Wrapping type cork belt core mold pressing method
Through the three-mold design and two-fold filler molding process, the problem of wrapping molding of complex shapes and special-shaped items in the prior art is solved, and efficient molding and convenient installation of cork products are achieved, forming precision and production efficiency are improved.
Patent Information
- Application Number
- CN202411057820.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-15
AI Technical Summary
The existing cork molding technology is difficult to make wrap-type molding products of complex shapes and special-shaped items, and the existing technology requires the design of the product into two parts for bonding and installation, resulting in inconvenient installation and poor molding.
The three-mold design is adopted, including the lower mold silo, pre-pressed mold and molding. Through two fillers and precisely controlled molding processes, the cork raw materials are evenly distributed and tightly wrapped, and the molding accuracy and installation convenience are improved.
It realizes cork-wrapped molding of items of complex shapes and sizes, reducing material waste, improving product density and consistency, and improving production efficiency and operating smoothness.
Smart Images

Figure CN118952550A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of molding technology, and in particular relates to a wrapped cork core molding method. Background Art
[0002] The existing cork molding technology mainly uses mold molding to make wrapped molded products. The molded cork products are then installed at the locations where the items need to be wrapped. If they are installed at both ends of the items, they can be directly put on for installation; if they need to be installed in the middle of the items, the cork molded products are easily damaged if they are directly put on.
[0003] Therefore, in the prior art, the cork molded product is designed to be divided into two parts, which are then glued and installed at the middle end of the object after the molding is completed. However, if the object needs to be installed at a position where the cork molded product is irregular, or the object is a set that cannot fit tightly because it is not of uniform size, or the position where it needs to be installed is irregular, the cork molded product can only be designed to be divided into two parts, which are then glued and installed after the molding is completed. Summary of the invention
[0004] The purpose of this application is to provide a wrapped cork core molding method, which improves the molding accuracy, adaptability and installation convenience of cork products through a three-mold design of a lower mold silo, a pre-pressing upper mold and a molding upper mold, combined with two fillings and a precisely controlled molding process, and realizes cork wrapped molding of objects with complex shapes and sizes.
[0005] In order to achieve the above objectives, the solution of this application is: In a first aspect, an embodiment of the present application provides a wrapped cork core molding method, comprising: Three molds are made according to the object to be molded, and the three molds include a lower mold silo, a pre-pressing upper mold and a forming upper mold; Carry out the first filling and pre-pressing, prepare the cork raw material, divide the cork raw material into two parts by weight, add half of the cork raw material into the lower mold silo, and scrape the other half of the cork raw material flat, install the pre-pressing upper mold for pre-pressing molding; After the pre-pressing is completed, the pre-pressing upper mold is removed to form a pre-pressing space, and the object to be molded is placed in the pre-pressing space; The second filling and molding is performed, and the remaining half of the cork raw material is added to the part of the object to be molded that is not in the pre-pressing space, and the molding upper mold is installed for molding.
[0006] According to the above method of the embodiment of the present application, the following additional technical features may also be provided: Furthermore, a cork raw material is prepared, wherein the cork raw material is a mixture formed by uniformly stirring cork particles and oily polyurethane, and the cork raw material is equally divided into two parts according to the weight of the cork raw material.
[0007] Furthermore, the proportion of cork particles is divided into 30% of 12 mesh cork particles, 30% of 24 mesh cork particles, 20% of 30 mesh cork particles and 20% of 40 mesh cork particles by weight, the moisture content of the cork particles is between 8% and 12%, and the oily polyurethane is added according to the weight of the cork particles, and the addition ratio is between 10% and 15%.
[0008] Further, the upper molding mold is installed for compression molding, including heating at a set temperature. After the compression molding is completed, the molded product is taken out for cooling and solidification.
[0009] Further, heating is performed at a set temperature, wherein the temperature ranges from 100° C. to 110° C., and the heating time increases with the increase in the thickness of the article to be molded.
