Graphite composite material and preparation method and application thereof

By using high-temperature doping and graphitization treatment technology in the negative electrode materials of lithium-ion batteries, heteroatom doping porous graphite is formed and heat treatment is carried out in carbon source gas and silicon source gas, the negative electrode materials of lithium-ion batteries are solved in the fast charging and The shortcomings in high-speed charging performance have significantly improved the circulation performance and safety of the material.

CN118954497APending Publication Date: 2024-11-15SHENZHEN GOLD MEDAL NEW ENERGY TECH CO LTD

Patent Information

Application Number
CN202411038191.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing lithium-ion battery anode materials have limited improvements in fast charging and large-scale charging performance, and the circulation performance and safety of the materials need to be further improved.

Method used

By mixing raw materials coke, sodium and inorganic pore-forming agent, high-temperature doping and graphitization, heteroatom-doped porous graphite is formed, and heat treatment is performed in the mixed gas of carbon source gas and silicon source gas to form a coated content. 硅的无定形碳结构,提升材料的快充性能和循环能力。

Benefits of technology

It significantly improves the fast charging performance, cycle performance and high-speed charging capacity of the negative electrode material of lithium-ion battery, improves the specific capacity and electronic conductivity of the material, improves the interface impedance, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954497A_ABST
    Figure CN118954497A_ABST
Patent Text Reader

Abstract

The invention discloses a graphite composite material and a preparation method and application thereof.The preparation method comprises the following steps that raw materials including coke, sodium and an inorganic pore forming agent are mixed to be uniform, then the temperature of the mixture is increased to 900-1000 DEG C, heat preservation is conducted, then the temperature is increased to 1000-1400 DEG C, heteroatom gas is introduced for doping, and then the mixture is cooled to the room temperature; finally, carrying out graphitization treatment to obtain the heteroatom doped porous graphite. And carrying out heat treatment on the heteroatom-doped porous graphite under the condition of introducing mixed gas to obtain the graphite composite material. According to the preparation method of the graphite composite material, metal sodium and an inorganic pore-forming agent are doped in raw material coke, in the heating process, sodium ions are volatilized to expand the interlayer spacing of carbon, the inorganic pore-forming agent forms pores to form a porous structure, and heteroatom-doped porous graphite is obtained through heteroatom doping; then, under the condition that mixed gas of carbon source gas and silicon source gas is introduced into the heteroatom-doped porous graphite, the surface of the material is coated with silicon-containing amorphous carbon, and the fast charging performance of the graphite composite material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of secondary batteries, and in particular to a method for preparing a graphite composite material, the graphite composite material and applications thereof. Background Art

[0002] As a green and environmentally friendly new energy, lithium-ion batteries have the advantages of good reliability, high safety, small size and light weight. They have been widely used in digital products, electric vehicles, military products and other fields. With the vigorous development of the new energy industry, the development of lithium-ion batteries is in full swing, but the requirements for the service life, safety and low cost of lithium-ion batteries are also getting higher and higher. At present, lithium-ion batteries are also developing in the direction of long life, high safety, high rate and low cost.

[0003] The negative electrode material is one of the key factors that restrict the energy density and rate charge and discharge performance of lithium-ion batteries. The negative electrode materials used in energy storage batteries are mainly selected from raw materials with high isotropy, artificial graphite materials with low specific surface area and low expansion. However, as the new SEI film expands during the cycle, it consumes lithium ions, causing the cycle performance to decrease during the charge and discharge process.

[0004] Compared with natural graphite negative electrode materials, artificial graphite negative electrode materials have better performance, and artificial graphite negative electrode materials have become the mainstream of power battery negative electrode materials. At present, the raw materials used to prepare artificial graphite lithium-ion battery negative electrode materials are mainly coke raw materials, including: needle coke, petroleum coke, and asphalt coke.

[0005] As the market's demand for fast charging of lithium-ion batteries increases, artificial graphite is required to have excellent fast charging performance, and the factors that affect its graphite fast charging performance mainly include: particle size, carbon coating amount, interface impedance, material interlayer spacing, etc. Currently, commercial artificial graphite mainly improves the fast charging performance of the material by reducing the aggregate particle size and increasing the material coating amount, but the improvement is limited. Patent application number CN201410787061.7 discloses a fast-charging graphite lithium-ion battery negative electrode material and a preparation method thereof, which mainly comprises (1) mixing, heating, kneading, and crushing a mixture containing a graphite precursor and asphalt; (2) heat treating at 300-700°C under inert gas protection; (3) graphitizing. The fast-charging graphite lithium-ion battery negative electrode material prepared by this method has an average particle size D50 of 5-15μm and a specific surface area of ​​2.0m 2 / g or less, the first discharge capacity of the battery made of the fast-charging graphite lithium-ion battery negative electrode material is above 355mAh / g, the first charge and discharge efficiency is above 90%, the fast charging and rate performance are good, but the improvement on the high-rate charging of the fast-charging graphite lithium-ion battery negative electrode material is not significant. Summary of the invention

[0006] Based on this, it is necessary to provide a method for preparing a graphite composite material that can solve the above problems.

