Sheet heater

By using a laminated structure of high-strength, high-insulating sheet and fluorine-based adhesive on the heated body on the curved surface, the tensile stress problem of the sheet-shaped heater on the curved surface is solved, and high insulation characteristics and construction properties are achieved Improvement.

CN118947221APending Publication Date: 2024-11-12TOMOEGAWA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030854.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-02-16
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When a sheet-shaped heater is installed on a heated body with a curved surface, tensile stress burden is prone to occur, resulting in deformation of the heater and changes in resistance value, and the prior art is difficult to effectively solve this problem.

Method used

The laminated structure of a high-strength high-insulating sheet, a first adhesive layer, a first insulation layer, a second adhesive layer and a heating layer is adopted to ensure that the ratio of the thickness of the first insulation layer to the total thickness reaches 0.10 or more, and The sheet-shaped heater formed by using a fluorine-based adhesive was able to reduce tensile stress on the curved surface and maintain high insulation properties by the adhesive having a solubility test with a solvent solubility test.

Benefits of technology

It realizes the reduction of tensile stress burden under the bending surface and maintains high insulation characteristics, improves the constructionability and heat resistance of the heater, and avoids changes in resistance value caused by bending of the heater.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118947221A_ABST
    Figure CN118947221A_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a sheet-shaped heater which, when disposed on a curved surface of a body to be heated, such as a pipe, has a curved surface, can reduce the load of tensile (elongation) stress and has high insulation characteristics. This problem is solved by a sheet-like heater in which a high-strength, high-insulating sheet in which reinforcing fibers are impregnated with a fluororesin, a first adhesive layer, a first insulating layer, a second adhesive layer, and a heat generating layer are laminated in this order, the sheet-like heater being characterized in that: the high-strength, high-insulating sheet and the main surface of the first adhesive layer are in close contact with each other; the first adhesive layer and the main surface of the first insulating layer are in close contact with each other, the second adhesive layer and the main surface of the heat generating layer are in close contact with each other, and the ratio (h1 / Htotal) of the thickness (h1) of the first insulating layer to the total thickness (Htotal) of the high-strength high-insulating sheet, the first adhesive layer, and the first insulating layer is 0.10 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to sheet heaters. Background Art

[0002] Conventionally, heaters described in Patent Documents 1 to 4 have been proposed as heaters for heating pipes and the like.

[0003] Patent Document 1 describes a planar heater having a sheet heating element formed by connecting a lead wire to a terminal portion connected to a conductive heating element, and a sheet heating element having a thermal expansion coefficient of 8×10 -5 ℃ or less, are sandwiched and heat-fused together from both sides by heat-fusible fluororesin layers A. Furthermore, a heat diffusion material layer is provided on each surface of the heat-fusible fluororesin layer A on both sides, and another heat-fusible fluororesin layer B is provided on the surface of the heat diffusion material layer. It is also recorded that: According to this planar heater, because it has a heat diffusion material layer, even if the conductive heating element is extremely thin, during the heat fusion process based on resin heating during manufacturing, the force that causes deformation due to resin shrinkage is suppressed by the heat diffusion material layer pressed against the resin, and therefore will not be transmitted to the conductive heating element itself. Therefore, the planar heater will not deform into a wavy shape or warp, and can be accurately made into a flat planar heater. Therefore, it can be made into a stable specified shape, and even when immersed in the heated liquid, the planar heater can be reliably and completely immersed.

[0004] Patent Document 2 describes a planar heating element characterized by being formed by laminating insulating sheaths on both sides of a metal resistor having a heating circuit, separated by a heat-melting adhesive layer, and integrating them. A heat-melting fluororesin is used as the heat-melting adhesive layer, and glass cloth impregnated with polytetrafluoroethylene (hereinafter referred to as "PTFE") and sintered is used as the insulating sheath. The disclosure further states that, according to this planar heating element, a PFA film or FEP film is sandwiched between PTFE-impregnated glass cloths as a heat-melting adhesive layer, and the metal resistor is sandwiched and heat-welded by applying heat and pressure, thereby obtaining a planar heating element having heat resistance of 200°C or higher for continuous use. Because PTFE-impregnated glass cloth is used as the insulating sheath, deformation such as warping does not occur with temperature increases or decreases, and the mechanical strength is also high.

[0005] Patent Document 3 describes a planar heater comprising a heat-generating layer and first fluororubber layers disposed on both surfaces thereof, wherein the first fluororubber layers have a durometer A hardness of 65 or less according to JIS K 6253. The patent document also states that this planar heater can provide a planar heater having improved thermal conductivity, in which the heat-generating layer is covered with a fluororubber layer.

[0006] Patent Document 4 describes a fluororubber planar heater characterized by comprising a heater element and a fluororubber sheet bonded to the heater element, the fluororubber sheet comprising glass cloth and a fluororubber layer impregnated with an adhesion-strengthening agent. The patent also states that this fluororubber planar heater exhibits excellent heat resistance, cold resistance, acid resistance, oil resistance, and solvent resistance, and, as a rubber elastic body, excellent flexibility and impact resistance.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 2016-110757

[0010] Patent Document 2: Japanese Utility Model Application Laid-Open No. 4-66087

[0011] Patent Document 3: Japanese Patent Application Laid-Open No. 2015-122212

[0012] Patent Document 4: Japanese Patent Application Laid-Open No. 2007-224208 Summary of the Invention

[0013] Problems to be solved by the invention

[0014] When a sheet heater is installed on a curved surface of a heated object such as a pipe, tensile stress is applied to the outer circumference of the sheet heater. The present invention provides a sheet heater having high insulation properties while reducing tensile stress even when installed on a curved surface of a heated object such as a pipe.

