Optical film, polarizing plate, and image display device
By using a cured resin composition of a specific proportion in the optical film, the problems of low moisture permeability, surface hardness and bending resistance in the prior art are solved, and excellent optical film performance is achieved, suitable for polarizing plates and image displays Device.
Patent Information
- Application Number
- CN202380028556.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-22
- Filing Date
- 2023-06-15
- Publication Date
- 2024-11-12
AI Technical Summary
现有技术难以在光学膜中实现低透湿性、表面硬度和耐弯曲性的兼顾,尤其是在薄型化基材和严苛的固化条件下,导致制造工序增加和基材收缩引起的褶皱问题。
Using a cured resin composition laminated on a transparent substrate, the composition contains compound A with more than 2 reactive functional groups, compound B with more than 1 bromine atoms, and compound C with more than 3 reactive functional groups, and light is combined with The polymerization initiator D has a ratio of 30 to 60 mass %, a ratio of 10 to 25 mass %, and a film thickness of 3 to 20 μm. Low moisture permeability and hardness are achieved by specific curing conditions.
An optical film with excellent moisture permeability, high surface hardness, low curlability and bending resistance is achieved. It is suitable for polarizing plates and image display devices, reducing process complexity during manufacturing and defects caused by substrate shrinkage.
Smart Images

Figure CN118946833A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an optical film, a polarizing plate and an image display device. Background Art
[0002] The quality of image display devices is greatly affected by moisture in the atmosphere. For example, when the polarizer of a polarizing plate absorbs moisture, the display including the polarizing plate warps, causing light leakage. Therefore, improvement is achieved by using a polarizing plate protective film with low moisture permeability.
[0003] For example, Patent Document 1 describes a barrier laminate having improved barrier properties by laminating an organic layer formed of an organic compound having a cyclic structure and an inorganic layer of a silicon compound on a substrate film. Patent Document 2 describes a curable composition containing an epoxy compound having a halogen element as a sealant for an organic EL display element.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2014 / 136590
[0007] Patent Document 2: International Publication No. 2020 / 149384 Summary of the invention
[0008] Problems to be solved by the invention
[0009] In order to reduce the moisture permeability of an optical film such as a polarizing plate protective film, it is difficult to sufficiently reduce the moisture permeability by only providing an organic layer on a substrate. On the other hand, only providing an inorganic layer on a substrate may result in insufficient adhesion to the substrate or cracks in the inorganic layer. When an inorganic layer is provided, it is preferred to stack an organic layer and an inorganic layer as described in Patent Document 1, but this results in an increase in the number of manufacturing steps.
[0010] In Patent Document 2, the thickness of the cured sealant is set to 100 μm, thereby achieving a heat release rate of 40 g / (m 2 However, in recent years, due to the thinning of optical films, the thickness of the substrate has become less than 100 μm. From the perspective of thinning, it is not preferable to provide a cured film thicker than the substrate. In addition, in order to obtain a 100 μm thick cured film, for example, several thousand mJ / cm 2 UV irradiation or at 100°C
[0011] The above heating is performed for several hours, but in the roll-to-roll method of continuously producing optical films at a conveying speed of tens of meters per minute, it is impossible to set such harsh curing conditions. In addition, depending on the material of the substrate, the shrinkage caused by heat is large, so at 100°C
[0012] Under the above heating conditions, wrinkles are generated due to shrinkage of the substrate. Therefore, the sealant composition for organic EL elements cannot be applied to optical films.
[0013] An object of the present invention is to provide an optical film which is excellent in low moisture permeability and has surface hardness, low curling and bending resistance, and a polarizing plate and an image display device using the optical film.
[0014] Means for solving problems
[0015] The optical film of the present invention comprises a cured film of a curable resin composition on at least one surface of a transparent substrate, wherein the curable resin composition comprises: a compound (A) having two or more reactive functional groups in one molecule and one or more alicyclic hydrocarbons or aromatic rings in one molecule; a compound (B) having one or more reactive functional groups in one molecule and one or more bromine atoms in one molecule; a compound (C) having three or more reactive functional groups in one molecule; and a photopolymerization initiator (D), wherein the reactive functional groups of the compounds (A), (B) and (C) are any one of ethylenically unsaturated bond groups, epoxy groups and oxetane groups, wherein the content ratio of the compound (A) in the total solid content of the curable resin composition is 30 to 60% by mass, the content ratio of the compound (B) is 30 to 60% by mass, the content ratio of the compound (C) is 10 to 25% by mass, and the thickness of the cured film is 3 to 100 μm.
