Talcum powder modified biochar composite material as well as preparation method and application thereof
Through the co-thermopyrolysis method of talc powder and biochar and the introduction of dicyandiamide, an efficient talc powder modified biochar composite material is formed, which solves the problem of limited passivation effect of heavy metals in clay mineral passivator and realizes the small amount Better repair effects of heavy metal pollution in soil.
Patent Information
- Application Number
- CN202411082941.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-08
AI Technical Summary
Existing clay mineral passivators have limited passivation effects in soil, and excessive use may damage the soil structure, affect plant root growth, and reduce crop yield.
The co-thermopyrolysis method of talc powder and biochar is used to form a talc powder modified biochar composite with a porous structure and high adsorption capacity, and dicyandiamide is introduced at a specific opportunity to improve the heavy metal passivation ability of the composite material.
At a smaller dose, the passivation effect of soil heavy metals is significantly improved, the heavy metal adsorption capacity of composite materials is improved, the damage to soil structure is reduced, and the soil pollution repair effect is achieved.
Smart Images

Figure BDA0004984307300000071 
Figure BDA0004984307300000081 
Figure BDA0004984307300000082
Abstract
Description
Technical Field
[0001] The invention relates to the field of heavy metal passivators, and in particular to a talc-modified biochar composite material and a preparation method and application thereof. Background Art
[0002] Clay minerals are the main minerals that make up clay rocks and soils. They are formed by weathering, hydrothermal and hot spring water, and sedimentation on rocks. They mainly include kaolinite, illite, montmorillonite, vermiculite, talc, and sepiolite. Clay minerals are an important component of soil colloids. They have strong polarity and adsorption due to their high stability, large specific surface area, and large ion exchange capacity. They play a huge role in repairing soil heavy metal pollution. Currently, commonly used natural mineral passivators include montmorillonite, attapulgite, sepiolite, and limestone. After these passivators are applied to the soil, they can transform heavy metals from an exchangeable state to a stable state through adsorption, precipitation, complexation, ion exchange, and oxidation-reduction, thereby reducing the mobility and bioavailability of heavy metals.
[0003] Clay minerals as passivating agents for soil remediation have the advantages of large specific surface area, strong adsorption, high stability, etc. They can increase soil pH and improve soil physical and chemical properties. However, excessive application of clay minerals may also damage soil structure, affect plant root growth and reduce crop yields. Therefore, it is of great significance to improve the heavy metal passivation effect of clay minerals, so as to achieve better soil heavy metal pollution remediation effect at a smaller dosage. Summary of the invention
[0004] In order to solve the technical problem that clay minerals have limited effect in passivating heavy metals, the present invention provides a method for preparing a talc-modified biochar composite material. The preparation method composites biochar and talc together through co-thermal pyrolysis, which can achieve better heavy metal passivation effect.
[0005] The specific technical scheme of the present invention is: In a first aspect, the present invention provides a method for preparing a talc-modified biochar composite material, comprising the following steps: mixing talc with a biomass material, and co-pyrolyzing the biomass material under oxygen-limited conditions until the biomass material is carbonized and sintered together with the talc to obtain a talc-modified biochar composite material.
[0006] Biomass materials can form biochar with a porous structure after pyrolysis and carbonization. The present invention adopts the method of co-thermal pyrolysis of talcum powder and biomass materials, and can use talcum powder to cover the surface of biochar formed after the carbonization of biomass materials with irregular particles, thereby increasing the specific surface area of biochar, and introducing more functional groups that can fix heavy metal ions on its surface. At the same time, biochar can use its good adsorption to fix heavy metal ions. In the above manner, the combined biochar and talcum powder can cooperate with each other, so that the heavy metal passivation ability of the composite material is significantly improved compared with the use of biochar and talcum powder alone, so when used for soil heavy metal pollution remediation, better effects can be achieved at a smaller dosage.
[0007] Preferably, the mass ratio of the biomass material to talcum powder is 1:1-2.
[0008] Preferably, the co-thermal pyrolysis process specifically includes: heating to 500-550° C. at 25-30° C. / min and maintaining for 1-1.5 h.