[0010] Furthermore, the molded article is cooled and solidified, including placing the molded article in a room temperature environment and cooling and solidifying it for 24 hours.
[0011] Furthermore, both the pre-pressing upper mold and the molding upper mold are positioning molds, which are used to determine the fixed position during the molding process.
[0012] Furthermore, the molding pressure ranges from 20 tons per square meter to 100 tons per square meter.
[0013] Furthermore, the time interval between pre-pressing and compression molding cannot exceed 5 minutes.
[0014] Compared with the prior art, the wrapped cork core molding method provided by the embodiment of the present application has the following beneficial technical effects: The embodiment of the present application ensures the uniform distribution of the cork raw material in the mold by means of two fillings and molding. The first half of the raw material pre-pressing not only allows the cork to be initially formed, but also provides a stable foundation for the subsequent placement of the object to be molded and the re-addition of cork raw material, which helps to reduce material waste and improve the density and consistency of the final product; after the object to be molded is placed in the pre-pressing space, the second filling is performed to ensure that the cork raw material can tightly and evenly wrap the object to be molded. This method can effectively cope with the production of complex shapes or products that require a high degree of fit; the three-mold structure is used for step-by-step operation, making the entire molding process more orderly and efficient, and each step of the operation has a clear purpose and steps, which reduces confusion and errors in the operation, thereby improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 A schematic diagram showing the process of the wrapped cork core molding method according to an embodiment of the present application is shown; Figure 2The structural diagram of the pre-pressing upper mold in the embodiment of the present application is shown; Figure 3 A schematic diagram showing the first addition of cork raw materials to the lower mold silo of an embodiment of the present application; Figure 4 The structure diagram of the upper molding die in the embodiment of the present application is shown; Figure 5 A schematic diagram showing the second addition of cork raw materials to the lower mold silo of an embodiment of the present application is shown. DETAILED DESCRIPTION
[0016] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. It is to be understood that the specific embodiments described herein are only used to explain the present application, rather than to limit the present application. It should also be noted that, for ease of description, only some structures related to the present application are shown in the accompanying drawings, rather than all structures. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0017] The terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device comprising a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to these processes, methods, products or devices.
[0018] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0019] like Figure 1 As shown, the embodiment of the present application provides a wrapped cork core molding method, comprising the following steps: Step 101, making three molds according to the object to be molded, the three molds including a lower mold silo, a pre-pressing upper mold and a molding upper mold.
[0020] The production of the three molds in the embodiment of the present application requires comprehensive consideration of the shape, size, material properties and molding process requirements of the molded objects. The specific production method is a common technical means for those skilled in the art and will not be repeated here.
[0021] like Figures 2 to 5As shown, the lower mold silo in the embodiment of the present application is mainly used to store and position the cork raw materials to be molded, ensuring that the cork raw materials are stable and easy to control during the molding process. According to the shape and size of the molded object, a reasonable lower mold silo structure is designed, including the volume, shape, inlet and outlet positions of the lower mold silo. The lower mold silo should be able to firmly support the cork raw materials to prevent movement or deformation during the molding process.
[0022] The pre-pressing upper mold is used to perform preliminary compression on the cork raw material to improve the density and uniformity of the cork raw material and prepare for subsequent molding. According to the final shape of the object to be molded, the cavity shape and size of the pre-pressing upper mold are designed. The cavity should be slightly larger than the size of the molded object. The larger size is based on the thickness required for the final cork wrapping. The lower mold silo also provides the feeding space required for the second addition of cork raw materials to allow the cork raw materials to have a certain space during the pre-pressing process. Figure 3 and Figure 5 They are respectively a schematic diagram of adding cork raw materials for the first time to the lower mold silo of an embodiment of the present application and a schematic diagram of adding cork raw materials for the second time to the lower mold silo of an embodiment of the present application.
