Chloroprene polymer latex and dip-molded article

CN118946625APending Publication Date: 2024-11-12DENKA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030233.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing chloroprene-based polymer latex is difficult to achieve the same high softness and feel as natural rubber and polyisoprene impregnated molded products, especially in medical glove applications.

Method used

By adjusting the weight average molecular weight and monomer unit ratio in the chloroprene polymer latex, combining the calcium solidification liquid and thermal drying treatment, an impregnated molded film with an apparent hardness of 25.0 IRHD or above and 40.0 IRHD or below was prepared. Ensure it has sufficient tensile strength for breakage and excellent feel.

Benefits of technology

It has achieved the flexibility and feel of chloroprene-based polymer latex impregnated molded products, with a similar feel to natural rubber and polyisoprene, and has sufficient tensile strength to break, suitable for medical and industrial gloves, etc. application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005058921240000011
    Figure BDA0005058921240000011
  • Figure BDA0005058921240000251
    Figure BDA0005058921240000251
  • Figure BDA0005058921240000291
    Figure BDA0005058921240000291
Patent Text Reader

Abstract

The purpose of the present invention is to provide a chloroprene polymer latex with which a dip-molded article of a chloroprene polymer having sufficient tensile strength at break and excellent texture can be obtained. According to the present invention, provided is a chloroprene polymer latex which contains a chloroprene polymer, and which has an apparent hardness of 25.0-40.0 IRHD (inclusive) and a thickness of 0.60 + / -0.10 mm of a dip-molded film containing the chloroprene polymer latex as measured at 23 DEG C using a Wallace micro-autodurometer. The dip-molded article film having a thickness of 0.60 + / -0.10 mm is obtained by overlapping a plurality of dip-molded article films having a thickness of 0.15-0.25 mm; the immersion-molded film having a thickness of 0.15-0.25 mm is obtained by immersing a ceramic mold, to which a calcium-based solidification liquid adheres, in a chloroprene polymer latex composition containing the chloroprene polymer latex by an immersion solidification method and molding the ceramic mold, and thermally drying the molded immersion-molded film at 150 DEG C for 60 minutes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a chloroprene polymer latex and a dip-molded article, and more particularly to a chloroprene polymer latex containing a chloroprene polymer and a dip-molded article obtained using the chloroprene polymer latex composition. Background Art

[0002] Chloroprene-based polymers are known as materials for dip-molded products such as medical surgical gloves, medical examination gloves, industrial gloves, balloons, catheters, rubber boots, and the like.

[0003] Various technologies have been proposed for chloroprene polymer latex for dip-molded products with improved flexibility of chloroprene polymers and dip-molded products of chloroprene polymers. Patent Document 1 describes a polychloroprene latex for use in dip-molded products, which contains 100 parts by mass of modified polychloroprene obtained by copolymerizing chloroprene and methacrylic acid, 90 to 150 parts by mass of water, 1 to 5 parts by mass of an emulsifier, and 0.5 to 2.5 parts by mass of potassium ions, and has a pH of 7 to 14. Patent Document 2 describes a mercaptan-modified polychloroprene latex for use in dip-molded products, wherein chloroprene and 2,3-dichloro-1,3-butadiene are copolymerized, and in the 13C-solid NMR spectrum of the polychloroprene, the peak area (A) of 126.2 to 127.6 ppm, the peak area (B) of 122.0 to 126.2 ppm, and the peak area (C) of 129.9 to 130.3 ppm are in the ranges shown by the following general formula (I). Patent Document 3 describes a chloroprene polymer latex for use in dip-molded products, which contains a high molecular weight polymer and a low molecular weight polymer, and can achieve both excellent softness and mechanical properties in a vulcanized rubber prepared by dip molding. Patent Document 4 describes a chloroprene polymer latex obtained by copolymerizing a chloroprene monomer with an isoprene monomer which is a raw material of isoprene rubber. The latex has excellent flexibility and exhibits mechanical properties even under mild vulcanization conditions.

[0004] [Number 1]

[0005]

[0006] [Prior art documents]

[0007] [Patent Document]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 2014-114342

[0009] [Patent Document 2] International Publication No. 2019 / 009038

[0010] [Patent Document 3] Japanese Patent Application Publication No. 2019-143002

[0011] [Patent Document 4] International Publication No. 2021-132460 Summary of the invention

[0012] Problem that the invention aims to solve

[0013] Chloroprene-based polymer latex has been used as a rubber latex raw material for coating films of dip-molded articles such as gloves, balloons, boots, and catheters. In particular, in medical rubber gloves, there is a tendency to seek high softness similar to that of dip-molded articles obtained using natural rubber or polyisoprene, and there is a desire to develop a chloroprene-based polymer latex that can provide a dip-molded article with excellent hand feel when formed into a dip-molded article film.

[0014] Therefore, a main object of the present invention is to provide a chloroprene polymer latex which can provide a chloroprene polymer dip-molded product having sufficient tensile strength at break and excellent hand feel.

[0015] Solutions for solving problems

[0016] According to the present invention, there is provided a chloroprene polymer latex, which contains a chloroprene polymer, wherein the apparent hardness of a dip-molded film containing the chloroprene polymer latex and having a thickness of 0.60±0.10 mm measured at 23° C. using a Wallace micro-automatic hardness tester is 25.0 IRHD or more and 40.0 IRHD or less,

[0017] The aforementioned 0.60±0.10 mm thick dip-molded film is formed by overlapping a plurality of 0.15 to 0.25 mm thick dip-molded films.

[0018] The dip-molded film having a thickness of 0.15 to 0.25 mm is obtained by dipping a ceramic mold to which a calcium-based coagulation liquid is attached into a chloroprene polymer latex composition containing the chloroprene polymer latex by an immersion coagulation method, and heat-drying the obtained dip-molded film at 150° C. for 60 minutes.

[0019] Various embodiments of the present invention are described below. The embodiments described below can be combined with each other.

[0020] Preferably, in the above-mentioned chloroprene polymer latex, when the chloroprene polymer latex is freeze-dried, dissolved in tetrahydrofuran, and the soluble component is measured by gel permeation chromatography, at least a peak with a weight average molecular weight of 3,000 to 80,000 is detected.

[0021] Preferably, the above-described chloroprene polymer latex contains 2,3-dichloro-1,3-butadiene monomer units.

[0022] Preferably, the chloroprene polymer latex described above contains 1 to 25% by mass of 2,3-dichloro-1,3-butadiene monomer units based on 100% by mass of the total of the chloroprene monomer units and the 2,3-dichloro-1,3-butadiene monomer units.

[0023] Preferably, in the above-described chloroprene polymer latex, the toluene-insoluble content in the solid content obtained by freeze-drying the chloroprene polymer latex is 45 to 85% by mass.

[0024] According to another aspect of the present invention, there is provided a dip-molded product using the above-described chloroprene polymer latex.

[0025] Preferably, the above-mentioned dip-molded product contains a metal oxide and an antioxidant.

[0026] Preferably, the aforementioned dip-molded article is industrial / general household gloves, medical gloves, balloons, catheters or boots.

[0027] Furthermore, in the present invention, "JIS" means Japanese Industrial Standards.

[0028] Effects of the Invention

[0029] According to the present invention, there is provided a chloroprene polymer latex which can provide a dip-molded product of the chloroprene polymer having sufficient tensile strength at break and being soft and having excellent hand feel. DETAILED DESCRIPTION

[0030] Hereinafter, the mode for implementing the present invention will be described in detail. In addition, the present invention is not limited to the embodiment described below.

[0031] 1. Chloroprene polymer latex

[0032] First, the chloroprene polymer latex according to one embodiment of the present invention will be described.

[0033] 1.1 Chloroprene polymers

[0034] The chloroprene polymer described in this embodiment is a polymer containing monomer units from 2-chloro-1,3-butadiene (hereinafter, also referred to as chloroprene). In addition, the chloroprene polymer of one embodiment of the present invention may also be a copolymer of chloroprene and other monomers copolymerizable with chloroprene, and as other monomers, 1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, isoprene, styrene, methacrylic acid, acrylonitrile, sulfur, etc. can be listed, and other monomers may also be used in combination with two or more of them. The chloroprene polymer of one embodiment of the present invention preferably contains monomer units from 2,3-dichloro-1,3-butadiene. The chloroprene polymer of one embodiment of the present invention may not contain sulfur, and the chloroprene polymer of one embodiment of the present invention may also be a polymer that does not have a -SS- structure derived from sulfur in the main chain.

