Electrochemical device and method for manufacturing electrochemical device

By using activated carbon as the positive electrode material in the winding electrochemical equipment and adopting specific winding processes and structural design, the rewinding problem caused by electrolyte impregnation is solved, the yield and reliability of the equipment are improved, and the electrode is ensured. The stability of the distance and the performance of the distance.

CN118946943APending Publication Date: 2024-11-12PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029925.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing winding electrochemical equipment is prone to rolling back after the electrolyte is impregnated, resulting in a deviation between electrode distances, an increase in internal resistance and a deviation in performance, making it difficult to manufacture at high yield and insufficient reliability.

Method used

The winding body structure including activated carbon as the positive electrode material, the belt-shaped negative electrode and the belt-shaped diaphragm is adopted. The winding body is formed by a specific winding shaft clamping and rotating process to ensure that the positive electrode and the negative electrode face each other and the diaphragm is placed on the diaphragm. The upper reinforcement area is wound several times to prevent winding from being offset and slack.

Benefits of technology

A winding electrochemical device with high reliability is achieved with high yield, which suppresses diaphragm deterioration and electrode distance deviation, and improves the stability and performance of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946943A_ABST
    Figure CN118946943A_ABST
Patent Text Reader

Abstract

The disclosed electrochemical device is provided with a wound body (1) comprising a belt-shaped positive electrode (2) containing activated carbon as a positive electrode active material, a belt-shaped negative electrode (3), and a belt-shaped separator (4). The winding body (1) comprises a winding shaft part (1a) formed by being clamped by a winding shaft and a winding part (1b) connected with the winding shaft part (1a). The winding shaft portion (1a) includes a portion of one end side of the negative electrode (3) and a portion of one end side of the separator (4). In a wound body (1), a positive electrode (2), a negative electrode (3), and a separator (4) are wound such that both surfaces of the positive electrode (2) face the negative electrode (3).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an electrochemical device and a method for manufacturing an electrochemical device. Background Art

[0002] As an example of an electrochemical device, a double-layer capacitor has a long life, can be quickly charged, and has excellent output characteristics. Therefore, double-layer capacitors are widely used in backup power supplies, etc. Examples of electrochemical devices include wound electrochemical devices and stacked electrochemical devices. In the past, various wound-type power storage devices have been proposed.

[0003] Patent document 1 (Japanese Patent Publication No. 2017-188541) discloses the following: "A method for manufacturing a capacitor, the capacitor having a capacitor element in which an anode foil and a cathode foil are stacked and a separator is wound, the manufacturing method being characterized by comprising the following processing: forming a support portion that supports the anode foil by integrating the anode foil with the separator, and winding the anode foil, the cathode foil, and the separator while applying a tensile force to the wound separator through the support portion to the anode foil."

[0004] Patent document 2 (Japanese Patent Publication No. 2020-188193) discloses the following: “A wound capacitor comprising a capacitor element and an outer casing for housing the capacitor element in a state impregnated with an electrolyte, the wound capacitor being characterized in that the capacitor element has a wound body and an element fixing tape, the wound body being formed by winding an electrode foil as an anode and an electrode foil as a cathode via a sheet-like diaphragm, the element fixing tape being wound around the outer circumference of the wound body to maintain the wound state of the electrode foil as the anode, the electrode foil as the cathode, and the diaphragm, at one end of the element fixing tape, in the electrode foil as the anode and the electrode foil as the cathode, the terminal end face of the electrode foil arranged radially inwardly of the wound body and the starting end face of the element fixing tape at the beginning of the winding are arranged opposite to each other in the winding direction of the wound body, and the other end is fixed to the surface of the element fixing tape.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2017-188541

[0008] Patent Document 2: Japanese Patent Application Publication No. 2020-188193 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] Currently, a wound electrochemical device that can be manufactured with high yield and has high reliability is sought. Under such circumstances, one of the objects of the present disclosure is to provide a wound electrochemical device that can be manufactured with high yield and has high reliability.

[0011] In an electrochemical device including a wound body, the wound body sometimes cannot maintain the state when the device is manufactured and becomes loose (winding up). In particular, when the wound body expands due to the immersion of the electrolyte, it is easy to wind up. When the wound body winds up, the distance between the electrodes deviates. As a result, problems such as an increase in internal resistance and an increase in performance deviation occur.

[0012] Therefore, an electrochemical device that is not prone to winding up of a wound body is currently sought. One of the objectives of the present disclosure is to provide an electrochemical device that is not prone to winding up of a wound body.

[0013] The novel features of the present invention are described in the appended claims, but the present invention, both in structure and content, as well as other objects and features of the present invention, will be further understood through the following detailed description with reference to the accompanying drawings.

[0014] Means used to solve problems

[0015] One aspect disclosed relates to a first method for manufacturing an electrochemical device. The electrochemical device includes a wound body, the wound body consisting of a strip-shaped positive electrode containing activated carbon as a positive electrode material, a strip-shaped negative electrode, and a strip-shaped separator disposed between the positive electrode and the negative electrode, the first manufacturing method sequentially comprising: step (i), clamping a portion of one end side of the negative electrode and a portion of one end side of the separator by a first winding shaft and a second winding shaft; and step (ii), in a state where the first winding shaft and the second winding shaft clamp the portion of the negative electrode and the portion of the separator, rotating the first winding shaft and the second winding shaft to wind up the positive electrode, the negative electrode, and the separator, thereby forming the wound body, wherein in step (ii), the positive electrode, the negative electrode, and the separator are wound so that both sides of the positive electrode face the negative electrode.

[0016] One aspect disclosed relates to a first electrochemical device. The first electrochemical device includes a wound body, the wound body including a strip-shaped positive electrode containing activated carbon as a positive electrode active material, a strip-shaped negative electrode, and a strip-shaped separator arranged between the positive electrode and the negative electrode, wherein the wound body includes a winding shaft portion formed by being clamped by a winding shaft and a winding portion connected to the winding shaft portion, the winding shaft portion includes a portion of one end side of the negative electrode and a portion of one end side of the separator, and in the wound body, the positive electrode, the negative electrode, and the separator are wound so that both sides of the positive electrode are opposite to the negative electrode.

[0017] One aspect of the disclosure relates to a second manufacturing method of an electrochemical device. The electrochemical device includes a wound body, which is composed of a strip-shaped positive electrode containing activated carbon as a positive electrode material, a strip-shaped negative electrode, and a strip-shaped separator disposed between the positive electrode and the negative electrode. In this second manufacturing method,

[0018] The separator includes a strip-shaped first separator and a strip-shaped second separator.

[0019] The manufacturing method sequentially includes:

[0020] Step (I), only a part of one end side of the first separator and the second separator is clamped by a winding shaft; and

[0021] Step (II), maintaining the state of Step (I), directly rotating the winding shaft, and winding the positive electrode, the negative electrode, the first separator, and the second separator to form the wound body.

[0022] The winding shaft is composed of a first winding shaft and a second winding shaft having a semi-circular cross-section, and the semi-circular cross-section has a diameter with a length A.

[0023] The first separator has an average thickness T1.

[0024] The second separator has an average thickness T2.

[0025] In Step (II),

[0026] (a) The distance B between one end of the negative electrode on the winding shaft side and the winding shaft and the length A satisfy πA < B, and

[0027] (b) The winding is performed under the condition that the distance C between one end of the positive electrode on the winding shaft side and one end of the negative electrode, the length A, the average thickness T1, and the average thickness T2 satisfy π(A + (T1 + T2) × 2n) < C (where n is the number of turns of only the first separator and the second separator).

[0028] One aspect of the disclosure relates to a second electrochemical device. This second electrochemical device includes a wound body, which is composed of a strip-shaped positive electrode containing activated carbon as a positive electrode active material, a strip-shaped negative electrode, and a strip-shaped separator disposed between the positive electrode and the negative electrode. Among them,

[0029] The separator includes a strip-shaped first separator and a strip-shaped second separator.

[0030] The wound body includes a winding shaft portion formed by being clamped by a winding shaft and a winding portion connected to the winding shaft portion.

[0031] The winding shaft portion is composed of the first diaphragm and the second diaphragm,

[0032] The winding shaft portion includes a first end portion as a boundary with the winding portion and a second end portion on the opposite side of the first end portion.

[0033] The winding portion includes a reinforcing portion, wherein only the first separator and the second separator are wound around the reinforcing portion for one or more times between the first end portion and one end of the negative electrode on the winding axis side.

[0034] In the wound body, a surface of the positive electrode on the winding axis side faces the negative electrode.

[0035] One aspect disclosed relates to a third electrochemical device. The third electrochemical device includes a wound body, the wound body comprising a strip-shaped first electrode, a strip-shaped second electrode, and a strip-shaped separator disposed at least between the first electrode and the second electrode, the outermost periphery of the second electrode being disposed outside the outermost periphery of the first electrode, the vicinity of the outer peripheral end of the second electrode being bent and the outer peripheral end of the second electrode being in contact with the separator.