[0023] In addition, a reasonable pressure control system needs to be designed to ensure that uniform and stable pressure can be applied during the pre-pressing process. The pressure should be determined according to the properties of the cork raw material and the requirements of the molding process.
[0024] In this embodiment, a heating system is also designed. Heating can make the cork raw material quickly molded during molding, shorten the molding time, and improve production efficiency. The preheating temperature and time are controlled by the heating system.
[0025] The upper molding die is used to further compress and mold the pre-pressed cork raw material to obtain the final product shape. The cavity shape and size of the upper molding die should be completely consistent with the requirements of the final product to ensure the dimensional accuracy and appearance quality of the product.
[0026] The pre-pressing upper mold and the molding upper mold in the embodiments of the present application are both positioning molds, which are used to determine the fixed position during the molding process. The positioning mold is a type of mold used in mold design to ensure the accuracy of the fixed position during the molding process. It mainly uses a built-in positioning device or structure to achieve precise positioning of the material or workpiece in the mold, thereby ensuring the dimensional accuracy and shape consistency of the product.
[0027] Positioning the mold can reduce product defects caused by position deviation, such as dimensional deviation, shape distortion, etc., thereby improving the qualification rate and quality of the product. And because the positioning mold can ensure the stability of the molding process, it can reduce the time and manpower wasted on adjusting the mold position and improve production efficiency.
[0028] In the embodiment of the present application, the molding pressure ranges from 20 tons per square meter to 100 tons per square meter, which is a relatively flexible parameter that can be adjusted according to specific conditions. The molding pressure is usually adjusted by the pressure control system of the machine to meet the product requirements of different materials, sizes and shapes.
[0029] Adjusting the molding pressure is one of the key steps to ensure product quality. Too low a pressure may lead to problems such as poor product molding, insufficient density or dimensional deviation; while too high a pressure may damage the mold, reduce product strength or increase production costs. Therefore, in actual production, it is necessary to accurately adjust the molding pressure according to the specific conditions of the product and the design requirements of the mold.
[0030] Step 102, performing the first filling and pre-pressing, adding half of the cork raw material into the lower mold silo, and scraping the half of the cork raw material flat, installing the pre-pressing upper mold for pre-pressing molding.
[0031] In the embodiment of the present application, the first filling and pre-pressing are performed to ensure the initial positioning and forming of the cork raw material in the mold. Specifically, it is necessary to first ensure that the lower mold silo and the pre-pressing upper mold are clean, undamaged and well-matched, check whether there are impurities or residues in the mold cavity, and clean them, and then prepare the cork raw material according to the process requirements and ensure that its quality meets the standards.
[0032] In this embodiment, the cork raw material is a mixture formed by uniformly stirring cork particles and oily polyurethane, wherein the proportion of the cork particles is (calculated by weight percentage): 30% of the 12-mesh cork particles are larger particles that help provide the skeleton and support of the mixture; 30% of the 24-mesh cork particles are medium-sized particles that help fill the gaps between large particles and increase the density of the mixture; 20% of the 30-mesh cork particles are smaller particles that can further refine the structure of the mixture and improve surface smoothness; 20% of the 40-mesh cork particles are the finest particles and are used to fill smaller gaps to make the mixture more uniform and compact.
[0033] The moisture content of the cork particles is controlled between 8% and 12%. Specifically, controlling the moisture content of the cork particles during the molding and heating process helps promote the chemical reaction and physical bonding between the cork particles and the oily polyurethane, thereby accelerating the curing process. Water can serve as a reaction medium, allowing the oily polyurethane to better penetrate between the cork particles and form a stronger structure.
[0034] Strictly controlling the moisture content helps ensure uniform mixing and distribution of cork particles and oil-based polyurethane, thereby avoiding local strength deficiencies or defects during the molding process. At the same time, the appropriate moisture content also helps improve the weather resistance, wear resistance and service life of the product.
