A polyimide-based composite dielectric film and its preparation method and application in electrical insulation
By introducing fluorenyl and aluminum oxide clusters on the polyimide molecular chain, a polyimide composite dielectric film was prepared, which solved the problem of poor insulation characteristics of polyimide dielectric materials, significantly improved the breakdown field strength and Insulation performance, suitable for electrical insulation devices in new energy vehicles and other fields.
Patent Information
- Application Number
- CN202311549291.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-11-21
AI Technical Summary
The inherent insulation characteristics of polyimide dielectric materials are poor, which leads to the problem of insulation failure in new energy vehicle drive motors.
By introducing fluorenyl and aluminum oxide clusters on the polyimide molecular chain, polyimide composite dielectric film was prepared by in-situ synthesis method, and imidized by dropping addition of sec-butoxide aluminum and infrared lamp irradiation. , a modified polyimide material with excellent insulating properties is formed.
It significantly improves the breakdown field strength of polyimide materials, improves insulation performance, and has a simple process and low cost. It is suitable for a wide range of applications of electrical insulating devices.
Smart Images

Figure CN117683351B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polyimide-based composite dielectric film and a preparation method thereof and application in electrical insulation, belonging to the technical field of polyimide-based modified composite materials and preparation thereof. Background Art
[0002] In the drive motor of new energy vehicles, the motor has uneven air gap electric field strength and concentrated electric field at the R corner due to structural reasons. In addition, the internal structure of the winding is compact, and heat is difficult to conduct away in time, resulting in heat accumulation. Under the combined effect of multiple factors, it is easy to cause motor insulation failure. In recent years, with the widespread application of drive motors for new energy vehicles, higher requirements have been put forward for motor insulation systems.
[0003] Polyimide (PI) is an excellent engineering plastic with wide applications and good performance. Due to its aromatic heterocyclic structure, polyimide has excellent mechanical properties, electrical properties, radiation resistance, electrical insulation properties and chemical stability. In recent years, with the advancement of science and technology and the increasing convenience of transportation modes such as motor vehicles and ships, the voltage level of drive motors has also increased, and the importance of polyimide in insulation systems has become increasingly prominent. Therefore, the preparation of polyimide composite films with good insulation properties is of great significance to the development of society.
[0004] At present, in order to solve the problem of poor intrinsic insulation performance of polyimide, most of the research uses inorganic materials as fillers to introduce into the polymer matrix to synthesize inorganic / polymer composite materials. However, inorganic nanoparticles have a large specific surface area, and the introduction of high-mass fraction inorganic fillers will lead to problems such as inorganic particle agglomeration, resulting in carrier traps or defects inside the material, leading to increased energy loss, and reducing the breakdown field strength of the composite material, thus causing insulation failure of the device. Therefore, in the current technology, starting from the molecular structure of polyimide, optimizing its insulation performance from the intrinsic structure has become an important research hotspot.
[0005] Therefore, for polyimide dielectric materials, how to design polyimide-based composite dielectric materials that intrinsically have excellent insulation properties has become an existing technical problem. Summary of the invention
[0006] In order to solve the technical problem that the existing polyimide dielectric materials have poor intrinsic insulation properties, the present invention provides a polyimide-based composite dielectric film and a preparation method thereof and application in electrical insulation, especially application in polyimide intrinsic modification technology.
[0007] The technical solution of the present invention:
[0008] One of the purposes of the present invention is to provide a method for preparing a polyimide-based composite dielectric film, the method comprising the following steps:
[0009] (1) preparing a glue solution by polycondensation of diamine and dianhydride;
[0010] The diamine includes a fluorene-containing diamine;
[0011] (2) adding aluminum sec-butoxide dropwise to the glue solution and stirring under vacuum conditions to obtain a modified glue solution;
[0012] (3) A wet film is prepared by a coating method using a modified adhesive solution, and the wet film is subjected to an imidization treatment after being irradiated by an infrared lamp to obtain a polyimide-based composite dielectric film.
[0013] It is further defined that the specific operation process of (1) is: adding diamine to an organic solvent, stirring to completely dissolve it, and then adding dianhydride, and subjecting it to polycondensation reaction under vacuum conditions to obtain a glue solution (fPAA).
[0014] It is further defined that the diamine is 9,9-bis(4-amino-3-fluorophenyl)fluorene and diaminodiphenyl ether in a molar ratio of 1:(1-50).