[0036] Effects of the Invention

[0037] According to one aspect of the present disclosure, a wound electrochemical device that can be manufactured with high yield and has high reliability can be obtained. According to another aspect of the present invention, an electrochemical device in which the wound body is less likely to unwind can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1A This is a cross-sectional view schematically showing one step of the manufacturing method according to the first embodiment.

[0039] Figure 1B yes Figure 1A Top view of the .

[0040] Figure 2 This is a cross-sectional view schematically showing an example of a wound body produced by the production method of the first embodiment.

[0041] Figure 3 This is a partially exploded perspective view schematically showing the electrochemical device according to the first embodiment.

[0042] Figure 4A This is a cross-sectional view schematically showing one step of the manufacturing method of the second embodiment.

[0043] Figure 4B yes Figure 4A Top view of the .

[0044] Figure 5This is a cross-sectional view schematically showing an example of a wound body produced by the production method of the second embodiment.

[0045] Figure 6 This is a partially exploded perspective view schematically showing the electrochemical device according to the second embodiment.

[0046] Figure 7 This is a cross-sectional view schematically showing a part of an example of a wound body used in the electrochemical device of the third embodiment.

[0047] Figure 8 This is a diagram schematically showing one step of an example of a method for producing a wound body.

[0048] Fig. 9 This is a partially exploded perspective view schematically showing an example of an electrochemical device according to the third embodiment. DETAILED DESCRIPTION

[0049] In the following, embodiments of the present disclosure are illustrated, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values ​​and materials are sometimes illustrated, but other numerical values ​​and other materials can also be applied as long as the invention of the present disclosure can be implemented. In this specification, the record of "numerical value A to numerical value B" includes numerical value A and numerical value B, which can be read as "above numerical value A and below numerical value B". In the following description, when the lower limit and upper limit of numerical values ​​related to specific physical properties or conditions are illustrated, as long as the lower limit is not above the upper limit, any combination of the illustrated lower limits and the illustrated upper limits can be performed.

[0050] Hereinafter, the electrochemical devices (D1), (D2) and (D3) will be described. As long as no technical contradiction occurs, at least a part of the structure of each of the electrochemical devices (D1), (D2) and (D3) may be combined.

[0051] (First method for manufacturing an electrochemical device)

[0052] The first manufacturing method of the present embodiment is a method for manufacturing an electrochemical device, which includes a winding body composed of a strip-shaped positive electrode containing activated carbon as a positive electrode material, a strip-shaped negative electrode, and a strip-shaped separator arranged between the positive electrode and the negative electrode. The first manufacturing method is sometimes referred to as "manufacturing method (M1)" hereinafter. Manufacturing method (M1) includes steps (i) and (ii) in sequence. These steps are described below.

[0053] Step (i) is a step of sandwiching a portion of one end side of the negative electrode and a portion of one end side of the separator by the first winding shaft and the second winding shaft. The first winding shaft and the second winding shaft are not limited, as long as they are members that serve as winding shafts when forming the wound body. For example, the first winding shaft and the second winding shaft are rod-shaped bodies with semicircular cross-sections.

[0054] In addition, the separator may include a first separator and a second separator. In this case, step (i) may be a process in which a portion of one end side of the negative electrode, a portion of one end side of the first separator, and a portion of one end side of the second separator are clamped by the first winding shaft and the second winding shaft. In this case, the negative electrode may be clamped between the first separator and the second separator. Alternatively, step (i) may be a process in which a portion of one end side of the negative electrode and a portion of one end side of the first separator are clamped by the first winding shaft and the second winding shaft. In addition, the strip-shaped separator may be bent and two sheets may be overlapped, and the two overlapping separators may be used as the first separator and the second separator.

[0055] Step (ii) is a step of winding the positive electrode, the negative electrode and the separator by rotating the first winding shaft and the second winding shaft in a state where a portion of the negative electrode and a portion of the separator are clamped by the first winding shaft and the second winding shaft to form the above-mentioned wound body. In step (ii), the positive electrode, the negative electrode and the separator are wound in a manner such that both sides of the positive electrode face the negative electrode.

[0056] The winding of step (ii) is performed while maintaining the state of step (i) (i.e., a state in which a portion of the negative electrode and a portion of the separator are sandwiched by the first winding axis and the second winding axis). In addition, the positive electrode, the negative electrode, and the separator are wound during the winding to form a wound body composed of them.

[0057] The positive electrode, the negative electrode, and the separator can be wound in such a manner that both sides of the positive electrode face the negative electrode, for example, as follows. For the portion close to the winding axis, firstly only the negative electrode and the separator are wound without the positive electrode, and then the positive electrode, the negative electrode, and the separator are wound together. Next, for the peripheral portion of the wound body, they are wound in such a manner that the negative electrode is arranged on the outside of the positive electrode. By doing so, the wound body can be formed in such a manner that both sides of the positive electrode face the negative electrode.

[0058] In the manufacturing method (M1), the negative electrode and the separator are wound together on the winding axis, so that the winding deviation of the negative electrode can be prevented. Therefore, according to the manufacturing method (M1), a highly reliable wound electrochemical device can be manufactured with a high yield.

[0059] In the manufacturing method (M1), a winding body is formed in such a manner that both sides of the positive electrode are opposite to the negative electrode. According to this structure, degradation of the diaphragm can sometimes be suppressed. In the case where a part of the positive electrode has a portion that is not opposite to the negative electrode (non-opposite portion), hydrogen ions (H+) generated at the positive electrode are difficult to diffuse, and thus a local acidic atmosphere is formed in this portion. In an acidic atmosphere, the diaphragm undergoes a dehydration reaction, and water is generated in the battery cell, causing rapid degradation of the battery cell. According to the manufacturing method (M1), a winding body in which the non-opposite portion of the positive electrode does not exist can be manufactured, and thus these problems can be suppressed.

[0060] In the manufacturing method (M1), in step (i), a portion of the above-mentioned one end side of the negative electrode and a portion of the above-mentioned one end side of the separator can be clamped by the first winding shaft and the second winding shaft, so that one end of the negative electrode protrudes from between the first winding shaft and the second winding shaft. According to this structure, since the negative electrode is bent twice at the winding shaft portion, the winding deviation can be particularly suppressed. In this case, a portion of the one end side of the negative electrode and a portion of the one end side of the separator can be clamped by the first winding shaft and the second winding shaft, so that one end of the negative electrode and one end of the separator protrude from between the first winding shaft and the second winding shaft.

[0061] In the manufacturing method (M1), in the step (i), the positive electrode does not need to be sandwiched between the first winding axis and the second winding axis. According to this structure, both surfaces of the positive electrode can be completely opposed to the negative electrode.

[0062] Through the above steps, a winding body can be formed. As needed, the obtained winding body is sealed in an outer body together with an electrolyte. In addition, as needed, before or after the production of the winding body, a lead is connected to the positive electrode and / or the negative electrode. By doing so, an electrochemical device is obtained. The electrochemical device can be used as a power storage device.

[0063] (Electrochemical Equipment)

[0064] The first electrochemical device of the present embodiment includes a wound body, which is composed of a strip-shaped positive electrode containing activated carbon as a positive electrode active material, a strip-shaped negative electrode, and a strip-shaped separator arranged between the positive electrode and the negative electrode. The first electrochemical device is sometimes referred to as "electrochemical device (D1)" below. The electrochemical device (D1) can be manufactured using the manufacturing method (M1), but can also be manufactured using a manufacturing method other than the manufacturing method (M1). Since the matters described about the manufacturing method (M1) can be applied to the electrochemical device (D1), repeated descriptions are sometimes omitted. In addition, the matters described about the electrochemical device (D1) can be applied to the manufacturing method (M1).

[0065] In the electrochemical device (D1), the winding body includes a winding shaft portion formed by being clamped by winding shafts (e.g., two winding shafts), and a winding portion connected to the winding shaft portion. The winding shaft portion includes a portion of one end side of the negative electrode and a portion of one end side of the separator. In the winding body, the positive electrode, the negative electrode, and the separator are wound in such a manner that the two sides of the positive electrode are opposite to the negative electrode.

[0066] When the winding shaft includes a first winding shaft and a second winding shaft, the winding shaft portion is a portion sandwiched by the first winding shaft and the second winding shaft when manufacturing the winding body. In one example, the winding shaft portion is configured to divide the cylindrical space existing in the center of the winding body into two semi-cylindrical spaces.

[0067] In the electrochemical device (D1), the negative electrode and the separator are bent at the boundary between the winding shaft and the winding portion. Therefore, in the electrochemical device (D1), the occurrence of winding deviation or loosening of the winding body can be suppressed. Therefore, the electrochemical device (D1) can be manufactured with high yield and high reliability.

[0068] In the electrochemical device (D1), the winding body may further include a protrusion connected to the winding shaft portion on the opposite side of the winding portion. The protrusion may include the above-mentioned one end of the negative electrode. Alternatively, the protrusion may include the above-mentioned one end of the negative electrode and the above-mentioned one end of the separator. According to these structures, since the negative electrode is bent twice before and after the protrusion, the winding body can be particularly suppressed from loosening.