[0007] In addition, it is also necessary to provide a graphite composite material prepared by the preparation method of the graphite composite material and the application of the graphite composite material.

[0008] A method for preparing a graphite composite material comprises the following steps:

[0009] The raw materials of coke, sodium and inorganic pore-forming agent are mixed uniformly, and then the mixture is heated to 900-1000°C and kept warm for 1h-6h, and then heated to 1000-1400°C and introduced with heteroatom gas for 2h-6h for doping, and finally heated to 2800-3200°C for graphitization treatment for 12h-48h to obtain heteroatom-doped porous graphite;

[0010] The heteroatom-doped porous graphite is heat-treated under the condition of introducing a mixed gas to obtain a graphite composite material, wherein the mixed gas is a mixed gas of a carbon source gas and a silicon source gas in a volume ratio of 100:1-10.

[0011] In one embodiment, in the operation of uniformly mixing the raw coke, sodium and the inorganic pore former, the mass ratio of the raw coke, the sodium and the inorganic pore former is 100:1-5:1-5.

[0012] In one embodiment, the operation of uniformly mixing the raw coke, sodium and the inorganic pore-forming agent is: grinding and uniformly mixing the raw coke, sodium and the inorganic pore-forming agent.

[0013] In one embodiment, in the operation of introducing the heteroatom gas for 2h-6h for doping, the heteroatom gas is selected from at least one of ammonia, hydrogen sulfide, boron hydride and phosphine, and the flow rate of the heteroatom gas is 100ml / min-500ml / min.

[0014] In one embodiment, the raw coke is selected from at least one of petroleum coke, oil-based needle coke, coal-based needle coke and asphalt coke;

[0015] The inorganic pore former is selected from at least one of Na2CO3, K2CO3, NaNO3 and KNO3.

[0016] In one embodiment, the heteroatom-doped porous graphite is heat treated under the condition of passing a mixed gas, the heat treatment temperature is 700°C-1000°C, the heat treatment time is 30min-300min, and the flow rate of the mixed gas is 100ml / min-500ml / min.

[0017] In one embodiment, the carbon source gas is selected from at least one of alkanes, alkenes and alkynes, and the silicon source gas is silane.

[0018] In one embodiment, the carbon source gas is at least one of methane, ethane, ethylene, acetylene and propyne; the silicon source gas is at least one of trichlorosilane, tetrachlorosilane, dichlorosilane, monosilane and disilane.

[0019] A graphite composite material is prepared by the above-mentioned graphite composite material preparation method.

[0020] Application of the above graphite composite materials in the field of energy storage devices.

[0021] The preparation method of the graphite composite material of the present invention comprises the following steps: by doping metallic sodium and an inorganic pore-forming agent into the raw coke, sodium ions are volatilized during heating to expand the interlayer spacing of carbon, thereby shortening the resistance to insertion and extraction of lithium ions and improving the fast charging performance of the material; at the same time, the inorganic pore-forming agent forms pores to form a porous structure, so that after graphitization treatment, a porous graphite material with a large interlayer spacing is obtained, the liquid retention performance and isotropy of the material are improved, the kinetic performance of the material is improved, and heteroatom-doped porous graphite is obtained by heteroatom doping, the electronic conductivity of the material is improved at the defects of the raw coke, and the rate performance is improved; then, the heteroatom-doped porous graphite is heat-treated under the condition of passing a mixed gas of carbon source gas and silicon source gas to obtain a graphite composite material, so that silicon-containing amorphous carbon is coated on the surface of the material, the interface impedance is improved and the specific capacity is increased, and the fast charging performance of the graphite composite material is improved without reducing the specific capacity of the prepared graphite composite material.

[0022] In combination with specific embodiments, the resistivity, interlayer spacing and OI value of the graphite composite material prepared by the preparation method of the graphite composite material of the present invention are significantly better than those of the comparative example. The first discharge capacity, first charge and discharge efficiency, and liquid absorption capacity of the negative electrode sheet prepared using this graphite composite material are significantly higher than those of the comparative example. The constant current ratio, cycle performance and high-rate charging capacity of the soft-pack battery prepared using this graphite composite material are significantly better than those of the comparative example.

[0023] Specifically, the graphite composite material prepared by the preparation method of the graphite composite material of the present invention has a specific capacity of ≥365 mAh / g, a first efficiency of ≥92%, and a specific surface area of ​​2m 2 / g~3m 2 / g, powder OI value ≤2.5.

[0024] In addition, in the preparation method of the graphite composite material of the present invention, amorphous carbon is deposited on the outer layer of heteroatom-doped porous graphite by vapor deposition, so as to reduce the specific surface area of ​​the core material and improve the initial efficiency. At the same time, the amorphous carbon has high electronic conductivity and stable structure, so as to further improve the cycle and rate performance. At the same time, a small amount of nano-silicon is deposited in the porous graphite, and the specific capacity of the graphite material is improved by relying on the high specific capacity of the nano-silicon itself. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] in:

[0027] Figure 1 The present invention is a flow chart of a method for preparing a graphite composite material according to one embodiment.

