Macromolecular well wall protective agent and preparation method thereof
By using copolymerization reactions of vinyl monomer, silane coupling agent and surfactant in the well wall protection agent, polymer well wall protection agent was prepared, which solved the insufficient stability of the existing well wall protection agent under complex geological conditions. The problem of this paper has achieved improved stability and safety of well walls in high temperature and high pressure environments, and is suitable for a variety of drilling fluid systems.
Patent Information
- Application Number
- CN202411184722.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing well wall protection agents have insufficient stability, poor temperature and pressure resistance under complex geological conditions, and have high environmental pollution and cost, and insufficient comprehensive performance, so they cannot effectively cope with complex and changing geological conditions and environmental protection requirements.
The polymer well wall protection agent is prepared by copolymerization reaction under the action of water-soluble initiator to form a tough protective film to adapt to ultra-high temperature and ultra-high pressure environment.
Significantly improve the stability of the well wall, prevent well collapse and well leakage, is suitable for a variety of drilling fluid systems, enhance the application scope, ensure the safety and efficiency of drilling operations, and meet environmental protection requirements.
Smart Images

Figure CN118930713A_ABST
Abstract
Description
Technical Field
[0001] The invention provides a polymer well wall protective agent and a preparation method thereof, belonging to the technical field of petroleum drilling. Background Art
[0002] As the global demand for oil and gas resources continues to grow, oil and gas drilling operations have expanded significantly in terms of geographic scope and depth. This results in complex and variable formation conditions often encountered during drilling, such as soft formations, salt formations, easily collapsed formations, and high-pressure formations. In order to meet the drilling needs under these extreme conditions, the advancement of drilling fluid technology is crucial, which largely relies on the research and development of new drilling fluid treatment agents. Wellbore instability can lead to complex situations such as well collapse and well leakage, which seriously affects drilling efficiency and safety and increases drilling costs. In order to maintain wellbore stability, wellbore protectors are usually added to the drilling fluid. Wellbore protectors can enhance the stability of the wellbore by forming a protective film on the wellbore.
[0003] Existing wellbore protective agents are mainly composed of a variety of polymers (such as polyacrylamide, polyvinyl alcohol, etc.) and chemical additives (such as salts, alcohols, silicates, etc.). These protective agents can provide a certain wellbore stabilization effect under conventional formation conditions. However, under certain conditions, existing wellbore protective agents have the following problems and limitations: insufficient stability, poor temperature and pressure resistance. Some wellbore protective agents may pollute the environment, have high costs, and insufficient comprehensive performance. Therefore, the development of a wellbore protective agent with better performance to adapt to complex and changeable geological conditions and environmental protection requirements has become a technical problem that needs to be solved urgently in the current oil and gas drilling field. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a polymer well wall protective agent and a preparation method thereof. The polymer well wall protective agent of the present invention is obtained by copolymerization of vinyl monomer, silane coupling agent and anionic and nonionic composite surfactant under the action of water-soluble initiator. The polymer well wall protective agent of the present invention has good stability and good temperature and pressure resistance during use.
[0005] The technical solution adopted by the present invention is:
[0006] A method for preparing a polymer well wall protective agent comprises the following steps:
[0007] (1) Preparation of a monomer mixture: Methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and a silane coupling agent are uniformly mixed at 30 to 40° C. to obtain 100 parts by weight of a monomer mixture; wherein the mass ratio of methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and silane coupling agent is (45 to 60):(15 to 25):(5 to 10):(1 to 2):(2 to 8);
[0008] (2) Preparation of an initiator aqueous solution: Weigh 0.5 to 1 parts by weight of a water-soluble initiator, mix the water-soluble initiator with water to prepare an initiator aqueous solution with a mass fraction of 1%;
[0009] (3) Preparation of anionic and nonionic composite surfactant solution: Add 80 to 100 parts by weight of water to a reaction bottle, add alkylphenol ether sulfosuccinate sodium salt, octylphenol polyoxyethylene ether-10 and allyloxy nonylphenol propanol polyoxyethylene (10) ether ammonium sulfate in a mass ratio of (1 to 2): (0.3 to 1): (0.2 to 1) respectively under stirring, and stir evenly to obtain an anionic and nonionic composite surfactant solution with a mass fraction of 5% to 10%;
[0010] (4) Preparation of seed emulsion: 20-30 parts by weight of the monomer mixture in step (1) are added dropwise to the reaction bottle in step (3), and stirred evenly in a constant temperature water bath at 60-80° C.; 20%-30% of the initiator aqueous solution is weighed and slowly added dropwise to the reaction bottle, and the addition is controlled to be completed within 20-30 minutes. After the addition is completed, stirring is continued for 20-30 minutes to obtain a seed emulsion;
[0011] (5) Preparation of polymer well wall protective agent: Keep a constant temperature water bath at 60-80°C, add the remaining monomer mixed solution of step (1) to the seed emulsion of step (4), and control the addition to be completed within 40-60 minutes, and at the same time, add the remaining initiator solution of step (2), and control the addition to be completed within 60-70 minutes. After the addition is completed, continue to keep the reaction in a constant temperature water bath at 60-80°C for 20-40 minutes, and cool to room temperature to obtain the polymer well wall protective agent.
