Preparation method of nanofiber adsorption material for deeply removing nickel complex in water body and nickel complex wastewater recycling technology

By preparing aminated and sulfur-containing nanofiber adsorption materials, using electrospinning technology and dynamic column adsorption cycle regeneration technology, the problem of low removal efficiency of nanofibers on nickel complexes is solved, and efficient removal and resource utilization are achieved , reducing the cost of treatment and the risk of secondary pollution.

CN118949934AActive Publication Date: 2024-11-15CHONGQING UNIVERSITY OF SCIENCE AND TECHNOLOGY

Patent Information

Application Number
CN202411115498.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-15
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

Existing nanofibers have low removal efficiency for nickel complexes, high processing costs, limited circulation and regeneration performance, risk of secondary pollution, and difficult to reap nickel ions.

Method used

Aminated and sulfur-containing nanofibers are prepared using raw materials such as polyvinyl alcohol, polyaniline, and polyacrylonitrile. Nanofiber adsorption materials are prepared through electrostatic spinning technology, and nickel network is realized through dynamic column adsorption and desorption liquid circulation and regeneration technology. Deep removal and resource utilization of the compound.

Benefits of technology

It improves the removal efficiency of nickel complexes, reduces the treatment cost, reduces the risk of secondary pollution, and realizes the resource utilization of nickel ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949934A_ABST
    Figure CN118949934A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nanofiber adsorption materials, and particularly discloses a preparation method of a nanofiber adsorption material for deep removal of a nickel complex in a water body and a nickel complex wastewater recycling technology, the preparation method comprises the following steps: taking polyvinyl alcohol, polyaniline, polyacrylonitrile and polypropylene as raw materials; adding an oxidizing agent into the polyvinyl alcohol solution for reaction, and then introducing amino; introducing amido into the polyaniline solution through a cross-linking agent; introducing the polyacrylonitrile solution into amido; introducing amido into the polypropylene substrate; adding a sulfur-containing reagent to prepare a spinning solution of a polymer containing sulfur adsorption sites; the spinning solution is used as a raw material and is prepared into nanofibers, and the nanofibers are washed and dried to prepare the nanofiber adsorption material for deeply removing the nickel complex in the water body. The adsorbent provides strong adsorption capacity, can effectively adsorb nickel complexes in wastewater, improves the removal efficiency of the nickel complexes, and has higher selectivity and affinity to the nickel complexes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanofiber adsorption materials, and in particular to a method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water and a technology for recycling nickel complex wastewater. Background Art

[0002] At present, nanofiber adsorption material is a material with strong adsorption capacity made by utilizing the characteristics of nanofibers. Nanofibers, as a new type of fiber material with a diameter at the nanometer level, have extremely high length and specific surface area, which makes nanofibers have significant advantages in adsorption, filtration, and enhancement. The large specific area and surface activity of nanofibers give them strong adsorption capacity and can be used to remove harmful substances, dyes and heavy metal pollutants in water. A large amount of nickel-containing complex wastewater is generated in the electroplating, metallurgy and other industries. These nickel-complex wastewaters are chemically stable, not easy to precipitate, have strong migration ability, and are more harmful.

[0003] However, in the prior art, ordinary nanofibers have low removal efficiency for nickel complexes, high treatment costs, and limited recycling performance, so there is a potential risk of secondary pollution. Nickel is an important non-renewable metal resource, and it is of great significance to treat nickel complex wastewater and recover nickel ion resources from it. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water and a nickel complex wastewater resource recovery technology, aiming to solve the technical problems in the prior art that ordinary nanofibers have low removal efficiency for nickel complexes, high treatment costs, limited recycling performance, the risk of secondary pollution, and difficulty in nickel ion resource recovery.