[0069] In the electrochemical device (D1), the winding axis portion may not include the positive electrode. According to this structure, both surfaces of the positive electrode can be completely opposed to the negative electrode.

[0070] The following describes examples of the structure and structural members of the electrochemical device (D1). As structural members other than the characteristic portions of the present disclosure, known structural members can be applied.

[0071] The electrochemical device (D1) includes a winding body, for example, a cylindrical shape. The electrochemical device (D1) can be an electric double layer capacitor (EDLC) or a storage device other than this (for example, a lithium ion capacitor). When the electrochemical device (D1) is an electric double layer capacitor, polarized electrodes can be used for the positive and negative electrodes. The polarized electrode contains an electrode material (active substance) capable of adsorbing and desorbing ions. Charging and discharging are performed by adsorbing and desorbing ions by the electrode material. When the electrochemical device (D1) is a lithium ion capacitor, a polarized electrode can be used as the positive electrode, and a non-polarized electrode can be used as the negative electrode. The negative electrode used in lithium ion secondary batteries can be used as the negative electrode of the non-polarized electrode. Examples of such negative electrodes include negative electrode active materials (for example, graphite) capable of absorbing and releasing lithium ions.

[0072] (Second method for manufacturing an electrochemical device)

[0073] The second manufacturing method of the present embodiment is a manufacturing method of an electrochemical device including a wound body, which is composed of a strip-shaped positive electrode containing activated carbon as a positive electrode material, a strip-shaped negative electrode, and a strip-shaped separator disposed between the positive electrode and the negative electrode. Hereinafter, this second manufacturing method may sometimes be referred to as "manufacturing method (M2)". The separator includes a strip-shaped first separator and a strip-shaped second separator. The manufacturing method (M2) sequentially includes step (I) and step (II). These steps will be described below.

[0074] Step (I) is a step of clamping only a part of one end side of the first separator and the second separator by a winding shaft. The winding shaft is composed of a first winding shaft and a second winding shaft. Both the first winding shaft and the second winding shaft have a semi-circular cross section (for example, a cross section that is half of a perfect circle), and the semi-circle has a diameter of length A (mm).

[0075] Step (II) is a step of winding the positive electrode, the negative electrode, and the first separator and the second separator while maintaining the state of step (I) to form the above-mentioned wound body.

[0076] The strip-shaped first separator has an average thickness T1 (mm). The strip-shaped second separator has an average thickness T2 (mm). In addition, the strip-shaped separator can be bent and two sheets can be overlapped, and the two overlapped sheets of the separator can be used as the first separator and the second separator.

[0077] In an example of the manufacturing method (M2), winding is performed in step (II) in a manner that satisfies the following conditions (a) and (b).

[0078] (a) The distance B (mm) between one end of the negative electrode on the winding shaft side and the winding shaft and the length A satisfy πA < B.

[0079] (b) The distance C (mm) between one end of the positive electrode on the winding shaft side and one end of the negative electrode, the length A, the average thickness T1, and the average thickness T2 satisfy π(A + (T1 + T2) × 2n) < C (where n is the number of turns of only winding the first separator and the second separator). More specifically, n is the number of turns of only winding the first separator and the second separator on the winding shaft side, and is the number of turns of the first separator and the second separator in the part that becomes the reinforcing portion.

[0080] In another example of the manufacturing method (M2), in step (II), winding is performed in a manner that satisfies the following conditions (a') and (b').

[0081] (a') After winding the first separator and the second separator one or more times, start winding the negative electrode.

[0082] (b') The surface of the positive electrode on the winding shaft portion side faces the negative electrode.

[0083] When the condition (a) or (a') is satisfied, the negative electrode does not contact the winding axis. Therefore, damage to the negative electrode can be suppressed. As a result, a highly reliable electrochemical device can be manufactured with a high yield.

[0084] By satisfying condition (b) or (b'), on the winding axis side, it is possible to prevent a portion of the positive electrode from becoming a portion that is not opposite to the negative electrode (non-opposite portion). According to this structure, degradation of the diaphragm can sometimes be suppressed. In the case where a portion of the positive electrode has a non-opposite portion that is not opposite to the negative electrode, in the non-opposite portion, negative ions are adsorbed and gathered near the positive electrode during charging, and on the other hand, since there is no negative electrode to adsorb positive ions, the positive ions gather in the diaphragm, destroying the ion balance. As a result, the diaphragm may be carbonized. According to the manufacturing method (M2), a winding body in which a non-opposite portion of the positive electrode is not present can be manufactured, so these problems can be suppressed.

[0085] In one example of step (II), first, a stacked structure of "first separator / second separator" is wound, then a stacked structure of "first separator / negative electrode / second separator" is wound, and then a stacked structure of "first separator / negative electrode / second separator / positive electrode" is wound.

[0086] In the step (II), winding may be performed so as to satisfy the following condition (c) or (c').

[0087] (c) The distance B and length A satisfy 2πA <B。

[0088] (c') After only the first separator and the second separator are wound for two or more times, winding of the negative electrode is started.

[0089] By satisfying the condition (c) or (c'), the portion of the winding body where only the separator is wound (the portion on the central side of the winding body) can be strengthened. Therefore, when the winding shaft is pulled out after the winding is completed, a short circuit caused by the breakage of the separator can be suppressed. The distance B and the length A can satisfy B≤3πA. That is, the number of turns of only the first separator and the second separator can be three or less.

[0090] In step (II), a winding body can be formed in a manner that the two sides of the positive electrode are opposite to the negative electrode. According to this structure, the degradation of the separator can be particularly suppressed. As described above, by satisfying condition (b) or (b'), the two sides of the positive electrode close to the winding axis are opposite to the negative electrode. For the peripheral portion of the winding body, they are wound in a manner that the negative electrode is arranged on the outside of the positive electrode. By doing so, a winding body can be formed in a manner that the two sides of the positive electrode are opposite to the negative electrode.

[0091] In step (I), only the first diaphragm and the second diaphragm can be clamped by the winding shaft so that the first diaphragm and the second diaphragm protrude from between the first winding shaft and the second winding shaft. According to this structure, since the diaphragm is bent twice before and after the winding shaft, the winding deviation of the diaphragm can be suppressed. Therefore, a more reliable electrochemical device can be manufactured with a higher yield.

[0092] Through the above steps, a winding body can be formed. As needed, the obtained winding body is sealed in an outer body together with an electrolyte. In addition, as needed, before or after the production of the winding body, a lead is connected to the positive electrode and / or the negative electrode. By doing so, an electrochemical device is obtained. The electrochemical device can be used as a power storage device.

[0093] (Electrochemical Equipment)

[0094] The second electrochemical device of this embodiment includes a wound body, which is composed of a strip-shaped positive electrode containing activated carbon as a positive electrode active material, a strip-shaped negative electrode, and a strip-shaped separator arranged between the positive electrode and the negative electrode. The second electrochemical device is sometimes referred to as "electrochemical device (D2)" below. The electrochemical device (D2) can be manufactured using the manufacturing method (M2). Since the matters described about the manufacturing method (M2) can be applied to the electrochemical device (D2), repeated descriptions are sometimes omitted. In addition, the matters described about the electrochemical device (D2) can be applied to the manufacturing method (M2).

[0095] The diaphragm includes a first diaphragm in the form of a strip and a second diaphragm in the form of a strip. The winding body includes a winding shaft portion formed by clamping a winding shaft and a winding portion connected to the winding shaft portion. The winding shaft portion is composed only of the first diaphragm and the second diaphragm. The winding shaft portion includes a first end portion as a boundary with the winding portion and a second end portion on the opposite side of the first end portion. The winding portion includes a reinforcing portion that only winds the first diaphragm and the second diaphragm for more than one cycle between the first end portion and one end portion on the winding shaft portion side of the negative electrode. In the winding body, the surface of the positive electrode on the winding shaft portion side is opposite to the negative electrode.

[0096] The winding shaft portion is formed by being sandwiched between the first winding shaft and the second winding shaft. In one example, the winding shaft portion is arranged so as to divide a cylindrical space existing in the center of the winding body into two semi-cylindrical spaces.

[0097] According to the electrochemical device (D2), the effects obtained by satisfying the above conditions (a) (or (a')) and (b) (or (b')) can be obtained. Therefore, the electrochemical device (D2) can be manufactured with high yield and has high reliability.

[0098] In the reinforcement portion of the electrochemical device (D2), only the first separator and the second separator may be wound two or more times.

[0099] In the electrochemical device (D2), both sides of the positive electrode may face the negative electrode.

[0100] The wound body of the electrochemical device (D2) may be composed of only the first separator and the second separator, and include a protrusion protruding from the second end portion.

[0101] Hereinafter, examples of the structure and structural members of the electrochemical device (D2) will be described. As structural members other than the characteristic portions of the present disclosure, known structural members can be applied.

