Natural sodium bentonite clay with improved rheological properties
By preparing and treated sodium bentonite clay, the problems of insufficient rheological performance and dispersion difficulties in the prior art are solved, and improved thickening efficiency and rapid dispersion effect in water-based formulations are achieved, reducing the need for shear force.
Patent Information
- Application Number
- CN202380030329.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-06
- Filing Date
- 2023-04-03
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to provide bentonite clays with improved rheology properties, especially in water-based formulations, which exhibit improved thickening efficiency, while requiring rapid dispersion in water or aqueous formulations and reducing the need to apply shear forces.
By preparing an aqueous slurry, non-sodium bentonite impurities are removed and spray-dried in a spray drying device, thereby preparing a exchangeable sodium ion content of 100 mmol/100 g or less and a exchangeable calcium ion content of 18 mmol/100 g or less Solid-treated sodium bentonite clay.
The treated bentonite clay with improved thickening efficiency in water-based formulations is achieved, which can be quickly dispersed in water or aqueous formulations, and reduces the need for applying shear forces, providing better rheological properties.
Smart Images

Figure BDA0005059394470000111 
Figure BDA0005059394470000121 
Figure BDA0005059394470000122
Abstract
Description
[0001] The present invention relates to a method for treating a natural clay material comprising sodium bentonite, an overtreated natural sodium bentonite clay obtained by the method, the use of the overtreated natural sodium bentonite clay and a method for controlling the rheology of an aqueous composition.
[0002] Different types of bentonite are named after their primary cation. For industrial use, bentonite is divided into two main categories: sodium bentonite and calcium bentonite. Sodium bentonite is more valuable, but calcium bentonite is more common. Naturally occurring sodium bentonite is usually not very pure. Often, they carry a lot of inert minerals as impurities in the mineral, which detracts from their use as rheological additives.
[0003] Natural calcium bentonite can be converted to sodium bentonite, called sodium enrichment or sodium activation, by an ion exchange process that exhibits many of the properties of sodium bentonite. The usual practice is to add 5-10% of a soluble sodium salt (such as sodium carbonate) to wet calcium bentonite, mix thoroughly, and allow time for ion exchange to occur, with water used to remove the exchanged calcium. Some of the properties of sodium-enriched calcium bentonite (such as viscosity of the suspension and fluid loss) are not exactly the same as those of natural sodium bentonite. For example, if the exchanged cations are not adequately removed, residual calcium carbonate will form, which can result in reduced properties of artificial sodium bentonite.
[0004] CN 111269606 A describes a method for modifying calcium bentonite powder into sodium bentonite powder, which comprises treating calcium bentonite with a sodium cation source in the presence of water, preparing an aqueous slurry, then centrifuging, adjusting the pH and drying.
[0005] CN 102283860 A relates to a method for preparing a montmorillonite preparation, and belongs to the field of pharmaceutical technology. The embodiment describes treating bentonite with water, removing sand, and spray drying the resulting suspension.
[0006] There is a need to provide bentonite clays with improved rheological properties, in particular bentonites that exhibit improved thickening efficiency in water-based formulations. In addition, it is highly desirable that clays be easily and rapidly dispersed in water or aqueous formulations while reducing the need to apply shear forces.
[0007] The present invention provides a method for treating a natural clay material containing sodium bentonite, comprising:
[0008] i) preparing an aqueous slurry of a natural clay material comprising sodium bentonite,
[0009] ii) removing non-sodium bentonite impurities from the aqueous slurry, and
[0010] iii) removing water from the aqueous slurry by spray drying in a spray drying apparatus to produce a solid treated sodium bentonite clay,
[0011] The solid treated bentonite clay has an exchangeable sodium ion content of 100 mmol / 100 g or less and an exchangeable calcium ion content of 18 mmol / 100 g or less, calculated on a clay dry weight basis.
[0012] The process of the present invention provides a treated bentonite clay having improved thickening efficiency in water-based formulations. In addition, the treated clay can be easily and quickly dispersed in water or aqueous formulations, and the need to apply shear forces is reduced.