[0012] Preferably, the silane coupling agent in step (1) is γ-methacryloxypropyltrimethoxysilane.
[0013] Preferably, the water-soluble initiator in step (2) is one of azobisisobutylamidine hydrochloride and azobisisobutylimidazoline hydrochloride.
[0014] Compared with the prior art, the present invention has the following technical effects:
[0015] 1) High efficiency and stability: This type of polymer well wall protective agent can form a tough protective film on the well wall, significantly improving the stability of the well wall under complex geological conditions and effectively preventing drilling accidents such as well collapse and well leakage.
[0016] 2) Good temperature and pressure resistance: This type of polymer well wall protective agent is adapted to ultra-high temperature and ultra-high pressure formation environments, and can maintain its performance without degradation under extreme conditions, ensuring the safety and efficiency of drilling operations.
[0017] 3) Wide adaptability: This polymer wellbore protective agent is suitable for various types of drilling fluid systems and is not limited by the type and formula of drilling fluid, which enhances its application range in different drilling operations. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a particle size distribution diagram of the polymer well wall protective agent prepared in Example 1 of the present invention;
[0019] Figure 2 This is an infrared spectrum of the polymer well wall protective agent prepared in Example 1 of the present invention;
[0020] Figure 3 This is a photo of the agglomeration of sodium bentonite after being immersed in the aqueous solution of the polymer well wall protective agent prepared in Example 1 of the present invention and centrifuged;
[0021] Figure 4 This is a scanning electron microscope photo of sodium bentonite after drying;
[0022] Figure 5 This is a scanning electron microscope photograph of sodium bentonite after being soaked in the polymer well wall protective agent solution prepared in Example 1 of the present invention, centrifuged, agglomerated, and dried. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical scheme and advantages of the present invention clearer, the preferred embodiments of the present invention are further described in detail in conjunction with the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Example 1
[0025] (1) Methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane were mixed uniformly at 30° C. to obtain 100 g of a monomer mixture; wherein the mass ratio of methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane was 50:20:10:1:6;
[0026] (2) Take 0.5 g of azobisisobutylamidine hydrochloride and add water to prepare an initiator aqueous solution with a mass fraction of 1%;
[0027] (3) Add 100g of water to the reaction flask, add sodium salt of alkylphenol ether sulfosuccinate, octylphenol polyoxyethylene ether-10 and allyloxy nonylphenol propanol polyoxyethylene (10) ether ammonium sulfate in a mass ratio of 1:0.5:0.3 under stirring, and stir evenly to obtain a 10% mass fraction of anionic and nonionic composite surfactant solution; weigh 20g of the monomer mixture described in step (1), slowly drip it into the reaction flask with a constant pressure dropping funnel, and stir evenly in a constant temperature water bath at 80°C; then slowly drip 20% of the initiator aqueous solution prepared in step (2), control the dripping to be completed within 20 minutes, and continue stirring for 20 minutes; pour the remaining monomer mixture in step (1) into the constant pressure dropping funnel, control the monomer mixture to be dripped within 40 to 60 minutes, and at the same time drip the remaining initiator solution in step (2), control the initiator aqueous solution to be dripped within 60 to 70 minutes. After all the additions were completed, the reaction was continued at 80° C. for 30 min. The obtained product was cooled to room temperature to obtain a polymer well wall protective agent.