[0028] Figure 2 This is the SEM image of the graphite composite material prepared in Example 1. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] In the present invention, the descriptions involving "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0031] Combination Figure 1 The present invention discloses a method for preparing a graphite composite material according to an embodiment of the present invention, comprising the following steps:

[0032] S10, mixing the raw materials of coke, sodium and inorganic pore-forming agent uniformly, then heating the mixture to 900°C-1000°C and keeping it for 1h-6h, then heating it to 1000°C-1400°C and introducing heteroatom gas for 2h-6h for doping, and finally heating it to 2800°C-3200°C for graphitization treatment for 12h-48h to obtain heteroatom-doped porous graphite.

[0033] In S10, by doping metallic sodium and inorganic pore-forming agents into the raw coke, sodium ions volatilize during the heating process to expand the interlayer spacing of carbon, shorten the insertion and extraction resistance of lithium ions, and improve the fast charging performance of the material. At the same time, the inorganic pore-forming agent forms pores to form a porous structure, so that after graphitization treatment, a porous graphite material with a large interlayer spacing is obtained, which improves the material's liquid retention performance and its isotropy, and the material's kinetic properties. Heteroatom-doped porous graphite is obtained by heteroatom doping, and the electronic conductivity of the material is improved at the defects of the raw coke, thereby improving the rate performance.

[0034] It should be noted that, in S10, the operation of heat treating the mixture needs to be performed under a protective gas atmosphere unless otherwise specified. The protective gas atmosphere may be a nitrogen atmosphere, a helium atmosphere, a neon atmosphere, an argon atmosphere, or the like.

[0035] Preferably, in the present embodiment, in the operation of uniformly mixing the raw coke, sodium and the inorganic pore former, the mass ratio of the raw coke, sodium and the inorganic pore former is 100:1-5:1-5.

[0036] Preferably, in this embodiment, the operation of uniformly mixing the raw coke, sodium and inorganic pore-forming agent is: grinding and uniformly mixing the raw coke, sodium and inorganic pore-forming agent.

[0037] In general, the grinding can be ball milling. Specifically, the operation of uniformly mixing the raw coke, sodium and inorganic pore-forming agent is as follows: adding the raw coke, sodium and inorganic pore-forming agent into a ball mill, controlling the rotation speed to 100 rpm to 500 rpm and ball milling for 1 h to 12 h.

[0038] Preferably, in this embodiment, in the operation of introducing heteroatom gas for 2h-6h for doping, the heteroatom gas is selected from at least one of ammonia, hydrogen sulfide, borohydride and phosphine, and the flow rate of the heteroatom gas is 100ml / min-500ml / min.

[0039] Preferably, in the present embodiment, the raw coke is selected from at least one of petroleum coke, oil-based needle coke, coal-based needle coke and asphalt coke.

[0040] Petroleum coke is a black solid coke produced by cracking and coking vacuum residue of petroleum at 500-550℃ in a coking unit. It is generally considered to be an amorphous carbon body, or a highly aromatized high molecular carbide, a carbon body with a needle-shaped or granular structure containing tiny graphite crystals.

[0041] Petroleum coke can be used as a raw material for energy storage materials to prepare artificial graphite or porous carbon, thereby increasing the added value of petroleum coke.

[0042] Needle coke is a porous solid with a silver-grey appearance and metallic luster. It is a high-quality variety of carbon materials. Its structure has obvious flow texture, is slightly elliptical, and has a large aspect ratio. It has a fibrous or needle-like texture and feels smooth to the touch. Needle coke has the characteristics of high carbon, low sulfur, low nitrogen, and low ash. It has outstanding electrochemical and mechanical properties after graphitization. It is an anisotropic high-end carbon material that is easy to graphitize.

[0043] Needle coke can be divided into two types: oil-based needle coke and coal-based needle coke. Needle coke produced from petroleum residue is oil-based needle coke; needle coke produced from coal tar pitch and its fractions is coal-based needle coke.

[0044] Pitch coke is the solid residue obtained after high-temperature dry distillation or delayed coking of coal tar pitch. Coal tar pitch has the characteristics of abundant resources, low price, high carbon content, good fluidity, and easy graphitization. It is one of the most important and basic matrix precursors in the production of various carbon materials.

[0045] Preferably, in this embodiment, the inorganic pore former is selected from at least one of Na2CO3, K2CO3, NaNO3 and KNO3.

[0046] Pore-forming agents such as Na2CO3, K2CO3, NaNO3 and KNO3 decompose at high temperatures to release gases, thereby forming holes inside the material and achieving pore formation.

[0047] S20, heat-treating the heteroatom-doped porous graphite under the condition of introducing a mixed gas to obtain a graphite composite material.