[0102] The electrochemical device (D2) includes a winding body, for example, a cylindrical shape. The electrochemical device (D2) may be an electric double layer capacitor (EDLC) or an electrical storage device other than this (for example, a lithium ion capacitor). When the electrochemical device (D2) is an electric double layer capacitor, polarized electrodes can be used for the positive and negative electrodes. The polarized electrode contains an electrode material (active substance) capable of adsorbing and desorbing ions. Charging and discharging are performed by adsorbing and desorbing ions by the electrode material. When the electrochemical device (D2) is a lithium ion capacitor, a polarized electrode can be used as the positive electrode, and a non-polarized electrode can be used as the negative electrode. The negative electrode used in a lithium ion secondary battery can be used as the negative electrode of the non-polarized electrode. Examples of such negative electrodes include negative electrode active materials (for example, graphite) capable of absorbing and releasing lithium ions.

[0103] (Third Electrochemical Device)

[0104] Hereinafter, the third electrochemical device of the present embodiment is sometimes referred to as "electrochemical device (D3)". The electrochemical device (D3) of the present embodiment includes a wound body, which is composed of a strip-shaped first electrode, a strip-shaped second electrode, and a strip-shaped separator arranged at least between the first electrode and the second electrode. The outermost periphery of the second electrode is arranged outside the outermost periphery of the first electrode. The vicinity of the outer peripheral end of the second electrode is bent so that the outer peripheral end of the second electrode abuts against the separator. The outer peripheral end of the second electrode is sometimes referred to as "outer peripheral end (E2)" hereinafter.

[0105] According to the above structure, the outer peripheral end (E2) abuts against the surface of the diaphragm. As a result, the positional deviation between the outer peripheral end (E2) and the diaphragm is suppressed, and the winding body is suppressed. This structure can be achieved by bending the vicinity of the outer peripheral end (E2) of the second electrode. Therefore, compared with the method of fixing the outer periphery of the winding body with tape, this method can easily implement the process at a low cost.

[0106] There is no particular limitation on the polarity of the first electrode and the second electrode. For example, the first electrode may be a positive electrode and the second electrode may be a negative electrode, or the first electrode may be a negative electrode and the second electrode may be a positive electrode. Alternatively, the first electrode may be an anode and the second electrode may be a cathode, or the first electrode may be a cathode and the second electrode may be an anode. Alternatively, the first electrode and the second electrode may have an undefined polarity. As described below, the separator generally includes a first separator and a second separator.

[0107] The following describes the first and second examples of the method for bending the outer peripheral end (E2). In the first example, the vicinity of the outer peripheral end (E2) of the second electrode is bent toward the inside of the winding body, and the outer peripheral end (E2) abuts against the separator existing on the inner side of the outer peripheral end (E2). The vicinity of the outer peripheral end (E2) is bent toward the inside, so that the separator can be pressed by the bent surface that abuts against the separator, thereby suppressing the distance between the electrodes ( Figure 7 By reducing the deviation of the distance between the first electrode 2 and the second electrode 3), it is possible to suppress the deviation of the resistance value which is a characteristic of the device and stabilize the resistance value.

[0108] In the first example, two diaphragms (a first diaphragm and a second diaphragm) are preferably stacked on the inner side of the peripheral end (E2). From another point of view, it is preferred that the peripheral end (E2) is opposite to the second electrode on the inner side through the diaphragm. According to this structure, it is possible to prevent the peripheral end (E2) from damaging the diaphragm and causing a short circuit between the first electrode and the second electrode.

[0109] The second example can be adopted when there is a diaphragm on the outside of the peripheral end (E2) of the second electrode. In the second example, the vicinity of the peripheral end (E2) of the second electrode is bent toward the outside of the winding body, and the peripheral end (E2) abuts against the diaphragm present on the outside of the peripheral end (E2). By bending the vicinity of the peripheral end (E2) toward the outside, the above-mentioned effect (stabilization of the resistance value) can be obtained. In addition, when the vicinity of the peripheral end (E2) is bent toward the outside, even if the peripheral end (E2) breaks through the diaphragm, the peripheral end (E2) does not contact the first electrode. Therefore, the short circuit between the first electrode and the second electrode can be further suppressed.

[0110] Typically, the first electrode includes a first current collector and a first composite layer formed on both sides of the first current collector, and the second electrode includes a second current collector and a second composite layer formed on both sides of the second current collector. In the electrochemical device (D3), the second current collector can be exposed at the end face of the peripheral end while being clamped by the second composite layer. By exposing the second current collector to the end face, the second current collector and the diaphragm are not easily offset. In addition, since the second current collector is clamped by the composite layer, the edge of the second current collector is properly protected, which can prevent the diaphragm from being damaged by the edge of the second current collector.

[0111] The position of the bent portion (bend portion) of the second electrode can be located at a distance of more than 0.01 mm, more than 0.1 mm, or more than 0.2 mm from the outer peripheral end (E2) of the second electrode. The position of the bend portion can be within a range of less than 0.5 mm or less than 0.3 mm from the outer peripheral end (E2) of the second electrode. For example, the bent portion (bend portion) of the second electrode may exist in a range of 0.01 mm to 0.5 mm (for example, a range of 0.1 mm to 0.5 mm) from the outer peripheral end (E2) of the second electrode. According to this structure, the effect of preventing the winding body from winding back is particularly high. In addition, these distances are distances measured along the length direction of the electrode.

[0112] The second electrode is bent at an angle α (refer to Figure 8 ) is 90° or less. Angle α may be 5° or more, 15° or more, or 30° or more. Angle α may be 90° or less, 60° or less, 45° or less, or 30° or less. Angle α may be in the range of 15 to 60°, in the range of 30 to 60°, or in the range of 15 to 45°.

[0113] In the electrochemical device (D3), the vicinity of the outer peripheral end of the first electrode (hereinafter sometimes referred to as "outer peripheral end (E1)") may be bent so that the outer peripheral end (E1) of the first electrode abuts against the separator. According to this structure, the deviation of the first electrode and the separator can be suppressed. Therefore, the winding back of the wound body can be particularly suppressed.

[0114] The direction in which the outer peripheral end (E1) of the first electrode is bent may be inward or outward. The direction in which the outer peripheral end (E1) of the first electrode is bent may be the same as or different from the direction in which the outer peripheral end (E2) of the second electrode is bent (inward or outward).

[0115] Hereinafter, examples of the structure and structural members of the electrochemical device (D3) will be described. As structural members other than the characteristic portions of the present disclosure, known structural members can be applied.

[0116] The electrochemical device (D3) includes a winding body, for example, in a cylindrical shape. The electrochemical device (D3) may be an electric double layer capacitor (EDLC) or a storage device other than this (for example, a lithium ion capacitor). Alternatively, the electrochemical device may be another capacitor or a battery. The first electrode and the second electrode of the electrochemical device (D3) may use electrodes corresponding to the device, or may use known electrodes corresponding to the device.

[0117] In the case where the electrochemical device (D3) is a double-layer capacitor, the positive electrode and the negative electrode can use polarized electrodes. The polarized electrode contains an electrode material (active material) that can adsorb and desorb ions. Charging and discharging are carried out by adsorbing and desorbing ions by the electrode material. In the case where the electrochemical device (D3) is a lithium ion capacitor, a polarized electrode can be used as the positive electrode, and a non-polarized electrode can be used as the negative electrode. The negative electrode used in a lithium ion secondary battery can be used as the negative electrode of the non-polarized electrode. Examples of such negative electrodes include negative electrode active materials (such as graphite) that can absorb and release lithium ions.

[0118] Hereinafter, examples of components when the electrochemical devices (D1) and (D2) are double-layer capacitors will be described. When the electrochemical devices (D1) and (D2) are electrochemical devices other than double-layer capacitors, electrodes, separators, and electrolytes can be selected according to their types.

[0119] (positive electrode)

[0120] The positive electrode (positive electrode plate) includes a strip-shaped positive electrode current collector and positive electrode mixture layers disposed on both sides of the positive electrode current collector. The positive electrode mixture layers contain activated carbon as a positive electrode material (active material).

[0121] The positive electrode mixture layer contains activated carbon as a positive electrode material as an essential component. The positive electrode material may contain carbon materials other than activated carbon. Examples of such carbon materials include carbon nanotubes, graphite, graphene, etc. As raw materials for activated carbon, for example, wood, coconut shells, pulp waste, coal or coal-based asphalt obtained by thermal decomposition thereof, heavy oil or petroleum-based asphalt obtained by thermal decomposition thereof, phenolic resin, petroleum coke, coal coke, etc. can be cited. The activated carbon is preferably activated carbon after activation treatment.

[0122] The positive electrode mixture layer may contain other components in addition to the positive electrode material (active material). Examples of other components include a binder, a conductive material, etc. As a binder, resin materials such as polytetrafluoroethylene (PTFE), carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), etc. are used. As a conductive material, carbon black (such as acetylene black, etc.) is used.