[0015] Solutions for solving problems

[0016] The present inventors have conducted intensive studies to solve the above-mentioned problems and have completed the present invention.

[0017] The present invention is the following (1) to (6).

[0018] (1) A sheet heater comprising:

[0019] High-strength, high-insulation sheet with fluororesin impregnated in the reinforcing fiber;

[0020] a first adhesive layer;

[0021] a first insulating layer;

[0022] a second adhesive layer; and

[0023] Heating layer,

[0024] The high-strength and high-insulation sheet and the main surface of the first adhesive layer are in close contact with each other.

[0025] The first adhesive layer and the main surface of the first insulating layer are in close contact with each other.

[0026] The second adhesive layer and the main surface of the heat generating layer are in close contact with each other.

[0027] The thickness (h1) of the first insulating layer is the sum of the thickness (H1) of the high-strength and high-insulating sheet, the first adhesive layer, and the first insulating layer. total ) ratio (h1 / H total ) is greater than 0.10.

[0028] (2) The sheet heater according to (1) above, wherein the total thickness is 200 to 800 μm.

[0029] (3) The sheet heater according to (1) or (2) above, wherein the thickness of the high-strength and high-insulation sheet is 100 to 300 μm.

[0030] The thickness of the first adhesive layer is 5 to 50 μm.

[0031] (4) The sheet heater according to any one of (1) to (3) above, wherein the heat generating layer is formed of a metal fiber sheet.

[0032] (5) A sheet heater according to any one of (1) to (4) above, wherein the first adhesive layer and / or the second adhesive layer is formed of a fluorine-based adhesive having a ratio of a storage modulus (E2) at 70°C to a storage modulus (E1) at 25°C (percentage: E2 / E1×100) of 8 to 92%.

[0033] (6) The sheet heater according to any one of (1) to (5) above, wherein the first adhesive layer is formed of a fluorine-based adhesive having a solubility of 5 to 30% by mass as determined by a solvent solubility test.

[0034] The solvent solubility test is as follows: 1000 g of tetrahydrofuran (THF) is placed in a 2 L plastic bottle, the temperature is adjusted to 23° C., and while stirring at 600 rpm using a medium viscosity stirrer using a disperser blade with a blade diameter of 40 mm as a stirring blade, 1 to 50 g of a granular sample with a diameter of 0.5 to 2.0 cm is added. After 24 hours, it is confirmed whether all the sample has dissolved. If all the sample has dissolved, 1 to 50 g of the sample is added again and dissolved after 24 hours. This operation is repeated to determine the maximum amount that can be dissolved (solubility).

[0035] Effects of the Invention

[0036] According to the present invention, a sheet heater having high insulation properties can be provided which can reduce the tensile (elongation) stress burden when arranged on a curved surface of a heated object such as a pipe. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a cross-section (schematic cross-sectional view) showing a preferred embodiment of the heater of the present invention cut along a direction perpendicular to its main surface. DETAILED DESCRIPTION

[0038] The present invention will be described.

[0039] The present invention is a sheet heater, which is laminated in this order: a high-strength, high-insulation sheet having reinforcing fibers impregnated with a fluororesin, a first adhesive layer, a first insulating layer, a second adhesive layer, and a heat-generating layer, wherein the high-strength, high-insulation sheet and the main surface of the first adhesive layer are in close contact with each other, the first adhesive layer and the main surface of the first insulating layer are in close contact with each other, the second adhesive layer and the main surface of the heat-generating layer are in close contact with each other, and the thickness (h1) of the first insulating layer is 1 / 2 of the total thickness (H1) of the high-strength, high-insulation sheet, the first adhesive layer, and the first insulating layer. total ) ratio (h1 / H total ) is greater than 0.10.

[0040] Hereinafter, such a sheet heater is also referred to as a "heater of the present invention."

[0041] The heater of the present invention will be described using drawings showing preferred embodiments thereof.

[0042] Figure 1 A cross section is shown when a suitable embodiment of the heater of the present invention is cut in a direction perpendicular to its main surface. Figure 1 is a schematic cross-sectional view, therefore, Figure 1 Dimensions shown may differ from actual dimensions.

[0043] Figure 1The heater 1 of the present invention shown in the figure is stacked in order: a high-strength high-insulation sheet 3, a first adhesive layer 5, a first insulating layer 7, a second adhesive layer 9, a heating layer 11, a third adhesive layer 13, and a second insulating layer 15. The main surfaces of the adjacent layers are in close contact with each other. In other words, in the heater of the present invention, the main surfaces of the first insulating layer 7 and the second adhesive layer 9 do not need to be in close contact with each other, and other layers can be included between these layers. Figure 1 In the case of the preferred embodiment shown in FIG. 1 , the main surfaces of the first insulating layer 7 and the second adhesive layer 9 are in close contact with each other. Similarly, in the heater of the present invention, the main surfaces of the heating layer 11, the third adhesive layer 13, and the second insulating layer 15 may not be in close contact with each other, but Figure 1 In the suitable manner shown, the layers are closely attached.

[0044] The heater of the present invention may not have the third adhesive layer and the second insulating layer, and is preferably Figure 1 The layers are present in the manner shown.

[0045] <High Strength High Insulation Sheet>

[0046] The high-strength and high-insulation sheet 3 is a sheet in which reinforcing fibers are impregnated with a fluororesin, and has high strength and high insulation properties.