[0048] The mixed gas is a mixed gas of a carbon source gas and a silicon source gas in a volume ratio of 100:1-10.

[0049] The heteroatom-doped porous graphite is heat-treated under the condition of introducing a mixed gas of a carbon source gas and a silicon source gas, so that silicon-containing amorphous carbon is coated on the surface of the heteroatom-doped porous graphite, the interface impedance is improved, and the fast charging performance of the prepared graphite composite material is improved without reducing the specific capacity of the prepared graphite composite material.

[0050] The mixed gas is a mixture of carbon source gas and silicon source gas. Silicon source gas is introduced into porous graphite to deposit nano-silicon, thereby increasing the specific capacity of the graphite material, and the porous structure can reduce the expansion of nano-silicon. Since nano-silicon has high activity, in order to avoid gas production or combustion when nano-silicon comes into contact with electrolyte or air, it is necessary to coat its surface with amorphous carbon with good stability to reduce its activity and increase the electronic conductivity of the material.

[0051] Specifically, the prepared graphite composite material includes a core of a heteroatom-doped porous graphite material and a shell of a silicon-doped amorphous carbon material covering the core.

[0052] In addition, in the preparation method of the graphite composite material of the present invention, amorphous carbon is deposited on the outer layer of heteroatom-doped porous graphite by vapor deposition, the specific surface area of ​​the core material is reduced, the initial efficiency is improved, and the amorphous carbon has high electronic conductivity and stable structure, which further improves the cycle and rate performance. At the same time, a small amount of nano-silicon is deposited in the porous graphite, and the specific capacity of the graphite material is improved by relying on the high specific capacity of the nano-silicon itself.

[0053] It should be noted that in S20, in order to save carbon source gas and silicon source gas, the heteroatom-doped porous graphite is heat-treated under the condition of passing a mixed gas, and then cooled to room temperature under a protective gas atmosphere. The protective gas atmosphere can be a nitrogen atmosphere, a helium atmosphere, a neon atmosphere, an argon atmosphere, etc.

[0054] Preferably, in this embodiment, in the operation of heat treating the heteroatom-doped porous graphite under the condition of passing a mixed gas, the heat treatment temperature is 700°C-1000°C, the heat treatment time is 30min-300min, and the flow rate of the mixed gas is 100ml / min-500ml / min.

[0055] Generally speaking, the carbon source gas refers to a gas containing carbon, especially a gas that can be carbonized under high temperature conditions.

[0056] Generally speaking, the silicon source gas refers to a gas containing silicon, especially a gas that can be silicidated under high temperature conditions.

[0057] Preferably, in this embodiment, the carbon source gas is selected from at least one of alkanes, alkenes and alkynes, and the silicon source gas is silane.

[0058] Specifically, in this embodiment, the carbon source gas is at least one of methane, ethane, ethylene, acetylene and propyne, and the silicon source gas is at least one of trichlorosilane, tetrachlorosilane, dichlorosilane, monosilane and disilane.

[0059] The preparation method of this graphite composite material of the present invention, by doping metallic sodium and inorganic pore-forming agent in raw coke, sodium ions volatilize to expand the interlayer spacing of carbon during heating, shorten the insertion and extraction resistance of lithium ions, and improve the fast charging performance of the material. At the same time, the inorganic pore-forming agent forms a porous structure, so that after graphitization, a porous graphite material with a large interlayer spacing is obtained, the liquid retention performance of the material and its various isotropies are improved, the dynamic properties of the material are improved, and heteroatom-doped porous graphite is obtained by heteroatom doping, and the electronic conductivity of the material is improved at the defects of the raw coke, and the rate performance is improved. Then, the heteroatom-doped porous graphite is heat-treated under the condition of passing a mixed gas of carbon source gas and silicon source gas to obtain a graphite composite material, so that amorphous carbon containing silicon is coated on the surface of the material, the interface impedance is improved, and the fast charging performance of the graphite composite material is improved without reducing the specific capacity of the prepared graphite composite material.

[0060] In combination with specific embodiments, the resistivity, interlayer spacing and OI value of the graphite composite material prepared by the preparation method of the graphite composite material of the present invention are significantly better than those of the comparative example. The first discharge capacity, first charge and discharge efficiency, and liquid absorption capacity of the negative electrode sheet prepared using this graphite composite material are significantly higher than those of the comparative example. The constant current ratio, cycle performance and high-rate charging capacity of the soft-pack battery prepared using this graphite composite material are significantly better than those of the comparative example.

[0061] Specifically, the graphite composite material prepared by the preparation method of the present invention has a specific capacity of ≥365 mAh / g, a first efficiency of ≥92%, and a specific surface area of ​​2 2 / g~3m 2 / g, powder OI value ≤2.5.

[0062] The present invention also discloses a graphite composite material prepared by the above-mentioned graphite composite material preparation method in an embodiment.