[0009] In a second aspect, the present invention provides a method for preparing a talc-modified biochar composite material, comprising the following steps: (1) Under oxygen-limited conditions, the biomass material is heated to 332-337° C. at a rate of 25-30° C. / min, maintained for 3-6 min, and cooled to obtain a preliminary pyrolysis material; (2) loading dicyandiamide in the preliminary pyrolysis material and talc respectively; (3) Under oxygen-limited conditions, the preliminary pyrolysis material loaded with dicyandiamide was calcined at 390-400°C for 10-15 min, talcum powder loaded with dicyandiamide was added and mixed, the temperature was raised to 500-550°C and calcined for 50-60 min, and then calcined at 750-800°C for 1-1.5 h to obtain a talc-modified biochar composite material.
[0010] By loading dicyandiamide in the preliminary pyrolysis material, dicyandiamide is completely decomposed after being roasted at 750-800°C, and a relatively stable nitrogen doping can be formed in the obtained biochar. The lone pair of electrons in these nitrogen atoms can form a coordination bond with heavy metal ions, thereby improving the adsorption capacity of biochar for heavy metal ions. The present invention loads dicyandiamide after the biomass material is pyrolyzed to a specific stage, and then continues to perform pyrolysis and carbonization, which can produce the following effects: if dicyandiamide is loaded after biochar is made, dicyandiamide is not easy to penetrate and bind to it because the pore wall of the biochar has formed a dense carbon layer; if dicyandiamide is loaded too early, dicyandiamide is not easy to decompose and firmly bind to the biomass material during the initial pyrolysis of the biomass material, and is easy to volatilize and lose; and the dicyandiamide loading time in the present invention can make dicyandiamide penetrate better and reduce its loss in the early stage of pyrolysis of the biomass material, so it is conducive to forming more nitrogen doping sites in the biochar, thereby improving the heavy metal passivation ability of the final obtained material.
[0011] Dicyandiamide is a weak base with a positive charge in an aqueous solution. It can be combined with the lamellae of talcum powder to form an intercalation layer. During roasting, dicyandiamide is converted into gas and escapes from the interlayer, which can expand the interlayer distance, increase the disorder degree of the talcum powder structure, and then increase the surface activity of the talcum powder, so that it has better heavy metal passivation ability. In addition to playing the above-mentioned role, the dicyandiamide loaded in the talcum powder is added to the talcum powder loaded with dicyandiamide at a specific stage of pyrolysis and carbonization of biomass materials (after the initial pyrolysis material loaded with dicyandiamide is roasted at 390-400°C for a certain period of time). At this time, the pyrolysis gas production rate of the biomass material slows down, and part of the dicyandiamide escaping from the interlayer of the talcum powder can be attached to the biomass material, thereby forming more nitrogen doping sites.
[0012] Preferably, in step (1), the biomass material is rice husk powder.
[0013] Preferably, the mass ratio of the biomass material to talcum powder is 1:1-2.
[0014] Preferably, in step (3), the heating rates to 390-400°C and to 500-550°C are both 25-30°C / min, and the heating rate to 750-800°C is 25-35°C / min.
[0015] Preferably, the process of step (2) specifically comprises: fully immersing the preliminary pyrolysis material and talcum powder in a dicyandiamide solution respectively, taking them out and drying them.
[0016] Furthermore, the concentration of the dicyandiamide solution is 0.05-0.1 g / mL, and the mass ratio of the preliminary pyrolysis material and talc to dicyandiamide is 1:1-2.
[0017] In a third aspect, the present invention provides a talc-modified biochar composite material, wherein the talc-modified biochar composite material is obtained by the above-mentioned preparation method.
[0018] In a fourth aspect, the present invention provides the use of the talc-modified biochar composite material in a heavy metal passivator.
[0019] In a fifth aspect, the present invention provides an application of the talc-modified biochar composite material in remediating heavy metal pollution in soil.