[0047] Here, the reinforcing fiber refers to a fiber with high strength and may be any conventionally known reinforcing fiber. Examples of the material of the reinforcing fiber include glass, aramid (aromatic polyamide resin), and carbon fiber.

[0048] The reinforcing fibers preferably have a cross-sectional diameter (equivalent circle area diameter) of approximately 5 to 10 μm.

[0049] The reinforcing fibers are preferably fibers woven flat into a sheet. In other words, they are preferably woven.

[0050] The high-strength and high-insulation sheet 3 is a sheet in which the above-mentioned reinforcing fibers are impregnated with a fluororesin.

[0051] The fluororesin is not particularly limited, and examples thereof include polytetrafluoroethylene (PTFE), a vinylidene fluoride-hexafluoropropylene copolymer, and a vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene copolymer.

[0052] The reinforcing fibers may be primed and then impregnated with a fluororesin.

[0053] The high-strength and high-insulation sheet 3 is preferably a woven fabric of glass fiber, that is, glass cloth impregnated with PTFE.

[0054] The thickness of the high-strength and high-insulation sheet is not limited, but is preferably 100 to 300 μm, and more preferably 125 to 200 μm.

[0055] In addition, the thickness of the high-strength and high-insulation sheet is a value measured as follows.

[0056] In getting Figure 1 After taking a magnified photograph (200x) of a cross section perpendicular to the main surface of the heater of the present invention as shown, the thickness of the high-strength, high-insulation sheet was measured at 100 randomly selected locations in the magnified photograph, and the simple average value of these values ​​was calculated. The obtained average value was then used as the thickness of the layer.

[0057] Note that the thicknesses of other layers described later (first adhesive layer 5 , first insulating layer 7 , second adhesive layer 9 , heat generating layer 11 , third adhesive layer 13 , second insulating layer 15 , and other layers) are also values ​​measured by the same method.

[0058] <First Adhesive Layer, Second Adhesive Layer, Third Adhesive Layer>

[0059] The first adhesive layer 5 , the second adhesive layer 9 , and the third adhesive layer 13 will be described.

[0060] They can be the same way or they can be different ways.

[0061] The main surface of the first adhesive layer 5 is in close contact with the main surfaces of the high-strength and high-insulation sheet 3 and the first insulating layer 7 .

[0062] The main surface of the second adhesive layer 9 is in close contact with the main surfaces of the first insulating layer 7 and the heat generating layer 11 .

[0063] The main surface of the third adhesive layer 13 is in close contact with the main surfaces of the heat generating layer 11 and the second insulating layer 15 .

[0064] The first adhesive layer 5 , the second adhesive layer 9 , and the third adhesive layer 13 are preferably formed of an adhesive α.

[0065] Examples of the adhesive α include fluorine-based adhesives, silicone-based rubbers, silicone-based pressure-sensitive adhesives, and polyimide-based adhesives.

[0066] Here, examples of the fluorine-based adhesive include fluorine-based rubber and fluorine-based elastomers (PFA, etc.).

[0067] The adhesive α preferably has a fluorine content of 64% by mass or less, and more preferably 57 to 60% by mass.

[0068] Here, the fluorine content in the adhesive α refers to a value obtained by quantitatively analyzing combustion gas of a fluororesin by absorbing the combustion gas of the fluororesin in an absorbing liquid according to JIS K 7217, using a method for analyzing combustion gas of plastics, and performing quantitative analysis according to 34.1 of JIS K 0102.

[0069] The adhesive α is preferably a fluorine-based adhesive, and has an unsaturated bond content in the range of 0.1 to 20%, more preferably in the range of 0.1 to 10%.

[0070] Here, the content of unsaturated bonds contained in the adhesive α is determined by 1 The calculation was performed based on the ratio of the cumulative amount of the peak derived from the unsaturated bond hydrogen of the alkyl chain (4.5 to 6.0 ppm) to the cumulative amount of the peak derived from the saturated bond hydrogen in the spectrum obtained by H-NMR (solid-state NMR) measurement.

[0071] The adhesive α is preferably a fluorine-based adhesive, and has a storage elastic modulus (E1) at 25° C. of 0.2 to 15 MPa, more preferably 1 to 10 MPa.

[0072] Here, the storage elastic modulus (E1) of the adhesive α at 25°C is defined as the value obtained at 25°C by measuring a 400 μm thick adhesive layer using a dynamic thermoelasticity measuring apparatus at a measurement frequency of 10 Hz while heating the temperature from 0°C to 120°C at a rate of 3°C / min.

[0073] The adhesive α is preferably a fluorine-based adhesive, and has a storage modulus (E2) at 70° C. of 0.1 to 10 MPa, more preferably 0.5 to 8 MPa.

[0074] Here, the storage modulus (E2) of the adhesive α at 70°C is defined as the value obtained at 70°C by measuring a 400 μm thick adhesive layer using a dynamic thermoelasticity measuring apparatus at a measurement frequency of 10 Hz while heating the layer from 0°C to 120°C at a rate of 3°C / min.

[0075] The adhesive α is preferably a fluorine-based adhesive, and the ratio of the storage modulus (E2) at 70°C to the storage modulus (E1) at 25°C (percentage: E2 / E1×100) is 8 to 92%, more preferably 20 to 85%.

[0076] The inventors have discovered that if at least one of the group consisting of the first adhesive layer 5, the second adhesive layer 9 and the third adhesive layer 13 is formed of a fluorine-based adhesive having a ratio of the storage modulus (E2) at 70°C to the storage modulus (E1) at 25°C (percentage: E2 / E1×100) of 8 to 92% (preferably 20 to 85%), then when the heater of the present invention is arranged on a curved surface of a heated body such as a pipe, core set is likely to occur.