[0016] 20μm.
[0017] The polarizing plate and the image display device according to the present invention include the above-mentioned optical film.
[0018] Effects of the Invention
[0019] According to the present invention, it is possible to provide an optical film which is excellent in low moisture permeability and has both surface hardness, low curling and bending resistance, and a polarizing plate and an image display device using the optical film. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] [ Figure 1 ] Figure 1 It is a cross-sectional view showing a schematic structure of an optical film according to an embodiment. DETAILED DESCRIPTION
[0021] Figure 1It is a cross-sectional view showing a schematic structure of an optical film according to an embodiment.
[0022] The optical film 1 includes a transparent substrate 2 and a cured film 3 of a curable resin composition laminated on one surface of the transparent substrate 2. In the present embodiment, the cured film 3 is laminated on one surface of the transparent substrate 2, but the cured film 3 may be provided on both surfaces of the transparent substrate 2.
[0023] The transparent substrate 2 is a film that becomes the base of the optical film 1, and is formed of a material with excellent transmittance of visible light. As the transparent substrate 2, any one of an acrylic substrate, a triacetyl cellulose substrate, a cycloolefin polymer substrate, a cycloolefin copolymer substrate, a polyethylene terephthalate substrate, a polycarbonate substrate, a polyimide-based substrate, and a polyamide-based substrate can be used. In order to reduce the moisture permeability of the optical film 1, the lower the moisture permeability of the transparent substrate 2 itself, the more preferably. Therefore, in the case of manufacturing an optical film 1 with extremely low moisture permeability, for example, an acrylic substrate, a cycloolefin substrate, etc. are preferably used.
[0024] The thickness of the transparent substrate 2 is not particularly limited, and for example, a substrate with a thickness of 10 to 200 μm can be used. In order to reduce the thickness of the optical film 1, the thickness of the transparent substrate 2 is preferably 10 to 100 μm, more preferably 20 to 60 μm.
[0025] The cured film 3 is a functional layer that imparts low moisture permeability and surface hardness to the optical film 1. The film thickness of the cured film 3 is preferably 3 to 20 μm, and more preferably 5 to 15 μm. When the film thickness of the cured film 3 is less than 3 μm, the surface hardness of the optical film 1 is reduced, and low moisture permeability becomes difficult, so it is not preferred. When the film thickness of the cured film 3 exceeds 20 μm, the optical film 1 curls due to the shrinkage during the curing of the curable resin composition, which reduces the workability (handling property) of the optical film 1 during manufacturing or processing, so it is not preferred. In addition, when the film thickness of the cured film 3 exceeds 20 μm, when the optical film 1 is bent, cracks are easily generated on the surface of the cured film 3, so it is not preferred.
[0026] The curable resin composition for forming the cured film 3 contains the following compounds (A) to
[0027] (D).
[0028] Compound (A): A compound having two or more reactive functional groups in one molecule and one or more alicyclic hydrocarbons or aromatic rings in one molecule
[0029] Compound (B): a compound having one or more reactive functional groups in one molecule and one or more bromine atoms in one molecule
[0030] Compound (C): A compound having three or more reactive functional groups in one molecule
[0031] Photopolymerization initiator (D)
[0032] The reactive functional group possessed by the compounds (A), (B) and (C) is preferably any one of a methacryloyl group, an epoxy group and an oxetanyl group.
[0033] The compounds (A) and (B) are components that constitute the basic skeleton of the cured film 3 and impart low moisture permeability to the cured film 3 .
[0034] When gas permeates (passes) in a polymer such as the cured film 3, the gas molecules pass through the free volume portion (molecular gaps generated by the movement of the molecular chain). Therefore, it is believed that the larger the free volume of the polymer, the easier it is for the gas to permeate. In addition, the smaller the molecular diameter of the gas, the easier it is to permeate the polymer. In the present invention, the compound (B) in the curable resin composition has a halogen atom (bromine atom) with an atomic radius larger than that of hydrogen. The halogen atom reduces the free volume in the molecule and thus hinders the water molecules from passing through the cured film 3. As a result, the optical film 1 can be made less permeable to moisture. In addition, when the compound (A) or (B) has an aromatic ring, stacking (stacking) occurs due to the interaction of the aromatic rings, so that the molecules become close, which helps to reduce the permeability of the optical film 1.