[0020] Compared with the prior art, the present invention has the following advantages: (1) In the present invention, by co-thermal decomposition of talc and biomass materials, the biochar formed is sintered with the talc, and the two can cooperate with each other to give the composite material better heavy metal passivation ability; (2) In the present invention, during the co-thermal pyrolysis of talc and biomass materials, by introducing dicyandiamide at a specific time (loading dicyandiamide into the biomass materials at a specific stage of pyrolysis and carbonization of the biomass materials, and adding talc loaded with dicyandiamide), the heavy metal passivation ability of the composite material can be further improved. DETAILED DESCRIPTION
[0021] The present invention will be further described below in conjunction with the embodiments.
[0022] Overall embodiment A method for preparing a talc-modified biochar composite material comprises the following steps: mixing talc with a biomass material, and co-thermal pyrolysis under oxygen-limited conditions until the biomass material is carbonized and sintered together with the talc to obtain the talc-modified biochar composite material.
[0023] As a specific implementation manner, the mass ratio of the biomass material to talcum powder is 1:1-2.
[0024] As a specific implementation manner, the co-thermal pyrolysis process specifically includes: heating to 500-550° C. at 25-30° C. / min and maintaining for 1-1.5 hours.
[0025] A method for preparing a talc-modified biochar composite material comprises the following steps: (1) Under oxygen-limited conditions, the biomass material is heated to 332-337° C. at a rate of 25-30° C. / min, maintained for 3-6 min, and cooled to obtain a preliminary pyrolysis material; (2) loading dicyandiamide in the preliminary pyrolysis material and talc respectively; (3) Under oxygen-limited conditions, the preliminary pyrolysis material loaded with dicyandiamide was calcined at 390-400°C for 10-15 min, talcum powder loaded with dicyandiamide was added and mixed, the temperature was raised to 500-550°C and calcined for 50-60 min, and then calcined at 750-800°C for 1-1.5 h to obtain a talc-modified biochar composite material.
[0026] As a specific implementation, in step (1), the biomass material is rice husk powder.
[0027] As a specific implementation manner, the mass ratio of the biomass material to talcum powder is 1:1-2.
[0028] As a specific implementation method, the process of step (2) specifically includes: respectively soaking the preliminary pyrolysis material and talcum powder in 0.05-0.1 g / mL dicyandiamide solution, the mass ratio of the preliminary pyrolysis material and talcum powder to dicyandiamide is 1:1-2, and then taking out and drying.
[0029] As a specific implementation, in step (3), the heating rates to 390-400°C and to 500-550°C are both 25-30°C / min, and the heating rate to 750-800°C is 25-35°C / min.
[0030] In a third aspect, the present invention provides a talc-modified biochar composite material, wherein the talc-modified biochar composite material is obtained by the above-mentioned preparation method.
[0031] In a fourth aspect, the present invention provides the use of the talc-modified biochar composite material in a heavy metal passivator.
[0032] In a fifth aspect, the present invention provides an application of the talc-modified biochar composite material in remediating heavy metal pollution in soil. Specific embodiments The present invention is described below by specific examples. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. Without departing from the spirit and scope of the inventive concept, changes and advantages that can be thought of by those skilled in the art are included in the present invention, and the attached claims and any equivalents thereof are the protection scope of the present invention.
[0034] In the following examples, rice husk powder is obtained by drying and grinding rice husk from Yangdu Experimental Base of Zhejiang Academy of Agricultural Sciences. This source is only for illustration and does not limit the scope of the present invention.
[0035] Example 1: Preparation of talc-modified biochar composite (TBC) Take talcum powder and rice husk powder, mix them in a mass ratio of 1:1 and place them in a crucible. Under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace, heat them to 500°C at a rate of 25°C / min, maintain them for 90 minutes, cool them naturally to room temperature, grind them and pass them through a 100-mesh sieve to obtain a talcum powder-modified biochar composite material (denoted as TBC).
[0036] Example 2: Preparation of talc-modified biochar composite material (TNBC1) Step 1: Place the rice husk powder in a crucible, and heat it to 332°C at a rate of 25°C / min under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace, maintain for 6 minutes, and naturally cool to room temperature to obtain a preliminary pyrolysis material.