[0063] Specifically, in the present embodiment, the graphite composite material includes a core of a porous graphite material doped with heteroatoms and a shell of an amorphous carbon material doped with silicon covering the core.

[0064] The graphite composite material prepared by the preparation method of this graphite composite material of the present invention is obtained by doping metallic sodium and inorganic pore-forming agent in raw coke, and the interlayer spacing of carbon is expanded by volatilization of sodium ions during heating, which shortens the insertion and extraction resistance of lithium ions, improves the fast charging performance of the material, and the inorganic pore-forming agent forms a porous structure at the same time, so that after graphitization treatment, a porous graphite material with a large interlayer spacing is obtained, the liquid retention performance of the material and its various isotropies are improved, the dynamic properties of the material are improved, and heteroatom-doped porous graphite is obtained by heteroatom doping, and the electronic conductivity of the material is improved at the defects of raw coke, and the rate performance is improved. Then, the heteroatom-doped porous graphite is heat-treated under the condition of passing a mixed gas of carbon source gas and silicon source gas to obtain a graphite composite material, so that amorphous carbon containing silicon is coated on the surface of the material, the interface impedance is improved, and the fast charging performance of the graphite composite material is improved without reducing the specific capacity of the prepared graphite composite material.

[0065] In combination with specific embodiments, the resistivity, interlayer spacing and OI value of the graphite composite material prepared by the preparation method of the graphite composite material of the present invention are significantly better than those of the comparative example. The first discharge capacity, first charge and discharge efficiency, and liquid absorption capacity of the negative electrode sheet prepared using this graphite composite material are significantly higher than those of the comparative example. The constant current ratio, cycle performance and high-rate charging capacity of the soft-pack battery prepared using this graphite composite material are significantly better than those of the comparative example.

[0066] Specifically, the graphite composite material prepared by the preparation method of the graphite composite material of the present invention has a specific capacity of ≥365 mAh / g, a first efficiency of ≥92%, and a specific surface area of ​​2m 2 / g~3m 2 / g, powder OI value ≤2.5.

[0067] The invention also discloses the application of the graphite composite material in the field of energy storage devices.

[0068] For example, the graphite composite material can be applied to the field of secondary batteries.

[0069] Specifically, the graphite composite material can be used as a negative electrode material for lithium-ion secondary batteries.

[0070] In addition, the above-mentioned graphite composite materials can also be applied to fields such as supercapacitors.

[0071] The following are specific embodiments.

[0072] The key raw material information is as follows:

[0073] Oil-based needle coke: Liaoning Jinzhou Petrochemical Co., Ltd.; Model: 4#;

[0074] Sodium metal: Manufacturer: Guangdong Xiaoda Chemical Co., Ltd.; CAS: 7440-23-5;

[0075] Petroleum coke: Tianjin Mingxintai Petrochemical Co., Ltd.; Model: 2#A.

[0076] Example 1

[0077] A method for preparing a graphite composite material comprises the following steps:

[0078] 100g of oil-based needle coke, 3g of metallic sodium and 3g of Na2CO3 were added to a ball mill, ball-milled at a speed of 300rpm for 6h, and after being evenly mixed, transferred to a tubular furnace, heated to 950℃ under an argon atmosphere and kept warm for 3h, then heated to 1000℃, and ammonia gas was introduced at a flow rate of 100ml / min for 3h for doping, and finally heated to 3000℃ for graphitization treatment for 24h to obtain heteroatom-doped porous graphite;

[0079] The heteroatom-doped porous graphite is transferred to a tube furnace, heated to 800°C, and a mixed gas of methane and monosilane (the volume ratio of methane gas to monosilane gas is 100:5) is introduced at a flow rate of 300 ml / min for 120 minutes, and then cooled to room temperature in an argon inert atmosphere to obtain the desired graphite composite material. The prepared graphite composite material includes a core of a heteroatom-doped porous graphite material and a shell of a silicon-doped amorphous carbon material covering the core.

[0080] Example 2

[0081] A method for preparing a graphite composite material comprises the following steps:

[0082] 100g of petroleum coke, 1g of metallic sodium and 1g of K2CO3 were added to a ball mill, ball-milled at a speed of 100rpm for 12h, and after being evenly mixed, transferred to a tubular furnace, heated to 900℃ in an argon atmosphere and kept warm for 6h, then cooled to 1400℃, and hydrogen sulfide gas was introduced at a flow rate of 500ml / min for 2h for doping, and finally heated to 2800℃ for graphitization treatment for 48h to obtain heteroatom-doped porous graphite;

[0083] The heteroatom-doped porous graphite is transferred to a tube furnace, heated to 700°C, and a mixed gas of ethylene and disilane (the volume ratio of ethylene gas to disilane gas is 100:1) is introduced at a flow rate of 100 ml / min for 300 minutes, and then cooled to room temperature in an argon inert atmosphere to obtain the desired graphite composite material. The prepared graphite composite material includes a core of a heteroatom-doped porous graphite material and a shell of a silicon-doped amorphous carbon material covering the core.