[0123] The positive electrode current collector can use a strip of metal foil (e.g., aluminum foil). The thickness of the positive electrode current collector is not particularly limited. The thickness of the positive electrode current collector of the electrochemical device (D1) can be in the range of 10 μm to 50 μm (e.g., in the range of 15 μm to 30 μm). The thickness of the positive electrode current collector of the electrochemical device (D2) can be in the range of 10 μm to 50 μm (e.g., in the range of 20 μm to 30 μm). The surface of the positive electrode current collector can be roughened by etching or the like (the same applies to the negative electrode current collector).

[0124] (negative electrode)

[0125] The negative electrode (negative electrode plate) comprises a strip-shaped negative electrode current collector and a negative electrode mixture layer disposed on both sides of the negative electrode current collector. The negative electrode mixture layer comprises a negative electrode material (active substance). The negative electrode material comprises a negative electrode material (active substance) capable of adsorbing and desorbing ions. Examples of negative electrode materials include carbon materials, and the carbon materials exemplified as positive electrode materials can be used. Specifically, activated carbon, hard carbon, carbon nanotubes, graphite, graphene, etc. can be used as negative electrode materials.

[0126] The negative electrode mixture layer may contain other components in addition to the negative electrode material (active material). Examples of other components include a binder and a conductive material. The binder and the conductive material may be the same as those exemplified as the binder and the conductive material of the positive electrode.

[0127] The negative electrode current collector may be a strip of metal foil (e.g., aluminum foil). The thickness of the negative electrode current collector is not particularly limited. The thickness of the negative electrode current collector of the electrochemical device (D1) may be in the range of 5 μm to 50 μm (e.g., in the range of 5 μm to 20 μm). The thickness of the negative electrode current collector of the electrochemical device (D2) may be in the range of 10 μm to 50 μm (e.g., in the range of 20 μm to 30 μm).

[0128] The formation method of the above-mentioned electrodes (positive electrode and negative electrode) is not limited and can be formed by a known method. For example, the composite layer can be formed by the following method. First, a slurry is prepared by mixing an electrode material (active substance), a binder and / or a conductive material and a dispersion medium. Next, the obtained slurry is applied to the surface of a collector to form a coating. Next, the coating is dried and rolled to form a composite layer on the surface of the collector. By doing so, a composite layer is formed.

[0129] (Diaphragm)

[0130] The separator is arranged between the positive electrode and the negative electrode to prevent a short circuit between the positive electrode and the negative electrode. Examples of materials for the separator include insulating resins, glass, etc. Examples of separators include non-woven fabrics with cellulose as the main component, glass fiber mats, microporous films of polyolefins such as polyethylene, etc. The separator can use a known separator used in a double-layer capacitor or a lithium ion capacitor.

[0131] The thickness of the separator of the electrochemical device (D1) is not particularly limited, and may be in the range of 15 μm to 60 μm (eg, in the range of 20 μm to 40 μm).

[0132] The average thicknesses T1 and T2 of the separator of the electrochemical device (D2) are not particularly limited, and may be in the range of 10 μm to 50 μm (eg, in the range of 15 μm to 40 μm), respectively.

[0133] The average thickness of the diaphragm is determined by the following steps. First, a test piece of about 500 mm in length is folded into two layers, and the thickness is measured at five points at equal intervals. The average thickness is calculated by dividing the arithmetic mean of the thicknesses at the five points measured by the number of stacked sheets. Usually, the same diaphragm is used for the first diaphragm and the second diaphragm. In this case, the average thickness T1 of the first diaphragm can be set to the average thickness T2 of the second diaphragm.

[0134] (Electrolyte (electrolyte))

[0135] The electrolyte can use an electrolyte containing a solvent and an ionic substance. Examples of the electrolyte include non-aqueous electrolytes containing a non-aqueous solvent and an ionic substance. The ionic substance is dissolved in the solvent and contains cations and anions. The ionic substance may contain a low melting point compound (ionic liquid) that can exist as a liquid near room temperature. The concentration of the ionic substance in the electrolyte is, for example, 0.5 mol / L or more and 2.0 mol / L.

[0136] The solvent may further include a lactone compound. Examples of lactone compounds include β-propiolactone, γ-butyrolactone, γ-valerolactone, δ-valerolactone, etc. The lactone compound preferably includes γ-butyrolactone (GBL) because it has low viscosity even at low temperatures, is electrochemically stable within the voltage range of the device, and has a low gas release amount.

[0137] The solvent may contain other solvents besides the lactone compound. Examples of other solvents include: chain carboxylic acid esters such as methyl methyl propionate; chain carbonates such as diethyl carbonate; cyclic carbonates such as propylene carbonate; polyols such as ethylene glycol and propylene glycol; cyclic sulfones such as sulfolane; amides such as N-methylacetamide, N,N-dimethylformamide, and N-methyl-2-pyrrolidone; ethers such as 1,4-dioxane; ketones such as methyl ethyl ketone; and formaldehyde. The solvent may contain acetonitrile.

[0138] When the solvent is a mixed solvent of a lactone compound and other solvents, the ratio of the lactone compound to the solvent may be 50% by volume or more and 85% by volume or less.

[0139] Ionic substances include, for example, organic salts. Organic salts are salts in which at least one of anions and cations contains organic matter. As organic salts in which the cation contains organic matter, for example, quaternary ammonium salts can be cited. As organic salts in which the anion (or two ions) contains organic matter, for example, trimethylamine maleate, triethylamine borodisalicylate, ethyl dimethylamine phthalate, 1,2,3,4-tetramethylazo rhenium phthalate and 1,3-dimethyl-2-ethylidazoline phthalate can be cited.

[0140] Anions preferably include anions of fluorinated acids from the viewpoint of improving withstand voltage characteristics. Examples of anions of fluorinated acids include BF4- and / or PF6-. Organic salts preferably include cations of tetraalkylammonium and anions of fluorinated acids, for example. Specifically, examples include diethyldimethylammonium tetrafluoroborate (DEDMABF4), triethylmethylammonium tetrafluoroborate (TEMABF4), and the like.

[0141] In the case where the electrochemical device is a lithium ion capacitor (LIC), the ionic substance includes a lithium salt. The lithium salt is preferably a salt having a fluorine-containing anion. Among the salts having a fluorine-containing anion, at least one selected from the group consisting of LiBF4, LiPF6 and lithium bis(fluorosulfonyl)imide (LiN(SO2F)2) is more preferred. LiN(SO2F)2 is also called LiFSI or LFSI. Among the salts having a fluorine-containing anion, LFSI is less likely to produce by-products and has excellent stability.

[0142] Hereinafter, an example of the components of the electrochemical device (D3) in the case of a double-layer capacitor in which the first electrode is a positive electrode and the second electrode is a negative electrode will be mainly described. When the electrochemical device (D3) is an electrochemical device other than a double-layer capacitor, the electrodes, separators and electrolytes can be selected according to their types.

[0143] (positive electrode)

[0144] The positive electrode (positive electrode plate) includes a strip-shaped positive electrode current collector (first current collector) and positive electrode mixture layers (first mixture layers) disposed on both sides of the positive electrode current collector. The positive electrode mixture layers may contain activated carbon as a positive electrode material (active substance).

[0145] The positive electrode material may include carbon materials other than activated carbon. Such carbon materials include, for example, carbon nanotubes, graphite, graphene, etc. As raw materials for activated carbon, for example, wood, coconut shells, pulp waste, coal or coal-based asphalt obtained by thermal decomposition thereof, heavy oil or petroleum-based asphalt obtained by thermal decomposition thereof, phenolic resin, petroleum coke, coal cola, etc. can be cited. The activated carbon is preferably activated carbon after activation treatment.

[0146] The positive electrode mixture layer may contain other components in addition to the positive electrode material (active material). Examples of other components include a binder, a conductive material, etc. As a binder, resin materials such as polytetrafluoroethylene (PTFE), carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), etc. are used. As a conductive material, carbon black (such as acetylene black, etc.) is used.

[0147] The positive electrode current collector can be a strip of metal foil (e.g., aluminum foil). The thickness of the current collector is not particularly limited and can be in the range of 10 μm to 100 μm (e.g., 15 μm to 40 μm). The surface of the positive electrode current collector can be roughened by etching or the like (the same is true for the negative electrode current collector).

[0148] (negative electrode)

[0149] The negative electrode (negative electrode plate) includes a strip-shaped negative electrode current collector (second current collector) and a negative electrode mixture layer (second mixture layer) arranged on both sides of the negative electrode current collector. The negative electrode mixture layer contains a negative electrode material (active substance). The negative electrode material contains a negative electrode material (active substance) capable of adsorbing and desorbing ions. Examples of negative electrode materials include carbon materials, and the carbon materials exemplified as positive electrode materials can be used. Specifically, activated carbon, hard carbon, carbon nanotubes, graphite, graphene, etc. can be used as negative electrode materials.

[0150] The negative electrode mixture layer may contain other components in addition to the negative electrode material (active material). Examples of other components include a binder and a conductive material. The binder and the conductive material may be the same as those exemplified as the binder and the conductive material of the positive electrode.

[0151] The negative electrode current collector may be a strip of metal foil (eg, aluminum foil). The thickness of the current collector is not particularly limited, but may be in the range of 10 μm to 100 μm (eg, 15 μm to 40 μm).