[0077] The inventors have found that: in the heater of the present invention in which at least one of the first adhesive layer 5, the second adhesive layer 9 and the third adhesive layer 13 is formed by the fluorine-based adhesive as described above, if the heating layer is energized, the elastic modulus of the fluorine-based adhesive is reduced due to the heat emitted by the heating layer. Furthermore, if the heater of the present invention is deformed in such a manner as to be in close contact with the curved surface in the heated body in this state, the fluorine-based adhesive easily follows this deformation and deforms. Thereafter, if the heating layer is stopped from being energized while maintaining the heater of the present invention in close contact with the curved surface of the heated body, and the heater of the present invention is cooled to about room temperature, the elastic modulus of the fluorine-based adhesive becomes high, and therefore, the heater of the present invention is wound and shaped, and as a result, it is easy to arrange the heater of the present invention on the curved surface in the heated body having a curved surface, such as a pipe.

[0078] Furthermore, the present inventors have discovered that when the heater of the present invention is placed on a curved surface of a heated object such as a pipe, the heater of the present invention can be easily installed on the curved surface of the heated object if the heater of the present invention is pre-bent along the curved surface. If at least one of the first adhesive layer 5, the second adhesive layer 9, and the third adhesive layer 13 is formed from a fluorine-based adhesive having a storage modulus (E2) at 70°C relative to the storage modulus (E1) at 25°C (percentage: E2 / E1×100) of 8 to 92% (preferably 20 to 85%), the heater of the present invention can be easily bent pre-bent along the curved surface of the heated object.

[0079] As a method for bending the heater of the present invention before installation, the following method can be cited, for example: a cylinder having a curved surface with a curvature equal to that of the heated body and the heater of the present invention are placed in an oven, heated to about 110°C, and the heater of the present invention is wrapped around the outer surface of the cylinder in the oven to be bent. The cylinder with the heater of the present invention wrapped around it is taken out of the oven, cooled to about room temperature, and then the heater of the present invention is removed from the cylinder.

[0080] The adhesive α is preferably a fluorine-based adhesive, and its solubility as determined by a solvent solubility test is 5 to 30% by mass, preferably 10 to 28% by mass.

[0081] At least one selected from the group consisting of the first adhesive layer 5 , the second adhesive layer 9 , and the third adhesive layer 13 is preferably formed of such a fluorine-based adhesive.

[0082] Among these, the first adhesive layer 5 is preferably formed of a fluorine-based adhesive having a solubility of 5 to 30 mass % (preferably 10 to 28 mass %) as determined by a solvent solubility test.

[0083] Here, the solvent solubility test refers to the following test: 1000 g of tetrahydrofuran (THF) is placed in a 2 L plastic bottle, adjusted to 23°C, and while stirring at 600 rpm using a medium viscosity stirrer using a disperser blade with a blade diameter of 40 mm as a stirring blade, 1 to 50 g of a granular sample (adhesive α) with a diameter of 0.5 to 2.0 cm is added. After 24 hours, it is confirmed whether all the sample has dissolved. If all the sample has dissolved, 1 to 50 g of the sample (adhesive α) is added again and dissolved after 24 hours. This operation is repeated to determine the maximum amount that can be dissolved (solubility).

[0084] The thickness of the first adhesive layer 5 is not limited, but is preferably 5 to 50 μm, more preferably 20 to 30 μm.

[0085] The thickness of the second adhesive layer 9 is not limited, but is preferably 5 to 100 μm, more preferably 20 to 30 μm.

[0086] The thickness of the third adhesive layer 13 is not limited, but is preferably 5 to 100 μm, more preferably 20 to 30 μm.

[0087] <First Insulating Layer, Second Insulating Layer>

[0088] The first insulating layer 7 and the second insulating layer 15 will be described.

[0089] They can be the same way or they can be different ways.

[0090] The main surface of the first insulating layer 7 is in close contact with the main surfaces of the first adhesive layer 5 and the second adhesive layer 9. The first insulating layer 7 serves to electrically insulate the heat generating layer 11 from the high-strength and high-insulating sheet 3.

[0091] The main surface of the second insulating layer 15 is in close contact with the main surface of the third adhesive layer 13. When another layer is present on the main surface of the second insulating layer 15 where the third adhesive layer 13 is not present, the second insulating layer 15 serves to electrically insulate the other layer from the heat generating layer 11.

[0092] It is preferable that the first insulating layer 7 and the second insulating layer 15 have thermal conductivity in addition to insulating properties.

[0093] The first insulating layer 7 and the second insulating layer 15 are preferably formed of materials such as PET (polyethylene terephthalate), PI (polyimide), PP (polypropylene), PE (polyethylene), PEN (polyethylene naphthalate), TAC (cellulose triacetate), or ceramics. This is because these materials have high insulating properties. Among these, the first insulating layer 7 and the second insulating layer 15 formed of PI (polyimide) are preferred due to their excellent heat resistance and insulating properties.

[0094] The thickness ( h1 ) of the first insulating layer 7 is not limited, but is preferably 25 to 75 μm, and more preferably 40 to 60 μm.

[0095] The thickness of the second insulating layer 15 is not limited, but is preferably 10 to 50 μm, and more preferably 20 to 30 μm.