[0035] The compound (A) has a hydrophobic functional group (alicyclic hydrocarbon or aromatic ring), which reduces the moisture permeability of the optical film 1. The content of the compound (A) is 30 to 60% by mass of the total solid content of the curable resin composition. When the mixing ratio of the compound (A) deviates from this range, the mixing ratio of the compounds (B) and (C) cannot be within an appropriate range, which is not preferred.
[0036] The content of compound (B) is 30-60% by mass of the total solid content of the curable resin composition. By making the content of compounds (A) and (B) 30-60% by mass of the total solid content, the balance of the cyclic skeleton (alicyclic hydrocarbon or aromatic ring) and the halogen element with an atomic radius larger than hydrogen is good, and excellent low moisture permeability can be obtained. When the content of compound (B) is less than 30% by mass of the total solid content of the curable resin composition, it is difficult to show the low moisture permeability caused by bromine atoms, so it is not preferred. In addition, since the cured product of compound (B) is softer than the cured product of compound (A), when the content of compound (B) exceeds 60% by mass of the total solid content of the curable resin composition, the hardness deteriorates, so it is not preferred. In addition, compound (B) also helps to alleviate the curling of the cured film 3.
[0037] Compound (C) is mainly a component that crosslinks compounds (A) and (B) to impart hardness to the cured film 3. In order to impart the desired hardness to the cured film 3, compound (C) is preferably a polyfunctional compound of trifunctional or higher. The content of compound (C) is 10 to 25% by mass of the total solid content of the curable resin composition. When the content of compound (C) is less than 10% by mass of the total solid content of the curable resin composition, it is difficult to show hardness, so it is not preferred. On the other hand, when the content of compound (C) exceeds 25% by mass of the total solid content of the curable resin composition, the content of compounds (A) and (B) is relatively reduced, and low moisture permeability may become insufficient, so it is not preferred. In addition, when the content of compound (C) exceeds 25% by mass of the total solid content of the curable resin composition, the shrinkage of the curable resin composition during curing becomes stronger, thereby increasing the curling of the optical film 1, reducing the handling of the optical film 1 during manufacture and processing, and when the optical film 1 is bent, cracks are easily generated in the cured film 3, so it is not preferred.
[0038] In order to polymerize and cure the compounds (A) to (C), a photopolymerization initiator (D) is added. When the reactive functional groups of the compounds (A) to (C) are (meth)acryloyl groups, a free radical polymerization initiator is used as the photopolymerization initiator (D). In addition, when the reactive functional groups of the compounds (A) to (B) are epoxy groups or oxetanyl groups, a photoacid generator is used as the photopolymerization initiator.
[0039] As the compound (A), a compound having an alicyclic hydrocarbon or an aromatic ring and two or more (meth)acryloyl groups, or a compound having an alicyclic hydrocarbon or an aromatic ring and two or more epoxy groups or oxetanyl groups can be used.
[0040] Examples of the difunctional or higher-functional (meth)acrylates having an alicyclic hydrocarbon include dimethylol tricyclodecane di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, dicyclopentenyl di(meth)acrylate, dicyclopentadienyl di(meth)acrylate, bornyl di(meth)acrylate, isobornyl di(meth)acrylate, tricyclodecyl di(meth)acrylate, adamantyl di(meth)acrylate, adamantane dimethanol di(meth)acrylate, and the like. Acid ester, adamantane diethanol di(meth)acrylate, dihydroxymethyl dicyclopentane di(meth)acrylate, norbornane dihydroxymethyl di(meth)acrylate, cyclohexanedimethanol tri(meth)acrylate, adamantane tri(meth)acrylate, adamantane trimethanol tri(meth)acrylate, norbornane trihydroxymethyl tri(meth)acrylate, tricyclodecane trimethanol tri(meth)acrylate, perhydro-1,4,5,8-dimethylnaphthalene-2,3,7-(oxymethyl) tri(meth)acrylate.
[0041] Examples of the (meth)acrylate having two or more functions and having an aromatic ring include EO (ethylene oxide)-modified bisphenol A di(meth)acrylate, PO (propylene oxide)-modified bisphenol A di(meth)acrylate, ECH (ethylcyclohexane)-modified bisphenol A di(meth)acrylate, EO-modified bisphenol F di(meth)acrylate, ECH-modified hexahydrophthalic acid di(meth)acrylate, and ECH-modified phthalic acid di(meth)acrylate.