[0152] The formation method of the first electrode and the second electrode (positive electrode and negative electrode) is not limited and can be formed by a known method. For example, the composite layer can be formed by the following method. First, a slurry is prepared by mixing an electrode material (active substance), a binder and / or a conductive material, and a dispersion medium. Next, the obtained slurry is applied to the surface of the collector to form a coating. Next, the coating is dried and rolled to form a composite layer on the surface of the collector. By doing so, a composite layer is formed.

[0153] (Diaphragm)

[0154] The separator is arranged between the first electrode and the second electrode (positive electrode and negative electrode) to prevent a short circuit between the positive electrode and the negative electrode. Examples of materials for the separator include insulating resins, glass, etc. Examples of separators include non-woven fabrics with cellulose as the main component, glass fiber mats, microporous films of polyolefins such as polyethylene, etc. The separator can use a known separator used in a double-layer capacitor or a lithium-ion capacitor.

[0155] Usually, the diaphragm includes a first diaphragm in the form of a strip and a second diaphragm in the form of a strip. Alternatively, the diaphragm in the form of a strip may be folded and two diaphragms may be overlapped, and the two overlapped diaphragms may be used as the first diaphragm and the second diaphragm.

[0156] The average thickness of the separator is not particularly limited, and may be in the range of 10 μm to 100 μm (eg, in the range of 20 μm to 40 μm).

[0157] (Electrolytes)

[0158] The electrolyte (electrolyte) may be an electrolyte used in an electric double layer capacitor. For example, a non-aqueous solvent in which a solute (organic salt, inorganic salt, etc.) is dissolved may be used as the electrolyte.

[0159] (outer body)

[0160] The outer casing houses the wound body and the electrolyte (electrolyte). The outer casing is not particularly limited, and a known outer casing can be used. For example, the outer casing can be a bottomed cylindrical shell and a sealing body for sealing the shell.

[0161] (Method for manufacturing electrochemical device)

[0162] An example of a method for producing the electrochemical device (D3) is described below. The electrochemical device (D3) may also be produced by a method other than the method described below.

[0163] First, the structural components constituting the winding body are prepared. The first electrode and the second electrode (or the electrode sheet as these electrodes) can be formed by the above method. If necessary, the lead is connected to the electrode (or electrode sheet) in advance. Next, a winding process is performed. In the winding process, the winding body is formed by winding the first electrode, the second electrode and the separator in a manner such that the separator is arranged between the first electrode and the second electrode.

[0164] Before or during the winding step, a bending step is performed to bend the vicinity of the portion to be the outer peripheral end of the second electrode. The bending step is not particularly limited as long as the vicinity of the outer peripheral end of the second electrode can be bent.

[0165] In one example of the bending process, when the strip-shaped electrode sheet to be the second electrode is cut into a predetermined length, the second electrode can be bent while cutting. For example, a certain gap can be intentionally provided between the lower mold and the upper mold and the bending portion can be formed by cutting. The same method can be used to bend the outer peripheral end of the first electrode.

[0166] The steps after forming the wound body are not particularly limited, and the electrochemical device (D3) can be assembled by a known method. For example, the electrochemical device (D3) can be obtained by housing the wound body and the electrolyte in an outer casing.

[0167] Hereinafter, an example of an embodiment of the present disclosure is specifically described with reference to the accompanying drawings. The embodiment described below can be changed based on the above description. In addition, the matters described below can be applied to the above embodiment. In addition, in the embodiment described below, matters that are not essential to the invention of the present disclosure can be omitted.

[0168] (Implementation Method 1)

[0169] In Embodiment 1, examples of the manufacturing method (M1) and the electrochemical device (D1) are described. According to the manufacturing method and the electrochemical device of Embodiment 1, the above-mentioned effects can be obtained. Figure 1A and Figure 1B One step of the manufacturing method of embodiment 1 is shown. Figure 1A It is a cross-sectional view schematically showing a part of the process of manufacturing a wound body. Figure 1B yes Figure 1A Top view of the .

[0170] In the manufacturing method of embodiment 1, first, Figure 1A As shown, a portion of the negative electrode 3 on the side of one end 3e and a portion of the separator 4 on the side of one end 4e are clamped by a winding shaft 110 (a first winding shaft 111 and a second winding shaft 112). The winding shaft 110 includes a first winding shaft 111 and a second winding shaft 112. The first winding shaft 111 and the second winding shaft 112 are rod-shaped bodies with semicircular cross sections.

[0171] The strip-shaped positive electrode 2 includes a strip-shaped positive electrode current collector and a positive electrode mixture layer disposed on both sides of the positive electrode current collector. The strip-shaped negative electrode 3 includes a strip-shaped negative electrode current collector and a negative electrode mixture layer disposed on both sides of the negative electrode current collector. In addition, the positive electrode 2 and the negative electrode 3 are respectively connected to leads not shown in the figure.

[0172] The strip-shaped diaphragm 4 includes a strip-shaped first diaphragm 4a and a strip-shaped second diaphragm 4b. Figure 1A In the example shown, the first winding axis 111 and the second winding axis 112 sandwich a portion of the negative electrode 3 on the side of one end 3e, a portion of the first separator 4a on the side of one end 4ae, and a portion of the second separator 4b on the side of one end 4be. Figure 1A In the example shown, a portion of the negative electrode 3 on the side of one end 3e and a portion of the separator 4 on the side of one end 4e are sandwiched by the first winding shaft 111 and the second winding shaft 112, so that the negative electrode 3 end 3e and the separator 4 end 4e protrude from between the first winding shaft 111 and the second winding shaft 112. The positive electrode 2 is not sandwiched by the first winding shaft 111 and the second winding shaft 112.

[0173] Next, while a portion of the negative electrode 3 and a portion of the separator 4 are held between the winding shaft 110, the winding shaft 110 is rotated to form a winding body. Figure 1A The positive electrode 2 is also wound together with the negative electrode 3 and the separator 4 to form a wound body. In addition, the end of the outermost separator 4 and / or the end of the outermost negative electrode 3 can be fixed with tape.

[0174] Figure 2 1 is a cross-sectional view showing a state where the wound body 1 is placed in the outer casing 6. Figure 2 In the figure, a part of the wound body 1 is omitted. In addition, in each figure, the ratio of the size of each component is changed according to the actual ratio for easy understanding. For example, the actual ratio of the thickness of each component constituting the wound body 1 to the size of the outer casing 6 is Figure 2 The ratio shown is small. That is, Figure 2 In the figure, each member constituting the wound body 1 is drawn thicker than the actual thickness.

[0175] Figure 2 The winding body 1 shown includes a winding shaft portion 1a formed by being clamped by a winding shaft 110 (a first winding shaft 111 and a second winding shaft 112) and a winding portion 1b connected to the winding shaft portion 1a. The winding portion 1b is a portion around which the components of the winding body 1 are wound. The winding shaft portion 1a includes a portion on the side of one end 3e of the negative electrode 3 and a portion on the side of one end 4e of the separator 4. The winding shaft portion 1a illustrated in Embodiment 1 does not include the positive electrode 2.

[0176] Although the components constituting the winding shaft portion 1a (including at least the negative electrode 3 and the separator 4) are substantially integrated, they may not be integrated. The winding shaft portion 1a is generally located at a cross section ( Figure 2 In the cross section shown in the figure, it extends in a manner that radially intersects the central circular hollow portion.

[0177] The negative electrode 3 is present inside the innermost circumference of the positive electrode 2 and outside the outermost circumference of the positive electrode 2. Therefore, in the wound body 1, both sides of the positive electrode 2 face the negative electrode 3. As an example of a method for arranging the negative electrode 3 inside the innermost circumference of the positive electrode 2, Figure 1A In the case of winding as shown, the length L from the winding axis 110 to one end of the positive electrode 2 may be greater than the circumference of the winding axis 110 . In the example shown in Embodiment 1, the separator 4 is present at the outermost circumference, and the electrode plate is not in contact with the outer case 6 .

[0178] like Figure 2As shown, the wound body 1 illustrated in the first embodiment further includes a protrusion 1c connected to the winding shaft 1a on the opposite side of the winding portion 1b. The protrusion 1c includes one end 3e of the negative electrode 3. The negative electrode 3 and the separator 4 are bent before and after the winding shaft 1a.

[0179] The outer peripheral end of the separator 4 and / or the outer peripheral end of the negative electrode 3 may be fixed with tape. By fixing the outer peripheral end with tape, the winding start and winding end of the wound body 1 can be fixed. As a result, the sag of the wound body 1 can be particularly suppressed.

[0180] Figure 3 An example of an electrochemical device using the wound body 1 is shown. Figure 3 This is a partially cutaway perspective view of the electrochemical device 10 according to the first embodiment.