[0028] Example 2
[0029] (1) Methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane were mixed uniformly at 30° C. to obtain 100 g of a monomer mixture; wherein the mass ratio of methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane was 50:20:10:1:6;
[0030] (2) Take 0.5 g of azobisisobutylamidine hydrochloride and add water to prepare an initiator aqueous solution with a mass fraction of 1%;
[0031] (3) Add 100g of water to the reaction flask, add sodium salt of alkylphenol ether sulfosuccinate, octylphenol polyoxyethylene ether-10 and allyloxy nonylphenol propanol polyoxyethylene (10) ether ammonium sulfate in a mass ratio of 1.5:0.5:0.3 under stirring, and stir evenly to obtain a 10% mass fraction of anionic and nonionic composite surfactant solution; weigh 20g of the monomer mixture described in step (1), slowly drip it into the reaction flask with a constant pressure dropping funnel, and stir evenly in a constant temperature water bath at 80°C; then slowly drip 20% of the initiator aqueous solution prepared in step (2), control the dripping to be completed within 20 minutes, and continue stirring for 20 minutes; pour the remaining monomer mixture in step (1) into the constant pressure dropping funnel, control the monomer mixture to be dripped within 40 to 60 minutes, and at the same time drip the remaining initiator solution in step (2), control the initiator aqueous solution to be dripped within 60 to 70 minutes. After all the additions were completed, the reaction was continued at 80° C. for 30 min. The obtained product was cooled to room temperature to obtain a polymer well wall protective agent.
[0032] Example 3
[0033] (1) Methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane were mixed uniformly at 30° C. to obtain 100 g of a monomer mixture; wherein the mass ratio of methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane was 50:20:10:1:6;
[0034] (2) Take 0.5 g of azobisisobutylamidine hydrochloride and add water to prepare an initiator aqueous solution with a mass fraction of 1%;
[0035] (3) Add 100g of water to the reaction flask, add sodium salt of alkylphenol ether sulfosuccinate, octylphenol polyoxyethylene ether-10 and allyloxy nonylphenol propanol polyoxyethylene (10) ether ammonium sulfate in a mass ratio of 2:0.5:0.3 under stirring, and stir evenly to obtain a 10% mass fraction of anionic and nonionic composite surfactant solution; weigh 20g of the monomer mixture described in step (1), slowly drip it into the reaction flask with a constant pressure dropping funnel, and stir evenly in a constant temperature water bath at 80°C; then slowly drip 20% of the initiator aqueous solution prepared in step (2), control the dripping to be completed within 20 minutes, and continue stirring for 20 minutes; pour the remaining monomer mixture in step (1) into the constant pressure dropping funnel, control the monomer mixture to be dripped within 40 to 60 minutes, and at the same time drip the remaining initiator solution in step (2), control the initiator aqueous solution to be dripped within 60 to 70 minutes. After all the additions were completed, the reaction was continued at 80° C. for 30 min. The obtained product was cooled to room temperature to obtain a polymer well wall protective agent.
[0036] Example 4
[0037] (1) Methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane were mixed uniformly at 30° C. to obtain 100 g of a monomer mixture; wherein the mass ratio of methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane was 55:15:5:1.5:5;
[0038] (2) Take 1 g of azobisisobutylamidine hydrochloride and add water to prepare an initiator aqueous solution with a mass fraction of 1%;
[0039] (3) Add 80g of water to the reaction flask, add sodium salt of alkylphenol ether sulfosuccinate, octylphenol polyoxyethylene ether-10 and allyloxy nonylphenol propanol polyoxyethylene (10) ether ammonium sulfate in a mass ratio of 1.5:0.5:0.5 under stirring, and stir evenly to obtain an anionic and nonionic composite surfactant solution with a mass fraction of 8%; weigh 25g of the monomer mixture described in step (1), slowly drip it into the reaction flask with a constant pressure dropping funnel, and stir evenly in a constant temperature water bath at 70°C; then slowly drip 25% of the initiator aqueous solution prepared in step (2), control the dripping to be completed within 25 minutes, and continue stirring for 25 minutes; pour the remaining monomer mixture in step (1) into the constant pressure dropping funnel, control the monomer mixture to be dripped within 40-60 minutes, and at the same time drip the remaining initiator solution in step (2), control the initiator aqueous solution to be dripped within 60-70 minutes. After all the additions were completed, the reaction was continued at 70° C. for 30 min. The obtained product was cooled to room temperature to obtain a polymer well wall protective agent.