[0035] The addition ratio of oily polyurethane is between 10% and 15% of the weight of the cork particles. As a binder and reinforcing agent, oily polyurethane can significantly improve the cohesion and strength of the mixture. The appropriate addition ratio can ensure that the mixture maintains good shape stability during the molding process and has the required physical properties after molding.
[0036] Weigh various cork particles and oily polyurethane according to the above proportions, stir the cork particles and oily polyurethane thoroughly until the mixture is uniform, weigh the mixture according to the weight of the cork material required by the product setting, and divide it into two equal parts.
[0037] Add half of the prepared cork raw material into the lower mold silo, paying attention to even distribution to avoid local accumulation or gaps. Use appropriate tools, such as a scraper or scraper, to scrape the added cork raw material flat to ensure that its surface is flat and in close contact with the bottom of the mold. This step is to ensure that the raw material can be evenly stressed during the pre-pressing process.
[0038] Use a mold clamp or other fixing device to firmly fix the pre-pressing upper mold to the lower mold hopper. This step is to ensure that the mold will not move or loosen during the pre-pressing process.
[0039] After confirming that all preparations have been completed and are correct, perform the pre-pressing operation and set appropriate pressure and time parameters according to the process requirements. During the pre-pressing process, closely observe the deformation of the mold and the reading of the pressure gauge. When the predetermined pressure and time are reached, stop the pre-pressing.
[0040] Step 103, after the pre-pressing is completed, the pre-pressing upper mold is removed to form a pre-pressing space, and the object to be molded is placed in the pre-pressing space.
[0041] In the embodiment of the present application, it is first necessary to ensure that the pre-pressing operation has been completed and the cork raw material has been initially formed and has achieved the expected density and shape, and then remove the pre-pressing upper mold from the lower mold silo to ensure that the mold or the initially formed cork raw material is not damaged during the removal process.
[0042] After removing the pre-pressing upper mold, check whether the pre-pressing space formed in the lower mold silo meets the requirements. The pre-pressing space should have sufficient depth and shape to accommodate the items to be molded and allow the remaining cork raw materials to fill and wrap the items in the subsequent steps. If there are impurities or residues in the pre-pressing space, use appropriate tools to clean it. At the same time, ensure that the surface of the pre-pressing space is flat and clean so that the items to be molded can be placed stably in it.
[0043] Step 104, performing a second filling and molding, adding the remaining half of the cork raw material to the portion of the object to be molded that is not in the pre-compression space, and installing the molding upper mold for molding.
[0044] After the first filling and pre-pressing, and placing the object to be molded into the pre-pressing space, the next step is the second filling and molding process. Two portions of cork material are mixed at one time, weighed according to product requirements, and then divided into two, with one portion of cork material added each during the first pre-pressing and second molding.
[0045] Add the remaining cork raw materials to the part of the molded object that is not in the pre-pressing space. After confirming that the second filling is completed, place the molding upper mold accurately above the lower mold silo and ensure that it is aligned with the cavity of the lower mold silo. Use a mold clamping device or other fixing device to firmly fix the molding upper mold on the lower mold silo.
[0046] Set the parameters such as pressure, temperature and time of the molding according to the process requirements. The selection of these parameters should take into account the characteristics of the cork raw material, the size and shape of the object to be molded, and the performance requirements of the required product. After confirming that all preparations have been completed and are correct, the molding operation is carried out. During the molding process, closely observe the deformation of the mold and the reading of the pressure gauge, and adjust the molding parameters according to the actual situation to ensure a good molding effect. At the same time, pay attention to check the sealing and stability of the mold to prevent leakage or mold damage. When the predetermined molding time and pressure are reached, stop the molding.
[0047] In this embodiment, according to the process requirements, the heating temperature of the molding is set between 100°C and 110°C. This temperature range is conducive to the rapid solidification and molding of the cork raw material. After the molding is completed, the molded object is placed in a room temperature environment for cooling and solidification. This process usually takes 24 hours or longer, depending on the size, shape and characteristics of the raw materials of the product. During the cooling and solidification process, the product will gradually harden and achieve the desired physical properties.