[0035] The chloroprene polymer of one embodiment of the present invention can be obtained by mixing two or more different chloroprene polymers. The chloroprene polymer includes at least one selected from the group consisting of a homopolymer of chloroprene (2-chloro-1,3-butadiene), a copolymer of chloroprene and 1-chloro-1,3-butadiene, a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene, and a copolymer of chloroprene and 1-chloro-1,3-butadiene and 2,3-dichloro-1,3-butadiene, and more preferably includes at least one of a homopolymer of chloroprene and a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene.

[0036] The chloroprene polymer of one embodiment of the present invention may contain 50 to 100% by mass of monomer units derived from chloroprene, preferably 70 to 100% by mass, based on 100% by mass of the chloroprene polymer contained in the chloroprene polymer latex composition. The content of the monomer units derived from chloroprene may be, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100% by mass, and may be within a range between any two of the values ​​exemplified herein.

[0037] The chloroprene polymer of one embodiment of the present invention may contain 1 to 25% by mass of monomer units derived from 2,3-dichloro-1,3-butadiene, when the total of the chloroprene monomer units and the 2,3-dichloro-1,3-butadiene monomer units in the chloroprene polymer contained in the chloroprene polymer latex composition is 100% by mass. The content of the monomer units derived from 2,3-dichloro-1,3-butadiene is, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, or 25% by mass, and may be within the range between any two of the values ​​exemplified here.

[0038] The chloroprene-based polymer according to one embodiment of the present invention may contain a monomer unit derived from chloroprene and a monomer unit derived from 2,3-dichloro-1,3-butadiene, or may be composed of a monomer unit derived from chloroprene and a monomer unit derived from 2,3-dichloro-1,3-butadiene.

[0039] When the chloroprene polymer is a mixture of two or more different chloroprene polymers, the content of each monomer unit refers to the total of each monomer unit in all chloroprene polymers contained in the chloroprene polymer latex.

[0040] 1.2 Chloroprene polymer latex

[0041] The chloroprene polymer latex according to one embodiment of the present invention may be a latex in which a chloroprene polymer is dispersed in water, or a latex in which at least one selected from the group consisting of a homopolymer of chloroprene, a copolymer of chloroprene and 1-chloro-1,3-butadiene, a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene, and a copolymer of chloroprene and 1-chloro-1,3-butadiene and 2,3-dichloro-1,3-butadiene is dispersed in water, or a latex in which a homopolymer of chloroprene or a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene is dispersed in water.

[0042] 1.2.1 Apparent hardness of dip-molded films containing chloroprene polymer latex

[0043] The chloroprene polymer latex of the present invention has an apparent hardness of 25 IRHD or more and 40 IRHD or less of a dip-molded film containing the chloroprene polymer latex and having a thickness of 0.60±0.10 mm measured at 23° C. using a Wallace micro-automatic hardness tester. The apparent hardness of the dip-molded film containing the chloroprene polymer latex is, for example, 25.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, or 40.0 IRHD, and may be within a range between any two of the values ​​exemplified herein.

[0044] Here, the dip-molded film with a thickness of 0.60±0.10 mm is formed by overlapping a plurality of dip-molded films with a thickness of 0.15 to 0.25 mm, and the dip-molded film with a thickness of 0.15 to 0.25 mm can be molded by an immersion coagulation method, which is formed by immersing a ceramic mold with a calcium-based coagulation liquid in a chloroprene polymer latex composition containing a chloroprene polymer latex, and heat drying the molded dip-molded film at 150° C. for 60 minutes. In addition, the sample of the above shape is used in this measurement, and the international rubber hardness IRHD measured according to JIS K 6253-2 for other conditions is defined as the apparent hardness. In addition, the hardness measured by the above method according to JIS K 6253-1 is referred to as "apparent hardness".

[0045] The method for producing the dip-molded article and the method for measuring the "apparent hardness" (International Rubber Hardness IRHD) can be specifically described in the Examples.

[0046] The apparent hardness of the dip-molded film containing chloroprene polymer latex can be controlled by adjusting the type and amount of raw materials formulated during the production of the chloroprene polymer latex, as well as the polymerization conditions, and by adjusting the type (weight average molecular weight and the type and content of the monomer units contained, etc.) and amount of the chloroprene polymer contained in the chloroprene polymer latex.

[0047] 1.2.2 Weight average molecular weight of chloroprene polymer latex

[0048] The chloroprene polymer latex according to one embodiment of the present invention is preferably freeze-dried, dissolved in tetrahydrofuran, and subjected to gel permeation chromatography to detect a peak with a weight average molecular weight of 3,000 to 80,000, and more preferably a peak with a weight average molecular weight of 5,000 to 50,000. That is, the chloroprene polymer latex according to one embodiment of the present invention preferably contains a low molecular weight chloroprene polymer with a weight average molecular weight of 3,000 to 80,000, and more preferably contains a low molecular weight chloroprene polymer with a weight average molecular weight of 5,000 to 50,000.

[0049] When the weight average molecular weight of the low molecular weight chloroprene polymer is greater than the above lower limit, a dip molded product having a better tensile strength at break can be obtained. From the viewpoint of easily obtaining a better dip molded product, the weight average molecular weight of the low molecular weight chloroprene polymer may be greater than 10,000 or greater than 15,000.

[0050] When the weight average molecular weight of the low molecular weight chloroprene polymer is below the upper limit, a dip molded product with lower apparent hardness can be obtained. From the viewpoint of easily obtaining better flexibility, the weight average molecular weight of the low molecular weight chloroprene polymer may be 80,000 or less, 70,000 or less, 50,000 or less, or 30,000 or less.

[0051] The peak detected in the weight average molecular weight range of 3,000 to 80,000 is, for example, 3,000, 4,000, 5,000, 6,000, 7,000, 8,000, 9,000, 10,000, 11,000, 12,000, 13,000, 14,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, 21,000, 22,000, 23,000, 24,000, 25,000, 26,000, 27,000, 28,000, 29,000, 30,000, 31,000, 32,000, 33,000, 34,000, 35,000, 36,000, 37,000, 38,000, 39,000, 40,000, 41,000, 42,000, 43,000, 44,000 The amount may be in the range of 20,000, 30,000, 35,000, 40,000, 50,000, 60,000, 70,000, or 80,000, or may be in the range of 20,000, 30,000, 35,000, 40,000, 50,000, 60,000, 70,000, or 80,000, or may be in the range of 20,000, 30,000, 35,000, 40,000, 50,000, 60,000, 70,000, or 80,000, or may be in the range of 20,000, 30,000, 35,000, 40,000, 50

[0052] Since the chloroprene polymer latex according to one embodiment of the present invention has the above-mentioned molecular weight distribution, the apparent hardness of the dip-molded film can be appropriately adjusted.

[0053] The chloroprene polymer latex according to one embodiment of the present invention preferably contains a high molecular weight chloroprene polymer having a weight average molecular weight of 500,000 to 1,500,000 when the chloroprene polymer latex is freeze-dried, dissolved in tetrahydrofuran, and the soluble component is measured by gel permeation chromatography. That is, the chloroprene polymer latex according to one embodiment of the present invention preferably contains a high molecular weight chloroprene polymer having a weight average molecular weight of 500,000 to 1,500,000. The weight average molecular weight of the peak detected in the weight average molecular weight range of 500,000 to 1,500,000 is, for example, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,200,000, 1,300,000, 1,400,000, or 1,500,000, or may be within the range between any two of the values ​​exemplified here.

[0054] The weight average molecular weight of the chloroprene polymer can be controlled by adjusting the formulation such as the type and amount of the chain transfer agent in the polymerization of each chloroprene polymer, the polymerization temperature, the polymerization time, the polymerization conversion rate, etc. In addition, by adjusting the weight average molecular weight of the chloroprene polymer and the mixing ratio of chloroprene polymers having different weight average molecular weights, the apparent hardness of the dip-molded product containing the chloroprene polymer latex can be adjusted.

[0055] The molecular weight distribution of the sol component soluble in tetrahydrofuran in the chloroprene polymer latex can be obtained by measuring the weight average molecular weight using gel permeation chromatography. Specifically, the chloroprene polymer latex is freeze-dried, dissolved in tetrahydrofuran, and the eluted component (sol component) is analyzed using gel permeation chromatography (GPC). The measurement conditions of GPC can be described in the examples.

[0056] Furthermore, the molecular weight distribution of the tetrahydrofuran-soluble sol component in the chloroprene polymer latex contained in the chloroprene polymer latex composition can be obtained by freeze-drying the chloroprene polymer latex composition, dissolving the chloroprene polymer latex composition in tetrahydrofuran, and analyzing the composition in the same manner. Furthermore, the molecular weight distribution of the tetrahydrofuran-soluble sol component in the chloroprene polymer latex contained in the dip-molded article can be obtained by dissolving the dip-molded article in tetrahydrofuran and analyzing the composition in the same manner.