[0042] Examples of the bifunctional or higher-functional epoxy compound having an alicyclic hydrocarbon include hydrogenated bisphenol A diglycidyl ether, 3,4-epoxycyclohexanecarboxylic acid 3',4'-epoxycyclohexylmethyl ester, bis(3,4-epoxycyclohexylmethyl) adipate, 4-vinylcyclohexene dioxide, and limonene dioxide.
[0043] Examples of bifunctional or higher-functional epoxy compounds having an aromatic ring include epoxy compounds having a bisphenol skeleton such as bisphenol A type and bisphenol F type, a naphthalene skeleton, a fluorene skeleton, and a biphenyl skeleton. A specific example of a bisphenol A type epoxy compound is 2,2-bis(4-glycidyloxyphenyl)propane.
[0044] Examples of bifunctional or higher-functional oxetane compounds having an alicyclic hydrocarbon or an aromatic ring include EO-modified hydrogenated bisphenol A bis(3-ethyl-3-oxetanyl methyl) ether, PO-modified hydrogenated bisphenol A bis(3-ethyl-3-oxetanyl methyl) ether, ethylene oxide (EO)-modified bisphenol A bis(3-ethyl-3-oxetanyl methyl) ether, and EO-modified bisphenol F (3-ethyl-3-oxetanyl methyl) ether.
[0045] As the compound (B), a compound having a bromine atom and any one of a (meth)acryloyl group, an epoxy compound, and an oxetanyl group can be used.
[0046] Examples of the compound (B) include 2,3-dibromopropyl (meth)acrylate, tribromophenyl (meth)acrylate, EO-modified tribromophenyl (meth)acrylate, EO-modified tetrabromobisphenol A di(meth)acrylate, PO-modified tribromophenyl (meth)acrylate, PO-modified tetrabromobisphenol A di(meth)acrylate, dibromophenyl glycidyl ether, dibromoneopentyl glycol diglycidyl ether, and 3-bromooxetane.
[0047] As the compound (C), trifunctional or higher-functional (meth)acrylates, trifunctional or higher-functional epoxy compounds, and trifunctional or higher-functional oxetane compounds can be used.
[0048] Examples of trifunctional or higher (meth)acrylates include tri(meth)acrylates such as trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, tri-2-hydroxyethyl isocyanurate tri(meth)acrylate, and glycerol tri(meth)acrylate; and trifunctional (meth)acrylate compounds such as pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, and ditrimethylolpropane tri(meth)acrylate. Polyfunctional (meth)acrylate compounds having three or more functions, such as pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, ditrimethylolpropane penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ditrimethylolpropane hexa(meth)acrylate, and dipentaerythritol polyacrylate; and polyfunctional (meth)acrylate compounds in which a part of these (meth)acrylates is substituted with an alkyl group or ε-caprolactone, etc.
[0049] Examples of the trifunctional or higher-functional epoxy compound include novolac epoxy compounds, diglycerol triglycidyl ether, pentaerythritol polyglycidyl ether, and 1,3,5-tris(2,3-epoxypropyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione.
[0050] Examples of the trifunctional or higher-functional oxetane compound include oxetane silicate, pentaerythritol tris(3-ethyl-3-oxetanylmethyl) ether, pentaerythritol tetrakis(3-ethyl-3-oxetanylmethyl) ether, dipentaerythritol hexa(3-ethyl-3-oxetanylmethyl) ether, dipentaerythritol penta(3-ethyl-3-oxetanylmethyl) ether, dipentaerythritol tetrakis(3-ethyl-3-oxetanylmethyl) ether, ditrimethylolpropane tetrakis(3-ethyl-3-oxetanylmethyl) ether, caprolactone-modified dipentaerythritol hexa(3-ethyl-3-oxetanylmethyl) ether, and caprolactone-modified dipentaerythritol penta(3-ethyl-3-oxetanylmethyl) ether.