[0040] Example 5
[0041] (1) Methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane were mixed uniformly at 30° C. to obtain 100 g of a monomer mixture; wherein the mass ratio of methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane was 45:25:5:1.5:2;
[0042] (2) Take 1 g of azobisisobutylamidine hydrochloride and add water to prepare an initiator aqueous solution with a mass fraction of 1%;
[0043] (3) Add 80g of water to the reaction flask, add sodium salt of alkylphenol ether sulfosuccinate, octylphenol polyoxyethylene ether-10 and allyloxy nonylphenol propanol polyoxyethylene (10) ether ammonium sulfate in a mass ratio of 1.5:0.5:0.8 under stirring, and stir evenly to obtain an anionic and nonionic composite surfactant solution with a mass fraction of 8%; weigh 25g of the monomer mixture described in step (1), slowly drip it into the reaction flask with a constant pressure dropping funnel, and stir evenly in a constant temperature water bath at 70°C; then slowly drip 25% of the initiator aqueous solution prepared in step (2), control the dripping to be completed within 25 minutes, and continue stirring for 25 minutes; pour the remaining monomer mixture in step (1) into the constant pressure dropping funnel, control the monomer mixture to be dripped within 40-60 minutes, and at the same time drip the remaining initiator solution in step (2), control the initiator aqueous solution to be dripped within 60-70 minutes. After all the additions were completed, the reaction was continued at 70° C. for 30 min. The obtained product was cooled to room temperature to obtain a polymer well wall protective agent.
[0044] Example 6
[0045] (1) Methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane were mixed uniformly at 30° C. to obtain 100 g of a monomer mixture; wherein the mass ratio of methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane was 60:15:8:1.5:4;
[0046] (2) Take 1 g of azobisisobutylamidine hydrochloride and add water to prepare an initiator aqueous solution with a mass fraction of 1%;
[0047] (3) Add 80g of water to the reaction flask, add sodium salt of alkylphenol ether sulfosuccinate, octylphenol polyoxyethylene ether-10 and allyloxy nonylphenol propanol polyoxyethylene (10) ether ammonium sulfate in a mass ratio of 1.5:0.5:1 under stirring, and stir evenly to obtain an anionic and nonionic composite surfactant solution with a mass fraction of 8%; weigh 25g of the monomer mixture described in step (1), slowly drip it into the reaction flask using a constant pressure dropping funnel, and stir evenly in a constant temperature water bath at 70°C; then slowly drip 25% of the initiator aqueous solution prepared in step (2), control the dripping to be completed within 25 minutes, and continue stirring for 25 minutes; pour the remaining monomer mixture in step (1) into the constant pressure dropping funnel, control the monomer mixture to be dripped within 40-60 minutes, and at the same time drip the remaining initiator solution in step (2), control the initiator aqueous solution to be dripped within 60-70 minutes. After all the additions were completed, the reaction was continued at 70° C. for 30 min. The obtained product was cooled to room temperature to obtain a polymer well wall protective agent.
[0048] Example 7
[0049] (1) Methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane were mixed uniformly at 30° C. to obtain 100 g of a monomer mixture; wherein the mass ratio of methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane was 50:20:5:2:5;
[0050] (2) Take 0.5 g of azobisisobutylimidazoline hydrochloride and add water to prepare an initiator aqueous solution with a mass fraction of 1%;
[0051] (3) Add 80g of water to the reaction flask, add sodium salt of alkylphenol ether sulfosuccinate, octylphenol polyoxyethylene ether-10 and allyloxy nonylphenol propanol polyoxyethylene (10) ether ammonium sulfate in a mass ratio of 1.5:0.8:0.8 under stirring, and stir evenly to obtain a 5% mass fraction of anionic and nonionic composite surfactant solution; weigh 20g of the monomer mixture described in step (1), slowly drip it into the reaction flask with a constant pressure dropping funnel, and stir evenly in a constant temperature water bath at 60°C; then slowly drip 20% of the initiator aqueous solution prepared in step (2), control the dripping to be completed within 20 minutes, and continue stirring for 20 minutes; pour the remaining monomer mixture in step (1) into the constant pressure dropping funnel, control the monomer mixture to be dripped within 40-60 minutes, and at the same time drip the remaining initiator solution in step (2), control the initiator aqueous solution to be dripped within 60-70 minutes. After all the additions were completed, the reaction was continued at 60° C. for 30 min. The obtained product was cooled to room temperature to obtain a polymer well wall protective agent.