[0057] The chloroprene polymer latex of the present invention can be obtained by mixing two or more chloroprene polymer latexes having different weight average molecular weights, or can be obtained by mixing two or more chloroprene polymer latexes having different weight average molecular weights to obtain a chloroprene polymer latex in which a peak of a weight average molecular weight within the above range is detected in the molecular weight distribution. When two or more chloroprene polymer latexes are mixed, the weight average molecular weight of each chloroprene polymer latex can be controlled by adjusting the formulation such as the type and amount of the chain transfer agent in the polymerization of each chloroprene polymer latex, the polymerization temperature, the polymerization time, the polymerization conversion rate, etc. When two or more chloroprene polymer latexes are used, the chloroprene polymer latex can be obtained by stirring and mixing the two or more chloroprene polymer latexes at 100 rpm for 2 minutes using a paddle.

[0058] The chloroprene polymer latex according to one embodiment of the present invention preferably contains a chloroprene polymer having a weight average molecular weight of 3,000 to 80,000 and a peak having a weight average molecular weight of 500,000 to 1,500,000 in the molecular weight distribution obtained when the chloroprene polymer latex is freeze-dried, dissolved in tetrahydrofuran, and the soluble component is measured by gel permeation chromatography. That is, the chloroprene polymer latex according to one embodiment of the present invention preferably contains a chloroprene polymer having a weight average molecular weight of 3,000 to 80,000 and a chloroprene polymer having a weight average molecular weight of 500,000 to 1,500,000.

[0059] The chloroprene polymer latex according to one embodiment of the present invention preferably contains 5 to 40% by mass of a chloroprene polymer having a weight average molecular weight of 3,000 to 80,000, based on 100% by mass of the chloroprene polymer contained in the chloroprene polymer latex. The chloroprene polymer latex according to one embodiment of the present invention may contain, for example, 5, 10, 15, 20, 25, 30, 35, or 40% by mass of a chloroprene polymer having a weight average molecular weight of 5,000 to 50,000, based on 100% by mass of the chloroprene polymer contained in the chloroprene polymer latex, or may be within the range between any two of the values ​​exemplified herein.

[0060] The chloroprene polymer latex according to one embodiment of the present invention preferably contains 60 to 95% by mass of a chloroprene polymer having a weight average molecular weight of 500,000 to 1,500,000, based on 100% by mass of the chloroprene polymer contained in the chloroprene polymer latex. The chloroprene polymer latex according to one embodiment of the present invention may contain, for example, 60, 65, 70, 75, 80, 85, 90, or 95% by mass of a chloroprene polymer having a weight average molecular weight of 500,000 to 1,500,000, based on 100% by mass of the chloroprene polymer contained in the chloroprene polymer latex, or may be within the range between any two of the values ​​exemplified herein.

[0061] By adjusting the content of the chloroprene polymers having different weight average molecular weights within the above numerical range, the apparent hardness can be more appropriately adjusted.

[0062] 1.2.3 2,3-Dichloro-1,3-butadiene copolymer content of chloroprene polymer in chloroprene polymer latex

[0063] The copolymerization amount of 2,3-dichloro-1,3-butadiene in the chloroprene polymer contained in the chloroprene polymer latex of one embodiment of the present invention is preferably 1 to 25% by mass, and more preferably 5 to 25% by mass, when the total of the monomer units derived from chloroprene and the monomer units derived from 2,3-dichloro-1,3-butadiene contained in the chloroprene polymer is 100% by mass. The copolymerization amount of this component is, for example, 1, 2, 5, 8, 9, 10, 12, 15, 20, or 25% by mass, and may be within the range between any two of the values ​​exemplified herein.

[0064] The chloroprene polymer contained in the chloroprene polymer latex of one embodiment of the present invention can more appropriately adjust the apparent hardness of the dip-molded film obtained by using the chloroprene polymer latex by setting the 2,3-dichloro-1,3-butadiene copolymerization amount within the numerical range, and it is easy to obtain a dip-molded product with sufficient tensile strength at break and better hand feel. The 2,3-dichloro-1,3-butadiene copolymerization amount can be adjusted by preparing two or more chloroprene polymer latexes with different copolymerization amounts of the component and adjusting their mixing ratio. In addition, the 2,3-dichloro-1,3-butadiene copolymerization amount in each chloroprene polymer latex can be adjusted by controlling the type and amount of raw materials blended during the polymerization of each chloroprene polymer latex, as well as the polymerization conditions.

[0065] Regarding the "2,3-dichloro-1,3-butadiene copolymerization amount", the chloroprene polymer latex or the chloroprene polymer latex composition can be used as the analysis object, and the chloroprene polymer latex or the chloroprene polymer latex composition can be cut into a dried product obtained by freezing, and the 2,3-dichloro-1,3-butadiene copolymerization amount in the chloroprene polymer latex (contained in the chloroprene polymer latex composition) can be obtained using a pyrolysis gas chromatography-mass spectrometer. In addition, the analysis object can also be a dip-molded product.

[0066] 1.2.4 Toluene-insoluble fraction of chloroprene polymer latex

[0067] The toluene insoluble matter (gel component) of the chloroprene polymer latex of one embodiment of the present invention can be 45 to 85% by mass, more preferably 60 to 80% by mass, relative to the solid content obtained by freeze-drying the chloroprene polymer latex. The toluene insoluble matter is, for example, 45, 50, 55, 60, 65, 70, 75, 80, 85% by mass, and can also be in the range between any two values ​​​​exemplified herein. By making the toluene insoluble matter fall within the above-mentioned numerical range, a more excellent tensile strength at break will be exhibited. This numerical range can be adjusted by preparing two or more chloroprene polymer latexes with different toluene insoluble matters and adjusting their mixing ratio. In addition, the toluene insoluble matter in each chloroprene polymer latex can be adjusted by controlling the type, amount, and polymerization conditions of the raw materials when the chloroprene polymer latex is polymerized.

[0068] The "toluene insoluble content" can be obtained by cutting 1 g of chloroprene polymer rubber obtained by freeze-drying the chloroprene polymer latex into 2 mm squares, dissolving the mixture in toluene for 16 hours, separating the insoluble components using a 200-mesh metal net after centrifugation, and measuring the weight after drying. The toluene insoluble content can be calculated using the following calculation formula.

[0069] (Mass of the solid obtained by separating and drying the gel component) / (Mass of the solid obtained by freeze-drying the latex containing the chloroprene polymer)×100

[0070] Furthermore, by analyzing a dried product obtained by freezing the chloroprene polymer latex composition using the chloroprene polymer latex composition as the analysis object in the same manner, the toluene-insoluble content in the chloroprene polymer latex contained in the chloroprene polymer latex composition can be determined. Furthermore, by analyzing a dip-molded article using the same manner as the analysis object, the toluene-insoluble content in the chloroprene polymer latex contained in the dip-molded article can be determined.

[0071] 1.2.5 Tensile Strength at Break of Dip-Molded Films Containing Chloroprene-Based Polymer Latex

[0072] In the case of the chloroprene polymer latex of one embodiment of the present invention, the tensile strength at break of the dip-molded product film containing the chloroprene polymer latex can be 16.0 MPa or more, preferably 17.0 MPa or more. The tensile strength at break is, for example, 16.0, 17.0, 18.0, 19.0, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0 MPa, or can be in the range between any two of the values ​​exemplified herein. The chloroprene polymer latex of one embodiment of the present invention is easy to have sufficient tensile strength at break and excellent hand feel by adjusting the type (weight average molecular weight and type and content of monomer units contained, etc.) and amount of the chloroprene polymer contained in the chloroprene polymer latex so that the apparent hardness is within the above-mentioned numerical range.

[0073] 1.2.6 Method for producing chloroprene polymer latex

[0074] Next, the method for producing the chloroprene polymer latex of the present invention will be described.

[0075] The method for producing chloroprene polymer latex may include a polymerization step of polymerizing a monomer containing chloroprene to obtain chloroprene polymer latex. In addition, the method for producing chloroprene polymer latex may include a mixing step of mixing two or more chloroprene polymer latexes having different weight average molecular weights.

[0076] In the polymerization step, the monomer includes chloroprene and may include other monomers copolymerizable with chloroprene. Examples of other monomers copolymerizable with chloroprene include 1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, isoprene, styrene, methacrylic acid, acrylonitrile, sulfur, and the like. The monomer may also include chloroprene and 2,3-dichloro-1,3-butadiene.