[0051] As the free radical polymerization initiator that can be used as the above-mentioned photopolymerization initiator (D), compounds such as acetophenone, benzophenone, thioxanthone, benzoin, and benzoin methyl ether can be preferably used. Examples of free radical polymerization initiators include: 2,2-ethoxyacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2,2-dimethoxy-phenylacetophenone, dibenzoyl, benzoin, benzoin methyl ether, benzoin ethyl ether, p-chlorobenzophenone, p-methoxybenzophenone, Michler'sketone, acetophenone, and 2-chlorothioxanthone. The content ratio of the free radical polymerization initiator (D) is preferably 0.1 to 5% by mass of the total solid content of the curable resin composition.
[0052] As the photoacid generator that can be used as the photopolymerization initiator (D), compounds such as aromatic diazonium salts, aromatic sulfonium salts, aromatic iodonium salts, and metallocene compounds can be preferably used. Examples of the photoacid generator include p-methoxybenzenediazonium hexafluorophosphate, diphenyl 4-thiophenoxyphenylsulfonium hexafluorophosphate, diphenyl 4-thiophenoxyphenylsulfonium hexafluoroantimonate, diphenyl iodonium hexafluorophosphate, diphenyl iodonium hexafluoroantimonate, triphenylsulfonium hexafluorophosphate, triphenylsulfonium hexafluoroantimonate, diphenyl [4- (phenylthio) phenyl] sulfonium hexafluorophosphate, diphenyl [4- (phenylthio) phenyl] sulfonium hexafluoroantimonate, diphenyl [4- (phenylthio) phenyl] sulfonium pentafluorohydroxyantimonate, diphenyl [4- (phenylthio) phenyl] sulfonium tris (pentafluoro) hydroxyantimonate. The photoacid generator is preferably present in an amount of 0.1 to 5.0% by mass of the total solid content of the curable resin composition.
[0053] In addition, the compounds (A) to (D) mentioned above may be used alone or in combination of two or more.
[0054] In order to improve the surface property of the coating film of the curable resin composition, a leveling agent may also be added. The content of the leveling agent is preferably 0.05 to 5.0% by mass of the solid content of the hard coat forming composition. There is no particular limitation on the compound that can be used as the leveling agent, and for example, F565 and RS-75 manufactured by DIC Corporation can be used.
[0055] A solvent may be added to the curable resin composition as needed. As the solvent, one of the following solvents may be used or a mixture of two or more thereof: alcohols such as methanol, ethanol, 1-propanol, 2-propanol, butanol, isopropanol, and isobutanol; ketones such as acetone, methyl ethyl ketone, cyclohexanone, and methyl isobutyl ketone; ketone alcohols such as diacetone alcohol; aromatic hydrocarbons such as benzene, toluene, and xylene; glycols such as ethylene glycol, propylene glycol, and hexylene glycol; glycol ethers such as ethyl cellosolve, butyl cellosolve, ethyl carbitol, butyl carbitol, diethyl cellosolve, diethyl carbitol, and propylene glycol monomethyl ether; esters such as dimethyl carbonate, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, butyl acetate, and amyl acetate; ethers such as dimethyl ether and diethyl ether; N-methylpyrrolidone and dimethylformamide.
[0056] In addition, various additives such as antistatic agents, defoaming agents, antioxidants, ultraviolet absorbers, infrared absorbers, colorants, light stabilizers, polymerization inhibitors, photosensitizers, antifouling agents, oleophobic agents, hydrophobic agents, and anti-fingerprint adhesion agents may be added to the curable resin composition as needed.
[0057] The coating method of the curable resin composition is not particularly limited, and for example, coating can be performed using a spin coater, roll coater, reverse roll coater, gravure coater, micro gravure coater, air knife coater, rod coater, wire bar coater, die coater, dip coater, spray coater, applicator, etc.
[0058] The optical film 1 involved in this embodiment has low moisture permeability and can therefore be used as a protective film for a polarizing plate. A polarizing plate can be made by pasting protective films on both sides of a polarizer formed by adsorbing iodine or a dye on a polyvinyl alcohol (PVA) film and orienting it. The optical film 1 involved in this embodiment can be pasted on both sides of the polarizer, or the optical film 1 involved in this embodiment can be pasted on one side of the polarizer and a film different from the optical film 1 can be pasted on the other side. As a film different from the optical film 1, a single-layer film composed of any one of a cycloolefin polymer, polyethylene terephthalate, and polymethyl methacrylate can be used.