[0015] In a further embodiment, the diamine is composed of 9,9-bis(4-amino-3-fluorophenyl)fluorene and diaminodiphenyl ether in a molar ratio of 1:(9-36).
[0016] In a further embodiment, the dianhydride is pyromellitic anhydride.
[0017] It is further defined that the organic solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methylpyrrolidone, and tetrahydrofuran mixed in any proportion.
[0018] In a further embodiment, the organic solvent is N,N-dimethylformamide or N,N-dimethylacetamide.
[0019] It is further defined that the polycondensation reaction temperature in (1) is -10°C to 40°C and the reaction time is 6h to 24h.
[0020] It is further defined that the polycondensation reaction temperature in (1) is -5°C to 10°C and the reaction time is 6h to 24h.
[0021] It is further defined that the molar ratio of diamine to dianhydride in (1) is 1:1.02 to 1.08.
[0022] It is further defined that the molar ratio of diamine to dianhydride in (1) is 1:1.02 to 1.04.
[0023] It is further defined that the mass fractions of the diamine and the dianhydride in the polycondensation reaction system are both 12% to 35%.
[0024] It is further defined that the specific operation process of (2) is: adding aluminum sec-butoxide into the glue solution at a certain volume fraction to obtain a modified glue solution (fPAA-AOC).
[0025] It is further defined that the volume fraction of aluminum sec-butoxide in the modified rubber solution of (2) is 0.5 vol% to 2 vol%.
[0026] It is further defined that the volume fraction of aluminum sec-butoxide in the modified rubber solution of (2) is 0.75 vol% to 1.5 vol%.
[0027] It is further defined that the vacuum conditions in (1) and (2) are achieved by a step vacuum method, and specifically, the vacuum gradient interval of each step vacuum is 1 Pa to 5 Pa, the vacuum rate is 1 Pa / min to 2 Pa / min, and the constant vacuum time of each step is 30 min to 180 min.
[0028] It is further defined that the vacuum conditions in (1) and (2) are achieved by a step vacuum method, and specifically, the vacuum gradient interval of each step vacuum is 1Pa to 5Pa, the vacuum rate is 1Pa / min to 2Pa / min, and the constant vacuum time of each step is 60min to 120min.
[0029] It is further defined that the specific operation process of (3) is: pouring the modified adhesive solution onto the surface of a clean glass substrate to coat the glass substrate to form a wet film, and then subjecting the film to infrared light irradiation and thermal imidization treatment, and then naturally cooling the film to room temperature to obtain a modified polyimide-AOC (fPI-AOC), which is a polyimide-based composite dielectric film.
[0030] It is further defined that: (3) the power of the mid-infrared lamp is 2000W and the irradiation time is 3s to 5s.
[0031] It is further defined that the imidization in (3) is achieved by gradient heating, and the specific temperature gradient interval of each stage of the gradient heating is 20°C to 50°C, the heating rate is 2°C / min to 15°C / min, and the constant temperature time of each stage is 30min to 120min.
[0032] It is further defined that the imidization in (3) is achieved by gradient heating, and the specific temperature gradient interval of each stage of the gradient heating is 20°C to 50°C, the heating rate is 2°C / min to 15°C / min, and the constant temperature time of each stage is 60min to 90min.
[0033] It is further defined that the coating method is blade coating, spin coating or drop coating.
[0034] It is further defined that the coating speed of the scraper coating is 10 to 25 cm / min and the time is 10 to 60 s.
[0035] It is further defined that the coating speed of the scraper coating is 15 to 20 cm / min and the time is 20 to 40 s.
[0036] The second object of the present invention is to provide a polyimide-based composite dielectric film obtained by the above preparation method, wherein the thickness of the film is 3 to 20 μm.
[0037] The third object of the present invention is to provide an application of the polyimide-based composite dielectric film, specifically, as a high-field insulator for the preparation of electrical insulation devices.
[0038] It is further defined that electrical insulation devices include, but are not limited to, the fields of fast charging and discharging technology such as new energy vehicles, AC and DC power transmission networks, high-frequency power transformers, and aerospace.