[0077] It is preferred to adjust the type and amount of each monomer so that the content of each monomer unit in the obtained chloroprene polymer falls within the above numerical range. As an example, the copolymerization amount of 2,3-dichloro-1,3-butadiene in the chloroprene polymer contained in the chloroprene polymer latex may be in the range of 1 to 25 mass % relative to 100 mass % of the total of the chloroprene monomer and 2,3-dichloro-1,3-butadiene contained in the chloroprene polymer. In this case, the amount of 2,3-dichloro-1,3-butadiene added before the start of emulsion polymerization is preferably in the range of 1 to 25 mass parts relative to 100 mass parts of the total of the chloroprene monomer and the 2,3-dichloro-1,3-butadiene monomer. From the viewpoint of controlling polymerization, the amount of 2,3-dichloro-1,3-butadiene added is more preferably 5 to 25 mass parts relative to 100 mass parts of the total of the chloroprene monomer and the 2,3-dichloro-1,3-butadiene monomer.

[0078] When producing chloroprene-based polymers, the raw monomers are polymerized by polymerization methods such as emulsion polymerization, solution polymerization, suspension polymerization, and bulk polymerization. Among these polymerization methods, emulsion polymerization is preferred because it has various advantages such as easy control, easy extraction of the polymer from the polymerization termination solution, and relatively high polymerization speed.

[0079] Emulsion polymerization is a type of free radical polymerization, in which raw monomers are put into a reaction tank together with a chain transfer agent, water, an alkali (for example, metal hydroxides such as potassium hydroxide and sodium hydroxide), an emulsifier (dispersant), a reducing agent (for example, sodium bisulfite), a polymerization initiator, etc., and polymerization is carried out.

[0080] The type of chain transfer agent used in emulsion polymerization is not particularly limited, and for example, long-chain alkyl mercaptans such as n-dodecyl mercaptan and tert-dodecyl mercaptan, dialkyl xanthogen disulfides such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide, and known chain transfer agents commonly used in emulsion polymerization of chloroprene such as iodoform can be used. The chain transfer agent is preferably a long-chain alkyl mercaptan, and more preferably n-dodecyl mercaptan.

[0081] By adjusting the type and amount of the chain transfer agent, the weight average molecular weight of the obtained chloroprene polymer latex can be adjusted.

[0082] For example, in order to obtain a latex containing a chloroprene polymer having a weight average molecular weight of 500,000 or more, that is, in order to obtain a chloroprene polymer latex in which a peak having a weight average molecular weight of 500,000 or more is detected in the molecular weight distribution, the amount of the chain transfer agent added before the start of emulsion polymerization is preferably 0.01 parts by mass or more relative to 100 parts by mass of the monomer (for example, 100 parts by mass of the total of chloroprene and 2,3-dichloro-1,3-butadiene). From the viewpoint of obtaining a chloroprene polymer latex in which a peak having a weight average molecular weight of 500,000 or more is detected, the amount of the chain transfer agent added is more preferably 0.02 to 0.05 parts by mass, for example, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09 parts by mass, or less than 0.10 parts by mass, and may also be within the range between any two of the numerical values ​​exemplified here. When the amount of the chain transfer agent, especially the long-chain alkyl mercaptan, added is 0.01 parts by mass or more, the storage stability of the latex is further improved, and when the amount added is less than 0.10 parts by mass, especially less than 0.05 parts by mass, the toluene insoluble matter increases, and the tensile strength at break of the dip-molded product containing the obtained chloroprene polymer latex is higher.

[0083] In order to obtain a chloroprene polymer latex having a weight average molecular weight of 3,000 to 80,000, that is, to obtain a chloroprene polymer latex having a peak of a weight average molecular weight of 3,000 to 80,000 detected in the molecular weight distribution, the amount of the chain transfer agent added before the start of the emulsion polymerization is preferably 0.5 to 10.0 parts by mass relative to 100 parts by mass of the monomer. In this case, the amount added is, for example, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, and may be within the range between any two of the numerical values ​​exemplified here.

[0084] Emulsifiers include anionic emulsifiers, nonionic emulsifiers, and the like. Examples of anionic emulsifiers include fatty acid salts such as potassium tallow fatty acid, partially hydrogenated potassium tallow fatty acid, potassium oleate, and sodium oleate; resin acid salts such as potassium rosinate, sodium rosinate, hydrogenated potassium rosinate, and hydrogenated sodium rosinate; alkylbenzene sulfonates such as sodium dodecylbenzene sulfonate; sodium salt of β-naphthalenesulfonic acid formalin condensate, and the like. Examples of nonionic emulsifiers include polyethylene glycol ester emulsifiers and polyvinyl alcohol. Among them, anionic emulsifiers are preferred, resin acid salts are preferred, rosin acids such as rosin acid and rosin acid salts are preferred, and at least one selected from the group consisting of potassium rosinate and sodium rosinate is more preferred. These emulsifiers may be used alone or in combination of two or more. The amount of the emulsifier used is preferably 1.0 to 6.5 parts by mass relative to 100 parts by mass of the monomer.

[0085] The emulsifier used in the emulsion polymerization preferably contains an anionic emulsifier, and more preferably contains a resinate, particularly rosin acids. By using rosin acids, aggregation of the rubber solid component and pH fluctuation can be prevented when blending with the base chloroprene polymer latex. Rosin acids include disproportionated rosin acid, conjugated resin acid, alkali metal salts of disproportionated rosin acid, alkali metal salts of conjugated resin acid, and the like.

[0086] In addition, in the method for producing the chloroprene polymer latex according to one embodiment of the present invention, in addition to the rosin acids, other commonly used emulsifiers and fatty acids may also be used in combination. As other emulsifiers, for example, an anionic emulsifier is preferably contained, and in addition to the above-mentioned anionic emulsifiers, metal salts of aromatic sulfinic acid formalin condensates, sodium dodecylbenzene sulfonate, potassium dodecylbenzene sulfonate, sodium alkyl diphenyl ether sulfonate, potassium alkyl diphenyl ether sulfonate, sodium polyoxyethylene alkyl ether sulfonate, sodium polyoxypropylene alkyl ether sulfonate, potassium polyoxyethylene alkyl ether sulfonate, potassium polyoxypropylene alkyl ether ether sulfonate, etc. may be cited.

[0087] The content of the anionic emulsifier other than rosin acid is preferably 0.2 to 1.0 mass % relative to 100 mass % of the chloroprene polymer contained in the chloroprene polymer latex. Therefore, the amount of the anionic emulsifier other than rosin acid added before the start of emulsion polymerization is preferably in the range of 0.2 to 0.9 mass parts relative to 100 mass parts of the monomers (for example, the total of chloroprene and 2,3-dichloro-1,3-butadiene).

[0088] The pH of the aqueous emulsion at the start of emulsion polymerization is preferably 10.5 to 13.5. The aqueous emulsion refers to a mixed solution of a chain transfer agent and monomers (chloroprene, 2,3-dichloro-1,3-butadiene, etc.) immediately before the start of emulsion polymerization, and also includes the case where the composition is changed by adding each component later or adding it in batches. If the pH of the aqueous emulsion at the start of emulsion polymerization is 10.5 or more, the polymerization reaction can be controlled more stably. If the pH is below 13.5, the excessive increase in viscosity during polymerization can be suppressed, and the polymerization reaction can be controlled more stably.

[0089] The polymerization temperature of the emulsion polymerization is preferably in the range of 5 to 55° C. It is more preferred that the temperature is 5° C. or higher because the emulsion does not freeze, and that the temperature is 55° C. or lower because the chloroprene monomer does not evaporate or boil.

[0090] As the polymerization initiator, potassium persulfate, benzoyl peroxide, ammonium persulfate, hydrogen peroxide, etc., which are generally used in radical polymerization, can be used.

[0091] The polymerization conversion rate is preferably in the range of 50 to 95%. The polymerization reaction is terminated by adding a polymerization terminator. When the polymerization conversion rate is 50% or more, the toluene insoluble matter tends to increase, and the strength of the obtained dip-molded film tends to increase. In addition, it is also advantageous in terms of production cost. When the polymerization conversion rate is lower than 95%, the reduction in polymerization reactivity due to the reduction in unreacted monomers can be avoided, and the reduction in productivity can be avoided.

[0092] Examples of the polymerization terminator include diethylhydroxylamine, thiodiphenylamine, 4-tert-butylcatechol, 2,2'-methylenebis-4-methyl-6-tert-butylphenol, etc. After the emulsion polymerization, unreacted monomers can be removed by a conventional method such as reduced pressure distillation.

[0093] Furthermore, to the chloroprene polymer latex obtained by the production method of one embodiment of the present invention, a freeze stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, a preservative, etc. may be optionally added after polymerization within a range that does not impair the effects of the present invention.