[0013] The starting material used in the process of the present invention is a natural clay material comprising sodium bentonite.Natural clay material is material obtained from clay mines and has not been treated or modified except by physical methods such as grinding or sieving to obtain the desired particle size.
[0014] Bentonite is a natural clay mineral, the main component of which is montmorillonite. Typically, bentonite contains 30 to 90% by weight of montmorillonite. The montmorillonites present in bentonite are sheet-like aluminosilicates stacked on top of each other. The sheets are usually slightly negatively charged. Therefore, they carry cations in the interlayers between the sheets to compensate for the negative charge of the layers. Their application is usually due to their high surface area and sheet-like structure, which gives them special advantages in gelling water or solvents or adsorbing specific substances or providing barrier properties. In most of these applications, the sheets need to be separated into single or small stacked sheets to achieve optimal performance. Bentonite can provide this expansion into sheets if the interlayer cations are singly charged, especially if the interlayer cations are sodium or lithium. Bentonite clays, which carry mainly divalent cations (Ca and Mg ions) between their layers, swell only slightly, and the individual aluminosilicate sheets cannot be completely separated from each other in water.
[0015] The natural clay material containing sodium bentonite used as the raw material of the present invention generally has a certain content of sodium ions. The content of sodium ions is appropriately expressed as the content of sodium ions that can be exchanged by ammonium chloride. Generally, the natural clay material containing sodium bentonite contains at least 20 mmol / 100g of sodium cations, as determined by ion exchange with ammonium chloride.
[0016] The sodium ion content can be determined by refluxing the natural clay material with excess ammonium chloride in water for 1 hour, then filtering and analyzing the filtrate by inductively coupled plasma optical emission spectrometry (ICP-OES).
[0017] In a preferred embodiment, the natural clay material comprising sodium bentonite comprises at least 30 mmol / 100 g of sodium cations, even more preferably at least 40 mmol / 100 g of sodium cations. Typically, the amount of sodium cations is in the range of 20 mmol / 100 g to 100 mmol / 100 g, preferably in the range of 30 to 90 mmol / 100 g.
[0018] The higher the exchangeable sodium ion content, the higher the sodium bentonite content of the natural clay material. The higher the sodium bentonite content, the better, as it means that less non-sodium bentonite material needs to be removed.
[0019] For the present invention, the natural clay material comprising sodium bentonite preferably has a swelling volume of 12 ml or more, determined by adding 2.0 g of the natural clay material comprising sodium bentonite to 100 ml of deionized water. Generally, a larger swelling volume indicates a higher content of sodium bentonite in the natural clay material, which is preferred. In some embodiments, the natural clay material comprising sodium bentonite preferably has a swelling volume of 15 ml or more, or 20 ml or more, such as 25 ml or more, or 30 ml or more. The swelling volume is generally 70 ml or less, or 60 ml or less.
[0020] The swelling volume can be determined visually. For this purpose, a measuring cylinder is filled with 100 ml of deionized water and 2 g of the corresponding clay material are added to the water in portions over a period of 30 minutes. 60 minutes after the addition of the last portion of clay material, the volume of the swelling material in the cylinder can be measured visually.
[0021] The natural clay material containing sodium bentonite used in the present invention includes sodium bentonite, and other materials, collectively referred to as non-sodium bentonite impurities. Suitably, the natural clay material containing sodium bentonite contains 10 to 90% by weight of sodium bentonite, calculated on the dry weight of the natural clay material. In a preferred embodiment, the content of sodium bentonite in the natural clay material is in the range of 30 to 90% by weight, calculated on the dry weight of the natural clay material.
[0022] The sodium bentonite content of the natural clay material can be determined by dispersing the natural clay material in water and then removing non-sodium bentonite impurities from the natural clay material by centrifugation at 3700 g for 10 minutes and drying the remaining aqueous phase.
[0023] The content of non-sodium bentonite impurities in the natural clay material is suitably in the range of 10 to 90% by weight, preferably 10 to 60% by weight, calculated on the dry weight of the natural clay material.