[0039] Beneficial effects:
[0040] The present invention introduces fluorene groups and aluminum oxide clusters into polyimide to prepare a modified polyimide flexible dielectric with excellent insulation properties, thereby solving the problem of poor intrinsic insulation properties of polyimide. Compared with the prior art, the polyimide-based composite dielectric prepared by the present invention has the following advantages:
[0041] (1) The present invention adopts an in-situ synthesis method to prepare a polyimide film material with high breakdown field strength by introducing a large volume group fluorene and a metal aluminum oxide cluster (-AOC) into a polyimide molecular chain. The DC breakdown field strength of the polyimide dielectric material at room temperature is 672.2 MV / m, which is 54.6% higher than that of the conventional polyimide dielectric material prepared by using pyromellitic anhydride and diaminodiphenyl ether. The DC breakdown field strength at 150°C is 651.9 MV / m, which is 56.9% higher than that of the conventional polyimide dielectric material prepared by using pyromellitic anhydride and diaminodiphenyl ether.
[0042] (2) The present invention introduces F atoms into the polyimide molecular chain. The F atoms have strong electronegativity and reduce the electron donation of the diamine through steric hindrance effect and inductive effect, thereby reducing the charge transfer complex between polymer chains and between molecules, thereby significantly improving the breakdown field strength of the polyimide. At the same time, the fluorene group is a large-volume group. Introducing it into the molecular chain of polyimide can destroy the arrangement of the chain and increase the free volume, thereby reducing the dielectric constant of the polyimide, and significantly improving the insulating properties of the polyimide material.
[0043] (3) Furthermore, the present invention introduces metal aluminum oxide clusters on the basis of polyimide molecular modification. After adding aluminum sec-butoxide, a large number of carboxyl groups in the polyamic acid glue are fixed by covalent bonds during the in-situ polymerization process, and the F atoms in the fluorene group are fixed by hydrogen bonds, and then separated during the thermal imidization process to form aluminum oxide clusters. This method does not require additional auxiliary dispersion steps, improves the problem of poor dispersibility of inorganic particles, and improves the insulation performance of the polyimide composite film.
[0044] (4) In addition, the present invention has the advantages of simple preparation process and required equipment, safety and reliability, low cost, and is more conducive to its wide application in electrical insulation devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a cross-sectional scanning electron microscope image of the polyimide-based composite dielectric material prepared in Comparative Example 1;
[0046] Figure 2 This is a cross-sectional scanning electron microscope image of the polyimide-based composite dielectric material prepared in Example 1;
[0047] Figure 3 This is a cross-sectional scanning electron microscope image of the polyimide-based composite dielectric material prepared in Comparative Example 2;
[0048] Figure 4 This is a cross-sectional scanning electron microscope image of the polyimide-based composite dielectric material prepared in Comparative Example 3;
[0049] Figure 5 This is a cross-sectional scanning electron microscope image of the polyimide-based composite dielectric material prepared in Comparative Example 4;
[0050] Figure 6 This is a cross-sectional scanning electron microscope image of the polyimide-based composite dielectric material prepared in Example 2;
[0051] Figure 7 This is a cross-sectional scanning electron microscope image of the polyimide-based composite dielectric material prepared in Example 3;
[0052] Figure 8 It is a comparative curve diagram of infrared spectra of polyimide-based composite dielectric materials prepared in Comparative Examples 1, 2, 3 and 4;
[0053] Fig. 9 It is a comparative curve diagram of infrared spectra of the polyimide-based composite dielectric materials prepared in Examples 1, 2, 3 and Comparative Example 2;
[0054] Fig.10 The dielectric spectrum of the polyimide-based composite dielectric material prepared in Comparative Examples 1-4 at room temperature;
[0055] Fig.11The dielectric spectra of the polyimide-based composite dielectric materials prepared in Examples 1, 2, 3 and Comparative Example 2 at room temperature;
[0056] Fig.12 The DC breakdown Weibull distribution spectrum of the polyimide-based composite dielectric material prepared in Comparative Examples 1-4 at room temperature;
[0057] Fig.13 The DC breakdown Weibull distribution spectrum of the polyimide-based composite dielectric material prepared in Comparative Examples 1-4 at 150° C.;
[0058] Fig.14 The DC breakdown Weibull distribution spectrum of the polyimide-based composite dielectric material prepared in Examples 1, 2, 3 and Comparative Example 2 at room temperature;
[0059] Fig.15 This is the DC breakdown Weibull distribution spectrum of the polyimide-based composite dielectric materials prepared in Examples 1, 2, 3 and Comparative Example 2 at 150°C. DETAILED DESCRIPTION
[0060] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0061] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0062] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0063] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.