[0059] In addition, the polarizing plate using the optical film 1 of the present embodiment can be used in combination with an image display panel such as a liquid crystal panel or an organic EL panel to form an image display device. The image display device may also have a touch panel. The polarizing plate using the optical film 1 of the present embodiment as a protective film has low moisture permeability and bending resistance, and therefore, for example, can be suitably used as an image display device provided on a curved surface in a vehicle.
[0060] As described above, in this embodiment, since the cured film 3 is formed using a curable resin composition containing the above-mentioned compounds (A), (B) and (C) in a specific ratio, an optical film 1 having a balance of low moisture permeability, surface hardness, low curling and bending resistance can be achieved.
[0061] Example
[0062] Hereinafter, embodiments for implementing the present invention will be described.
[0063] The materials used in Examples and Comparative Examples are as follows.
[0064] (A) A compound having two or more reactive functional groups in one molecule and one or more alicyclic hydrocarbons or aromatic rings in one molecule
[0065] (A-1): 2,2-bis(4-glycidyloxyphenyl)propane, B1796 (trade name), manufactured by Tokyo Chemical Industry Co., Ltd.
[0066] [Chemical formula 1]
[0067]
[0068] (A-2): 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate, Celloxide 2021P (trade name), manufactured by Daicel Corporation
[0069] [Chemical formula 2]
[0070]
[0071] (A-3): dimethylol-tricyclodecane diacrylate, Light Acrylate DCP-A (trade name), manufactured by Kyoeisha Chemical Co., Ltd.
[0072] [Chemical formula 3]
[0073]
[0074] (A-4): EO-modified bisphenol A diacrylate, Light Acrylate BP-4EAL (trade name), manufactured by Kyoeisha Chemical Co., Ltd.
[0075] [Chemical formula 4]
[0076]
[0077] (A') A compound having two or more reactive functional groups in one molecule and having no alicyclic hydrocarbon and aromatic ring
[0078] Triethylene glycol diacrylate, Light Acrylate 3EG-A (trade name), manufactured by Kyoeisha Chemical Co., Ltd.
[0079] [Chemical formula 5]
[0080]
[0081] (B) A compound having one or more reactive functional groups in one molecule and one or more bromine atoms in one molecule
[0082] (B-1): 2,4-dibromophenyl glycidyl ether, D4885 (trade name), manufactured by Tokyo Chemical Industry Co., Ltd.
[0083] [Chemical formula 6]
[0084]
[0085] (B-2): tribromophenyl acrylate, T3130 (trade name), manufactured by Tokyo Chemical Industry Co., Ltd.
[0086] [Chemical formula 7]
[0087]
[0088] (B-3): Dibromopropyl acrylate, A0910 (trade name), manufactured by Tokyo Chemical Industry Co., Ltd.
[0089] [Chemical formula 8]
[0090]
[0091] (B') A compound having one or more reactive functional groups and no bromine atom in one molecule
[0092] 1H,1H,2H,2H-nonafluorohexyl acrylate, N1107 (trade name), manufactured by Tokyo Chemical Industry Co., Ltd.
[0093] [Chemical formula 9]
[0094]
[0095] (C) Compounds having three or more reactive functional groups in one molecule
[0096] (C-1): Oxetanyl silicate, OXT191 (trade name), manufactured by Toagosei Co., Ltd.
[0097] [Chemical formula 10]
[0098]
[0099] (C-2): Pentaerythritol triacrylate, Light Acrylate PE-3A (trade name), manufactured by Kyoeisha Chemical Co., Ltd.
[0100] [Chemical formula 11]
[0101]
[0102] (C') A compound having two reactive functional groups in one molecule
[0103] 3-Ethyl-3-{[(3-ethyloxetan-3-yl)methoxy]}oxetane, OX-221 (trade name), manufactured by Toagosei Co., Ltd.
[0104] [Chemical formula 12]
[0105]
[0106] (D) Photopolymerization initiator
[0107] (D-1): 1-Hydroxycyclohexyl-phenyl ketone, Omnirad 184 (trade name), manufactured by IGM Resins BV
[0108] (D-2): Diphenyl 4-thiophenoxyphenylsulfonium hexafluoroantimonate, CPI-101A (trade name), manufactured by San-Apro Co., Ltd.
[0109] (E) Leveling agent
[0110] F565 (trade name), manufactured by DIC Co., Ltd.
[0111] Curable resin compositions were prepared containing compounds (A) to (E) in the amounts shown in Tables 1 to 4. In addition, the unit of the amount of each component shown in Tables 1 to 4 is parts by mass.