[0052] Example 8
[0053] (1) Methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane were mixed uniformly at 40° C. to obtain 100 g of a monomer mixture; wherein the mass ratio of methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane was 50:25:5:2:5;
[0054] (2) Take 0.5 g of azobisisobutylimidazoline hydrochloride and add water to prepare an initiator aqueous solution with a mass fraction of 1%;
[0055] (3) Add 80g of water to the reaction flask, add sodium salt of alkylphenol ether sulfosuccinate, octylphenol polyoxyethylene ether-10 and allyloxy nonylphenol propanol polyoxyethylene (10) ether ammonium sulfate in a mass ratio of 1.5:1:0.8 with stirring, and stir evenly to obtain a 5% mass fraction of anionic and nonionic composite surfactant solution; weigh 25g of the monomer mixture described in step (1), slowly drip it into the reaction flask with a constant pressure dropping funnel, and stir evenly in a constant temperature water bath at 60°C; then slowly drip 25% of the initiator aqueous solution prepared in step (2), control the dripping to be completed within 25 minutes, and continue stirring for 25 minutes; pour the remaining monomer mixture in step (1) into the constant pressure dropping funnel, control the monomer mixture to be dripped within 40-60 minutes, and at the same time drip the remaining initiator solution in step (2), control the initiator aqueous solution to be dripped within 60-70 minutes. After all the additions were completed, the reaction was continued at 60° C. for 30 min. The obtained product was cooled to room temperature to obtain a polymer well wall protective agent.
[0056] Example 9
[0057] (1) Methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane were mixed uniformly at 40° C. to obtain 100 g of a monomer mixture; wherein the mass ratio of methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane was 50:25:5:2:8;
[0058] (2) Take 0.5 g of azobisisobutylimidazoline hydrochloride and add water to prepare an initiator aqueous solution with a mass fraction of 1%;
[0059] (3) Add 80g of water to the reaction flask, add sodium salt of alkylphenol ether sulfosuccinate, octylphenol polyoxyethylene ether-10 and allyloxy nonylphenol propanol polyoxyethylene (10) ether ammonium sulfate in a mass ratio of 1.5:1:1 under stirring, and stir evenly to obtain a 5% mass fraction of anionic and nonionic composite surfactant solution; weigh 30g of the monomer mixture described in step (1), slowly drip it into the reaction flask with a constant pressure dropping funnel, and stir evenly in a constant temperature water bath at 60°C; then slowly drip 30% of the initiator aqueous solution prepared in step (2), control the dripping to be completed within 30 minutes, and continue stirring for 30 minutes; pour the remaining monomer mixture in step (1) into the constant pressure dropping funnel, control the monomer mixture to be dripped within 40 to 60 minutes, and at the same time drip the remaining initiator solution in step (2), control the initiator aqueous solution to be dripped within 60 to 70 minutes. After all the additions were completed, the reaction was continued at 60° C. for 30 min. The obtained product was cooled to room temperature to obtain a polymer well wall protective agent.
[0060] Example 10
[0061] (1) Methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane were mixed uniformly at 40° C. to obtain 100 g of a monomer mixture; wherein the mass ratio of methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and γ-methacryloxypropyl trimethoxysilane was 50:25:5:1.5:8;
[0062] (2) Take 0.5 g of azobisisobutylimidazoline hydrochloride and add water to prepare an initiator aqueous solution with a mass fraction of 1%;
[0063] (3) Add 90g of water to the reaction flask, add sodium salt of alkylphenol ether sulfosuccinate, octylphenol polyoxyethylene ether-10 and allyloxy nonylphenol propanol polyoxyethylene (10) ether ammonium sulfate in a mass ratio of 2:1:1 under stirring, stir evenly, and obtain a 5% mass fraction of anionic and nonionic composite surfactant solution; weigh 30g of the monomer mixture described in step (1), slowly drip it into the reaction flask with a constant pressure dropping funnel, and stir evenly in a constant temperature water bath at 60°C; then slowly drip 30% of the initiator aqueous solution prepared in step (2), control the dripping to be completed within 30 minutes, and continue stirring for 30 minutes; pour the remaining monomer mixture in step (1) into the constant pressure dropping funnel, control the monomer mixture to be dripped within 40 to 60 minutes, and at the same time drip the remaining initiator solution in step (2), control the initiator aqueous solution to be dripped within 60 to 70 minutes. After all the additions were completed, the reaction was continued at 60° C. for 30 min. The obtained product was cooled to room temperature to obtain a polymer well wall protective agent.