[0024] In most embodiments, the non-sodium bentonite impurities include at least one of feldspar, calcite, mica, quartz, cristobalite, dolomite, and calcium bentonite.
[0025] In step i) of the process of the present invention, an aqueous slurry of a natural clay material comprising sodium bentonite is prepared. The aqueous slurry can be prepared by mixing the natural clay material and water in a suitable container. The order in which the natural clay material and the water are added to the container is not important. It is also possible to add water and the natural clay material to the container simultaneously. Tap water or water of similar purity is very suitable for use. If desired, water of higher purity or deionized water can be used. However, from an economic point of view, the use of deionized water is not preferred.
[0026] Typically, the aqueous slurry contains 2 to 20% by weight of the natural sodium clay material containing sodium bentonite, calculated on the weight of the aqueous slurry. Although the method can also be carried out in an embodiment in which the amount of the natural sodium clay material containing sodium bentonite is less than 2% by weight of the aqueous slurry, such an embodiment is less attractive from an economic point of view because too much water must be handled. If the amount of the natural sodium clay material containing sodium bentonite exceeds 20% in the aqueous slurry, the viscosity of the slurry may become very high, which is not conducive to handling the aqueous slurry, such as stirring and pumping. In a preferred embodiment, the aqueous slurry contains 3 to 15% by weight of the natural sodium clay material containing sodium bentonite, calculated on the weight of the aqueous slurry.
[0027] In most embodiments, shear forces are applied to the aqueous slurry prepared in step i) of the method of the present invention. The shear forces can be applied by means known to those skilled in the art, such as by a mixer, agitator or dissolver, or a combination thereof. Applying shear forces can reduce the particle size of the slurry and / or result in a more uniform particle size distribution within the slurry.
[0028] In a preferred embodiment, at least one dispersant additive is present during the preparation of an aqueous slurry of a natural clay material comprising sodium bentonite. The presence of the dispersant additive reduces the viscosity of a slurry of a natural clay material comprising sodium bentonite and water at a given content. In addition, the presence of the dispersant additive may also improve the separation of non-sodium bentonite impurities in step ii) of the process of the present invention. Thus, the dispersant additive may improve the efficiency of the process.
[0029] Preferably, the dispersant additive comprises at least one of an organic polymer or oligomer and an inorganic phosphate or polyphosphate. Suitable organic polymers or oligomers include linear and branched polymers or oligomers with side chains or terminal carboxylic acid groups or their salts, phosphoric acid groups or their salts or phosphonate groups. Suitable polymer or oligomer types include polyesters and polyacrylate polymers and oligomers. The weight average molecular weight of the polymer or oligomer is usually in the range of 200 to 250000 g / mol, preferably in the range of 500 to 50000 g / mol.
[0030] If present, the amount of dispersant additive is suitably in the range of 0.5 to 5.0 wt %, calculated on the weight of the natural clay material comprising sodium bentonite. If the amount of dispersant additive is less than 0.5 wt %, the beneficial effects of the dispersant additive may not be fully realized.
[0031] In some embodiments, the dispersant additive may contain sodium ions. However, the amount of sodium ions introduced with the dispersant additive is always less than the amount of sodium ions required for sodium activation of the calcium bentonite.
[0032] In step ii) of the process of the present invention, non-sodium bentonite impurities are removed from the aqueous slurry. Non-sodium bentonite impurities are mainly present in the aqueous slurry in the form of solid particles or incompletely expanded materials, which can be separated from the aqueous phase by physical separation methods commonly known to those skilled in the art. Examples of suitable separation methods include sedimentation, decantation, flotation and centrifugation. If desired, these methods can also be combined or carried out continuously.
[0033] The non-sodium bentonite impurities removed include most of the crystalline impurities and low swelling amorphous minerals and low swelling clays, such as calcium bentonite. The more swelling sodium bentonite is not mainly removed but remains in the slurry.
[0034] As mentioned above, the non-sodium bentonite impurities to be removed generally include at least one of feldspar, calcite, mica, quartz, cristobalite, dolomite and calcium bentonite.