[0005] To achieve the above object, the present invention adopts a method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water, comprising the following steps: Step 1: using polyvinyl alcohol, polyaniline, polyacrylonitrile and polypropylene as raw materials, and fully dissolving the polyvinyl alcohol, polyaniline, polyacrylonitrile and polypropylene; Step 2: Add an oxidant to the polyvinyl alcohol solution to react and oxidize the alcohol hydroxyl group to a carbonyl group. Then add an amine-containing compound to introduce an amine group. The reaction temperature is 50-100°C and the reaction time is 4-24 hours. Adding an amine-containing compound and a cross-linking agent into a polyaniline solution to introduce amine groups into the polyaniline substrate, the reaction temperature is 60-140°C, and the reaction time is 2-72 hours; Transfer the polyacrylonitrile solution to the reactor, and add an amine-containing compound to introduce amine groups. The reaction temperature is 80-140°C and the reaction time is 2-48 hours. Add an initiator and an amine-containing compound to a polypropylene solution to introduce amine groups into a polypropylene substrate. The reaction temperature is 60-100°C and the reaction time is 2-48 hours. Step 3: Filter, wash and dry the product in the above step 2 to obtain an aminated polymer, disperse the aminated polymer in an anhydrous ethanol solution, add a sulfur-containing reagent, and control the pH value to 12-14, the reaction temperature to 50-78°C, and the reaction time to 10-24h; Step 4: filtering, washing and drying the product obtained in the above step 3 to obtain a sulfur-containing polymer, dissolving the sulfur-containing polymer in a mixed solvent of dimethyl sulfoxide and N,N-dimethylacetamide, wherein the volume ratio of dimethyl sulfoxide to N,N-dimethylacetamide solvent is 0.5-3, to obtain a spinning solution; Step 5: Using the spinning solution as raw material, an electrostatic spinning device is used to make it into nanofibers. After washing and drying, the nanofiber adsorption material for deep removal of nickel complexes in water is obtained.

[0006] Step 6: using the sulfur-containing nanofibers prepared in the above step 5 as an adsorbent, the sulfur-containing nanofibers are filled into an adsorption column by a wet method, and the nickel complex-containing wastewater is pumped into the adsorption column from bottom to top, that is, the nickel complex in the wastewater is removed; Step 7: After the sulfur-containing nanofibers are saturated in the dynamic column adsorption described in step 6 above, a desorption solution is introduced from top to bottom. The cyclic desorption can enrich the nickel ion solution concentration to 0.5-80g / L. After the regeneration solution is introduced, the cyclic adsorption of the nanofibers can be achieved; Step 8: Concentrate, cool, crystallize, filter and dry the nickel ion desorption solution in step 7 to obtain a nickel sulfate product.

[0007] Wherein, the polyvinyl alcohol is dissolved in water at a temperature of 80-95°C.

[0008] The polyaniline is dissolved in a mixed solution of N-methylpyrrolidone and N,N-dimethylacetamide, the mixed volume ratio of the mixed solution of N-methylpyrrolidone and N,N-dimethylacetamide is 0.5-2, and the temperature is 100-150°C.

[0009] Wherein, the polyacrylonitrile is dissolved in N,N-dimethylacetamide at a temperature of 70-105°C.

[0010] Wherein, the polypropylene is dissolved in N,N-dimethylacetamide at a temperature of 70-105°C.

[0011] Wherein, the oxidant is any one of sodium periodate, hydrogen peroxide and potassium permanganate.

[0012] Wherein, the amine-containing compound is any one of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethyleneimine and urea.

[0013] Wherein, the cross-linking agent is any one of dichloromethane and formaldehyde.

[0014] Wherein, the initiator is any one of potassium disulfate, ammonium peroxodisulfate and sodium peroxodisulfate.

[0015] Wherein, the sulfur-containing reagent is any one of carbon disulfide, trithiocyanic acid and dimercaptopropanol.

[0016] Wherein, the desorption liquid is a 0.5~4 mol / L sulfuric acid aqueous solution, and the regeneration liquid is a 0.5~2 mol / L sodium hydroxide aqueous solution.

[0017] The method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water and the technology for recycling nickel complex wastewater have the following beneficial effects: specific surface area and adsorption capacity; the nanofiber has a very large specific surface area and an extremely high surface area / volume ratio, which provides it with a strong adsorption capacity, can effectively adsorb nickel complexes in wastewater, improve the removal efficiency of nickel complexes, and deeply remove nickel complexes; when wastewater containing nickel complexes passes through the nanofiber adsorption material, the nickel complexes are effectively trapped in micropores, achieving efficient removal; the nanofiber adsorption material can be recycled, reducing treatment costs and the risk of secondary pollution; it has higher selectivity and affinity for nickel complexes, can treat wastewater containing nickel complexes, and realize its resource utilization by desorbing and enriching nickel ions. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 These are the SEM images and mapping images of the nanofiber adsorption material for deep removal of nickel complexes in water prepared in Example 1 of the present invention.