[0096] The shape and size of the main surfaces of the first insulating layer 7 and the second insulating layer 15 are not particularly limited. In order to electrically insulate the heat generating layer 11 from other layers, the main surfaces of the first insulating layer 7 and the second insulating layer 15 are typically the same size as or larger than the main surface of the heat generating layer 11.

[0097] In the heater of the present invention, the thickness of the first insulating layer (h1) is 1 / 2 of the total thickness (H1) of the high-strength and high-insulation sheet, the first adhesive layer, and the first insulating layer. total ) ratio (h1 / H total ) is 0.10 or more, preferably 0.15 or more, more preferably 0.20 or more.

[0098] The present inventors have found that, in this case, when the heater of the present invention is arranged on a curved surface of a heated object such as a pipe, the tensile (elongation) stress burden can be reduced.

[0099] In the past, it was desired to make the sheet heater as thin as possible from the viewpoint of the ease of being installed on a curved surface of a pipe, etc., specifically, the ease of being wound around the outer surface of a pipe, and the ease of heat conduction. However, the inventors have found that when the sheet heater is simply thinned, the tensile (elongation) stress burden increases, and the resistance value changes accompanying the elongation of the heating element. Furthermore, the inventors have found that even if the overall thickness of the sheet heater is thinned, the thickness of the first insulating layer (h1) is not thinned, but thickened instead. Specifically, the thickness of the first insulating layer (h1) is made thicker relative to the total thickness (H1) of the high-strength and high-insulation sheet, the first adhesive layer, and the first insulating layer. total ) ratio (h1 / H total ) becomes greater than 0.10, thereby reducing the tensile (elongation) stress burden.

[0100] <Heat-generating layer>

[0101] The heat generating layer 11 will be described.

[0102] The heat generating layer 11 may be any sheet-shaped heat generating layer that generates heat when electricity is passed through it.

[0103] The heat generating layer 11 may be, for example, a metal foil, a sheet of metal mesh, a sheet of metal fiber, or a carbon sheet.

[0104] The material of the heat generating layer 11 is not particularly limited as long as it generates heat when electricity is applied thereto, and is preferably stainless steel, and may also be Cu (copper), Al (aluminum), Ni (nickel), nickel-chromium alloy, or carbon.

[0105] The thickness of the heat generating layer 11 is preferably 10 to 600 μm, more preferably 20 to 150 μm, and preferably about 30 μm from the viewpoint of flexibility and strength.

[0106] The shape and size of the main surface of the heat generating layer 11 can be adjusted as appropriate depending on the shape and size of the object to be heated on which the sheet of the present invention is provided.

[0107] The resistance of the heat generating layer 11 is preferably 10 to 800Ω, more preferably 80 to 200Ω. If the resistance is too low, the temperature may rise too high due to excessive output. Conversely, if the resistance is too high, the temperature may rise too slowly due to insufficient output.

[0108] Here, the resistance of the heat generating layer is set to a value determined in accordance with JIS K 7194.

[0109] The heat generating layer 11 is preferably formed mainly of metal fibers, and more preferably formed only of metal fibers.

[0110] Here, "primarily" means 70% by mass or more. That is, the heat generating layer 75 preferably comprises 70% by mass or more of metal fibers. The proportion of metal fibers in the heat generating layer 75 is more preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more.

[0111] It should be noted that the ratio of the metal fibers contained in the heat generating layer 11 is determined by the following method.

[0112] In the SEM image obtained by magnifying the surface of the heating layer 11 to 1000 times using a scanning electron microscope (SEM), an image processing device is used to calculate the area occupied by the metal fibers (excluding gaps) in the field of view, and the area is converted into a volume ratio by multiplying it by the cube, and then the mass ratio is calculated by multiplying it by the specific gravity to calculate the metal fiber content.

[0113] The metal fibers are preferably metal fibers having a cross-sectional equivalent circle diameter of 2 to 100 μm (preferably 5 to 20 μm) and a length of 2 to 20 mm.

[0114] The heat generating layer 11 is preferably a sheet-like layer (metal fiber sheet) formed by complexly entwining a plurality of such metallic fibers. The metal fiber sheet may be formed solely of metal fibers, or may contain metal fibers and other fibers (e.g., resin fibers that function as a binder) as long as the heat generating properties are not impaired.

[0115] Here, the metal fibers constituting the metal fiber sheet are connected to each other to the extent that they are electrically connected. The metal fibers are preferably connected to each other at the connection points. For example, it is preferable that the metal fibers are fused to each other at the connection points by a process in which a portion of the metal fibers melts and then solidifies due to sintering at a high temperature.

[0116] The metal fiber sheet is preferably a SUS fiber sheet because of its high heat resistance and chemical resistance. Examples of the SUS fiber sheet include a stainless steel fiber sheet (for example, Tommy Filec SS, manufactured by Tomogawa Paper Co., Ltd.).

[0117] The basis weight of the metal fiber sheet is preferably 25 g / m 2 Above, preferably 50g / m 2 In addition, it is preferably 1000g / m 2 Below, more preferably 200g / m 2 the following.

[0118] In addition, the basis weight is set to the value calculated|required based on JIS P 8124.

[0119] The density of the metal fiber sheet is preferably 1.0 to 10.0 g / cm 3 , more preferably 1.4 to 2.0 g / cm 3 , preferably 1.7 g / cm 3 about.

[0120] It should be noted that the density of the metal fiber sheet is determined in accordance with JIS P 8118 and is expressed as a density (g / cm 3 ) = Basis weight (g / m 2 ) / (thickness (mm)×1000).