[0094] The method for producing a chloroprene polymer latex according to an embodiment of the present invention may further include a mixing step of mixing two or more chloroprene polymer latexes having different weight average molecular weights after the polymerization step. In the mixing step, the two or more chloroprene polymer latexes may be mixed by a known method. In the mixing step, for example, the chloroprene polymer latex may be obtained by stirring and mixing at 30 to 300 rpm using a paddle for 20 seconds to 3 minutes, for example, at 100 rpm for 2 minutes.

[0095] 2. Chloroprene polymer latex composition

[0096] The chloroprene polymer latex composition of one embodiment of the present invention includes a chloroprene polymer latex containing the chloroprene polymer of the present invention. The chloroprene polymer latex composition of one embodiment of the present invention may contain a metal oxide, an antioxidant, and other necessary agents in addition to the chloroprene polymer latex. The types and amounts of the metal oxide, antioxidant, and other necessary agents that the chloroprene polymer latex composition may contain will be described later as components that may be contained in the dip molded article.

[0097] 3. Method for producing chloroprene polymer latex composition

[0098] The method for producing the chloroprene polymer latex composition may include a raw material mixing step of mixing raw materials containing the chloroprene polymer latex, a metal oxide, an antioxidant, and other necessary reagents.

[0099] In the mixing step, an aqueous dispersion containing a metal oxide, an antioxidant, and other necessary reagents may be prepared in advance, and then the chloroprene polymer latex and the aqueous dispersion may be mixed.

[0100] The mixing step can be performed using a known mixing device such as a ball mill.

[0101] 4. Dip-molded articles (dip-molded articles coated with films)

[0102] The dip-molded article of one embodiment of the present invention is obtained by using the above-mentioned chloroprene polymer latex composition containing chloroprene polymer latex. The dip-molded article of this embodiment can be obtained by dip-molding the above-mentioned chloroprene polymer latex composition alone or after blending with other chloroprene polymer latex compositions. The dip-molded article of the present invention can be a dip-molded article obtained by heat drying the dip-molded article obtained by dip-molding the chloroprene polymer latex composition containing chloroprene polymer latex by dip coagulation method at 150°C for 60 minutes. The dip-molded article of the present invention has sufficient tensile strength at break and excellent hand feel. The dip-molded article can be suitably used as industrial / general household gloves, medical gloves, balloons, catheters and boots.

[0103] The dip molded article of the present invention may have the components contained in the above-mentioned chloroprene polymer latex. In addition, the dip molded article may contain a chloroprene polymer as a base polymer, and when the dip molded article is set to 100 mass%, it may contain 70 mass% or more of the chloroprene polymer, preferably 80 mass% or more, and more preferably 90 mass% or more. When the dip molded article is set to 100 mass%, the content of the chloroprene polymer in the dip molded article is, for example, 70, 75, 80, 85, 90, 95, 96, 97, 98, 99, 100 mass%, and may also be within the range between any two of the values ​​exemplified here.

[0104] The dip molded article of the present invention may contain metal oxides and antioxidants. The dip molded article of the present invention has sufficient tensile strength at break and excellent hand feel regardless of whether a vulcanizing agent and a vulcanization accelerator are added. In addition, the chloroprene polymer latex composition of one embodiment of the present invention may not contain a vulcanizing agent and a vulcanization accelerator, and may not contain sulfur and vulcanization accelerators such as thiuram, dithiocarbamate, thiourea, guanidine, xanthate, and thiazole. The components that the dip molded article of the present invention may contain are described in detail below.

[0105] 4.1 Metal oxides

[0106] The dip-molded product of the chloroprene polymer of the present invention may contain a metal oxide.

[0107] The metal oxide contained in the chloroprene polymer latex composition for obtaining the dip-molded product is not particularly limited, and examples thereof include zinc oxide, lead oxide, lead tetraoxide, magnesium oxide, aluminum oxide, iron oxide, beryllium oxide, titanium oxide, etc. The metal oxide preferably contains zinc oxide. Zinc oxide is generally considered to function as a supplement for the dechlorination atoms of the chloroprene polymer. In addition, these metal oxides may be used alone or in combination of two or more.

[0108] The amount of the metal oxide added is preferably 0.5 to 15.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer latex contained in the chloroprene polymer latex composition used to obtain the dip-molded product. If the amount of the metal oxide added is 0.5 parts by mass or more, an improvement in the tensile strength at break can be expected due to the cross-linking effect between the polymers. If the amount of the metal oxide added is 15.0 parts by mass or less, a dip-molded product with excellent softness can be obtained. In addition, from the viewpoint of the physical balance between the softness and tensile strength at break of the obtained dip-molded product, the amount of the metal oxide added is more preferably 0.5 to 5.0 parts by mass. In addition, the dip-molded product of the present invention may not contain a metal oxide.

[0109] 4.2 Antioxidants

[0110] The dip-molded product of the chloroprene polymer of the present invention may contain an antioxidant.

[0111] The antioxidant is not particularly limited, and phenolic antioxidants, amine antioxidants, heat-resistant antioxidants (aging) agents, ozone-resistant antioxidants, etc. can be used. When the obtained dip-molded product is used for medical gloves, a phenolic antioxidant can be used from the viewpoints of color tone, texture, and hygiene of the dip-molded product. In particular, the above-mentioned effect of hindered phenolic antioxidants is stronger. Examples of hindered phenolic antioxidants include 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 4,4'-butylene(3-methyl-6-tert-butylphenol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), a butylation product of p-cresol and dicyclopentadiene, 2,5'-di-tert-butylhydroquinone, and 2,5'-di-tert-amylhydroquinone. Among them, generally, from the viewpoint of being dispersible in water-based materials, a butylation reaction product of p-cresol and dicyclopentadiene is preferred. In addition, these compounds may be used alone or in combination of two or more.

[0112] The amount of the antioxidant added is preferably 0.5 to 10.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer latex contained in the chloroprene polymer latex composition used to obtain the dip molded product. The amount of the antioxidant added is, for example, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0 parts by mass, and may also be within the range between any two of the values ​​exemplified herein. If the amount of the antioxidant added is 0.5 parts by mass or more, the effect of suppressing the change in color tone of the dip molded product can be obtained. If the amount of the antioxidant added is 10.0 parts by mass or less, the stability of the chloroprene polymer latex composition can be ensured. In addition, from the viewpoint of the physical balance between the softness and the breaking strength of the obtained dip molded product, the amount of the antioxidant added is more preferably 0.5 to 5.0 parts by mass. In addition, the dip molded product of the present invention may also not contain an antioxidant.

[0113] 4.3 Vulcanizing agents and vulcanization accelerators

[0114] The dip-molded article of the chloroprene polymer of one embodiment of the present invention may also contain a vulcanizing agent and / or a vulcanization accelerator. In addition, the chloroprene polymer latex composition used to obtain the dip-molded article may also be free of sulfur and the above-mentioned thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthate-based, thiazole-based and other vulcanization accelerators. That is, the dip-molded article of the chloroprene polymer latex composition includes one containing a vulcanizing agent but not containing a vulcanization accelerator, one containing no vulcanizing agent but containing a vulcanization accelerator, one containing a vulcanizing agent and a vulcanization accelerator, and one containing no vulcanizing agent and a vulcanization accelerator. Whether to prepare a vulcanizing agent and a vulcanization accelerator can be determined according to the expected dip-molded article.

[0115] Examples of the vulcanizing agent include sulfur, but are not limited thereto. The amount of the vulcanizing agent added may be 0 to 10.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer latex contained in the chloroprene polymer latex composition. The amount of the vulcanizing agent added may be, for example, 0, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, or may be within the range between any two of the values ​​exemplified herein.

[0116] Vulcanization accelerator refers to a reagent added during the vulcanization of raw rubber to increase the vulcanization rate by reacting with the vulcanizing agent, shorten the vulcanization time, lower the vulcanization temperature, reduce the vulcanizing agent, and improve the physical properties of the vulcanized rubber. It usually refers to a reagent that promotes sulfur vulcanization reaction.

[0117] Commonly used vulcanization accelerators for vulcanization of chloroprene polymer latex include, but are not limited to, thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthate-based, thiazole-based, etc. These can be used alone or in combination of two or more as needed.

[0118] Examples of the thiuram-based vulcanization accelerator include tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide, and bis(pentamethylene)thiuram tetrasulfide.

[0119] Examples of the dithiocarbamate-based vulcanization accelerator include sodium dibutyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, copper dimethyldithiocarbamate, iron (III) dimethyldithiocarbamate, tellurium diethyldithiocarbamate, and the like. Zinc dibutyldithiocarbamate is particularly preferably used.