[0020] Figure 2 This is an infrared spectrum of the nanofiber adsorption material for deep removal of nickel complexes in water prepared in Example 1 of the present invention.

[0021] Figure 3It is a schematic diagram of dynamic column adsorption of nanofiber adsorption material for deep removal of nickel complexes in water prepared in Example 2 of the present invention.

[0022] Figure 4 It is a dynamic column adsorption penetration curve diagram of the nanofiber adsorption material for deep removal of nickel complexes in water prepared in Example 1 of the present invention.

[0023] Figure 5 This is the X-ray diffraction spectrum of the nickel sulfate product prepared by resource utilization of nickel-containing complex wastewater in Example 3 of the present invention. DETAILED DESCRIPTION

[0024] To achieve the above object, the present invention adopts a method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water, comprising the following steps: Step 1: using polyvinyl alcohol, polyaniline, polyacrylonitrile and polypropylene as raw materials, and fully dissolving the polyvinyl alcohol, polyaniline, polyacrylonitrile and polypropylene; Step 2: Add an oxidant to the polyvinyl alcohol solution to react and oxidize the alcohol hydroxyl group to a carbonyl group. Then add an amine-containing compound to introduce an amine group. The reaction temperature is 50-100°C and the reaction time is 4-24 hours. Adding an amine-containing compound and a cross-linking agent into a polyaniline solution to introduce amine groups into the polyaniline substrate, the reaction temperature is 60-140°C, and the reaction time is 2-72 hours; Transfer the polyacrylonitrile solution to the reactor, and add an amine-containing compound to introduce amine groups. The reaction temperature is 80-140°C and the reaction time is 2-48 hours. Add an initiator and an amine-containing compound to a polypropylene solution to introduce amine groups into a polypropylene substrate. The reaction temperature is 60-100°C and the reaction time is 2-48 hours. Step 3: Filter, wash and dry the product in the above step 2 to obtain an aminated polymer, disperse the aminated polymer in an anhydrous ethanol solution, add a sulfur-containing reagent, and control the pH value to 12-14, the reaction temperature to 50-78°C, and the reaction time to 10-24h; Step 4: filtering, washing and drying the product obtained in the above step 3 to obtain a sulfur-containing polymer, dissolving the sulfur-containing polymer in a mixed solvent of dimethyl sulfoxide and N,N-dimethylacetamide, wherein the volume ratio of dimethyl sulfoxide to N,N-dimethylacetamide solvent is 0.5-3, to obtain a spinning solution; Step 5: Using the spinning solution as raw material, an electrostatic spinning device is used to make it into nanofibers. After washing and drying, the nanofiber adsorption material for deep removal of nickel complexes in water is obtained.

[0025] Step 6: using the sulfur-containing nanofibers prepared in the above step 5 as an adsorbent, the sulfur-containing nanofibers are filled into an adsorption column by a wet method, and the nickel complex-containing wastewater is pumped into the adsorption column from bottom to top, that is, the nickel complex in the wastewater is removed; Step 7: After the sulfur-containing nanofibers are saturated in the dynamic column adsorption described in step 6 above, a desorption solution is introduced from top to bottom. The cyclic desorption can enrich the nickel ion solution concentration to 0.5-80 g / L. After the regeneration solution is introduced, the cyclic adsorption of the nanofibers can be achieved; Step 8: Concentrate, cool, crystallize, filter and dry the nickel ion desorption solution in step 7 to obtain a nickel sulfate product.

[0026] Furthermore, the polyvinyl alcohol is dissolved in water at a temperature of 80-95°C.

[0027] Furthermore, the polyaniline is dissolved in a mixed solution of N-methylpyrrolidone and N,N-dimethylacetamide, the mixed volume ratio of the mixed solution of N-methylpyrrolidone and N,N-dimethylacetamide is 0.5-2, and the temperature is 100-150°C.

[0028] Furthermore, the polyacrylonitrile is dissolved in N,N-dimethylacetamide at a temperature of 70-105°C.

[0029] Furthermore, the polypropylene is dissolved in N,N-dimethylacetamide at a temperature of 70-105°C.

[0030] Furthermore, the oxidant is any one of sodium periodate, hydrogen peroxide and potassium permanganate.

[0031] Furthermore, the amine-containing compound is any one of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethyleneimine and urea.