[0121] The metal fiber sheet can be manufactured by a dry nonwoven fabric manufacturing method or a wet papermaking method. In the case of manufacturing by the wet papermaking method, a plurality of metallic fibers with a cross-sectional equivalent circle diameter of 2 to 100 μm and a length of 2 to 20 mm are stirred in a dispersion medium (water, organic solvent, etc.), and then an organic coagulant is added. The sheet is made using a square hand-made papermaking device (manufactured by Toyo Seiki Co., Ltd., etc.), and a drying device using iron plate photography is used to obtain a sheet with a basis weight of 50 to 1100 g / m 2 The dried sheet is then calcined at 400-1300°C to obtain a metal fiber sheet. It should be noted that, as a rule, it is preferred that no organic aggregating agent remain in the metal fiber sheet.

[0122] <Heat Diffusion Layer>

[0123] As described above, the heater 1 of the present invention is stacked in sequence with a high-strength and high-insulation sheet 3, a first adhesive layer 5, a first insulating layer 7, a second adhesive layer 9 and a heating layer 11 (preferably further stacked in sequence with a third adhesive layer 13 and a second insulating layer 15), and the main surfaces of adjacent layers are tightly bonded to each other.

[0124] Furthermore, a heat diffusion layer may be further provided on the main surface of the high-strength and high-insulation sheet 3 where the first adhesive layer 5 is not present.

[0125] If the heat diffusion layer is provided, the heat generated by the heat generating layer is diffused, and the object to be heated can be heated more uniformly.

[0126] The method of bonding the thermal diffusion layer to the main surface of the high-strength and high-insulation sheet 3 where the first adhesive layer 5 is not present is not particularly limited, but bonding using the aforementioned adhesive α is preferred.

[0127] The thermal conductivity of the heat diffusion layer in the plane direction is preferably higher than the thermal conductivity of the heat generating layer in the plane direction, because the heat diffusion capability is further improved.

[0128] Here, the thermal conductivity of the thermal diffusion layer is measured at room temperature by a known measurement method such as laser flash thermal diffusivity measurement (eg, LFA series manufactured by NETZSCH) or optical AC thermal diffusivity measurement (eg, LaserPit series manufactured by ADVANCE-RIKO).

[0129] The heat diffusion layer is preferably formed of a metal such as carbon, aluminum, copper, zinc, lead, gold, or silver, or a ceramic such as aluminum oxide or aluminum nitride.

[0130] The heat diffusion layer is preferably formed of a carbon thin film because it has excellent flexibility and high thermal conductivity in the extension direction.

[0131] The thickness of the heat diffusion layer is not particularly limited, but is preferably 5 to 300 μm, more preferably 15 to 200 μm, and even more preferably about 100 μm.

[0132] The total thickness of the sheet of the present invention is not limited, but is preferably 200 to 800 μm, more preferably 200 to 500 μm, and even more preferably 300 to 450 μm.

[0133] Example

[0134] The present invention will be described with reference to the following examples, but the present invention is not limited to the following examples.

[0135] [Experiment 1]

[0136] <Example 1>

[0137] Prepare Figure 1 Sheet heater in the manner shown.

[0138] Details of each layer are shown below.

[0139] High-strength and high-insulation sheet: PTFE cloth (manufactured by Chunghsing Chemical Industry Co., Ltd., FGF-500-8), thickness 170 μm

[0140] First adhesive layer: a layer made of a fluorine-based adhesive, 25 μm thick

[0141] First insulation layer: polyimide film, thickness 50μm

[0142] Second adhesive layer: Same as the first adhesive layer (thickness 25 μm)

[0143] Heating layer: Stainless steel paper (Tommy Filec SS, manufactured by Tomogawa Paper Co., Ltd.), thickness 30 μm

[0144] ·Third adhesive layer: Same as the first and second adhesive layers (thickness 25 μm)

[0145] Second insulating layer: Same as the first insulating layer (thickness 25 μm)

[0146] In addition, the thickness of each layer is a value measured by the above-mentioned method.

[0147] The fluorine-based adhesive used to form the first, second, and third adhesive layers had a solubility within the range of 5 to 30% by mass, as determined by the aforementioned solvent solubility test. A high-powered general-purpose blender, BLH1200, manufactured by Shinto Scientific Co., Ltd., was used as a medium-pressure blender in the solvent solubility test.

[0148] The fluorine content of the fluorine-based adhesive was measured by the aforementioned method and found to be within a range of 57 to 60% by mass.

[0149] The unsaturated bond content of the fluorine-based adhesive was measured by the aforementioned method and found to be within a range of 0.1 to 10%.

[0150] The storage elastic modulus (E1) of the fluorine-based adhesive at 25° C. was measured by the aforementioned method and was found to be 5.58 MPa.

[0151] Furthermore, the storage elastic modulus (E2) of this fluorine-based adhesive at 70° C. was measured by the aforementioned method and was found to be 3 MPa.

[0152] With respect to the sheet heater obtained in Example 1, strain (measured value) was measured.

[0153] The method for measuring the strain (measured value) is as follows.

[0154] After the strain gauge of a strain gauge (FLAB-1-11-3LJCT, manufactured by Tokyo Shoki Laboratory) was fixed to the upper side of the heating element layer with an adhesive in the same direction as the winding direction, the adhesive layer 13 and the third insulating layer 15 were laminated. The strain immediately after lamination was set to zero, and the strain measurement value when the layer was wound onto a 27 mm diameter cylinder was read.

[0155] The results are shown in Table 1. Table 1 also shows the values ​​of elongation (%) calculated as one ten-thousandth of the measured values.