[0037] Step 2: According to the mass volume ratio of 1g:20mL, the preliminary pyrolysis material is added into a 0.1g / mL dicyandiamide solution (the solvent is water), ultrasonically immersed for 1h, then taken out and dried to obtain a preliminary pyrolysis material loaded with dicyandiamide.
[0038] Step 3: Take talcum powder of the same mass as the rice husk powder, add it into a 0.1 g / mL dicyandiamide solution (the solvent is water) at a mass volume ratio of 1 g:20 mL, immerse it in ultrasound for 1 hour, take it out, dry it, and obtain talcum powder loaded with dicyandiamide.
[0039] Step 4: Place the preliminary pyrolysis material loaded with dicyandiamide in a crucible, and heat it to 400°C at a rate of 25°C / min under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace. After holding for 10 minutes, add talcum powder loaded with dicyandiamide and mix well. Continue to heat it to 500°C at a rate of 25°C / min, hold for 60 minutes, and then heat it to 800°C at a rate of 35°C / min and roast for 1 hour. Naturally cool to room temperature, grind and pass through a 100-mesh sieve to obtain a talc-modified biochar composite material (denoted as TNBC1).
[0040] Example 3: Preparation of talc-modified biochar composite material (TNBC2) Step 1: Place the rice husk powder in a crucible, and heat it to 337°C at a rate of 30°C / min under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace, maintain for 3 minutes, and naturally cool to room temperature to obtain a preliminary pyrolysis material.
[0041] Step 2: According to the mass volume ratio of 1g:20mL, the preliminary pyrolysis material is added into a 0.05g / mL dicyandiamide solution (the solvent is water), ultrasonically immersed for 1.5h, then taken out and dried to obtain a preliminary pyrolysis material loaded with dicyandiamide.
[0042] Step 3: Take talcum powder of the same mass as the rice husk powder, add it to a 0.05 g / mL dicyandiamide solution (the solvent is water) at a mass volume ratio of 1 g:20 mL, ultrasonically immerse it for 1.5 hours, then take it out and dry it to obtain talcum powder loaded with dicyandiamide.
[0043] Step 4: Place the preliminary pyrolysis material loaded with dicyandiamide in a crucible, and heat it to 390°C at a rate of 30°C / min under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace. After holding for 15 minutes, add talcum powder loaded with dicyandiamide and mix well. Continue to heat it to 550°C at a rate of 30°C / min, hold for 50 minutes, and then heat it to 750°C at a rate of 25°C / min and roast it for 1.5 hours. Naturally cool to room temperature, grind it and pass it through a 100-mesh sieve to obtain a talc-modified biochar composite material (denoted as TNBC2).
[0044] Example 4: Preparation of talc-modified biochar composite material (TNBC3) Step 1: Take talcum powder and rice husk powder, mix them in a crucible in a mass ratio of 1:1, and heat them to 500°C at a rate of 25°C / min under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace. After maintaining for 90 minutes, naturally cool to room temperature, grind and pass through a 100-mesh sieve to obtain a composite material.
[0045] Step 2: According to the mass volume ratio of 1 g:20 mL, the composite material was added into a 0.1 g / mL dicyandiamide solution (the solvent was water), ultrasonically immersed for 1 hour, then taken out and dried to obtain a composite material loaded with dicyandiamide.
[0046] Step 3: Place the composite material loaded with dicyandiamide in a crucible, and heat it to 400°C at a rate of 25°C / min under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace. After holding for 10 minutes, continue to heat it to 500°C at a rate of 25°C / min, hold it for 60 minutes, and then heat it to 800°C at a rate of 35°C / min and roast it for 1 hour. Naturally cool it to room temperature, grind it and pass it through a 100-mesh sieve to obtain a talc-modified biochar composite material (denoted as TNBC3).
[0047] Example 5: Preparation of talc-modified biochar composite material (TNBC4) Step 1: Place the rice husk powder in a crucible, and heat it to 250°C at a rate of 25°C / min under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace, maintain for 6 minutes, and naturally cool to room temperature to obtain a preliminary pyrolysis material.