[0032] Furthermore, the cross-linking agent is any one of dichloromethane and formaldehyde.

[0033] Furthermore, the initiator is any one of potassium disulfate, ammonium peroxodisulfate and sodium peroxodisulfate.

[0034] Furthermore, the sulfur-containing reagent is any one of carbon disulfide, thiocyanate and dimercaprol.

[0035] Furthermore, the desorption liquid is a 0.5-4 mol / L sulfuric acid aqueous solution, and the regeneration liquid is a 0.5-2 mol / L sodium hydroxide aqueous solution.

[0036] In this embodiment, the specific surface area and adsorption capacity of the nanofibers are extremely large in specific surface area and extremely high in surface area / volume ratio, which provide them with strong adsorption capacity, can effectively adsorb nickel complexes in wastewater, improve the removal efficiency of nickel complexes, and deeply remove nickel complexes. When wastewater containing nickel complexes passes through the nanofiber adsorption material, the nickel complexes will be effectively retained in the micropores to achieve efficient removal. The nanofiber adsorption material can be recycled, which reduces the treatment cost and the risk of secondary pollution. It has higher selectivity and affinity for nickel complexes, can treat wastewater containing nickel complexes and realize its resource utilization by desorption and enrichment of nickel ions.

[0037] Embodiment 1, the present invention also provides a method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water, comprising the following steps: Using polypropylene as raw material, a 10% polypropylene N,N-dimethylacetamide solution was obtained at 120°C; Take 20 mL and transfer it to the reactor, add 5 mL of polyethyleneimine and 20 mg of potassium persulfate, and react at 80 °C for 12 h; The aminated polymer was obtained by washing, filtering and drying. 5 g of the aminated polymer was weighed into a reactor, 100 mL of anhydrous ethanol and 25 mL of carbon disulfide were added, and the pH value was controlled to 14 with sodium hydroxide, and the reaction was carried out at 70° C. for 10 h. After washing, drying and baking, a sulfur-containing polymer is obtained, 2 g of the sulfur-containing polymer is weighed and dissolved in 20 mL of a mixed solvent of dimethyl sulfoxide and N,N-dimethylacetamide in a solution system ratio of 1:1 at 120° C., and after cooling to room temperature, a spinning solution is obtained; The spinning solution is used as a raw material and an electrostatic spinning device is used to make it into nanofibers. After drying, the nanofiber adsorption material for deep removal of nickel complexes in water is obtained.

[0038] The SEM image of the nanofiber adsorption material for deep removal of nickel complexes in water prepared in Example 1 is shown in Figure 1 The infrared spectrum of the nanofiber adsorbent material used for deep removal of nickel complexes in water is shown in Figure 2 .

[0039] Example 2: Take 2.0 g of the nanofiber adsorbent material for deep removal of nickel complexes in water prepared in Example 1 and load it into an adsorption column with a diameter of 10 mm and a height of 100 mm. Use a peristaltic pump to control the nickel-containing wastewater to pass through the adsorption column at a flow rate of 1 mL / min, and take the effluent at different times and measure its nickel ion concentration. See the schematic diagram. Figure 3 .

[0040] Determination of structure Figure 4As shown, no nickel complex was detected in the effluent before 480 min.

[0041] Example 3: The circulating desorption enriched liquid obtained in Example 2 is concentrated, cooled, crystallized, filtered and dried to obtain a nickel sulfate product, thereby realizing the resource utilization of nickel ions in the nickel complex wastewater. The XRD pattern of the nickel sulfate product is shown in FIG. Figure 5 , in accordance with the standard spectrum of nickel sulfate hexahydrate (NiSO 4 6H 2 O-PDF#08-0470).

[0042] What is disclosed above is only a preferred embodiment of the present invention, and it certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiment and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.