[0181] Figure 3 The electrochemical device 10 shown is a double-layer capacitor. The electrochemical device 10 includes a winding body (capacitor element) 1. A lead 5a is connected to the positive electrode 2, and a lead 5b is connected to the negative electrode 3. The winding body 1 is housed in a cylindrical outer casing 6 together with an electrolyte (not shown). The material of the outer casing 6 can be, for example, metals such as aluminum, stainless steel, copper, iron, and brass. The opening of the outer casing 6 is sealed by a sealing member 7. The leads 5a and 5b are led out to the outside in a manner that passes through the sealing member 7. The sealing member 7 can be formed by an elastic member such as rubber (for example, butyl rubber).

[0182] (Implementation Method 2)

[0183] In Embodiment 2, examples of a manufacturing method (M2) and an electrochemical device (D2) are described. According to the manufacturing method and the electrochemical device of Embodiment 2, the above-mentioned effects can be obtained. Figure 4A and 4B A step of the manufacturing method of embodiment 2 is shown. Figure 4A It is a cross-sectional view schematically showing a part of the process of manufacturing a wound body. Figure 4B yes Figure 4A Top view of the .

[0184] In the manufacturing method of embodiment 2, first, as Figure 4A As shown, a portion of the end 4e side of the diaphragm 4 is clamped by the winding shaft 110 (the first winding shaft 111 and the second winding shaft 112). The winding shaft 110 includes the first winding shaft 111 and the second winding shaft 112. The first winding shaft 111 and the second winding shaft 112 are respectively rod-shaped bodies with a semicircular cross-section, and the semicircle has a diameter of length A.

[0185] The strip-shaped positive electrode 2 includes a strip-shaped positive electrode current collector and a positive electrode mixture layer disposed on both sides of the positive electrode current collector. The strip-shaped negative electrode 3 includes a strip-shaped negative electrode current collector and a negative electrode mixture layer disposed on both sides of the negative electrode current collector. In addition, the positive electrode 2 and the negative electrode 3 are respectively connected to leads not shown in the figure.

[0186] The strip-shaped diaphragm 4 includes a strip-shaped first diaphragm 4a and a strip-shaped second diaphragm 4b. Figure 4A In the example shown, the first winding shaft 111 and the second winding shaft 112 sandwich a portion of the first diaphragm 4a on the side of one end 4ae and a portion of the second diaphragm 4b on the side of one end 4be. Figure 4A In the example shown, a portion of the one end 4e side of the separator 4 is clamped by the first winding shaft 111 and the second winding shaft 112 so that the one end 4e of the separator 4 protrudes by a length D (mm) from between the first winding shaft 111 and the second winding shaft 112. The positive electrode 2 and the negative electrode 3 are not clamped by the first winding shaft 111 and the second winding shaft 112. The negative electrode 3 is arranged between the first separator 4a and the second separator 4b.

[0187] Reference Figure 4A , the distance between the end 3e of the winding axis 110 side of the negative electrode 3 and the winding axis 110 is set to distance B (mm). In addition, the distance between the end 2e of the winding axis 110 side of the positive electrode 2 and the end 3e of the negative electrode 3 is set to distance C (mm). The above description applies to the relationship between the length A, the distance B, the distance C, the length D, the average thickness T1 and the average thickness T2. In addition, the length A, the distance B, the distance C and the length D are Figure 4A When measuring these lengths and distances on a formed roll, the roll can be flattened and measured. Alternatively, the lengths and distances can be measured along the circumference of the roll based on an image of the end face or cross section of the roll.

[0188] Next, while a portion of the separator 4 is held by the winding shaft 110, the winding shaft 110 is rotated to form a wound body. Figure 4A At this time, the positive electrode 2 is also rolled up together with the negative electrode 3 and the separator 4 to form a wound body including them.

[0189] Figure 5 1 is a cross-sectional view showing a state where the wound body 1 is placed in the outer casing 6. Figure 5 In the figure, a part of the wound body 1 is omitted. In addition, in each figure, the ratio of the size of each component is changed according to the actual ratio for easy understanding. For example, the actual ratio of the thickness of each component constituting the wound body 1 to the size of the outer casing 6 is Figure 5 The ratio shown is small. That is, Figure 5 In the figure, each member constituting the wound body 1 is drawn thicker than the actual thickness.

[0190] Figure 5 The wound body 1 shown includes a winding shaft portion 1a formed by being sandwiched between winding shafts 110 (a first winding shaft 111 and a second winding shaft 112) and a winding portion 1b connected to the winding shaft portion 1a. The winding portion 1b is a portion where the constituent elements of the wound body 1 are wound.

[0191] The winding shaft portion 1a is composed only of the diaphragm 4 (the first diaphragm 4a and the second diaphragm 4b). The winding shaft portion 1a includes a first end portion 1as as a boundary with the winding portion 1b and a second end portion 1at on the opposite side of the first end portion 1as. The winding body 1 is composed only of the first diaphragm 4a and the second diaphragm 4b, and includes a protrusion 1c protruding from the second end portion 1at. Due to the presence of the protrusion 1c, the diaphragm 4 is bent before and after the winding shaft portion 1a.

[0192] The wound portion 1b includes a reinforcing portion 1bx between the first end portion 1as and one end 3e of the winding axis portion of the negative electrode 3, where only the first separator 4a and the second separator 4b are wound around for more than one turn. Figure 5 In the example shown, the number of turns n is 1. In addition, the reinforcement portion 1bx may be wound around only the first diaphragm 4a and the second diaphragm 4b for one or more turns. The reinforcement portion wound around only the first diaphragm 4a and the second diaphragm 4b may be wound around three turns or less or two turns or less.

[0193] Although the components (diaphragms 4a and 4b) constituting the winding shaft portion 1a are generally integrated, they may not be integrated. The winding shaft portion 1a is generally perpendicular to the central axis of the winding body 1 in a cross section ( Figure 5 In the cross section shown in the figure, it extends in a manner that radially intersects the central circular hollow portion.

[0194] The negative electrode 3 is present inside the innermost circumference of the positive electrode 2 and outside the outermost circumference of the positive electrode 2. Therefore, in the wound body 1, both sides of the positive electrode 2 face the negative electrode 3. As an example of a method for arranging the negative electrode 3 inside the innermost circumference of the positive electrode 2, Figure 4A In the case of winding as shown, the distance C can be made larger than the circumference of the winding body present inside the positive electrode 2. For example, the above condition (b) can be satisfied. In addition, in the example shown in Embodiment 2, the separator 4 is present on the outermost periphery, and the electrode plate is not in contact with the outer casing 6.

[0195] Figure 6 An example of an electrochemical device using the wound body 1 is shown. Figure 6 This is a partially cutaway perspective view of an electrochemical device 20 according to the second embodiment.

[0196] Figure 6The electrochemical device 20 shown is a double-layer capacitor. The electrochemical device 20 includes a winding body (capacitor element) 1. A lead 5a is connected to the positive electrode 2, and a lead 5b is connected to the negative electrode 3. The winding body 1 is housed in a cylindrical outer casing 6 together with an electrolyte (not shown). The material of the outer casing 6 can be, for example, metals such as aluminum, stainless steel, copper, iron, and brass. The opening of the outer casing 6 is sealed by a sealing member 7. The leads 5a and 5b are led out to the outside in a manner that passes through the sealing member 7. The sealing member 7 can be formed by an elastic member such as rubber (for example, butyl rubber).

[0197] (Implementation 3)

[0198] In Embodiment 3, an example of an electrochemical device (D3) and a method for producing the same will be described. According to the electrochemical device of Embodiment 3, the above-mentioned effects can be obtained.

[0199] Figure 7 A partial cross-sectional view showing an example of a wound body of an electrochemical device (D3) according to the third embodiment. Figure 7 1 shows a state where the wound body 1 is accommodated in the outer casing 6. Figure 7 In FIG. 1 , only a part of the outer peripheral portion of the wound body 1 is shown.

[0200] Figure 7 The wound body 1 shown is formed by winding a strip-shaped first electrode 2, a strip-shaped second electrode 3, and a separator 4. The separator 4 is arranged between the first electrode 2 and the second electrode 3. The separator 4 includes a first separator 4a and a second separator 4b.

[0201] like Figure 7 As shown, the outermost circumference of the second electrode 3 is arranged outside the outermost circumference of the first electrode 2. In addition, the separator 4 is present outside the outermost circumference of the second electrode 3. Therefore, the second electrode 3 and the outer case 6 are not in contact.

[0202] The vicinity of the outer peripheral end 3e of the second electrode 3 is bent, and as a result, the outer peripheral end 3e abuts against the diaphragm 4. Specifically, the outer peripheral end 3e abuts against the surface of the diaphragm 4 at an angle. According to this structure, the above-mentioned effect can be obtained.

[0203] The outer peripheral end 3e faces the inner second electrode 3 via the stacked first and second separators 4a and 4b. With this structure, even if the outer peripheral end 3e damages the separator, a short circuit between the first electrode 2 and the second electrode 3 can be prevented.