[0156] <Example 2>

[0157] The same experiment as in Example 1 was conducted except that the thickness of the first insulating layer was set to 25 μm.

[0158] The results are shown in Table 1.

[0159] <Example 3>

[0160] The same experiment as in Example 1 was conducted except that a PTFE cloth (FGF-500-10 manufactured by Chunghsoo Chemical Industry Co., Ltd.) having a thickness of 250 μm was used as the high-strength and high-insulation sheet.

[0161] The results are shown in Table 1.

[0162] <Example 4>

[0163] The same experiment as in Example 1 was conducted except that the thickness of the first adhesive layer was set to 50 μm.

[0164] The results are shown in Table 1.

[0165] <Example 5>

[0166] A fluorine-based adhesive layer (25 μm thick) and a polyimide coating (50 μm thick) were additionally formed between the first insulating layer and the second adhesive layer in Example 1. Specifically, the high-strength, high-insulation sheet, first adhesive layer, first insulating layer, fluorine-based adhesive layer (25 μm thick), polyimide coating (50 μm thick), second adhesive layer, heat-generating layer, third adhesive layer, and second insulating layer were laminated in this order.

[0167] And, except for this, the same experiment as in Example 1 was performed.

[0168] The results are shown in Table 1.

[0169] <Example 6>

[0170] The same experiment as in Example 1 was conducted except that a 50 μm-thick PTFE cloth (FGF-500-2 manufactured by Chunghsoo Chemical Industry Co., Ltd.) was used as the high-strength and high-insulation sheet and the thickness of the first insulating layer was set to 25 μm.

[0171] The results are shown in Table 1.

[0172] <Example 7>

[0173] The same experiment as in Example 1 was conducted except that PTFE cloth (FGF-500-6 manufactured by Chunghsoo Chemical Industry Co., Ltd.) with a thickness of 125 μm was used as the high-strength and high-insulation sheet.

[0174] <Example 8>

[0175] The same experiment as in Example 1 was conducted except that the thickness of the first adhesive layer was set to 20 μm.

[0176] The results are shown in Table 1.

[0177] <Example 9>

[0178] The same experiment as in Example 1 was conducted except that the thickness of the first insulating layer was set to 75 μm.

[0179] The results are shown in Table 1.

[0180] <Comparative Example 1>

[0181] The same experiment as in Example 1 was conducted except that PTFE cloth (FGF-500-10 manufactured by Chunghsoo Chemical Industry Co., Ltd.) with a thickness of 250 μm was used as the high-strength and high-insulation sheet and the thickness of the first insulating layer was set to 25 μm.

[0182] The results are shown in Table 1.

[0183] <Comparative Example 2>

[0184] As a high-strength and high-insulation sheet, a PTFE cloth (manufactured by Chunghsing Chemical Industry Co., Ltd., FGF-500-10) with a thickness of 250 μm was used, the thickness of the first adhesive layer was set to 50 μm, and the thickness of the first insulating layer was set to 25 μm. Except for this, the same experiment as in Example 1 was conducted.

[0185] The results are shown in Table 1.

[0186] <Comparative Example 3>

[0187] A 30 μm thick aluminum layer was attached using an adhesive to the main surface (the main surface without the first adhesive layer) of the high-strength, high-insulation sheet of the sheet heater in Comparative Example 1. The adhesive used here was the same as that used to form the first adhesive layer, and the thickness of the adhesive layer X formed by the adhesive used to attach the aluminum layer was 25 μm.

[0188] Except for this, the same experiment as in Comparative Example 1 was performed.

[0189] The results are shown in Table 1.

[0190] [Table 1]

[0191]

[0192] As shown in Table 1, it can be confirmed that if the thickness of the first insulating layer (h1) is equal to the total thickness (H total ) ratio (h1 / H total ) is 0.10 or more, the elongation % becomes lower, which is preferred.

[0193] On the other hand, in the case of Comparative Examples 1 to 3 in which the value was less than 0.1, the elongation % was high.

[0194] [Experiment 2]

[0195] <Example 10>

[0196] The first, second, and third adhesive layers in Example 1 were formed from a fluorine-based adhesive having a storage modulus (E2) at 70°C relative to the storage modulus (E1) at 25°C (percentage: E2 / E1 × 100) of 50%. The thickness was set to 25 μm, similar to Example 1. The remaining high-strength, high-insulation sheet, first insulating layer, heat-generating layer, and second insulating layer were identical to those in Example 1, producing a sheet heater.

[0197] Then, a test was conducted in which the sheet-shaped heater was wound around a stainless steel pipe having an outer diameter of 42.7 mm and an inner diameter of 35.7 mm.

[0198] The details are as follows.

[0199] First, the stainless steel pipe and the sheet heater were placed in an oven whose interior was adjusted to 110° C., and heated for 30 minutes.

[0200] Next, while the stainless steel pipe and the sheet heater were heated in an oven, the sheet heater was wound around the stainless steel pipe, and this state was maintained for 10 minutes.

[0201] Next, the stainless steel pipe around which the sheet-shaped heater was wound was taken out of the oven in this state and naturally cooled to room temperature in the room.

[0202] Next, the sheet heater was removed from the stainless steel pipe, and the inner diameter of the sheet heater formed into a cylindrical shape or a partial shape thereof was measured.

[0203] This inner diameter was then compared with the outer diameter of the stainless steel pipe (42.7 mm). If the inner diameter of the deformed sheet heater exceeded the outer diameter of the stainless steel pipe by 10 mm or more, it was determined that the winding was not fixed (indicated by "X" in Table 2). If it did not exceed 10 mm or more, it was determined that the winding was fixed (indicated by "O" in Table 2).