[0120] Examples of the thiourea-based vulcanization accelerator include ethylenethiourea, N,N′-diethylthiourea, trimethylthiourea, and N,N′-diphenylthiourea.

[0121] Examples of the guanidine-based vulcanization accelerator include 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, and di-o-tolylguanidine salt of dicatechol borate.

[0122] Examples of the xanthate-based vulcanization accelerator include butyl zinc xanthate and isopropyl zinc xanthate.

[0123] Examples of the thiazole vulcanization accelerator include 2-mercaptobenzothiazole, di-2-benzothiazole disulfide, 2-mercaptobenzothiazole zinc salt, cyclohexylamine salt of 2-mercaptobenzothiazole, and 2-(4′-morpholinodithio)benzothiazole.

[0124] The amount of the vulcanization accelerator added may be 0 to 5.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer latex contained in the chloroprene polymer latex composition. The amount of the vulcanization accelerator added may be, for example, 0, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, or may be within the range between any two of the values ​​exemplified herein.

[0125] 4.4 Shape of the Dip-molded Product

[0126] The thickness of the dip-molded article (e.g., minimum thickness) may be 0.01 to 0.50 mm. The thickness of the dip-molded article may be, for example, 0.01, 0.05, 0.10, 0.20, 0.30, 0.40, or 0.50 mm, or may be within the range between any two of the values ​​exemplified herein. The thickness of the dip-molded article may be adjusted by the time the molding die is immersed in the polymer latex composition, the solid content concentration of the chloroprene polymer latex composition, and the like. When the thickness of the dip-molded article is to be reduced, the immersion time may be shortened or the solid content concentration of the chloroprene polymer latex composition may be reduced.

[0127] 4.5 Apparent hardness of the impregnated product

[0128] The dip-molded article of one embodiment of the present invention has an apparent hardness of a dip-molded article film having a thickness of 0.60±0.10 mm, measured at 23°C using a Wallace micro-automatic hardness tester, preferably being greater than 25.0 IRHD and less than 40.0 IRHD. Here, the dip-molded article film having a thickness of 0.60±0.10 mm may be formed by overlapping multiple dip-molded articles having a thickness of 0.15 to 0.25 mm. The apparent hardness of the dip-molded article film is more preferably less than 37.0 IRHD. If the hardness value is less than 40.0 IRHD, the texture and feel of the dip-molded article film are excellent, and it has sufficient tensile strength at break. The apparent hardness of the dip molded article according to one embodiment of the present invention is, for example, 25.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, 40.0 IRHD, and may be within the range between any two of the values ​​exemplified herein. The apparent hardness of the dip molded article can be controlled by adjusting the type and amount of raw materials blended during the production of the chloroprene polymer latex, and the polymerization conditions, and by adjusting the type (weight average molecular weight and the type and content of the monomer units contained, etc.) and amount of the chloroprene polymer contained in the chloroprene polymer latex.

[0129] In addition, the sample of the above shape is used in the measurement, and the international rubber hardness IRHD measured according to JIS K 6253-2 is defined as the apparent hardness under other conditions. In addition, the hardness measured by the above method according to JIS K 6253-1 is called "apparent hardness". The manufacturing method of the dip molded product and the method for measuring the "apparent hardness" of the international rubber hardness IRHD can be described in the examples.

[0130] 4.6 Tensile strength at break of impregnated products

[0131] The tensile strength at break of the dip-molded article of one embodiment of the present invention may be 16.0 MPa or more, preferably 17.0 MPa or more. The tensile strength at break is, for example, 16.0, 17.0, 18.0, 19.0, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0 MPa, or may be within the range between any two values ​​exemplified herein. Here, the tensile strength at break of the dip-molded article is the tensile strength at break measured in accordance with JIS K 6251:2017.

[0132] As described above, the dip-molded article according to one embodiment of the present invention has an excellent texture and has sufficient tensile strength at break regardless of whether a vulcanizing agent, a vulcanization accelerator, or a cross-linking agent is added.

[0133] Latex containing conventional chloroprene rubber has been used as a rubber latex raw material for coating films of dip-molded articles such as gloves, balloons, boots, and catheters. On the other hand, in particular for medical rubber gloves, there is a tendency to seek for dip-molded articles made of chloroprene-based polymers with high flexibility similar to that of dip-molded articles obtained using natural rubber or polyisoprene, and an improved feel of the dip-molded article (film).

[0134] As described above, the dip-molded article according to one embodiment of the present invention has flexibility, has sufficient tensile strength at break even without containing sulfur, a vulcanization accelerator that is questionable in terms of sanitation, and has sufficiently excellent texture.

[0135] The dip-molded article obtained from the chloroprene polymer latex of the present embodiment may also contain sulfur or a vulcanization accelerator. However, even if the dip-molded article does not contain sulfur and a vulcanization accelerator, it has a hand feel equal to or better than that of a vulcanized dip-molded article obtained from a conventional chloroprene polymer latex. Therefore, the chloroprene polymer latex of the present embodiment is suitable for use as a raw material for a dip-molded article (dip-molded article coating).

[0136] 5. Method for manufacturing dip-molded articles

[0137] The method for producing the dip-molded article containing a chloroprene-based polymer of the present invention may include:

[0138] a molding step of molding the chloroprene polymer latex composition containing the chloroprene polymer by an immersion coagulation method using a calcium-based coagulation liquid to obtain an immersion molded body; and

[0139] In the drying step, the obtained impregnated body is subjected to a heat drying treatment to obtain an impregnated product.

[0140] The molding method when manufacturing the impregnation molded body of one embodiment of the present invention is not particularly limited, and molding can be performed according to a common method. As molding methods, for example, an impregnation coagulation method, a simple impregnation method, a thermosensitive impregnation method, an electrodeposition method, etc. can be cited. From the viewpoint of easy manufacture and easy acquisition of an impregnation molded body of a certain thickness, an impregnation coagulation method can be used. Specifically, a ceramic molding mold coated with a calcium-based coagulation liquid is immersed in a chloroprene polymer latex composition, and the chloroprene polymer latex composition is coagulated. Then, after removing water-soluble impurities by leaching, it is dried, and then a coating (rubber coating) of an impregnation molded body is formed by heating and vulcanization, and then the coating of the impregnation molded body is demoulded. Thus, a film-like impregnation molded body can be obtained.

[0141] In addition, the method for manufacturing an impregnated molded product of one embodiment of the present invention may include a step of subjecting the obtained impregnated molded product to a heat drying treatment and vulcanizing the unvulcanized impregnated molded product. The heat drying temperature may be appropriately set according to the composition of the chloroprene polymer latex composition, and may be 100 to 220° C. or 120 to 150° C. The heat drying temperature may be, for example, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, or 220° C., or may be within the range between any two of the values ​​exemplified herein. The heat drying time may be appropriately set according to the composition of the chloroprene polymer latex composition, the shape of the unvulcanized molded product, etc., and may be 10 to 300 minutes. The heat drying time is, for example, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300 minutes, and may be within the range between any two of the values ​​exemplified herein. As an example, the dip molded article of one embodiment of the present invention may be obtained by heat drying at 150° C. for 60 minutes.

[0142] [Example]

[0143] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to these examples. In the following examples relating to the synthesis of chloroprene polymer latex, unless otherwise specified, "parts by mass" refers to the amount relative to 100 parts by mass of the total of chloroprene monomer and 2,3-dichloro-1,3-butadiene monomer before the start of emulsion polymerization. In addition, "% by mass" refers to the amount relative to 100% by mass of the chloroprene polymer contained in the chloroprene polymer latex.

[0144] [Synthesis example A1]

[0145] <Preparation of Chloroprene Polymer Latex>

[0146] In a polymerization tank having an internal volume of 40 liters, 91 parts by mass of chloroprene monomer, 9 parts by mass of 2,3-dichloro-1,3-butadiene monomer, 0.02 parts by mass of n-dodecyl mercaptan, 76.5 parts by mass of pure water, 18 parts by mass of gum rosin-based disproportionated rosin acid potassium (aqueous solution, solid content 25%) (manufactured by Arakawa Chemical Industries, Ltd., trade name: RONDIS K-25), 0.80 parts by mass of potassium hydroxide, and 0.50 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation) were added. The pH of the aqueous emulsion before the start of polymerization was 13.2. 0.1 parts by mass of potassium persulfate was added as a polymerization initiator, and polymerization was carried out at a polymerization temperature of 15° C. under a nitrogen gas stream. When the polymerization conversion rate reached 83%, 0.01 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, thereby obtaining a latex.