[0035] After the separation step, the aqueous slurry is recovered and water is removed from the aqueous slurry by spray drying in a spray drying apparatus to produce a solid treated sodium bentonite clay.
[0036] If desired, shear forces may be applied to the aqueous slurry prior to removing the water by spray drying. Commonly known techniques for applying shear forces may be used for this optional treatment step. Examples of suitable methods for applying shear forces include treatment with a high speed dissolver or passing the slurry through an orifice under pressure.
[0037] In step iii) of the process of the present invention, water is removed from the aqueous slurry by spray drying in a spray drying apparatus to produce a solid treated sodium bentonite.
[0038] It has been found that spray drying is an essential feature of the process of the present invention and that drying methods other than spray drying result in solid treated sodium bentonite having inferior properties.
[0039] Spray drying devices take a liquid stream and separate the solute or suspension into solids and the solvent into vapor. The solids are usually collected in a drum or cyclone separator. The liquid input stream is sprayed through a nozzle into a hot vapor stream and evaporates. Solids are formed when the water quickly leaves the droplets. Nozzles are usually used to make the droplets as small as possible, thereby maximizing heat transfer and water evaporation rate. The droplet size is usually between 20 and 180 μm, depending on the nozzle. There are two main types of nozzles: high-pressure single-fluid nozzles (50 to 300 bar) and two-fluid nozzles: one fluid is the liquid to be dried and the other is a compressed gas (usually air at 1 to 7 bar). In addition to using nozzles to atomize liquids, rotary atomizers can also be used. The working principle of a rotary atomizer is centrifugal energy; this energy is used to produce a high relative velocity between the fluid and the air, which is essential for atomization. A rotary atomizer includes a rotating surface. This surface can be in the form of a flat disk or a bladed disk, a cup, or a slotted wheel. The liquid first flows radially outward in the disk and is then released from the outer boundary of the disk at a relatively very high speed. Atomization depends on the flow rate of the liquid and the rotation speed of the disk.
[0040] Spray dryers can dry products very quickly compared to other drying methods. They can also convert solutions (or slurries) into dry powders in one step, thus simplifying the process.
[0041] The inlet air temperature of the spray drying apparatus is generally in the range of 150 to 600°C, preferably in the range of 200 to 450°C.
[0042] The spray drying step results in the removal of water and provides treated sodium bentonite solid particles. Typically, the treated sodium bentonite still contains a residual amount of water, for example, the water content is 20.0 wt% or less, based on the total weight of the treated sodium bentonite. Preferably, the water content is in the range of 0.1 to 18.0 wt%, more preferably in the range of 0.5 to 15.0 wt%, based on the total weight of the treated sodium bentonite.
[0043] The present invention also relates to treated sodium bentonite obtainable by or obtained by the process of the present invention.
[0044] The treated sodium bentonite is in the form of particles. The particles generally have a shape in which all three dimensions are of similar order of magnitude, rather than a needle-like or plate-like shape in which one or two dimensions significantly exceed the other. Typically, the length, width and height of the particles differ from each other by less than 35%.
[0045] Suitably, the particles have a d50 number average particle size in the range of 5 to 60 μm, preferably 8 to 40 μm, as determined by laser diffraction.
[0046] The particles typically have a morel-like structure. This means that the particles have an irregular surface characterized by a network of ridges.
[0047] The treated sodium bentonite clay obtained by the process of the present invention suitably has a crystalline impurity content of less than 10 wt%, preferably less than 5 wt%, more preferably less than 3 wt%.
[0048] The treated sodium bentonite clay has an exchangeable sodium ion content of 100 mmol / 100 g or less and an exchangeable calcium ion content of 18 mmol / 100 g or less, calculated on a clay dry weight basis.
[0049] The amount of exchangeable sodium ions is preferably in the range of 50 to 100 mmol / 100 g of the treated sodium bentonite, more preferably in the range of 50 to 90 mmol / 100 g.
[0050] The amount of exchangeable calcium ions is preferably in the range of 2 to 18 mmol / 100 g of the treated sodium bentonite, more preferably in the range of 2 to 15 mmol / 100 g.