[0204] There is no limitation on the method of bending the outer peripheral end 3e. For example, the outer peripheral end 3e may be bent by clamping it with a clamp or the like. Figure 8As shown, a bend portion 3c can be formed near the outer peripheral end 3e of the second electrode 3. The bend portion 3c extends linearly along a direction perpendicular to the length direction of the second electrode 3 (a direction parallel to the outer peripheral end 3e). As described above, the distance L from the outer peripheral end 3e to the bend portion 3c can be in the range of 0.01 mm to 0.5 mm. The angle α at which the second electrode 3 is bent at the bend portion 3c can be set to the above range.

[0205] The second electrode 3 is formed to be connected to other components (the first electrode 2 and the separator 4). Figure 8 When the second electrode 3 is wound in the direction of arrow A, the bent portion 3c is bent toward the inside of the wound body. Figure 8 When the winding is carried out in the direction of the arrow B, the bent portion 3c is bent toward the outside of the wound body. In this way, a wound body is formed.

[0206] In addition, lead wires may be preliminarily connected to the wound first electrode 2 and the wound second electrode 3. In addition, the separator 4 at the outermost periphery of the wound body may be fixed with an adhesive tape.

[0207] Fig. 9 An example of an electrochemical device using the wound body 1 is shown. Fig. 9 This is a partially cutaway perspective view of an electrochemical device 30 according to the third embodiment.

[0208] Fig. 9 The electrochemical device 30 shown is a double-layer capacitor. The electrochemical device 30 includes a winding body (capacitor element) 1. A lead 5a is connected to the first electrode 2, and a lead 5b is connected to the second electrode 3. The winding body 1 is housed in a cylindrical outer casing 6 together with an electrolyte (not shown). The material of the outer casing 6 can be, for example, metals such as aluminum, stainless steel, copper, iron, and brass. The opening of the outer casing 6 is sealed by a sealing member 7. The leads 5a and 5b are led out to the outside in a manner that passes through the sealing member 7. The sealing member 7 can be formed by an elastic member such as rubber (for example, butyl rubber). As described above, the vicinity of the outer peripheral end of the second electrode 3 is bent.

[0209] Industrial Applicability

[0210] The present disclosure can be utilized in an electrochemical device and a method for manufacturing the same.

[0211] Although the present invention has been described according to the currently preferred embodiments, such disclosure should not be construed as limiting. For those skilled in the art to which the present invention belongs, various modifications and changes will undoubtedly become apparent after reading the above disclosure. Therefore, the appended claims should be construed as covering all modifications and changes that do not depart from the true spirit and scope of the present invention.

[0212] Description of Reference Numerals

[0213] 1: Winding body

[0214] 1a: Winding shaft

[0215] 1b: Winding section

[0216] 1bx: Strengthening

[0217] 1c: Protrusion

[0218] 2: Positive electrode, first electrode

[0219] 3: Negative electrode, second electrode

[0220] 3c: Bending part

[0221] 3e: peripheral end

[0222] 4: Diaphragm

[0223] 4a: First diaphragm

[0224] 4b: Second diaphragm

[0225] 10: Electrochemical device (first electrochemical device)

[0226] 20: Electrochemical device (second electrochemical device)

[0227] 30: Electrochemical device (third electrochemical device)

[0228] 110: Winding shaft

[0229] 111: First winding axis

[0230] 112: Second winding axis

Claims

1. A method for manufacturing an electrochemical device, the electrochemical device comprising a wound body, the wound body comprising a strip-shaped positive electrode containing activated carbon as a positive electrode material, a strip-shaped negative electrode, and a strip-shaped separator disposed between the positive electrode and the negative electrode, wherein: The manufacturing method of the electrochemical device successively includes: Step (i), clamping a part of one end side of the negative electrode and a part of one end side of the separator by a first winding shaft and a second winding shaft; and Step (ii), in a state where the first winding shaft and the second winding shaft clamp the part of the negative electrode and the part of the separator, rotating the first winding shaft and the second winding shaft to wind the positive electrode, the negative electrode, and the separator, thereby forming the wound body, In step (ii), the positive electrode, the negative electrode, and the separator are wound in such a manner that both sides of the positive electrode face the negative electrode.

2. The manufacturing method according to claim 1, wherein: In step (i), the part of the negative electrode and the part of the separator are clamped by the first winding shaft and the second winding shaft in such a manner that one end of the negative electrode protrudes between the first winding shaft and the second winding shaft.

3. The manufacturing method according to claim 1 or 2, wherein: In step (i), the positive electrode is not clamped by the first winding shaft and the second winding shaft.

4. An electrochemical device, the electrochemical device includes a wound body, the wound body is composed of a strip-shaped positive electrode containing activated carbon as a positive electrode active material, a strip-shaped negative electrode, and a strip-shaped separator disposed between the positive electrode and the negative electrode, wherein, The wound body includes a wound shaft portion formed by being clamped by a winding shaft and a wound portion connected to the wound shaft portion, The wound shaft portion includes a part of one end side of the negative electrode and a part of one end side of the separator, In the wound body, the positive electrode, the negative electrode, and the separator are wound in such a manner that both sides of the positive electrode face the negative electrode.

5. The electrochemical device according to claim 4, wherein, The wound body further includes a protruding portion, the protruding portion is connected to the wound shaft portion on the opposite side of the wound portion, The protruding portion includes the one end of the negative electrode.

6. The electrochemical device according to claim 4 or 5, wherein: The wound shaft portion does not include the positive electrode.

7. A manufacturing method of an electrochemical device, the electrochemical device includes a wound body, the wound body is composed of a strip-shaped positive electrode containing activated carbon as a positive electrode material, a strip-shaped negative electrode, and a strip-shaped separator disposed between the positive electrode and the negative electrode, wherein, The separator includes a strip-shaped first separator and a strip-shaped second separator, The manufacturing method successively includes: Step (I), only clamping a part of one end side of the first separator and the second separator by a winding shaft; and Step (II), while maintaining the state of step (I), rotating the winding shaft to wind the positive electrode, the negative electrode, the first separator, and the second separator, thereby forming the wound body, The winding shaft is composed of a first winding shaft and a second winding shaft having a semi-circular cross-section, and the semi-circular cross-section has a diameter with a length A, The first separator has an average thickness T1, The second separator has an average thickness T2, In step (II), (a) The distance B between one end of the winding shaft side of the negative electrode and the winding shaft and the length A satisfy πA < B, and (b) The winding is performed in a state where the distance C between one end on the winding axis side of the positive electrode and one end of the negative electrode, the length A, the average thickness T1, and the average thickness T2 satisfy π(A + (T1 + T2)×2n) < C, where n is the number of turns of only the first separator and the second separator.

8. The manufacturing method according to claim 7, wherein: In the step (II), the winding is performed in a state where the distance B and the length A satisfy 2πA < B.

9. The manufacturing method according to claim 7 or 8, wherein: In the step (II), the winding body is formed in such a manner that both surfaces of the positive electrode face the negative electrode.

10. An electrochemical device, the electrochemical device including a winding body, the winding body being composed of a strip-shaped positive electrode containing activated carbon as a positive electrode active material, a strip-shaped negative electrode, and a strip-shaped separator disposed between the positive electrode and the negative electrode, where, the separator includes a strip-shaped first separator and a strip-shaped second separator, the winding body includes a winding axis portion formed by being clamped by a winding axis and a winding portion connected to the winding axis portion, the winding axis portion is composed of only the first separator and the second separator, the winding axis portion includes a first end portion serving as a boundary between the winding portion and the winding axis portion side end of the negative electrode, and a second end portion opposite to the first end portion, the winding portion includes a reinforcing portion, and the reinforcing portion winds the first separator and the second separator more than one turn between the first end portion and the winding axis portion side end of the negative electrode, In the winding body, the surface of the positive electrode on the winding axis portion side faces the negative electrode.

11. The electrochemical device according to claim 10, wherein: In the reinforcing portion, the first separator and the second separator are wound more than two turns.

12. The electrochemical device according to claim 10 or 11, wherein: Both surfaces of the positive electrode face the negative electrode.

13. The electrochemical device according to any one of claims 10 to 12, wherein: The winding body includes a protruding portion, the protruding portion being composed of only the first separator and the second separator and protruding from the second end portion.

14. An electrochemical device, where, including a winding body, the winding body being composed of a strip-shaped first electrode, a strip-shaped second electrode, and at least a strip-shaped separator disposed between the first electrode and the second electrode, the outermost periphery of the second electrode is disposed outside the outermost periphery of the first electrode, the vicinity of the outer peripheral end of the second electrode is bent, and the outer peripheral end of the second electrode abuts against the separator.

15. The electrochemical device according to claim 14, where, the vicinity of the outer peripheral end of the second electrode is bent toward the inside of the winding body, the outer peripheral end of the second electrode abuts against the separator existing inside the outer peripheral end of the second electrode.

16. The electrochemical device according to claim 14 or 15, wherein: In the range from 0.01 mm to 0.5 mm from the outer peripheral end of the second electrode, there is a portion where the second electrode is bent.

17. The electrochemical device according to any one of claims 14 to 16, wherein: The vicinity of the outer peripheral end of the first electrode is bent, and the outer peripheral end of the first electrode abuts against the separator.