[0147] The latex was subjected to reduced pressure distillation to remove unreacted monomers and a portion of water, thereby obtaining a chloroprene polymer latex having a solid content of 60%.

[0148] [Synthesis Examples A2 to A5]

[0149] Chloroprene polymer latex samples of Synthesis Examples A2 to A5 were prepared by the same procedure as Synthesis Example A1 except that the addition amount of 2,3-dichloro-1,3-butadiene and n-dodecyl mercaptan as a chain transfer agent, the polymerization temperature, and the polymerization conversion rate were changed as shown in Table 1 below.

[0150] [Synthesis example B1]

[0151] <Preparation of Chloroprene Polymer Latex>

[0152] In a polymerization tank having an internal volume of 40 liters, 91 parts by mass of chloroprene monomer, 9 parts by mass of 2,3-dichloro-1,3-butadiene monomer, 3.0 parts by mass of n-dodecyl mercaptan, 76.5 parts by mass of pure water, 18 parts by mass of gum rosin-based disproportionated rosin acid potassium (aqueous solution, solid content 25%) (manufactured by Arakawa Chemical Industries, Ltd., trade name: RONDIS K-25), 0.80 parts by mass of potassium hydroxide, and 0.50 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation) were added. The pH of the aqueous emulsion before the start of polymerization was 13.1. 0.1 parts by mass of potassium persulfate was added as a polymerization initiator, and polymerization was carried out at a polymerization temperature of 30° C. under a nitrogen gas stream. When the polymerization conversion rate reached 83%, 0.01 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, thereby obtaining a latex.

[0153] The latex was subjected to reduced pressure distillation to remove unreacted monomers, thereby obtaining a chloroprene polymer latex having a solid content of 60%.

[0154] [Synthesis Examples B2 to B8]

[0155] Chloroprene polymer latex samples of Synthesis Examples B2 to B8 were prepared in the same manner as Synthesis Example B1 except that the addition amount of 2,3-dichloro-1,3-butadiene and n-dodecyl mercaptan as a chain transfer agent, the polymerization temperature, and the polymerization conversion rate were changed as shown in Table 1 below.

[0156] The latex was subjected to reduced pressure distillation to remove unreacted monomers, thereby obtaining a chloroprene polymer latex having a solid content of 60%.

[0157] The following analyses were performed using the obtained chloroprene polymer latex. The results are shown in Table 1.

[0158] <Measurement of Weight Average Molecular Weight of Each Chloroprene Polymer Latex>

[0159] The obtained chloroprene polymer latex was freeze-dried, dissolved in THF (tetrahydrofuran), and the weight average molecular weight of the eluted component (sol component) was measured by gel permeation chromatography (GPC). The detected peak can be obtained as a weight average molecular weight converted to polystyrene, and the measurement was performed under the conditions described below.

[0160] <Weight Average Molecular Weight Measurement by Gel Permeation Chromatography>

[0161] GPC measurement was performed under the following conditions. The weight average molecular weight was determined in terms of polystyrene.

[0162] · Gel permeation chromatography (GPC) measuring device: Gel permeation chromatograph (HLC-8320) manufactured by Tosoh Corporation

[0163] ·Chromatographic column: TSKgel ALPHA-M manufactured by Tosoh Corporation

[0164] ·Eluent: Tetrahydrofuran (manufactured by Kanto Chemical)

[0165] Eluent flow rate: 1.0ml / min

[0166] Column temperature: 40℃

[0167] ·Detection method: Differential refractive index (RI) meter

[0168] Calibration curve: Prepared using standard polystyrene

[0169] <Determination of Copolymerization Amount of 2,3-Dichloro-1,3-butadiene>

[0170] The rubber sample of the chloroprene polymer obtained by freeze-drying the obtained chloroprene polymer latex was cut into a test piece of 0.05 mg, and measured by a pyrolysis gas chromatography-mass spectrometer to obtain the area ratio of the peak derived from chloroprene to the peak derived from 2,3-dichloro-1,3-butadiene. The content (mass %) of the monomer unit of 2,3-dichloro-1,3-butadiene in the chloroprene polymer was obtained using a calibration curve of the area ratio of the peak derived from chloroprene to the peak derived from 2,3-dichloro-1,3-butadiene and the content of 2,3-dichloro-1,3-butadiene.

[0171] <Measurement by pyrolysis gas chromatography-mass spectrometry>

[0172] The measurement conditions of the pyrolysis gas chromatography-mass spectrometer are as follows.

[0173] Device name: HP5890-II

[0174] Chromatographic column: (Film thickness 1.0μm)

[0175] Column temperature: 50℃(5min)→10℃ / min→150℃→25℃ / min→300℃

[0176] Inlet temperature: 250℃

[0177] Detector temperature: 280°C

[0178] Detector: FID

[0179] <Determination of Toluene Insoluble Content of Chloroprene Polymer Latex>

[0180] 1 g of the solid component (chloroprene polymer rubber) obtained by freeze-drying the obtained chloroprene polymer latex was cut into 2 mm squares, placed in a conical beaker, and dissolved in toluene for 16 hours. After that, centrifugation was performed, and the gel component was separated using a 200-mesh metal mesh, and the weight after drying was measured. The toluene insoluble content was calculated by the following calculation formula.

[0181] (Mass of the solid obtained by separating and drying the gel component) / (Mass of the solid obtained by freeze-drying the chloroprene polymer latex)×100 [Table 1]

[0182]

[0183] [Example 1]

[0184] When the total amount of the chloroprene polymer latex of Synthesis Example A1 and the chloroprene polymer latex of Synthesis Example B1 was 100 parts by mass, 80 parts by mass of the sample of Synthesis Example A1 and 20 parts by mass of the sample of Synthesis Example B1 were stirred and mixed at 100 rpm for 2 minutes using a paddle to obtain the chloroprene polymer latex of Example 1.

[0185] <Measurement of Weight Average Molecular Weight of Chloroprene Polymer Latex>

[0186] The mixed chloroprene polymer latex was freeze-dried, dissolved in tetrahydrofuran, and the soluble component was measured by gel permeation chromatography (GPC), and a peak with a weight average molecular weight (Mw) of 22,715 was confirmed. The conditions for GPC measurement were the same as those for the weight average molecular weight measurement in the above-mentioned synthesis examples.

[0187] <Copolymerization Amount of 2,3-dichloro-1,3-butadiene in Chloroprene-Based Polymer Contained in Chloroprene-Based Polymer Latex>

[0188] The copolymerization amount of 2,3-dichloro-1,3-butadiene (content of 2,3-dichloro-1,3-butadiene monomer unit) of the chloroprene polymer rubber obtained by freeze-drying the mixed chloroprene polymer latex was measured and found to be 9.5% by mass. From this analysis value, it was confirmed that the copolymerization amount of 2,3-dichloro-1,3-butadiene in the chloroprene polymer in the mixed latex was roughly consistent with the copolymerization amount of 2,3-dichloro-1,3-butadiene in each latex (analysis value) and the calculated value calculated from the mixing ratio of each chloroprene polymer latex in the mixed latex, and was roughly correlated with the addition amount of 2,3-dichloro-1,3-butadiene in each latex and the calculated value calculated from the mixing ratio of each chloroprene polymer latex in the mixed latex. In addition, the conditions of this measurement are the same as those of the thermal decomposition gas chromatography measurement in the above-mentioned synthesis examples.

[0189] <Determination of Toluene Insoluble Content of Chloroprene Polymer Latex>

[0190] The toluene-insoluble content of the solid component (chloroprene polymer rubber) obtained by freeze-drying the mixed chloroprene polymer latex was measured to be 67% by mass. From this analysis value, it was confirmed that the toluene-insoluble content of the chloroprene polymer latex was roughly correlated with the toluene-insoluble content of each mixed chloroprene polymer latex and the calculated value calculated from the mixing ratio.

[0191] <Preparation of Dip-Molded Product (Dip-Molded Product Film Sample)>

[0192] (Preparation of Chloroprene Polymer Latex Composition)

[0193] A chloroprene polymer latex composition was prepared by mixing 100 parts by mass of the solid content of the chloroprene polymer latex with an aqueous dispersion, and adding water to adjust the total solid content concentration of the formulation to 30% by mass. The aqueous dispersion was prepared by mixing 2 parts by mass of type 2 zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 2 parts by mass of dibutyl dithiocarbamic acid (trade name "Nocceler BZ", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 1 part by mass of sulfur, 0.1 part by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), and 10.7 parts by mass of water at 20° C. for 16 hours using a ceramic ball mill. The obtained chloroprene polymer latex composition contained 2 parts by mass of type 2 zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 2 parts by mass of dibutyl dithiocarbamic acid (trade name "Nocceler BZ", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 1 part by mass of sulfur, 0.1 part by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), and water, based on 100 parts by mass of the solid content of the chloroprene polymer latex.