[0051] The amount of exchangeable sodium and calcium ions is suitably determined by a method comprising refluxing the treated clay material with excess ammonium chloride in water for 1 hour, then filtering and analysing the filtrate by inductively coupled plasma optical emission spectroscopy (ICP-OES). Excess ammonium chloride means that the amount of ammonium chloride is higher than the amount of exchangeable ions present in the treated clay material. Suitably, 120 mg of the treated clay material is refluxed with 8 ml of an aqueous solution of ammonium chloride having a concentration of 2 mol / l.
[0052] The treated sodium bentonite clay obtained by the method of the present invention is very suitable for controlling the rheology of aqueous compositions. In particular, the treated sodium bentonite clay can be easily dispersed in a variety of aqueous compositions and produce a desired rheological effect. Therefore, the present invention also relates to the use of the treated sodium bentonite clay for controlling the rheology of aqueous compositions.
[0053] The present invention also relates to a method of controlling the rheology of an aqueous composition comprising adding to the aqueous composition the treated sodium bentonite clay obtained by the method of the present invention.
[0054] In the above uses or methods, the treated sodium bentonite is suitably added to the aqueous composition in an amount ranging from 0.1 to 7.0 wt %, preferably ranging from 0.1 to 5.0 wt %, based on the total weight of the aqueous composition.
[0055] When the treated sodium bentonite is added to an aqueous composition, the viscosity of the aqueous composition generally increases. The greater the amount of treated sodium bentonite, the greater the increase in viscosity. In some embodiments, the addition of treated sodium bentonite results in thixotropic behavior of the aqueous composition.
[0056] The aqueous composition can be any liquid aqueous composition, the viscosity of which should increase or should have thixotropy. The aqueous composition is a composition in which the main or only liquid diluent used is water. Preferably, the aqueous composition contains less than 35 wt %, 25 wt %, 20 wt % or even less than 10 wt % of (volatile) organic solvent, based on the total weight of water and organic solvent in the liquid formulation. In some embodiments, the aqueous composition does not contain an organic solvent. The aqueous composition may contain a water-soluble organic or inorganic compound, for example an ionic compound, such as a salt.
[0057] Examples of suitable aqueous liquid compositions include coating compositions, (pre)polymer compositions, pigment concentrates, ceramic products, sealants, cosmetic preparations, adhesives, casting compounds, lubricants, inks, cleaning agents, liquids for gas or oil production, putties, metalworking fluids, sprayable liquids such as deposition aids for crop protection, wax emulsions, liquids for energy storage media such as batteries, liquids for electrical or electronic components, casting or potting compositions and building materials.
[0058] Aqueous compositions as coating compositions or inks can be used in various fields of application, such as automotive coatings, architectural coatings, protective coatings (such as marine coatings or bridge coatings), can and coil coatings, wood and furniture coatings, industrial coatings, plastic coatings, wire enamels, food and seed coatings, leather coatings (for natural and artificial leather), color resists (for liquid crystal displays). Coatings include pasty materials, which usually have a high content of solids and a low content of liquid components, such as pigment pastes or effect pigment pastes (using pigments based on aluminum, silver, brass, zinc, copper, bronze (such as gold bronze), iron oxide-aluminum); other examples of effect pigments are interference pigments and pearlescent pigments, such as metal oxide-mica pigments, bismuth oxide chloride or basic lead carbonate.
[0059] Cosmetic compositions may be all types of aqueous liquid compositions used for personal care and health purposes. Examples are lotions, creams, pastes such as toothpaste, foams such as shaving foams, gels such as shaving gels and shower gels, pharmaceutical compounds in gel-like delivery forms, shampoos, liquid soaps, nail polishes, lipsticks and hair lotions.
[0060] Preferred wax emulsions are aqueous dispersions of wax particles formed from waxes that are solid at room temperature.
[0061] Sprays (preferably used as deposition aids) may be formulated with the treated sodium bentonite of the invention to reduce drift. For example, they may contain fertilizers or herbicides, fungicides and other pesticides.