[0064] Comparative Example 1
[0065] Refer to Example 1, except that no methyl methacrylate is added.
[0066] Comparative Example 2
[0067] Refer to Example 1, except that no vinyl acetate is added.
[0068] Comparative Example 3
[0069] Refer to Example 1, except that no pentaerythritol triacrylate is added.
[0070] Comparative Example 4
[0071] The same method as in Example 1 was used, except that γ-methacryloxypropyltrimethoxysilane was not added.
[0072] Comparative Example 5
[0073] Refer to Example 1, except that no acrylamide is added.
[0074] Comparative Example 6
[0075] Refer to Example 1, the only difference is that the concentration of the anionic and nonionic composite surfactant solution is adjusted to 3%.
[0076] Comparative Example 7
[0077] Refer to Example 1, the only difference is that the concentration of the anionic and nonionic composite surfactant solution is adjusted to 12%.
[0078] Performance Testing
[0079] 1. Particle size test
[0080] The polymer well wall protective agent prepared in Example 1 was diluted with deionized water to a mass concentration of 0.1%, and after ultrasonic dispersion treatment for 30 minutes, the particle size was measured using a British Malvern Zetasizer Nano ZS laser scattering particle size analyzer at a test temperature of 25°C. The particle size test results are shown in Figure 1 .
[0081] Depend on Figure 1 It can be seen that the particle size of the polymer well wall protective agent prepared in Example 1 of the present invention presents a unimodal distribution, the particle size distribution range is narrow, the polydispersity coefficient is 0.221, and the particle size is 87.17 nm, indicating that the polymer well wall protective agent prepared by emulsion polymerization has high stability.
[0082] 2. Infrared test
[0083] The polymer well wall protective agent prepared in Example 1 was purified, dried, and ground into powder. The infrared structure was tested by the potassium bromide tablet method using a VECTOR-22 Fourier transform infrared spectrometer from Bruker, Germany, with a scanning range of 4000-500 cm -1 , resolution 4cm -1 . Infrared test results see Figure 2 .
[0084] Depend on Figure 2 It can be seen that 3226.83cm -1 The amino stretching vibration absorption peak is 2933.37cm -1 The absorption peak of C=O in the product is generally at 1720cm -1 Therefore, 1726.24cm -1 The bending vibration characteristic peaks around 1440.79cm -1 -CH2 bending vibration absorption peak; 1188.72cm -1 、1137.92cm -1 The absorption peak of C—O—C vibration indicates the successful introduction of ester group. -1 The Si-O-Si stretching vibration absorption peak is 846.72 cm -1 The bending vibration absorption peak of Si-O is at 1675-1640cm -1 No characteristic absorption peak of C=C stretching vibration was observed, which indicates that there is no unreacted vinyl monomer in the sample and no residual monomer in the polymer product. The results show that the prepared polymer well wall protective agent contains characteristic functional groups of various monomers in the molecular structure design.
[0085] 3. Application performance testing
[0086] The polymer well wall protective agent prepared in Examples 1 to 10 was tested for its application performance according to the following steps:
[0087] (1) The stability of the polymer well wall protective agent emulsion prepared in Examples 1 to 10 was determined by using a centrifuge. The specific method was as follows: 10 mL of the polymer well wall protective agent emulsion prepared in Examples 1 to 10 was respectively transferred into a 10 mL centrifuge tube, placed in a centrifuge, and centrifuged at a speed of 1500 r / min for 15 min. The emulsion was taken out after the centrifuge was stopped and the state of the emulsion was observed, and it was recorded whether the emulsion had precipitation or stratification.
[0088] (2) Accurately weigh 2 g of the centrifuged polymer well wall protective agent emulsion (1) in a dry and clean 250 mL beaker, add 98 mL of deionized water, and stir evenly with a glass cup for later use.
[0089] (3) Weigh 10 g of sodium bentonite and place it in an electric constant temperature drying oven at 105°C ± 1°C for 6 h. Take it out and place it in a desiccator to cool to room temperature for later use.
