Pervious concrete based on recycled aggregate loaded nano TiO2 and preparation method thereof

By synthesizing nano-titanium dioxide in situ on the surface of recycled aggregate and forming a layered structure, combined with a modified carbon fiber network, the problem of easy detachment of nano-photocatalytic materials was solved, thereby improving the pollutant degradation efficiency and stability of concrete.

CN118955046AInactive Publication Date: 2024-11-15CHANGCHUN INST OF TECH +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411018643.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The nano-photocatalytic materials on the surface of recycled aggregates are easily detached due to external environmental factors and rainwater erosion, and have weak bonding force. The utilization rate of nano-titanium dioxide inside concrete is low, which affects the degradation performance of pollutants.

Method used

Nano-titanium dioxide is synthesized in situ on the surface of recycled aggregate to form a core-shell material with a heterogeneous interface. It forms a cross- or arranged sheet structure with graphite-phase carbon nitride nanosheets and molybdenum disulfide nanosheets. Combined with modified carbon fibers and fish scale powder, it forms an effective stress transfer network to enhance the bonding force.

Benefits of technology

This improved the stability and utilization rate of nano-photocatalytic materials, enhanced the degradation performance and durability of concrete against pollutants, and ensured a strong bond between the composite photocatalytic materials and concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004966504670000141
    Figure BDA0004966504670000141
Patent Text Reader

Abstract

The invention discloses pervious concrete based on recycled aggregate loaded nano TiO2 and a preparation method of the pervious concrete, and belongs to the technical field of concrete materials. Comprising the following components in parts by mass: 350 to 400 parts of natural aggregate, 200 to 250 parts of recycled aggregate, 210 to 230 parts of cement, 240 to 260 parts of spun yarn, 60 to 90 parts of mineral powder, 12 to 15 parts of a reinforcing material, 10 to 20 parts of a composite nano titanium dioxide photocatalytic material, 0.8 to 1 part of sodium tripolyphosphate, 5 to 10 parts of a water reducing agent and 250 to 270 parts of water. The nanometer titania-loaded hollow nanometer material is filled between the nanometer sheet layers to form a concave-convex layer structure, so that the reflection and the reflection distance of visible light are increased; the fish scale powder and the recycled aggregate are combined through hydrogen bonds, so that the recycled aggregate can be connected to form a more effective stress transfer network, and the situation that the nano photocatalytic material is very easy to fall off due to the effects of environmental factors, abrasion, rain wash and the like on the concrete is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete materials, in particular to a permeable concrete based on recycled aggregate loaded with nano-TiO2 and a preparation method thereof. Background Art

[0002] Recycled aggregate permeable concrete is also called porous concrete or sandless concrete. Permeable concrete is composed of a thin layer of cement slurry coated on the surface of coarse aggregate, which are bonded together to form a honeycomb structure with evenly distributed pores. Therefore, it has a high porosity and permeability coefficient, which is conducive to rainwater infiltration, and has the advantages of noise reduction, heat insulation and good air permeability and water permeability. Nano-titanium dioxide is a good semiconductor photocatalyst with the advantages of low toxicity, stable chemical properties and strong light absorption. It can absorb photon energy to form redox potential on its surface, oxidize and reduce automobile exhaust into harmless substances such as water, carbon dioxide and salt. When rainwater enters the underground through permeable concrete, it can wash away the photocatalytic products attached to the surface of photocatalytic permeable concrete.

[0003] Recycled aggregates attach nano-photocatalytic materials through surface pores, and the binding force is weak, which makes the nano-photocatalytic materials on the surface of recycled aggregates easily affected by external environmental factors, wear, rain erosion, etc., causing the nano-photocatalytic materials to fall off easily, affecting the concrete's degradation performance for atmospheric pollutants; directly adding nano-titanium dioxide into concrete hinders the contact area between nano-titanium dioxide and the light source, resulting in low utilization rate of nano-titanium dioxide, which is not conducive to its promotion and application. Summary of the invention

[0004] The purpose of the present invention is to provide a permeable concrete based on recycled aggregate loaded nano-TiO2 and a preparation method thereof: a carbon iron zinc hollow nano-material is mixed with tetrabutyl titanate, and after hydrothermal treatment, nano-titanium dioxide is synthesized in situ on the surface of the carbon iron zinc hollow nano-material to form a core-shell material with a heterogeneous interface, thereby reducing the chance of photogenerated electron-hole recombination; the loaded nano-titanium dioxide hollow nano-material is deposited on the surface of a graphite phase carbon nitride nano-sheet, and then mixed with a molybdenum disulfide nano-sheet; the surface of the graphite phase carbon nitride nano-sheet is then mixed with a molybdenum disulfide nano-sheet to form a mutually crossed or arranged sheet structure, and the sheet structure can absorb external forces to produce The stress generated is avoided, and the photocatalytic performance of the loaded nano-titanium dioxide hollow nanomaterials is reduced due to the brittle hollow structure. The loaded nano-titanium dioxide hollow nanomaterials are filled between the graphite phase carbon nitride nanosheets and the molybdenum disulfide nanosheets to form a concave-convex layer structure, which increases the reflection and reflection distance of visible light. After the fish scale powder is deposited on the surface of the carbon fiber, it reacts with acrylamide and acrylic acid. The fish scale powder in the modified carbon fiber is combined with the recycled aggregate through hydrogen bonds, which can connect the recycled aggregate to form a more effective stress transfer network, thereby preventing the concrete from being affected by local environmental factors, wear, rain erosion, etc., which causes the nano-photocatalytic material to fall off easily.