[0064] Comparative Example 1
[0065] Step 1: In a 250 ml round-bottom flask, 1.897 g of diaminodiphenyl ether and 0.202 g of 9,9-bis(4-amino-3-fluorophenyl)fluorene are dissolved in 25.0 ml of N,N-dimethylacetamide. Under a water bath temperature of 0° C., 2.225 g of pyromellitic anhydride is added to the solution in batches at a uniform speed, and the solution is stirred under a gradient vacuum to obtain a modified polyamic acid glue solution.
[0066] The gradient vacuum was carried out in six steps, 25Pa→20Pa→15Pa→10Pa→5Pa→1Pa, the vacuum rate was 1°C / min, each vacuum process was maintained for 120min, and after stirring for 12h, a modified polyamic acid glue solution with a solid content of about 15% was obtained;
[0067] Step 2: Place the modified polyamic acid glue solution in a vacuum oven for degassing treatment, and then coat it on a glass substrate by a scraping process with a scraping speed of 25 cm / min and a scraping time of 30 s. Then, it is subjected to a gradient heating thermal imidization treatment. The gradient heating is carried out in seven steps: 60°C → 80°C → 150°C → 200°C → 250°C → 300°C → 350°C. The heating rate is 5°C / min, and the insulation time of each insulation process is 60 minutes. Finally, a modified polyimide film with a thickness of 7 μm is prepared, which is recorded as fPI-18.
[0068] Figure 1 This is a cross-sectional SEM photograph of the polyimide-based composite medium prepared in Comparative Example 1. Figure 1 It can be seen that the thickness of the modified polyimide-based composite medium is 7 μm, and the thickness is relatively uniform. Figure 1 It can also be seen that the prepared film has a smooth cross-section, basically free of defects such as holes, and has good density.
[0069] Example 1
[0070] Step 1: In a 250 ml round-bottom flask, 1.897 g of diaminodiphenyl ether and 0.202 g of 9,9-bis(4-amino-3-fluorophenyl)fluorene are dissolved in 25.0 ml of N,N-dimethylacetamide. Under a 0° C. water bath condition, 2.225 g of pyromellitic anhydride is added to the solution in batches at a uniform speed interval, and gradient vacuum stirring is performed to obtain a modified polyamic acid glue solution.
[0071] The gradient vacuum was carried out in six steps, 25Pa→20Pa→15Pa→10Pa→5Pa→1Pa, the vacuum rate was 1°C / min, each vacuum process was maintained for 120min, and after stirring for 12h, a modified polyamic acid glue solution with a solid content of about 15% was obtained;
[0072] Step 2: prepare two beakers, measure appropriate amounts of DMAC respectively, add 1 vol% aluminum sec-butoxide to one of the beakers, add appropriate amount of deionized water to the other beaker, and drop the solutions in the two beakers into the pre-polymerized modified polyamic acid glue solution, and stir under gradient vacuum. The gradient vacuum is carried out in six steps, 25pa→20pa→15pa→10pa→5pa→1pa, and the vacuum rate is 1°C / min. Each vacuum process is maintained for 120min. After stirring for 12h, a modified polyamic acid-AOC glue solution with a solid content of about 15% is obtained;
[0073] Step three, placing the modified polyamic acid-AOC glue solution in a vacuum oven for degassing treatment, and then coating it on a glass substrate by a scraping process with a scraping speed of 25 cm / min and a scraping time of 30 s, and then subjected to a gradient heating thermal imidization treatment. The gradient heating is carried out in seven steps, 60°C→80°C→150°C→200°C→250°C→300°C→350°C, with a heating rate of 5°C / min, and the insulation time of each insulation process is 60 min. Finally, a modified polyimide-AOC film with a thickness of 6 μm is prepared, which is recorded as AOC-1.
[0074] Figure 2 This is a cross-sectional SEM photograph of the modified polyimide-AOC prepared in Example 1. Figure 2 It can be seen that the thickness of the modified polyimide-AOC is 6 μm, and the thickness is relatively uniform and controllable, with no obvious visible clusters and good density.