[0090] (4) Pipette 5 mL of the aqueous solution of the polymer well wall protective agent prepared in (2) into a 10 mL centrifuge tube, weigh 0.5 g of the sodium bentonite in (3), put it into the centrifuge tube, then add 5 mL of the polymer well wall protective agent solution prepared in (2), shake well, store at room temperature for 2 h, put it into a centrifuge, centrifuge at a speed of 1500 r / min for 15 min, stop the centrifuge, take it out, and observe whether the sodium bentonite in the centrifuge tube is agglomerated.
[0091] Figure 3 This is a photo of the sodium bentonite agglomeration after being soaked in the aqueous solution of the polymer well wall protective agent prepared in Example 1 of the present invention and centrifuged. Figure 3 It can be seen that after being soaked in the aqueous solution of the polymer well wall protective agent, the polymer well wall protective agent can interact with the mineral salts on the surface of the sodium bentonite, wrap the sodium bentonite, and then prevent the clay from dispersing, plug the formation gaps, thereby maintaining the stability of the well wall and effectively protecting the reservoir.
[0092] The comparative example application performance test method is the same as above, and the stability of the comparative example emulsion and whether the sodium bentonite in the centrifuge tube is agglomerated are observed. The emulsion state after centrifugation of the embodiment and the comparative example and the agglomeration of the sodium bentonite are shown in Table 1.
[0093] Table 1
[0094] Example Emulsion state Sodium Bentonite Comparative Example Emulsion state Sodium Bentonite Example 1 Stable emulsion Unite into a block Comparative Example 1 Stable emulsion Relatively loose Example 2 Stable emulsion Unite into a block Comparative Example 2 Stable emulsion Relatively loose Example 3 Stable emulsion Unite into a block Comparative Example 3 Stable emulsion Relatively loose Example 4 Stable emulsion Unite into a block Comparative Example 4 Stable emulsion Relatively loose Example 5 Stable emulsion Unite into a block Comparative Example 5 Stable emulsion Relatively loose Example 6 Stable emulsion Agglomeration Comparative Example 6 Emulsion is unstable and stratified Unable to test Example 7 Stable emulsion Unite into a block Comparative Example 7 Stable emulsion Relatively loose, slightly clumped Example 8 Stable emulsion Unite into a block Example 9 Stable emulsion Unite into a block Example 10 Stable emulsion Unite into a block
[0095] As can be seen from Table 1, the polymer well wall protective agent emulsion prepared by the present application can still maintain a stable emulsion state after centrifugation, without stratification, precipitation and other phenomena, is easy to store for a long time, has a long shelf life, and can make sodium bentonite aggregate. This is because the polymer well wall protective agent prepared by the present invention is a polymer with a network cross-linked structure. From the perspective of its raw material components, pentaerythritol triacrylate is a polymerizable cross-linked monomer that can form a network cross-linked structure for the polymer; methyl methacrylate and γ-methacryloxypropyl trimethoxysilane are hard monomers, and the combination of the two can make the polymer molecule have a rigid segment and have certain strength and mechanical properties. At the same time, the amide group and ester group provided by acrylamide and vinyl acetate in the polymer structure can form hydrogen bonds with the mineral salt on the surface of sodium bentonite, and are connected to form a network structure through hydrogen bonds, wrapping the sodium bentonite. Therefore, the polymer prepared by the present invention can prevent clay from dispersing, block the formation gap, thereby maintaining the stability of the well wall and effectively protecting the reservoir. However, the comparative examples 1 to 5 in which the ingredients were adjusted could not cause the sodium bentonite to clump, that is, could not maintain the stability of the well wall. After reducing the ratio of the anionic and nonionic compound surfactants in comparative example 6, a stable emulsion could not be formed. After increasing the ratio of the anionic and nonionic compound surfactants in comparative example 7, although a relatively stable polymer emulsion could be formed, the waterproof performance of the polymer after film formation deteriorated due to the increase in the amount of surfactants. Therefore, the sodium bentonite could not be effectively film-formed, and the stability of the well wall could not be maintained.
[0096] 4. Scanning electron microscope test
[0097] (1) Weigh 10 g of sodium bentonite and place it in an electric constant temperature drying oven at 105°C ± 1°C for 6 h. Take it out and place it in a desiccator to cool to room temperature for later use.
[0098] (2) According to the application performance test method 3., the polymer well wall protective agent prepared in Example 1 was soaked in sodium bentonite, centrifuged, and agglomerated, and then kept at a constant temperature of 105°C ± 1°C for 6 hours, taken out and placed in a desiccator to cool to room temperature for use.