[0112] The coating solution prepared by diluting the adjusted curable resin composition with a solvent was applied to a TAC film (trade name: TJ40, manufactured by FUJIFILM Co., Ltd.) having a thickness of 40 μm using a wire bar coater so that the film thickness after curing becomes the value described in Tables 1 to 4. After heating in an oven at 60° C. for 1 minute to dry the coating film, the coating film was cured in a UV curing device in a nitrogen atmosphere (oxygen concentration of 500 ppm or less) at a cumulative light intensity of 200 mJ / cm 2 The coating film is cured by irradiating ultraviolet rays in a manner to obtain an optical film.
[0113] <Evaluation of optical film>
[0114] [Pencil hardness]
[0115] A scratch test was performed on the hard coating surface of the protective film A using a pencil (uni, manufactured by Mitsubishi Pencil Co., Ltd.) and a Clemens scratch tester (HA-301, manufactured by TESTERSANGYO Co., Ltd.) under the conditions of a load of 500 g and a scratch speed of 0.5 mm / sec. The scratch test was performed 5 times at each hardness while changing the hardness of the pencil. The case where there were two or more scratches on the surface of the cured film of the curable resin composition was considered NG, and the maximum hardness that did not become NG was determined based on the following criteria. The judgments of ○ and ◎ were considered acceptable.
[0116] ◎:≥3H
[0117] 0: 2H
[0118] △: H
[0119] ×: < less than H
[0120] [Bending resistance]
[0121] The optical film was cut into a sample of 3 cm × 10 cm in size, and the sample was wound onto an iron rod (mandrel) of a predetermined diameter (1φ to 8φ [mm]) with the cured film on the outside. The minimum diameter of the iron rod without cracks on the surface was used as the evaluation value of the bending resistance, and the sample was judged according to the following criteria. The judgments of ○ and ◎ were regarded as passing.
[0122] ◎: 2mmφ or less
[0123] 0:3mmφ
[0124] △: 4mmφ
[0125] ×: 5mmφ or more
[0126] A sample of 100 mm square was prepared by cutting the optical film. The sample was placed on a flat surface. The vertical distance (standing height) from the flat surface to the top of the four corners was measured in mm. The total of the measured values of the four corners was used as the evaluation value, and the evaluation was performed according to the following criteria. ○ and ◎ were considered acceptable.
[0127] ◎:0~5mm
[0128] ○: More than 5mm and less than 20mm
[0129] △: More than 20mm and less than 35mm
[0130] ×: More than 35 mm and less than 50 mm
[0131] [Moisture Permeability]
[0132] According to the moisture permeability test method (cup method) for moisture-proof packaging materials specified in JIS Z 0208:1976, the moisture permeability of the obtained optical film and the moisture permeability of the above-mentioned transparent substrate were measured under the conditions of 40°C and 90RH%. Based on the measured value of the moisture permeability of the optical film and the measured value of the moisture permeability of the transparent substrate, the moisture permeability of the cured film of the curable resin composition was calculated using the following formula (1), and the judgment was made according to the following criteria. It should be noted that formula (1) is based on "Barrier Chemistry of Packaging Materials (Basic Lecture on Packaging 5), p68-p72, written by Tsutomu Nakagawa, Japan Society of Packaging". The judgments of ○ and ◎ are set as pass.
[0133] 1 / a=1 / b+1 / c…Formula (1)
[0134] here
[0135] a: Moisture permeability of optical film
[0136] b: Moisture permeability of transparent substrate
[0137] c: Moisture permeability value of the curable resin composition layer.
[0138] ◎: c value is 100g / (m 2 ·Days) or less
[0139] ○: c value exceeds 100g / (m 2 ·day) and 175g / (m 2 ·Days) or less
[0140] △: c value exceeds 175g / (m 2 ·day) and 250g / (m 2 ·Days) or less
[0141] ×: c value exceeds 250g / (m 2 ·sky)
[0142] Tables 1 to 4 collectively show the composition of the curable resin composition in each Example and each Comparative Example, the evaluation values of the above-mentioned evaluation items, and the determination results.