[0075] Comparative Example 2
[0076] Step 1: In a 250 ml round-bottom flask, 2.0024 g of diaminodiphenyl ether was dissolved in 25.0 ml of N,N-dimethylacetamide. Under a 0° C. water bath condition, 2.225 g of pyromellitic anhydride was added to the solution in batches at a uniform speed, and the solution was stirred under gradient vacuum to obtain a polyamic acid glue solution.
[0077] Gradient vacuum stirring, the gradient vacuum is carried out in six steps, 25Pa→20Pa→15Pa→10Pa→5Pa→1Pa, the vacuum rate is 1℃ / min, each vacuum process is maintained for 120min, and after stirring for 12h, a polyamic acid glue solution with a solid content of about 15% is obtained;
[0078] Step 2: Place the polyamic acid glue solution in a vacuum oven for degassing treatment, and then coat it on a glass substrate by a scraping process with a scraping speed of 25 cm / min and a scraping time of 30 s. Then, it is subjected to a gradient heating thermal imidization treatment. The gradient heating is carried out in seven steps: 60°C → 80°C → 150°C → 200°C → 250°C → 300°C → 350°C. The heating rate is 5°C / min, and the insulation time of each insulation process is 60 minutes. Finally, a polyimide film with a thickness of 5 μm is prepared, which is recorded as PI.
[0079] Figure 3 is a cross-sectional SEM photograph of the polyimide-based composite medium prepared in Comparative Example 2; Figure 3 It can be seen that the thickness of the polyimide-based composite medium prepared by the in-situ synthesis method is 5 μm, the thickness is relatively uniform, and no obvious defects such as holes can be observed through the cross-sectional SEM image.
[0080] Comparative Example 3
[0081] Step 1, in a 250 ml round-bottom flask, 1.802 g of diaminodiphenyl ether and 0.384 g of 9,9-bis(4-amino-3-fluorophenyl)fluorene are dissolved in 25.0 ml of N,N-dimethylacetamide, and 2.225 g of pyromellitic anhydride is added to the solution in batches at a uniform interval under 0 ° C water bath conditions, and stirred to obtain a modified polyamic acid glue solution, and gradient vacuum stirring is performed in six steps, 25 Pa → 20 Pa → 15 Pa → 10 Pa → 5 Pa → 1 Pa, and the vacuum rate is 1 ° C / min, each vacuum process is maintained for 120 min, and after stirring for 12 hours, a modified polyamic acid glue solution with a solid content of about 15% is obtained;
[0082] Step 2: Place the polyamic acid glue solution in a vacuum oven for degassing treatment, and then coat it on a glass substrate by a scraping process with a scraping speed of 25 cm / min and a scraping time of 30 s. Then, it is subjected to a gradient heating thermal imidization treatment. The gradient heating is carried out in seven steps: 60°C → 80°C → 150°C → 200°C → 250°C → 300°C → 350°C. The heating rate is 5°C / min, and the insulation time of each insulation process is 60 minutes. Finally, a polyimide film with a thickness of 8 μm is prepared, which is recorded as fPI-9.
[0083] Figure 4 is a cross-sectional SEM photograph of the polyimide-based composite medium prepared in Comparative Example 3; Figure 4 It can be seen that the thickness of the modified polyimide-based composite medium is 8 μm. The thickness of the insulating dielectric material prepared by this preparation method is relatively uniform. Figure 4 It can be seen that the prepared film has a smooth cross-section, basically free of defects such as holes, and has good density.
[0084] Comparative Example 4
[0085] Step 1, in a 250 ml round-bottom flask, 1.948 g of diaminodiphenyl ether and 0.104 g of 9,9-bis(4-amino-3-fluorophenyl)fluorene are dissolved in 25.0 ml of N,N-dimethylacetamide, and 2.225 g of pyromellitic anhydride is added to the solution in batches at a uniform interval under a 0°C water bath condition, and stirred to obtain a modified polyamic acid glue solution, and gradient vacuum stirring is performed in six steps, 25 Pa → 20 Pa → 15 Pa → 10 Pa → 5 Pa → 1 Pa, and the vacuum rate is 1°C / min. Each vacuum process is maintained for 120 min, and after stirring for 12 hours, a modified polyamic acid glue solution with a solid content of about 15% is obtained;
[0086] Step 2: Place the polyamic acid glue solution in a vacuum oven for degassing treatment, and then coat it on a glass substrate by a scraping process with a scraping speed of 25 cm / min and a scraping time of 30 s. Then, it is subjected to a gradient heating thermal imidization treatment. The gradient heating is carried out in seven steps: 60°C → 80°C → 150°C → 200°C → 250°C → 300°C → 350°C. The heating rate is 5°C / min, and the insulation time of each insulation process is 60 minutes. Finally, a polyimide film with a thickness of 12 μm is prepared, which is recorded as fPI-36.