[0099] (3) The microstructure of sodium bentonite (1) and (2) was observed using a Japanese IT700HR non-leakage magnetic thermal field emission scanning electron microscope. The scanning electron microscope photos are shown in Figure 4 and Figure 5 .
[0100] Figure 4 This is a scanning electron microscope photo of sodium bentonite (magnification 500). Figure 5The following is a scanning electron microscope photograph (magnification 500) of sodium bentonite after being soaked in the aqueous solution of the polymer well wall protective agent of Example 1 and centrifuged to form agglomerates. It can be clearly seen that before being soaked in the aqueous solution of the polymer well wall protective agent, the sodium bentonite is in granular form, and there is no other substance between the particles; after being soaked in the aqueous solution, the polymer well wall protective agent forms a dense film on the surface of the sodium bentonite, and the film almost completely covers the sodium bentonite particles. This indicates that the polymer well wall protective agent prepared in this application has excellent film-forming properties, thereby maintaining the stability of the well wall and effectively protecting the reservoir.
[0101] The embodiments described above are part of the embodiments of the present invention, rather than all of the embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A method for preparing a polymer well wall protective agent, characterized in that: The following steps are involved: (1) Preparation of a monomer mixture: Methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and a silane coupling agent are uniformly mixed at 30 to 40° C. to obtain 100 parts by weight of a monomer mixture; wherein the mass ratio of methyl methacrylate, vinyl acetate, acrylamide, pentaerythritol triacrylate, and silane coupling agent is (45 to 60):(15 to 25):(5 to 10):(1 to 2):(2 to 8); (2) Preparation of an initiator aqueous solution: Weigh 0.5 to 1 parts by weight of a water-soluble initiator, mix the water-soluble initiator with water to prepare an initiator aqueous solution with a mass fraction of 1%; (3) Preparation of anionic and nonionic composite surfactant solution: Add 80 to 100 parts by weight of water to a reaction bottle, add alkylphenol ether sulfosuccinate sodium salt, octylphenol polyoxyethylene ether-10 and allyloxy nonylphenol propanol polyoxyethylene (10) ether ammonium sulfate in a mass ratio of (1 to 2): (0.3 to 1): (0.2 to 1) respectively under stirring, and stir evenly to obtain an anionic and nonionic composite surfactant solution with a mass fraction of 5% to 10%; (4) Preparation of seed emulsion: 20-30 parts by weight of the monomer mixture in step (1) are added dropwise to the reaction bottle in step (3), and stirred evenly in a constant temperature water bath at 60-80° C.; 20%-30% of the initiator aqueous solution is weighed and slowly added dropwise to the reaction bottle, and the addition is controlled to be completed within 20-30 minutes. After the addition is completed, stirring is continued for 20-30 minutes to obtain a seed emulsion; (5) Preparation of polymer well wall protective agent: Keep a constant temperature water bath at 60-80°C, add the remaining monomer mixed solution of step (1) to the seed emulsion of step (4), and control the addition to be completed within 40-60 minutes, and at the same time, add the remaining initiator solution of step (2), and control the addition to be completed within 60-70 minutes. After the addition is completed, continue to keep the reaction in a constant temperature water bath at 60-80°C for 20-40 minutes, and cool to room temperature to obtain the polymer well wall protective agent.
2. The method for preparing a polymer well wall protective agent according to claim 1, characterized in that: The silane coupling agent in step (2) is γ-methacryloxypropyltrimethoxysilane.
3. The method for preparing a polymer well wall protective agent according to claim 1, characterized in that: The water-soluble initiator in step (2) is one of azobisisobutylamidine hydrochloride and azobisisobutylimidazoline hydrochloride.
4. A polymer well wall protective agent, characterized in that: Prepared by any one of the methods of claims 1 to 3.
Citation Information
Patent Citations
Polymeric Compositions Agglomerating Compositions, Modified Solid Materials, And Methods For Making And Using Same
CN107683319A
Novel phase-change material with multiple phase-change temperatures
CN108504332A
Wall fixing agent for drilling fluid as well as preparation method and application of wall fixing agent
CN111748330A
Zwitterionic polymers comprising betaine-type units and use of zwitterionic polymers in drilling fluids
CN1894292A
Cementitious plugging wall solidifer for water-based drilling fluid, and a preparation method thereof and a water-based drilling fluid
US11578250B1