[0062] Preparations for construction purposes may be materials that are in liquid or pasty form during handling and processing; these water-containing materials are used in the construction industry and they become solid after a setting time, for example, hydraulic binders such as concrete, cement, mortar / plaster, tile adhesives and plaster.
[0063] Metalworking fluids are aqueous compositions used to treat metals and metal parts. Examples are cutting fluids, drilling fluids (used for drilling holes in metals), mold release agents (primarily aqueous emulsions, e.g., in aluminum die casting and foundry applications), foundry cleaning agents, foundry coatings, and liquids used for metal surface treatment (e.g., surface finishing, surface cleaning, and galvanizing).
[0064] Lubricants are water-containing compounds used for lubrication purposes, i.e. to reduce wear and friction losses or to improve cooling, force transmission, vibration damping, sealing effect and corrosion protection.
[0065] Liquid preparations used in gas and oil production are aqueous preparations used to develop and exploit mineral deposits. Aqueous drilling fluids or "drilling muds" are preferred examples. An example application is hydraulic fracturing.
[0066] Cleaning agents can be used to clean different types of objects. They help remove contaminants, residual dirt and adhering debris. Cleaning agents also include detergents (especially for cleaning textiles, their precursors and leather), cleaning agents and polishes, laundry preparations, fabric softeners and personal care products.
[0067] Preferred aqueous compositions include aqueous coating compositions, aqueous compositions comprising hydraulic binders, aqueous cleaning compositions and aqueous personal care compositions.
[0068] The above aqueous composition may contain other ingredients and additives commonly used in aqueous compositions, such as organic co-solvents, crosslinking agents, defoamers, dispersing aids and UV stabilizers. Although the treated sodium bentonite of the present invention has excellent thickening properties, it can also be used in combination with other rheology control agents if necessary.
[0069] Examples of other rheology control agents include polysaccharides (e.g. cellulose derivatives, guar gum, xanthan gum), urea compounds, (poly)amides, polyacrylates (e.g. alkali-soluble or swellable emulsions) or associative thickeners (e.g. polyurethane thickeners, aminoplast-based thickeners, hydrophobically modified alkali-soluble emulsion-type thickeners).
[0070] The treated sodium bentonite of the present invention may also be used as an adsorbent in certain compositions, for example, to absorb unwanted impurities. Example
[0071] Embodiment 1:
[0072] The natural sodium bentonite raw material clay is purchased in the market as "natural sodium bentonite powder", does not contain soda ash, has a moisture content of 8% by weight, and a montmorillonite content of more than 65% by weight. The analytical expansion volume in deionized water is 19 ml / 2g. Crystalline impurities are analyzed by powder X-ray diffraction. The amount of crystallized impurities is 12% by weight.
[0073] 250 kg of natural sodium bentonite powder was vigorously stirred into a slurry in 4800 kg of tap water using a propeller stirrer and a sawtooth dissolving disk for 30 minutes. The slurry was then purified by placing it on a Flottweg decanter centrifuge (with a centrifugal force of about 3700 G) to remove crystalline impurities and unexpanded mineral parts. By this decanter centrifugation, about 1 / 3 of the initial clay mass was removed. The removed materials included most of the crystalline impurities and low-expansion amorphous minerals and low-expansion clays, such as calcium bentonite. The sodium bentonite with better expansion was mainly not removed and remained in the slurry. By this treatment, the total crystalline impurities were reduced to about 2%.
[0074] To achieve perfect dispersion, the resulting slurry was additionally passed through a Manton-Gaulin homogenizer at a pressure of 150 bar.
[0075] The obtained slurry was dried in an Anhydro spray dryer with an inlet drying air temperature of 380°C. The spray feed rate was adjusted to achieve a moisture content of 6% by weight in the obtained dry powder. The spray dryer outlet temperature was in the range of 70°C to 100°C. The number average d50 particle size of the obtained powder was 15 μm. The treated sodium bentonite had an exchangeable sodium ion content of 61 mmol / 100 g and an exchangeable calcium ion content of 11 mmol / 100 g, calculated on the dry weight of the material.