[0087] Figure 5 is a cross-sectional SEM photograph of the polyimide-based composite medium prepared in Comparative Example 4; Figure 5 It can be seen that the thickness of the modified polyimide-based composite medium is 12 μm. The thickness of the insulating dielectric material prepared by this preparation method is relatively uniform. Figure 5 It can be seen that the prepared film has a smooth cross-section, basically free of defects such as holes, and has good density.
[0088] Example 2
[0089] Step 1: In a 250 ml round-bottom flask, 1.897 g of diaminodiphenyl ether and 0.202 g of 9,9-bis(4-amino-3-fluorophenyl)fluorene are dissolved in 25.0 ml of N,N-dimethylacetamide. Under a 0° C. water bath condition, 2.225 g of pyromellitic anhydride is added to the solution in batches at a uniform interval, and stirred to obtain a modified polyamic acid glue solution. The gradient vacuum is stirred in six steps, 25 Pa → 20 Pa → 15 Pa → 10 Pa → 5 Pa → 1 Pa, and the vacuum rate is 1° C. / min. Each vacuum process is maintained for 120 min. After stirring for 12 hours, a modified polyamic acid-AOC glue solution with a solid content of about 15% is obtained;
[0090] Step 2: prepare two beakers, measure appropriate amounts of DMAC respectively, add 0.75 vol% aluminum sec-butoxide to one of the beakers, add appropriate amount of deionized water to the other beaker, and drop the solutions in the two beakers into the pre-polymerized modified polyamic acid glue solution, and stir under gradient vacuum. The gradient vacuum is carried out in six steps, 25 Pa → 20 Pa → 15 Pa → 10 Pa → 5 Pa → 1 Pa, and the vacuum rate is 1 ° C / min. Each vacuum process is maintained for 120 min. After stirring for 12 hours, a modified polyamic acid-AOC glue solution with a solid content of about 15% is obtained;
[0091] Step three, placing the modified polyamic acid-AOC glue in a vacuum oven for degassing treatment, and then coating it on a glass substrate by a scraping process with a scraping speed of 25 cm / min and a scraping time of 30 s, and then subjected to a gradient heating thermal imidization treatment. The gradient heating is carried out in seven steps, 60°C→80°C→150°C→200°C→250°C→300°C→350°C, with a heating rate of 5°C / min, and the insulation time of each insulation process is 60 min. Finally, a modified polyimide-AOC film with a thickness of 6 μm is prepared, recorded as AOC-0.75.
[0092] Figure 6 The cross-sectional SEM photograph of the polyimide-based composite medium prepared in Example 2; Figure 6 It can be seen that the thickness of the modified polyimide-AOC insulating medium is 6 μm. The thickness of the insulating medium material prepared by the preparation method is relatively uniform. Figure 6 It can be seen that the prepared film has a smooth cross-section, basically no defects such as holes, and no obvious alumina clusters, and has good density.
[0093] Example 3
[0094] Step 1: In a 250 ml round-bottom flask, 1.897 g of diaminodiphenyl ether and 0.202 g of 9,9-bis(4-amino-3-fluorophenyl)fluorene are dissolved in 25.0 ml of N,N-dimethylacetamide. Under a 0° C. water bath condition, 2.225 g of pyromellitic anhydride is added to the solution in batches at a uniform interval, and stirred to obtain a modified polyamic acid glue solution. The gradient vacuum is stirred in six steps, 25 Pa → 20 Pa → 15 Pa → 10 Pa → 5 Pa → 1 Pa, and the vacuum rate is 1° C. / min. Each vacuum process is maintained for 120 min. After stirring for 12 hours, a modified polyamic acid-AOC glue solution with a solid content of about 15% is obtained;
[0095] Step 2, prepare two beakers, measure appropriate amounts of DMAC respectively, add 1.25 vol% aluminum sec-butoxide to one of the beakers, add appropriate amount of deionized water to the other beaker, add the solutions in the two beakers to the pre-polymerized modified polyamic acid glue, and stir under gradient vacuum. The gradient vacuum is carried out in six steps, 25pa→20pa→15pa→10pa→5pa→1pa, and the vacuum rate is 1°C / min. Each vacuum process is maintained for 120min. After stirring for 12h, a modified polyamic acid-AOC glue with a solid content of about 15% is obtained;
[0096] Step three, placing the modified polyamic acid-AOC glue solution in a vacuum oven for degassing treatment, and then coating it on a glass substrate by a scraping process with a scraping speed of 25 cm / min and a scraping time of 30 s, and then subjected to a gradient heating thermal imidization treatment. The gradient heating is carried out in seven steps, 60°C→80°C→150°C→200°C→250°C→300°C→350°C, with a heating rate of 5°C / min, and the insulation time of each insulation process is 60 min. Finally, a modified polyimide-AOC film with a thickness of 7 μm is prepared, recorded as AOC-1.25.