[0194] (Preparation of Dip-molded Film)

[0195] A ceramic cylinder (manufactured by Shinko Co., Ltd.) with an outer diameter of 50 mm and a length of 300 mm was immersed in a coagulation solution prepared by mixing 62 parts by mass of water, 35 parts by mass of calcium nitrate tetrahydrate, and 3 parts by mass of calcium carbonate for 1 second and then taken out. After drying for 3 minutes, it was immersed in a chloroprene polymer latex composition containing no sulfur and vulcanization accelerator prepared according to the above procedure for 2 minutes. Then, it was washed with running water at 45°C for 1 minute and dried at 150°C for 60 minutes to prepare an evaluation dip molded product (dip molded product coating).

[0196] <Evaluation of Dip Molded Product>

[0197] (film thickness)

[0198] The thickness (film thickness) of three locations in the center of the evaluation film was measured using a test piece thickness meter (manufactured by Kobun Keiki Co., Ltd., trade name: ASKER SDA-12), and the minimum thickness was determined as the thickness of the evaluation film.

[0199] (International Rubber Hardness IRHD Determination)

[0200] Three sheets of the chloroprene polymer impregnation molded product with a film thickness of 0.20 mm were overlapped to a thickness of 0.60 mm, and the IRHD hardness was measured using a Wallace micro-automatic hardness tester at 23°C, and the result was 31.6 IRHD. In addition, the number of films overlapped during the measurement can be changed according to the film thickness of the obtained impregnation molded product, and the total is 0.60±0.10 mm. In addition, the thickness of the impregnation molded product film can be adjusted to 0.15-0.25 mm. In addition, 3-4 impregnation molded product films with the above thickness can be overlapped to obtain an impregnation molded product film with a total thickness of 0.60±0.10 mm and used for measurement. The results are shown in Tables 2 and 3.

[0201] <Evaluation of the feel of dip-molded products>

[0202] The dip-molded article was touched by five subjects to evaluate the feel of the dip-molded article by touching the surface and stretching and bending the article. The evaluation was performed according to the following criteria, and the average value of the evaluation of each subject is shown as a rounded value.

[0203] (Hand feel evaluation criteria)

[0204] 3: Extremely soft, comfortable to touch, and has an excellent feel.

[0205] 2: Soft, no practical problems in touch, feels good.

[0206] 1: I can't feel the softness, it feels a bit hard and the feel is not good.

[0207] (Tensile strength at break)

[0208] The tensile strength at break was measured using the dip-molded film in accordance with JIS K 6251. The results are shown in Tables 2 and 3.

[0209] [Examples 2 to 12, Comparative Examples 1 to 5]

[0210] Dip-molded articles were prepared in the same manner as in Example 1 except that the formulation of the chloroprene polymer latex composition was changed to the conditions shown in Tables 2 and 3 below, and each dip-molded article film sample was produced and evaluated. In Examples 2, 3, 4, 5, 8, 9, 10, and Comparative Examples 2, 3, and 4, chloroprene polymer latexes having different detected weight average molecular weight peaks and / or 2,3-dichloro-1,3-butadiene copolymerization amounts were used. In Examples 6 and 7 and Comparative Examples 1 and 5, the mixing ratio of each chloroprene polymer latex was changed. In Example 11, zinc oxide and an antioxidant as a metal oxide were removed from the chloroprene polymer latex composition for obtaining a dip-molded article of the chloroprene polymer latex.

[0211] In Example 12, dibutyl dithiocarbamic acid as a vulcanization accelerator and sulfur as a vulcanizing agent were added to the chloroprene polymer latex composition for obtaining a dip-molded product of the chloroprene polymer latex.

[0212] [Table 2]

[0213]

[0214] [Table 3]

[0215]

[0216] As can be seen from Tables 1 to 3 above, the dip molded products (dip molded product films) obtained using the chloroprene polymer latex composition of the present invention in Examples 1 to 12 have low hardness values ​​of apparent hardness in the international rubber hardness, have excellent hand feel when made into dip molded products (dip molded product films), and have sufficient tensile strength at break.

[0217] In Comparative Example 1, the chloroprene polymer latex did not contain a chloroprene polymer with a low weight average molecular weight, and contained a large amount of toluene insoluble matter, namely, a very large amount of gel component, and had a high apparent hardness value. As a result, the texture of the obtained dip-molded product was deteriorated.

[0218] In Comparative Example 2, it is considered that since 2,3-dichloro-1,3-butadiene was not copolymerized in the chloroprene polymer latex, the influence of crystallinity was strong and the apparent hardness value was high. As a result, the texture of the obtained dip-molded product was poor.

[0219] In Comparative Example 3, the chloroprene polymer latex did not contain a chloroprene polymer having a low weight average molecular weight, and the apparent hardness was high. As a result, the texture was deteriorated.

[0220] In Comparative Example 4, it is considered that since the chloroprene polymer latex did not contain a chloroprene polymer with a low weight average molecular weight and 2,3-dichloro-1,3-butadiene was not copolymerized, the crystallinity had a strong influence and the apparent hardness value became high. As a result, the texture was deteriorated.

[0221] In Comparative Example 5, since only a low-molecular-weight chloroprene polymer existed in the chloroprene polymer latex, stickiness was severe during molding, and a dip-molded product could not be obtained.

[0222] As can be seen from Example 12, when a chloroprene polymer latex containing a dip-molded product having an apparent hardness of a film of a chloroprene polymer latex of a specific value or less is used, a dip-molded product having a sufficient tensile strength at break and excellent hand feel can be obtained even if a vulcanization accelerator or sulfur is contained. That is, the chloroprene polymer latex composition and the dip-molded product according to one embodiment of the present invention may contain sulfur or a vulcanization accelerator.

[0223] In addition, from Examples 2, 3 and Examples 8, 9 using Synthesis Examples B2, B3, B5, and B6, it can be seen that the weight average molecular weight value in the low molecular weight region affects the apparent hardness value, and there is a tendency that the larger the weight average molecular weight, the higher the hardness value. From the above, it was confirmed that the apparent hardness of the dip-molded film containing the chloroprene polymer latex of the present invention can be controlled by appropriately adjusting the weight average molecular weight of each chloroprene polymer contained in the chloroprene polymer latex, the type and amount of the monomer unit contained in the chloroprene polymer, and the blending ratio of each chloroprene polymer contained in the chloroprene polymer latex, and by adjusting the apparent hardness of the dip-molded film containing the chloroprene polymer latex, a dip-molded product with excellent hand feel can be obtained.

Claims

1. A chloroprene polymer latex comprising a chloroprene polymer, The apparent hardness of the dip-molded film containing the chloroprene polymer latex and having a thickness of 0.60±0.10 mm measured at 23° C. using a Wallace micro-automatic hardness tester is 25.0 IRHD or more and 40.0 IRHD or less. The impregnation film with a thickness of 0.60±0.10 mm is formed by overlapping a plurality of impregnation films with a thickness of 0.15 to 0.25 mm. The dip-molded film having a thickness of 0.15 to 0.25 mm is obtained by dipping a ceramic mold having a calcium-based coagulation liquid adhered thereto into a chloroprene polymer latex composition containing the chloroprene polymer latex by an immersion coagulation method, and heat-drying the obtained dip-molded film at 150° C. for 60 minutes.

2. The chloroprene polymer latex according to claim 1, in, The chloroprene polymer latex is freeze-dried, dissolved in tetrahydrofuran, and the soluble component is measured by gel permeation chromatography, whereby at least a peak having a weight average molecular weight of 3,000 to 80,000 is detected.

3. The chloroprene polymer latex according to claim 1 or 2, in, The chloroprene-based polymer contains 2,3-dichloro-1,3-butadiene monomer units.

4. The chloroprene polymer latex according to claim 3, in, The chloroprene polymer contains 1 to 25% by mass of the 2,3-dichloro-1,3-butadiene monomer unit relative to 100% by mass of the total of the chloroprene monomer unit and the 2,3-dichloro-1,3-butadiene monomer unit.

5. The chloroprene polymer latex according to any one of claims 1 to 4, in, The toluene-insoluble content of the solid content obtained by freeze-drying the chloroprene polymer latex is 45 to 85% by mass. 6 . A dip-molded product using the chloroprene polymer latex according to claim 1 .

7. The dip-molded article according to claim 6, comprising a metal oxide and an antioxidant.

8. The dip-molded article according to claim 7, which is industrial / general household gloves, medical gloves, balloons, catheters or boots.