[0048] Step 2: According to the mass volume ratio of 1g:20mL, the preliminary pyrolysis material is added into a 0.1g / mL dicyandiamide solution (the solvent is water), ultrasonically immersed for 1h, then taken out and dried to obtain a preliminary pyrolysis material loaded with dicyandiamide.
[0049] Step 3: Take talcum powder of the same mass as the rice husk powder, add it into a 0.1 g / mL dicyandiamide solution (the solvent is water) at a mass volume ratio of 1 g:20 mL, immerse it in ultrasound for 1 hour, take it out, dry it, and obtain talcum powder loaded with dicyandiamide.
[0050] Step 4: Place the preliminary pyrolysis material loaded with dicyandiamide in a crucible, and heat it to 400°C at a rate of 25°C / min under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace. After holding for 10 minutes, add talcum powder loaded with dicyandiamide and mix well. Continue to heat it to 500°C at a rate of 25°C / min, hold for 60 minutes, and then heat it to 800°C at a rate of 35°C / min and roast for 1 hour. Naturally cool to room temperature, grind and pass through a 100-mesh sieve to obtain a talc-modified biochar composite material (denoted as TNBC4).
[0051] Example 6: Preparation of talc-modified biochar composite material (TNBC5) Step 1: Place the rice husk powder in a crucible, and heat it to 332°C at a rate of 25°C / min under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace, maintain for 6 minutes, and naturally cool to room temperature to obtain a preliminary pyrolysis material.
[0052] Step 2: According to the mass volume ratio of 1g:20mL, the preliminary pyrolysis material is added into a 0.1g / mL dicyandiamide solution (the solvent is water), ultrasonically immersed for 1h, then taken out and dried to obtain a preliminary pyrolysis material loaded with dicyandiamide.
[0053] Step 3: The preliminary pyrolysis material loaded with dicyandiamide is placed in a crucible, and under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace, the temperature is raised to 400°C at a rate of 25°C / min, and maintained for 10 minutes. Then, talcum powder of the same mass as the rice husk powder is added and mixed, and the temperature is continued to be raised to 500°C at a rate of 25°C / min, maintained for 60 minutes, and then raised to 800°C at a rate of 35°C / min and roasted for 1 hour. The mixture is naturally cooled to room temperature, ground and sieved through a 100-mesh sieve to obtain a talc-modified biochar composite material (denoted as TNBC5).
[0054] Example 7: Preparation of talc-modified biochar composite material (TNBC6) Step 1: Place the rice husk powder in a crucible, and heat it to 332°C at a rate of 25°C / min under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace, maintain for 6 minutes, and naturally cool to room temperature to obtain a preliminary pyrolysis material.
[0055] Step 2: Take talcum powder of the same mass as the rice husk powder, mix it with the preliminary pyrolysis material to obtain a mixture; add the mixture into 0.1 g / mL dicyandiamide solution (the solvent is water) at a mass volume ratio of 1 g:20 mL, ultrasonically immerse it for 1 hour, then take it out and dry it to obtain a mixture loaded with dicyandiamide.
[0056] Step 3: Place the mixture loaded with dicyandiamide in a crucible, and in a tubular carbonization furnace under oxygen limited conditions (vacuum), heat it to 400°C at a rate of 25°C / min, hold it for 10 minutes, then continue to heat it to 500°C at a rate of 25°C / min, hold it for 60 minutes, and then heat it to 800°C at a rate of 35°C / min and roast it for 1 hour. Naturally cool it to room temperature, grind it and pass it through a 100-mesh sieve to obtain a talc-modified biochar composite material (denoted as TNBC6).
[0057] Comparative Example 1: Preparation of Biochar (BC) The rice husk powder was placed in a crucible and heated to 500°C at a rate of 25°C / min under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace. After maintaining for 90 minutes, it was naturally cooled to room temperature, ground and passed through a 100-mesh sieve to obtain biochar (BC).