[0097] Figure 7 This is a cross-sectional SEM photograph of the polyimide-based composite medium prepared in Example 3; Figure 7 It can be seen that the thickness of the modified polyimide-AOC insulating medium is 7 μm. The thickness of the insulating medium material prepared by the preparation method is relatively uniform. Figure 7 It can be seen that the prepared film has a smooth cross-section, basically free of defects such as holes, and there are a few visible metal aluminum oxide clusters, but due to the fixing effect of carboxyl groups and hydrogen bonds, its dispersion is still relatively uniform and has good density.
[0098] Effect example
[0099] The structure and performance of the polyimide-based composite dielectric materials obtained in Examples 1-3 and Comparative Examples 1-4 were characterized, and the results are as follows:
[0100] Figure 8 The infrared spectrum comparison curves of the polyimide-based composite dielectric materials prepared in Comparative Examples 1-4 are shown in FIG. Figure 8 It can be seen that the synthesized fPI is at 1784cm -1 The characteristic peak near 1726 cm -1 The symmetrical stretching vibration of the two carbonyl groups on the imide ring appeared, proving that the imidization of the film was successful.
[0101] Fig. 9 The infrared spectra of the polyimide-based composite dielectric materials prepared in Examples 1-3 and Comparative Example 2 are compared. Fig. 9It can be seen that the synthesized fPI-AOC has a peak at 1784 cm -1 The characteristic peak near 1726 cm -1 The symmetrical stretching vibration of the two carbonyl groups on the imide ring appeared, proving that the imidization of the film was successful.
[0102] Fig.10 The dielectric spectrum of the polyimide-based composite dielectric material prepared in Comparative Examples 1-4 at room temperature is Fig.10 It can be seen that the fPI prepared in Comparative Example 1 has the lowest dielectric constant. This is because the free volume of the fluorene group is large, which disrupts the linear structure of the polyimide molecular chain and increases its free volume. At the same time, fluorine has a strong electron-withdrawing ability, so the dielectric constant of the prepared polyimide is reduced, thereby reducing the dielectric constant.
[0103] Fig.11 The dielectric spectra of the polyimide-based composite dielectric materials prepared in Examples 1, 2, 3 and Comparative Example 2 at room temperature are as follows: Fig.11 It can be seen that with the increase of aluminum sec-butoxide content, the dielectric constant increases successively. This is because with the increase of aluminum sec-butoxide content, the content of aluminum oxide clusters in the modified polyimide-AOC composite film becomes larger successively, resulting in an increase in the dielectric constant, but the dielectric constant of the composite film still remains at a low level.
[0104] Fig.12 and Fig.13 The Weibull distribution diagrams of the DC breakdown field strength of the polyimide-based composite dielectric materials prepared in Comparative Examples 1-4 at room temperature and 150°C are shown in FIG. Fig.12 and Fig.13 It can be seen that the breakdown field strength of fPI-18 prepared in Comparative Example 1 is significantly higher than that of other polyimide-based composite dielectrics. The DC breakdown field strength at room temperature is 614.8 MV / m, which is 41.4% higher than that of the traditional polyimide dielectric material prepared by using pyromellitic anhydride and diaminodiphenyl ether. The DC breakdown field strength at 150°C is 603.5 MV / m, which is 45.2% higher than that of the traditional polyimide dielectric material prepared by using pyromellitic anhydride and diaminodiphenyl ether. This is because the fluorene group has a large free volume, which causes the destruction of the conjugated structure of the PI molecular chain, as well as the enhancement of the chain spacing and the reduction of the molecular chain packing density, which increases the free volume of the system. At the same time, the fluorene group contains F atoms, which have strong electronegativity. The electron donating property of the diamine is reduced through the steric hindrance effect and the inductive effect, and the charge transfer complex between polymer chains and molecules is reduced, thereby significantly improving the breakdown field strength of the modified polyimide.