[0048] In addition, in the compression molding process, the time interval between pre-pressing and compression molding is a key parameter, which directly affects the molding quality and production efficiency of the product. If the time interval is too long, the cork raw material after pre-pressing may become loose again due to the loss of some pressure, resulting in difficulty in achieving the ideal density and shape stability in the subsequent compression molding process.
[0049] Therefore, in the embodiment of the present application, the time interval between pre-pressing and compression molding cannot exceed 5 minutes. This is to ensure that compression molding is carried out immediately after the pre-pressing is completed to maintain the compression state and temperature of the raw materials, thereby facilitating the molding of the product.
[0050] Specifically, by reasonably arranging the production process between pre-pressing and compression molding, ensuring that the connection between the two is close and efficient, and by reducing unnecessary waiting time and operating steps, the time interval can be shortened. After the pre-pressing is completed, try to keep the temperature of the mold and cork raw material stable to avoid the temperature dropping too quickly and causing the raw material to harden. This can be achieved by setting an insulation device around the mold or adjusting the temperature control strategy of the heating system.
[0051] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.
[0052] The embodiments of the present application are described above in conjunction with the accompanying drawings, but the present application is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the guidance of the present application, ordinary technicians in this field can also make many forms without departing from the purpose of the present application and the scope of protection of the claims, all of which are within the protection of the present application.
Claims
1. A wrapped cork core molding method, characterized in that: The method comprises: Making three molds according to the object to be molded, the three molds comprising a lower mold silo, a pre-pressing upper mold and a forming upper mold; Performing the first filling and pre-pressing, preparing cork raw materials, dividing the cork raw materials into two parts by weight, adding half of the cork raw materials into the lower mold silo, and flattening the half of the cork raw materials, installing the pre-pressing upper mold for pre-pressing molding; After the pre-pressing is completed, the pre-pressing upper mold is removed to form a pre-pressing space, and the object to be molded is placed in the pre-pressing space; The second filling and molding is performed, and the remaining half of the cork raw material is added to the upper space after the molded object is placed in the lower mold silo, and the molding upper mold is installed for molding.
2. The wrapped cork core molding method according to claim 1, characterized in that: The cork raw material is prepared, wherein the cork raw material is a mixture formed by uniformly stirring cork particles and oily polyurethane, and the cork raw material is evenly divided into two parts according to the weight of the cork raw material.
3. The wrapped cork core molding method according to claim 2, characterized in that: The proportion of the cork particles is divided into 30% of 12-mesh cork particles, 30% of 24-mesh cork particles, 20% of 30-mesh cork particles and 20% of 40-mesh cork particles by weight. The moisture content of the cork particles is between 8% and 12%. The oily polyurethane is added according to the weight of the cork particles, and the addition ratio is between 10% and 15%.
4. The wrapped cork core molding method according to claim 1, characterized in that: The step of installing the upper molding die for compression molding includes heating at a set temperature. After the compression molding is completed, the molded product is taken out for cooling and solidification.
5. The wrapped cork core molding method according to claim 4, characterized in that: The heating is performed at a set temperature, wherein the temperature ranges from 100° C. to 110° C., and the heating time increases with the increase in the thickness of the article to be molded.
6. The wrapped cork core molding method according to claim 4, characterized in that: The step of cooling and curing the object to be molded comprises placing the object to be molded in a room temperature environment and cooling and curing it for 24 hours.
7. The wrapped cork core molding method according to claim 1, characterized in that: The pre-pressing upper mold and the forming upper mold are both positioning molds, which are used to determine the fixed position during the molding process.
8. The wrapped cork core molding method according to claim 1, characterized in that: The molding pressure ranges from 20 tons per square meter to 100 tons per square meter.
9. The wrapped cork core molding method according to claim 1, characterized in that: The time interval between the pre-pressing and the compression molding is no more than 5 minutes.