[0084] Example 3

[0085] A method for preparing a graphite composite material comprises the following steps:

[0086] 100g of pitch coke, 5g of metallic sodium and 5g of NaNO3 were added to a ball mill, ball-milled at a speed of 500rpm for 1h, and after being evenly mixed, transferred to a tubular furnace, heated to 1000℃ under an argon atmosphere and kept warm for 1h, then heated to 1400℃, and borohydride gas was introduced at a flow rate of 50ml / min for 6h for doping, and finally heated to 3200℃ for graphitization treatment for 12h to obtain heteroatom-doped porous graphite;

[0087] The heteroatom-doped porous graphite is transferred to a tube furnace, heated to 1000°C, and a mixed gas of acetylene and trichlorosilane (the volume ratio of acetylene gas to trichlorosilane gas is 100:10) is introduced at a flow rate of 500 ml / min for 30 minutes, and then cooled to room temperature in an argon inert atmosphere to obtain the desired graphite composite material. The prepared graphite composite material includes a core of a heteroatom-doped porous graphite material and a shell of a silicon-doped amorphous carbon material covering the core.

[0088] Example 4

[0089] A method for preparing a graphite composite material comprises the following steps:

[0090] 100g of oil-based needle coke, 1g of metallic sodium and 5g of Na2CO3 were added to a ball mill, ball-milled at a speed of 300rpm for 6h, and after being evenly mixed, transferred to a tubular furnace, heated to 950℃ under an argon atmosphere and kept warm for 3h, then heated to 1000℃, and ammonia gas was introduced at a flow rate of 100ml / min for 3h for doping, and finally heated to 3000℃ for graphitization treatment for 24h to obtain heteroatom-doped porous graphite;

[0091] The heteroatom-doped porous graphite is transferred to a tube furnace, heated to 800°C, and a mixed gas of methane and monosilane (the volume ratio of methane gas to monosilane gas is 100:5) is introduced at a flow rate of 300 ml / min for 120 minutes, and then cooled to room temperature in an argon inert atmosphere to obtain the desired graphite composite material. The prepared graphite composite material includes a core of a heteroatom-doped porous graphite material and a shell of a silicon-doped amorphous carbon material covering the core.

[0092] Example 5

[0093] A method for preparing a graphite composite material comprises the following steps:

[0094] 100g of oil-based needle coke, 5g of metallic sodium and 1g of Na2CO3 were added to a ball mill, ball-milled at a speed of 300rpm for 6h, and then transferred to a tubular furnace after being evenly mixed, and heated to 950℃ and kept for 3h under argon atmosphere, and then heated to 1000℃, and ammonia gas was introduced at a flow rate of 100ml / min for 3h for doping, and finally heated to 3000℃ for graphitization treatment for 24h to obtain heteroatom-doped porous graphite;

[0095] The heteroatom-doped porous graphite is transferred to a tube furnace, heated to 800°C, and a mixed gas of methane and monosilane (the volume ratio of methane gas to monosilane gas is 100:5) is introduced at a flow rate of 300 ml / min for 120 minutes, and then cooled to room temperature in an argon inert atmosphere to obtain the desired graphite composite material. The prepared graphite composite material includes a core of a heteroatom-doped porous graphite material and a shell of a silicon-doped amorphous carbon material covering the core.

[0096] Comparative Example 1

[0097] Comparative Example 1 is substantially the same as Example 1, except that metallic sodium and Na2CO3 are not added in Comparative Example 1.

[0098] The specific preparation process is as follows:

[0099] 100 g of oil-based needle coke was added to a ball mill and ball-milled at a speed of 300 rpm for 6 h. After being evenly mixed, it was transferred to a tubular furnace and heated to 950° C. and kept for 3 h under an argon atmosphere. Then, the temperature was raised to 1000° C. and ammonia gas was introduced at a flow rate of 100 ml / min for 3 h for doping. Finally, it was heated to 3000° C. and graphitized for 24 h to obtain porous graphite.

[0100] The porous graphite is transferred to a tube furnace, heated to 800°C, and a mixed gas of methane and monosilane (the volume ratio of methane gas to monosilane gas is 100:5) is introduced at a flow rate of 300 ml / min for 120 minutes, and then cooled to room temperature in an argon inert atmosphere to obtain the desired graphite composite material. The prepared graphite composite material includes a core of a porous graphite material and a shell of a silicon-doped amorphous carbon material covering the core.

[0101] Comparative Example 2

[0102] Comparative Example 2 is substantially the same as Example 1, except that no disilane gas is introduced into Comparative Example 2.