[0204] The results are shown in Table 2.

[0205] <Example 11>

[0206] In Example 10, the first adhesive layer, the second adhesive layer and the third adhesive layer are formed by a fluorine-based adhesive having a ratio of the storage modulus (E2) at 70°C to the storage modulus (E1) at 25°C (percentage: E2 / E1×100) of 50%, but in Example 11, the first adhesive layer, the second adhesive layer and the third adhesive layer are formed by a fluorine-based adhesive having a ratio of the storage modulus (E2) at 70°C to the storage modulus (E1) at 25°C (percentage: E2 / E1×100) of 70%.

[0207] Then, except for the above, the same operation as in Example 10 was carried out to produce a sheet heater, and the same test was carried out.

[0208] The results are shown in Table 2.

[0209] <Comparative Example 4>

[0210] In Example 10, the first adhesive layer, the second adhesive layer and the third adhesive layer are formed by a fluorine-based adhesive having a ratio of the storage modulus (E2) at 70°C to the storage modulus (E1) at 25°C (percentage: E2 / E1×100) of 50%, but in Comparative Example 4, the first adhesive layer, the second adhesive layer and the third adhesive layer are formed by a paraffin-based adhesive having a ratio of the storage modulus (E2) at 70°C to the storage modulus (E1) at 25°C (percentage: E2 / E1×100) of 5%.

[0211] Then, except for the above, the same operation as in Example 10 was carried out to produce a sheet heater, and the same test was carried out.

[0212] The results are shown in Table 2.

[0213] <Comparative Example 5>

[0214] In Example 10, the first adhesive layer, the second adhesive layer and the third adhesive layer are formed by a fluorine-based adhesive whose ratio of the storage modulus (E2) at 70°C to the storage modulus (E1) at 25°C (percentage: E2 / E1×100) is 50%, but in Comparative Example 4, the first adhesive layer, the second adhesive layer and the third adhesive layer are formed by a polyimide-based adhesive whose ratio of the storage modulus (E2) at 70°C to the storage modulus (E1) at 25°C (percentage: E2 / E1×100) is 100%.

[0215] Then, except for the above, the same operation as in Example 10 was carried out to produce a sheet heater, and the same test was carried out.

[0216] The results are shown in Table 2.

[0217] [Table 2]

[0218] <![CDATA[E2 / E1×100]]> Winding and shaping Example 10 50 ○ Example 11 70 ○ Comparative Example 4 5 × Comparative Example 5 100 ×

[0219] The sheet heaters obtained in Examples 10 and 11 were able to be well wound and set.

[0220] In contrast, the sheet heaters of Comparative Examples 4 and 5 could not be properly wound and fixed.

[0221] This application claims priority based on Japanese Patent Application No. 2022-056330, filed on March 30, 2022, and incorporates herein in its entirety the disclosed contents.

[0222] Description of Reference Numerals

[0223] 1. Heater of the present invention

[0224] 3. High strength and high insulation sheet

[0225] 5. First bonding layer

[0226] 7 First insulation layer

[0227] 9 Second adhesive layer

[0228] 11 Heating layer

[0229] 13 Third bonding layer

[0230] 15 Second insulation layer

Claims

1. A sheet heater, which is stacked in sequence: High-strength, high-insulation sheet with fluororesin impregnated in the reinforcing fiber; a first adhesive layer; a first insulating layer; a second adhesive layer; as well as Heating layer, The high-strength and high-insulation sheet and the main surface of the first adhesive layer are in close contact with each other. The first adhesive layer and the main surface of the first insulating layer are in close contact with each other, The second adhesive layer and the main surface of the heat generating layer are in close contact with each other. The thickness (h1) of the first insulating layer is equal to the total thickness (H1) of the high-strength and high-insulating sheet, the first adhesive layer, and the first insulating layer. total ) ratio (h1 / H total ) is greater than 0.

10.

2. The sheet heater according to claim 1, wherein the total thickness is 200 to 800 μm.

3. The sheet heater according to claim 1 or 2, wherein: The thickness of the high-strength and high-insulation sheet is 100 to 300 μm. The thickness of the first adhesive layer is 5-50 μm.

4. The sheet heater according to any one of claims 1 to 3, wherein The heat generating layer is formed of a metal fiber sheet.

5. The sheet heater according to any one of claims 1 to 4, wherein The first adhesive layer and / or the second adhesive layer is formed of a fluorine-based adhesive having a ratio of a storage modulus (E2) at 70° C. to a storage modulus (E1) at 25° C. (percentage: E2 / E1×100) of 8 to 92%.

6. The sheet heater according to any one of claims 1 to 5, wherein The first adhesive layer is formed of a fluorine-based adhesive having a solubility of 5 to 30% by mass as determined by a solvent solubility test. The solvent solubility test is as follows: 1000 g of tetrahydrofuran (THF) is put into a 2 L plastic bottle and adjusted to 23° C., and while stirring the bottle at 600 rpm using a medium viscosity stirrer using a disperser blade with a blade diameter of 40 mm as a stirring blade, 1 to 50 g of a granular sample with a diameter of 0.5 to 2.0 cm is added, and after 24 hours, it is confirmed whether all the sample has dissolved. If all the sample has dissolved, 1 to 50 g of the sample is added again and it is confirmed whether the sample has dissolved after 24 hours. This operation is repeated to determine the maximum amount (solubility) that can be dissolved.