[0058] Comparative Example 2: Preparation of attapulgite-modified biochar composite material (ABC) Take attapulgite and rice husk powder, mix them in a mass ratio of 1:1 and place them in a crucible. Under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace, heat them to 500°C at a rate of 25°C / min, maintain them for 90 minutes, cool them naturally to room temperature, grind them and pass them through a 100-mesh sieve to obtain attapulgite-modified biochar composite material (denoted as ABC).
[0059] Comparative Example 3: Preparation of Kaolin Modified Biochar Composite Material (KBC) Kaolin and rice husk powder were mixed in a crucible in a mass ratio of 1:1, and heated to 500 °C at a rate of 25 °C / min under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace. After maintaining for 90 min, the mixture was naturally cooled to room temperature, ground and sieved through a 100-mesh sieve to obtain a kaolin-modified biochar composite material (denoted as KBC).
[0060] Comparative Example 4: Preparation of Vermiculite-modified Biochar Composite (VBC) Vermiculite and rice husk powder were mixed in a crucible in a mass ratio of 1:1, and heated to 500°C at a rate of 25°C / min under oxygen-limited conditions (vacuuming) in a tubular carbonization furnace. After maintaining for 90 minutes, the mixture was naturally cooled to room temperature, ground and sieved through a 100-mesh sieve to obtain a vermiculite-modified biochar composite material (denoted as VBC).
[0061] Test example: Test arrangement for the passivation effect of heavy metals in soil: The potted test was carried out at the Mulberry Garden Experimental Base of Zhejiang Academy of Agricultural Sciences. The experiment selected a flower pot with a capacity of 1.5L, and laid two layers of filter paper at the bottom of the pot to prevent the soil from escaping from the pores at the bottom of the pot. 1kg of test soil was added to each pot, and 2g of fertilizer with N:P:K=2:1:1 was mixed in. After stirring evenly, the materials prepared in each embodiment and comparative example and talcum powder (TP) were applied to the soil respectively, and then each pot was irrigated with distilled water. The materials and talcum powder in each embodiment and comparative example were set to the following three addition amounts of 0.5%, 1.0%, and 2.0%; and a blank control was set, and the materials in each embodiment and comparative example were not added, which was recorded as CK. Then 6 Suzhou green seeds were planted in each pot, covered with about 2mm of soil, and 3 parallel groups were set for each treatment. During the growth period of Suzhou green, about 100mL of distilled water was sprayed every day before germination, and after germination, water was poured once every 2 days, about 200mL each time. The soil was sampled 45 days after planting, and the CaCl2 extraction method was used to detect the residual effective heavy metal content in the soil. The results are shown in Tables 1 to 3.
[0062] Table 1 Passivation effect of soil heavy metals at 0.5% dosage Table 2 Passivation effect of soil heavy metals at 1.0% dosage Table 3 Passivation effect of soil heavy metals at 2.0% dosage According to the test results in Tables 1 to 3, it can be seen that: (1) Compared with the blank control (CK), the heavy metal residues in the soil were significantly reduced after the materials prepared in the examples and comparative examples were applied, indicating that the materials prepared in the examples and comparative examples can play a role in passivating heavy metals in the soil to a certain extent.
[0063] (2) Compared with BC and TP, the heavy metal residues in the soil after the application of TBC were significantly lower; while the heavy metal residues in the soil of ABC, KBC and VBC at different dosages were mostly higher than those of TBC, and even higher than those of BC at some dosages. This indicates that after the activated carbon and talc are combined, the two can cooperate with each other, so that the passivation effect of the composite on soil heavy metals is significantly improved compared with the use of activated carbon and talc alone, and the effect is better than the composite of attapulgite, kaolin and vermiculite on activated carbon.
[0064] (3) Compared with TNBC3 and TNBC4, the heavy metal residue in the soil after the application of TNBC1 was significantly lower. This shows that in the process of preparing talc-modified biochar composite materials, loading dicyandiamide too early or too late will have an adverse effect on the heavy metal passivation ability of the resulting material. This is because if dicyandiamide is loaded after biochar is made, it is difficult for dicyandiamide to penetrate and bind to the pore wall of biochar because a dense carbon layer has been formed, and talc has been sintered with biochar, so the effect of dicyandiamide in expanding the spacing between talc layers is weakened; if dicyandiamide is loaded too early, it is difficult to decompose and firmly bind to the biomass material during the initial pyrolysis of the biomass material, and it is easy to volatilize and lose.