[0076] Embodiment 2:
[0077] 400 kg of natural sodium bentonite powder was added to a mixture of 3600 kg of tap water and 12 kg of BYK-155 / 35 polyacrylate dispersant and stirred into a slurry. For further treatment, the same procedure as in Example 1 was followed. The treated sodium bentonite had an exchangeable sodium ion content of 83 mmol / 100 g and an exchangeable calcium ion content of 12 mmol / 100 g, calculated on the dry weight of the material.
[0078] Embodiment 3:
[0079] 400 kg of natural sodium bentonite powder was added to a mixture of 3600 kg of tap water and 4 kg of sodium pyrophosphate dispersant and stirred into a slurry. For further treatment, the same procedure as in Example 1 was followed.
[0080] Comparative Example 1:
[0081] Natural sodium bentonite powder, supplied from a mine without purification, was ground to the same fineness and moisture as in Example 1. The exchangeable sodium ion content of the treated sodium bentonite was 72 mmol / 100 g and the exchangeable calcium ion content was 46 mmol / 100 g, calculated on the dry weight of the material.
[0082] Comparative Example 2:
[0083] The purified and homogenized slurry from Example 1 (before spray drying) was dried in a laboratory drying oven at 70° C. to a moisture content of less than 12% and ground in a laboratory grinder to the same fineness as in Example 1.
[0084] Comparative Example 3:
[0085] The purified and homogenized slurry from Example 1 (before spray drying) was dried in a drum dryer to a moisture content below 12% and ground in a laboratory grinder to the same fineness as in Example 1.
[0086] Comparative Example 4:
[0087] Optigel CK, a commercial product of BYK-Chemie GmbH: an artificial sodium bentonite prepared by activating calcium bentonite with alkali soda, processed in the same manner as in Example 1. The amount of exchangeable sodium ions in the treated sodium bentonite was 135 mmol / 100 g, and the amount of exchangeable calcium ions was 20 mmol / 100 g, calculated on the dry weight of the material.
[0088] Test Results
[0089] Viscosity in water
[0090] Clay (3.5% or 5%, calculated on the dry weight of clay) is added to deionized water at room temperature in a glass beaker with a diameter of 70 mm, totaling 200 grams of water and clay, thereby preparing a suspension. Add slowly under stirring, using a Pendraulik toothed cover disk (cowles disk) with a diameter of 4 cm mounted on a Pendraulik laboratory stirrer LD 50, and the stirring speed is 930 rpm. After complete addition, the dissolver speed is increased to 2800 rpm, and the dispersion time is 10 minutes. After dispersion, the viscosity is measured at a speed of 10 rpm in a Brookfield DVII. The value is read after a measuring time of 2 minutes. The glass beaker is then covered and stored at room temperature for a specified storage time (e.g., 1 hour, 1 day, 1 week) and then measured again.
[0091] Table 1
[0092]
[0093]
[0094] The results in Table 1 show that the thickening effect of the sodium bentonite treated according to the present invention is much faster than the thickening effect of the comparative sodium bentonite.
[0095] Alpina-Weiss coatings
[0096] 100 g of Alpinaweiβ Innenfarbe "Das Original" (flat latex paint, DAWSE) and 0.2 g of BYK-035 and 24.43 g of the 3.5% aqueous preparation described in Table 1 (pregel) or 17.0 g of the 5% aqueous preparation described in Table 1 (pregel) + 6.8 g of deionized water were added to a Delbrouck beaker no. 211. This was mixed for 5 minutes at 2800 rpm in a Pendraulik laboratory stirrer LD 50 with a toothed cowles disk with a diameter of 4 cm. It was then covered and stored at room temperature for 1 day. The viscosity was measured in a Brookfield DVII at a speed of 10 rpm. The value was read after a measuring time of 2 minutes.
[0097] Table 2
[0098]
[0099]
[0100] From Table 2 it can be inferred that the sodium bentonite treated according to the invention has a much better thickening effect in aqueous coatings than sodium activated Ca-bentonite treated in the same way.