[0105] Fig.14 and Fig.15The Weibull distribution diagrams of the DC breakdown field strength of the polyimide-based composite dielectric materials prepared in Examples 1, 2, 3 and Comparative Example 2 at room temperature and 150° C. are shown in FIG. Fig.14 and Fig.15 It can be seen that the breakdown field strength of AOC-1 prepared in Example 1 is significantly higher than that of other polyimide-based composite dielectrics. The DC breakdown field strength at room temperature is 672.2 MV / m, which is 54.6% higher than that of the traditional polyimide dielectric material prepared by using pyromellitic anhydride and diaminodiphenyl ether. The DC breakdown field strength at 150°C is 651.9 MV / m, which is 56.9% higher than that of the traditional polyimide dielectric material prepared by using pyromellitic anhydride and diaminodiphenyl ether. This is because the fluorene group has a large free volume, which causes the destruction of the conjugated structure of the PI molecular chain, as well as the enhancement of the chain spacing and the reduction of the molecular chain packing density, which increases the free volume of the system. At the same time, the fluorene group contains F atoms, which have strong electronegativity. The electron donating property of the diamine is reduced through the steric hindrance effect and the inductive effect, and the charge transfer complex between polymer chains and molecules is reduced. In addition, the metal aluminum oxide clusters introduce deep traps in the composite medium, which enhances its ability to capture charges, thereby significantly enhancing the breakdown field strength.
[0106] Although the present invention has been disclosed as above in the preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for preparing a polyimide-based composite dielectric film, characterized in that: include: (1) preparing a glue solution by polycondensation of diamine and dianhydride under vacuum conditions; The diamine includes a fluorene-containing diamine; The molar ratio of diamine to dianhydride in (1) is 1:1.02-1.08, and the mass fractions of diamine and dianhydride in the reaction system are both 12-35%; The diamine is composed of 9,9-bis(4-amino-3-fluorophenyl)fluorene and diaminodiphenyl ether in a molar ratio of 1:1 to 50; (2) adding aluminum sec-butoxide dropwise to the glue solution and stirring under vacuum conditions to obtain a modified glue solution; The volume fraction of aluminum sec-butoxide in the modified glue is 0.5 vol% to 2 vol%; (3) A wet film is prepared by a coating method using a modified adhesive solution, and the wet film is subjected to an imidization treatment after being irradiated by an infrared lamp to obtain a polyimide-based composite dielectric film.
2. The preparation method according to claim 1, characterized in that: The dianhydride is pyromellitic anhydride.
3. The preparation method according to claim 1, characterized in that: (1) The polycondensation reaction temperature is -10 to 40°C and the reaction time is 6 to 24 hours.
4. The preparation method according to claim 1, characterized in that: The vacuum conditions in (1) and (2) are achieved by a step vacuum method. Specifically, the vacuum gradient interval of each step vacuum is 1 to 5 Pa, the vacuum rate is 1 to 2 Pa / min, and the constant vacuum time of each step is 30 to 180 min.
5. The preparation method according to claim 1, characterized in that: (3) The power of the mid-infrared lamp is 2000W and the irradiation time is 3 to 5s.
6. The preparation method according to claim 1, characterized in that: (3) The intermediate imidization is achieved by gradient heating, wherein the specific temperature gradient interval of each section of the gradient heating is 20 to 50°C, the heating rate is 2 to 15°C / min, and the constant temperature time of each section is 30 to 120 min.
7. A polyimide-based composite dielectric film obtained by the preparation method according to any one of claims 1 to 6, characterized in that: The thickness is 3 to 20 μm.
8. An application of the polyimide-based composite dielectric film according to claim 7, characterized in that: Used in the preparation of electrical insulation devices.
Citation Information
Patent Citations
High-temperature energy storage hybrid polyetherimide dielectric film and preparation method and application thereof
CN112789326A
Low-dielectric copolyimide film and preparation method thereof
CN113563584A