[0065] (4) Compared with TNBC5, the heavy metal residues in the soil were significantly lower after the application of TNBC1, indicating that the heavy metal passivation capacity of talc-modified biochar composites can be improved by loading dicyandiamide in talc.
[0066] (5) Compared with TNBC6, the heavy metal residue in the soil after the application of TNBC1 was significantly lower. This shows that in the process of preparing talc-modified biochar composite materials, if the talc loaded with dicyandiamide is mixed with the biochar intermediate too early, the heavy metal passivation effect of the obtained material will be weakened. This is because if the talc loaded with dicyandiamide is added too early, the pyrolysis gas production rate of the biomass material is faster at this time, and the dicyandiamide escaping from the talc layer is not easy to adhere to the biomass material, resulting in poor effect of increasing the nitrogen doping sites on the biochar.
[0067] Unless otherwise defined, all technical terms and scientific terms used in the present invention have the same meanings as those commonly understood by ordinary technicians in the field to which the present disclosure belongs. Unless otherwise specified, the raw materials and equipment used in the present invention are conventional raw materials and equipment in the field and can be obtained from conventional commercial channels; unless otherwise specified, the methods used in the present invention are conventional methods in the field.
[0068] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a talc-modified biochar composite material, characterized in that: The following steps are involved: The talc powder is mixed with the biomass material, and co-thermal pyrolysis is performed under oxygen-limited conditions until the biomass material is carbonized and sintered together with the talc powder to obtain a talc-modified biochar composite material.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the biomass material to talcum powder is 1:1-2.
3. The preparation method according to claim 1, characterized in that: The co-thermal pyrolysis process specifically includes: heating to 500-550° C. at 25-30° C. / min and maintaining for 1-1.5 h.
4. A method for preparing a talc-modified biochar composite material, characterized in that: The following steps are involved: (1) Under oxygen-limited conditions, the biomass material is heated to 332-337°C at a rate of 25-30°C / min, maintained for 3-6 min, and cooled to obtain a preliminary pyrolysis material; (2) loading dicyandiamide in the preliminary pyrolysis material and talc respectively; (3) Under oxygen-limited conditions, the preliminary pyrolysis material loaded with dicyandiamide was calcined at 390-400°C for 10-15 min, and then talc loaded with dicyandiamide was added and mixed. The mixture was heated to 500-550°C and calcined for 50-60 min. Then, the mixture was calcined at 750-800°C for 1-1.5 h to obtain a talc-modified biochar composite material.
5. The preparation method according to claim 4, characterized in that: In step (1), the biomass material is rice husk powder.
6. The preparation method according to claim 4 or 5, characterized in that: The mass ratio of the biomass material to talcum powder is 1:1-2.
7. The preparation method according to claim 4, characterized in that: In step (3), the heating rates to 390-400°C and 500-550°C are both 25-30°C / min, and the heating rate to 750-800°C is 25-35°C / min.
8. A talc-modified biochar composite material, characterized in that: The talc-modified biochar composite material is obtained by the preparation method described in any one of claims 1 to 3, or by the preparation method described in any one of claims 4 to 7.
9. Use of the talc-modified biochar composite material according to claim 8 in a heavy metal passivator.
10. Use of the talc-modified biochar composite material according to claim 8 in remediating soil heavy metal pollution.
Citation Information
Patent Citations
Preparation and application of composite adsorbent for synchronously adsorbing trace amount of antibiotics and hexavalent chromium
CN108144579A
Biochar preparation method capable of increasing specific surface area of biochar
CN114836224A
Porous clay-based modified charcoal composite material as well as preparation method and application thereof
CN115400725A
Modified biochar as well as preparation method and application thereof
CN117482897A