Claims

1. A method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water. It is characterized in that The steps include: Step 1: using polyvinyl alcohol, polyaniline, polyacrylonitrile and polypropylene as raw materials, and fully dissolving the polyvinyl alcohol, polyaniline, polyacrylonitrile and polypropylene; Step 2: Add an oxidant to the polyvinyl alcohol solution to react and oxidize the alcohol hydroxyl group to a carbonyl group. Then add an amine-containing compound to introduce an amine group. The reaction temperature is 50-100°C and the reaction time is 4-24 hours. Adding an amine-containing compound and a cross-linking agent to a polyaniline solution to introduce amine groups into a polyaniline-based substrate, the reaction temperature is 60-140° C., and the reaction time is 2-72 hours; Transfer the polyacrylonitrile solution to the reactor, and add an amine-containing compound to introduce amine groups. The reaction temperature is 80-140°C and the reaction time is 2-48 hours. Add an initiator and an amine-containing compound to a polypropylene solution to introduce amine groups into a polypropylene substrate. The reaction temperature is 60-100°C and the reaction time is 2-48 hours. Step 3: Filter, wash and dry the product in the above step 2 to obtain an aminated polymer, disperse the aminated polymer in an anhydrous ethanol solution, add a sulfur-containing reagent, and control the pH value to 12-14, the reaction temperature to 50-78°C, and the reaction time to 10-24h; Step 4: filtering, washing and drying the product obtained in the above step 3 to obtain a sulfur-containing polymer, dissolving the sulfur-containing polymer in a mixed solvent of dimethyl sulfoxide and N,N-dimethylacetamide, wherein the volume ratio of dimethyl sulfoxide to N,N-dimethylacetamide solvent is 0.5-3, to obtain a spinning solution; Step 5: Using the spinning solution as a raw material, using an electrospinning device to make it into nanofibers, after washing and drying, the nanofiber adsorption material for deep removal of nickel complexes in water is obtained. Step 6: Using the sulfur-containing nanofibers prepared in the above step 5 as an adsorbent, the sulfur-containing nanofibers are filled into an adsorption column by a wet method, and the nickel complex wastewater is pumped into the adsorption column from bottom to top, that is, the nickel complex in the wastewater is removed; Step 7: After the sulfur-containing nanofibers are saturated in the dynamic column adsorption described in step 6 above, a desorption solution is introduced from top to bottom. The cyclic desorption can enrich the nickel ion solution concentration to 0.5-80 g / L. After the regeneration solution is introduced, the cyclic adsorption of the nanofibers can be achieved; Step 8: Concentrate, cool, crystallize, filter and dry the nickel ion desorption solution in step 7 to obtain a nickel sulfate product.

2. A method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water as claimed in claim 1, It is characterized in that The polyvinyl alcohol is dissolved in water at a temperature of 80-95°C.

3. A method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water as claimed in claim 1, It is characterized in that The polyaniline is dissolved in a mixed solution of N-methylpyrrolidone and N,N-dimethylacetamide, the mixed volume ratio of the mixed solution of N-methylpyrrolidone and N,N-dimethylacetamide is 0.5-2, and the temperature is 100-150°C.

4. A method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water as claimed in claim 1, It is characterized in that The polyacrylonitrile is dissolved in N,N-dimethylacetamide at a temperature of 70-105°C.

5. A method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water as claimed in claim 1, It is characterized in that The polypropylene is dissolved in N,N-dimethylacetamide at a temperature of 70-105°C.

6. A method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water as claimed in claim 1, It is characterized in that The oxidant is any one of sodium periodate, hydrogen peroxide and potassium permanganate.

7. A method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water as claimed in claim 1, It is characterized in that The amine-containing compound is any one of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethyleneimine and urea.

8. A method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water as claimed in claim 1, It is characterized in that The cross-linking agent is any one of dichloromethane and formaldehyde.

9. A method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water as claimed in claim 1, It is characterized in that The initiator is any one of potassium disulfate, ammonium peroxodisulfate, sodium peroxodisulfate and dicumyl peroxide.

10. The method for preparing a nanofiber adsorption material for deep removal of nickel complexes in water according to claim 1, It is characterized in that The sulfur-containing reagent is any one of carbon disulfide, thiocyanate and dimercaprol.

11. The nickel complex wastewater resource recovery technology according to claim 1, Features: The desorption liquid is a 0.5-4 mol / L sulfuric acid aqueous solution, and the regeneration liquid is a 0.5-2 mol / L sodium hydroxide aqueous solution.

Citation Information

Patent Citations

  • Modified polyaniline loaded polystyrene adsorption resin as well as preparation and application thereof

    CN117797783A

  • Preparation method of novel nanofiber adsorption material for treating nickel-containing wastewater

    CN118416868A

Cited By

  • Method for deeply separating similar metal elements based on Lewis acidity regulation

    CN119876605A