[0103] 100g of oil-based needle coke, 3g of metallic sodium and 3g of Na2CO3 were added to a ball mill, ball-milled at a speed of 300rpm for 6h, and after being evenly mixed, transferred to a tubular furnace, heated to 950℃ under an argon atmosphere and kept warm for 3h, then heated to 1000℃, and ammonia gas was introduced at a flow rate of 100ml / min for 3h for doping, and finally heated to 3000℃ for graphitization treatment for 24h to obtain heteroatom-doped porous graphite;

[0104] The heteroatom-doped porous graphite is transferred to a tube furnace, heated to 800°C, and methane gas is introduced at a flow rate of 300 ml / min for 120 minutes, and then cooled to room temperature in an argon inert atmosphere to obtain the desired graphite composite material. The prepared graphite composite material includes a core of a heteroatom-doped porous graphite material and a shell of an amorphous carbon material covering the core.

[0105] Test Case

[0106] 1. Physical and chemical properties test

[0107] 1.1) SEM test

[0108] The graphite composite material prepared in Example 1 was subjected to SEM test, and the test results are as follows: Figure 2 shown.

[0109] Depend on Figure 2 It can be seen that the graphite composite material prepared in Example 1 presents a secondary particle structure with a uniform size distribution, and its particle size is between 10-15 μm.

[0110] 1.2) Powder conductivity test:

[0111] The graphite composite materials prepared in Examples 1-5 and the graphite composite materials prepared in Comparative Examples 1-2 were pressed into block structures, and then the electrical conductivity of the powders was tested using a four-probe tester. The test results are shown in Table 1.

[0112] 1.3) Powder compaction density test

[0113] The graphite composite materials obtained in Examples 1-5 and the graphite composite materials obtained in Comparative Examples 1-2 were tested for powder compaction density. During the test, a certain mass of powder was weighed and placed in a mold, and a 2T pressure was used to press (using a powder compaction density meter, 1g of powder was placed in a fixed kettle and then pressed with a 2T pressure, and then the volume under compression was calculated for 10S, and the compaction density was calculated). At the same time, the specific surface area of ​​the material was tested in accordance with GB / T 24533-2019 "Graphite Negative Electrode Materials for Lithium Ion Batteries", and the test results are shown in Table 1.

[0114] 1.4) Powder OI value and interlayer distance

[0115] The OI value of the powder material and the interlayer spacing La of the material were tested by XRD. The test results are shown in Table 1.

[0116] Table 1

[0117]

[0118] It can be seen from Table 1 that the powder resistivity, interlayer spacing and OI value of the graphite composite materials prepared in Examples 1-5 are significantly better than those in Comparative Examples 1-2. The reason is that the graphite composite materials prepared in Examples 1-5 improve the isotropy of the graphite composite materials and reduce the OI value of the graphite composite materials by expanding the interlayer spacing and pore formation of the materials through metallic sodium.

[0119] 2. Button battery test

[0120] The graphite composite materials prepared in Examples 1-5 and the graphite composite materials prepared in Comparative Examples 1-2 were respectively used as negative electrode materials to assemble button-type batteries A1, A2, A3, A4, A5, B1 and B2.

[0121] The assembly method is as follows: add a binder, a conductive agent and a solvent to the negative electrode material, stir to make a slurry, apply it on a copper foil, dry and roll to obtain a negative electrode sheet. The binder used is LA132 binder, the conductive agent is SP, the negative electrode material is the graphite composite material in Examples 1-5 and Comparative Examples 1-2, and the solvent is double distilled water. The proportion of each component is: negative electrode material: SP: LA132: double distilled water = 95g: 1g: 4g: 220mL; the electrolyte is LiPF6 / EC+DEC (the concentration of LiPF6 is 1.2mol / L, and the volume ratio of EC and DEC is 1:1), the metal lithium sheet is the counter electrode, and the diaphragm is a polyethylene (PE) film. The button cell was assembled in an argon-filled glove box, and the electrochemical performance test was performed on a Wuhan Blue Power CT2001A battery tester. The charge and discharge voltage range was 0.005 V to 2.0 V, the charge and discharge rate was 0.1 C, and the charging DCR (50% SOC) was tested. The test results are shown in Table 2.

[0122] At the same time, the above negative electrode was taken to test the liquid absorption capacity of the electrode (1 ml of electrolyte was absorbed by a 10 ml pipette and dropped onto the electrode until the electrolyte on the electrode was completely absorbed, and the time t was recorded). The results are shown in Table 2.

[0123] Table 2

[0124]

[0125]

[0126] It can be seen from Table 2 that the first discharge capacity, first charge and discharge efficiency, and liquid absorption capacity of the button cell and negative electrode sheet using the graphite composite materials prepared in Examples 1-5 are significantly higher than those of the comparative example. The reason is that the graphite composite materials prepared in Examples 1-5 have a low powder resistivity to reduce DCR, and nano-silicon is deposited on the surface to increase the specific capacity of the material. At the same time, the graphite composite materials prepared in Examples 1-5 have a high specific surface area, which improves the liquid absorption capacity of the graphite composite materials prepared in Examples 1-5.