[0143] [Table 1]
[0144]
[0145] [Table 2]
[0146]
[0147] [Table 3]
[0148]
[0149] [Table 4]
[0150]
[0151] The optical films involved in Examples 1 to 7 were judged as ◎ or ○ in all evaluation items of pencil hardness, bending resistance, curling and moisture permeability. Therefore, it can be confirmed that by forming a cured film on a transparent substrate using a curable resin composition containing compounds (A), (B) and (C) in a specific ratio and setting the film thickness of the cured film within a specific range, an optical film having excellent low moisture permeability and having both surface hardness, low curling and bending resistance can be achieved.
[0152] In Comparative Example 1, since the compounds (A) and (B) were not used, the determination of the water vapor permeability was poor. Since the compounding ratio of the compound (C) was too high, the pencil hardness increased, but the determination of the bending resistance and the curling was poor.
[0153] In Comparative Example 2, the determination of water vapor permeability was poor because the compound (B) was not used. In addition, since the compound (B) is a material that forms a soft and less curled cured product, the determination of bendability and curling was poor because the compound (B) was not added.
[0154] In Comparative Example 3, since the compound (A) was not used, the determination of the water vapor permeability was poor. In addition, since the compounding ratio of the compound (B) was too high, the determination of the pencil hardness was poor.
[0155] In Comparative Example 4, since the compound (C) was not used, the pencil hardness was poor.
[0156] In Comparative Example 5, since the compound (A') having neither an alicyclic hydrocarbon nor an aromatic ring was used instead of the compound (A), the determination of the water vapor permeability was poor.
[0157] In Comparative Example 6, since the compound (B′) having no bromine atom was used instead of the compound (B), the determination of the water vapor permeability was poor.
[0158] In Comparative Example 7, since the compound (C′) having a reactive functional group number of less than 3 was used instead of the compound (C), the pencil hardness was poorly judged.
[0159] In Comparative Example 8, since the mixing ratio of the compound (A) was too large and the mixing ratio of the compound (B) was too small, the determination of the water vapor permeability was poor.
[0160] In Comparative Example 9, since the blending ratio of the compound (B) was too large, the determination of the pencil hardness was poor.
[0161] In Comparative Example 10, the determination of bending resistance and curling deteriorated because the compound (C) was mixed in too much proportion. In addition, when the compound (C) was mixed in too much proportion, the amount of compounds (A) and (B) that contribute to moisture permeability was relatively reduced, so the determination of moisture permeability deteriorated.
[0162] In Comparative Example 11, since the blending ratio of the compound (C) was too small, the determination of the pencil hardness was poor.
[0163] In Comparative Example 12, since the film thickness of the cured film was too thin, the determination of the pencil hardness and the water vapor permeability was poor.
[0164] In Comparative Example 13, since the film thickness of the cured film was too thick, the determination of the bending resistance and the curling was poor.
[0165] Industrial Applicability
[0166] The present invention can be used as an optical film used in image display devices and the like, and is suitable as a protective film for a polarizing plate used in image display devices, for example.
[0167] Explanation of symbols
[0168] 1 Optical film
[0169] 2 Transparent substrate
[0170] 3 cured film
Claims
1. An optical film having a cured film of a curable resin composition on at least one surface of a transparent substrate, The curable resin composition comprises: A compound (A) having two or more reactive functional groups in one molecule and one or more alicyclic hydrocarbons or aromatic rings in one molecule; A compound (B) having one or more reactive functional groups in one molecule and one or more bromine atoms in one molecule; A compound (C) having three or more reactive functional groups in one molecule; and Photopolymerization initiator (D), The reactive functional group of the compounds (A), (B) and (C) is any one of a (meth)acryloyl group, an epoxy group and an oxetane group, In the total solid content of the curable resin composition, the content ratio of the compound (A) is 30 to 60% by mass, the content ratio of the compound (B) is 30 to 60% by mass, and the content ratio of the compound (C) is 10 to 25% by mass. The thickness of the cured film is 3 to 20 μm.
2. The optical film according to claim 1, characterized in that: The transparent substrate is any one of an acrylic substrate, a triacetyl cellulose substrate, a cycloolefin polymer substrate, a cycloolefin copolymer substrate, a polyethylene terephthalate substrate, a polycarbonate substrate, a polyimide-based substrate, and a polyamide-based substrate. The optical film according to claim 1 or 2, which is a protective film for a polarizing plate. A polarizing plate comprising the optical film according to claim 1 or 2. 5 . An image display device comprising the optical film according to claim 1 .