[0101] Determination of Sagging Resistance of White Coatings
[0102] A white paint was prepared using the ingredients listed in Table 3 below.
[0103]
[0104]
[0105] Sag resistance measurement
[0106] Sag resistance is measured according to ASTM D440-84. This standard test method uses a drawdown blade with a series of grooves with increasing gaps. The paint is applied to the test card using a multi-groove applicator. The card is immediately hung vertically with the drawdown strip horizontal. Sag resistance is measured from the drawdown after the film has completely dried. The results indicate the maximum layer thickness that can be applied without the paint sagging.
[0107] The results are summarized in Table 4 below:
[0108] Clay Thickener Sagging(μm) Comparative Example 4 100 Comparative Example 1 100 Comparative Example 2 200 Example 1 250 Example 3 300
[0109] From Table 4 it can be concluded that the sodium bentonite treated according to the present invention provides better sag resistance in aqueous coatings than the comparative bentonite.
Claims
1. A method for treating a natural clay material comprising sodium bentonite, comprising: i) preparing an aqueous slurry of a natural clay material comprising sodium bentonite, ii) removing non-sodium bentonite impurities from the aqueous slurry, and iii) removing water from the aqueous slurry by spray drying in a spray drying apparatus to produce a solid treated sodium bentonite clay, The solid treated bentonite clay has an exchangeable sodium ion content of 100 mmol / 100 g or less and an exchangeable calcium ion content of 18 mmol / 100 g or less, calculated on a clay dry weight basis.
2. The method according to claim 1, wherein the swelling volume of the natural clay material comprising sodium bentonite is 12 ml or more, as determined by adding 2.0 g of the natural clay material comprising sodium bentonite to 100 ml of deionized water.
3. The method according to claim 1 or 2, wherein the non-sodium bentonite impurities include at least one of feldspar, calcite, mica, quartz, cristobalite, dolomite and calcium bentonite.
4. A process according to any one of the preceding claims, wherein the content of non-sodium bentonite impurities in the natural clay material comprising sodium bentonite is in the range of 10 to 90 wt. %, preferably in the range of 10 to 60 wt. %.
5. A method according to any one of the preceding claims, wherein in step i) shear forces are applied to the aqueous slurry.
6. A process according to any one of the preceding claims wherein a dispersant additive is present during the preparation of the aqueous slurry of the natural clay material comprising sodium bentonite.
7. The method of claim 6, wherein the dispersant additive comprises at least one of an organic polymer and an inorganic phosphate.
8. A process according to any one of the preceding claims wherein non-sodium bentonite impurities are removed from the aqueous slurry by sedimentation or centrifugation.
9. A process according to any one of the preceding claims, wherein the inlet air temperature of the spray drying apparatus is in the range of 150°C to 600°C.
10. A process according to any one of the preceding claims wherein the residual water content of the solid treated sodium bentonite is 20 wt% or less, calculated on the total weight of the solid treated sodium bentonite clay.
11. A treated sodium bentonite clay obtainable by the process of any one of the preceding claims.
12. The treated sodium bentonite clay according to claim 11, wherein the treated sodium bentonite clay is in the form of particles having a morel-like structure.
13. A treated sodium bentonite clay according to claim 11 or 12, wherein the particles have a d50 number average particle size in the range of 5 to 60 μm, as determined by laser diffraction.
14. Use of a treated sodium bentonite clay according to any one of claims 11 to 13 for controlling the rheology of an aqueous composition.
15. The use according to claim 14, wherein the aqueous composition is selected from the group consisting of an aqueous coating composition, an aqueous composition comprising a hydraulic binder, an aqueous cleaning composition and an aqueous personal care composition.
16. Use according to claim 14 or 15, wherein the treated sodium bentonite clay is added to the aqueous composition in an amount of 0.1 to 7.0 wt%, preferably 0.1 to 5.0 wt%, calculated on the total weight of the aqueous composition.
17. A method of controlling the rheology of an aqueous composition comprising adding the treated sodium bentonite clay according to any one of claims 11 to 13 to the aqueous composition.