[0127] 3. Soft pack battery test

[0128] The graphite composite materials prepared in Examples 1-5 and the graphite composite materials prepared in Comparative Examples 1-2 were used as negative electrode materials to prepare negative electrode plates. Lithium iron phosphate was used as the positive electrode, LiPF6 solution (solvent was EC+DEC, volume ratio was 1:1, LiPF6 concentration was 1.1 mol / L) was used as the electrolyte, and celegard2400 was used as the separator to prepare 2Ah soft-pack batteries A6, A7, A8, A9, A10, B3 and B4.

[0129] The cycle performance and rate performance of the soft-pack battery were then tested, and the test results are shown in Table 3.

[0130] Rate performance test conditions: charging rate: 1C / 2C / 3C / 5C, discharge rate 1C; voltage range: 2.8V-4.2V.

[0131] The cycle test conditions are: 1C / 1C, 2.8V-4.2V, temperature: 25±3℃, number of cycles, 500 cycles.

[0132] Table 3

[0133]

[0134]

[0135] It can be seen from Table 3 that the soft-pack batteries prepared from the graphite composite materials prepared in Examples 1-5 of the present invention have better constant current ratio and cycle performance, and the high-rate constant current ratio is significantly better than that of Comparative Examples 1-2. The reason is that the graphite composite materials prepared in Examples 1-5 have low powder resistivity and large interlayer spacing, which improves the fast charging performance of the graphite composite materials prepared in Examples 1-5, that is, improves the constant current ratio of the graphite composite materials prepared in Examples 1-5; at the same time, the graphite composite materials prepared in Examples 1-5 have excellent liquid absorption capacity, which improves the cycle performance of the material.

[0136] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a graphite composite material, characterized in that: The steps include: The raw materials of coke, sodium and inorganic pore-forming agent are mixed uniformly, and then the mixture is heated to 900-1000°C and kept warm for 1h-6h, and then heated to 1000-1400°C and introduced with heteroatom gas for 2h-6h for doping, and finally heated to 2800-3200°C for graphitization treatment for 12h-48h to obtain heteroatom-doped porous graphite; The heteroatom-doped porous graphite is heat-treated under the condition of introducing a mixed gas to obtain a graphite composite material, wherein the mixed gas is a mixed gas of a carbon source gas and a silicon source gas in a volume ratio of 100:1-10.

2. The method for preparing the graphite composite material according to claim 1, characterized in that: In the operation of uniformly mixing the raw coke, sodium and the inorganic pore-forming agent, the mass ratio of the raw coke, the sodium and the inorganic pore-forming agent is 100:1-5:1-5.

3. The method for preparing the graphite composite material according to claim 2, characterized in that: The operation of uniformly mixing the raw coke, sodium and the inorganic pore-forming agent is as follows: grinding and uniformly mixing the raw coke, sodium and the inorganic pore-forming agent.

4. The method for preparing the graphite composite material according to claim 2, characterized in that: In the operation of introducing the heteroatom gas for 2h-6h for doping, the heteroatom gas is selected from at least one of ammonia, hydrogen sulfide, boron hydride and phosphine, and the flow rate of the heteroatom gas is 100ml / min-500ml / min.

5. The method for preparing the graphite composite material according to claim 4, characterized in that: The raw coke is selected from at least one of petroleum coke, oil-based needle coke, coal-based needle coke and asphalt coke; The inorganic pore former is selected from at least one of Na2CO3, K2CO3, NaNO3 and KNO3.

6. The method for preparing a graphite composite material according to any one of claims 1 to 5, characterized in that: In the operation of heat treating the heteroatom-doped porous graphite under the condition of introducing a mixed gas, the heat treatment temperature is 700° C.-1000° C., the heat treatment time is 30 min-300 min, and the flow rate of the mixed gas is 100 ml / min-500 ml / min.

7. The method for preparing the graphite composite material according to claim 6, characterized in that: The carbon source gas is selected from at least one of alkanes, alkenes and alkynes, and the silicon source gas is silane.

8. The method for preparing the graphite composite material according to claim 7, characterized in that: The carbon source gas is at least one of methane, ethane, ethylene, acetylene and propyne; the silicon source gas is at least one of trichlorosilane, tetrachlorosilane, dichlorosilane, monosilane and disilane.

9. A graphite composite material, characterized in that: The graphite composite material is prepared by the method for preparing the graphite composite material according to any one of claims 1 to 8.

10. Use of the graphite composite material according to claim 9 in the field of energy storage devices.

Citation Information

Patent Citations

  • Preparation method of doped high-specific-surface-area activated carbon

    CN104150479A

  • Negative electrode material and preparation method and application thereof

    CN114188533A

  • Fast-charging graphite composite material and preparation method thereof

    CN115528231A

  • Quick-charging graphite composite material, preparation method thereof and battery

    CN117342552A

  • Preparation method of fast-charging silicon-carbon composite material and lithium ion battery

    CN118405693A

Cited By

  • Porous graphite negative electrode material and preparation method and application thereof

    CN119976825A

  • Heteroatom-doped calcined coke material as well as preparation method and application thereof