[0005] The technical problems to be solved by the present invention are as follows: the nano-photocatalytic materials are attached to the recycled aggregates through the surface pores, and the bonding force is weak, which makes the nano-photocatalytic materials on the surface of the recycled aggregates susceptible to external environmental factors, wear, rain erosion and the like, causing the nano-photocatalytic materials to fall off very easily, affecting the degradation performance of concrete for atmospheric pollutants; the nano-titanium dioxide is directly added into the concrete, which hinders the contact area between the nano-titanium dioxide and the light source, resulting in a low utilization rate of the nano-titanium dioxide, which is not conducive to promotion and application.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A permeable concrete based on recycled aggregate loaded with nano-TiO2 comprises the following components by mass: 350-400 parts of natural aggregate, 200-250 parts of recycled aggregate, 210-230 parts of cement, 240-260 parts of spun yarn, 60-90 parts of mineral powder, 12-15 parts of reinforcing material, 10-20 parts of composite nano-titanium dioxide photocatalytic material, 0.8-1 part of sodium tripolyphosphate, 5-10 parts of water reducer and 250-270 parts of water.

[0008] A method for preparing permeable concrete based on recycled aggregate loaded with nano-TiO2 comprises the following steps:

[0009] S1. The composite nano-titanium dioxide photocatalytic material and 1 / 3 water were mixed, stirred evenly, sodium tripolyphosphate was added, and stirred at a speed of 9000r / min for 20min to obtain a suspension;

[0010] S2. The suspension was mixed with the recycled aggregate and soaked for 24 h, and dried in an oven at 80 ° C for 30 min to obtain a recycled aggregate loaded with composite nano-titanium dioxide photocatalytic material;

[0011] S3. Mix the recycled aggregate loaded with composite nano-titanium dioxide photocatalytic material, natural aggregate, reinforcing material and 1 / 3 part of water, stir for 30 seconds, add cement, fine yarn, mineral powder and water reducing agent, stir for 60 seconds to obtain a solid mixture, and finally add the remaining water and stir for 2 minutes to obtain permeable concrete.

[0012] Furthermore, the recycled aggregate is prepared by the following steps: the waste concrete is crushed, passed through a 20-25 mesh sieve, washed with deionized water, and crushed by a crusher to obtain the recycled aggregate.

[0013] Furthermore, the particle size of the recycled aggregate is 2.9-3.5 mm, the water absorption rate is 6.65-6.71%, and the apparent density is 2500-2700 kg / m 3 , bulk density is 1500-1600kg / m 3 .

[0014] Furthermore, the natural aggregate particle size is 3.1-3.8 mm, the water absorption rate is 0.69-0.81%, and the dry density is 1500-1520 kg / m 3 .

[0015] Furthermore, the cement is silicate cement with a PO4 of 2.5 and a specific surface area of ​​320-350m 2 / kg, 28d compressive strength is 55.3-55.9MPa, initial setting time is 90-100min, and final setting time is 140-150min.

[0016] Furthermore, the apparent density of fine sand is 2600-2700 kg / m 3 , fineness modulus is 1.6-2.1, particle size is 0.25-0.1mm, and mud content is 0.6-1%.

[0017] Furthermore, the mineral powder is S95 grade slag powder with a density of 2.9-3.5g / cm 3 , with a specific surface area of ​​450-500m 2 / kg, water content is 0.2-1%, and 28d activity index is 95%.

[0018] Furthermore, the water reducing agent is selected from the HPWR-Q8011 polycarboxylic acid high efficiency water reducing agent produced by Shaanxi Qinfen Building Materials Co., Ltd., and the water reducing rate of the water reducing agent is 25%.

[0019] Furthermore, the composite nano-titanium dioxide photocatalytic material is prepared by depositing a nano-titanium dioxide-loaded hollow nanomaterial on the surface of a graphite phase carbon nitride nanosheet and then mixing it with a molybdenum disulfide nanosheet.

[0020] Furthermore, the particle size of the molybdenum disulfide nanosheets is 0.8-1.2 μm.

[0021] Furthermore, the graphite phase carbon nitride nanosheets are 0.5-0.8 μm.

[0022] Furthermore, the composite nano titanium dioxide photocatalytic material is specifically prepared by the following steps:

[0023] The loaded nano-titanium dioxide hollow nanomaterial is added into deionized water, stirred evenly, succinic acid and hydrochloric acid with a mass fraction of 36% are added, the reaction is carried out at 60°C for 1 hour, graphite phase carbon nitride nanosheets are added, the reaction is continued for 10 minutes, the precipitate is collected by centrifugation at a rate of 3000 rpm, the precipitate is dried in an oven at 70°C for 10 minutes to obtain a solid, the solid is placed in deionized water, molybdenum disulfide nanosheets and ethylene glycol are added, the reaction is stirred at 70°C for 10 minutes, filtered, washed with deionized water 3 times, and dried in an oven at 70°C for 10 minutes to obtain a composite nano-titanium dioxide photocatalytic material.

[0024] Among them, the nano-titanium dioxide loaded hollow nanomaterial reacts with the hydroxyl groups on the surface of the graphite phase carbon nitride nanosheets through 2-hydroxysuccinic acid, so that the nano-titanium dioxide loaded hollow nanomaterial is deposited on the surface of the graphite phase carbon nitride nanosheets in the form of chemical bonds. The graphite phase carbon nitride nanosheets serve as carriers of the core-shell materials of the heterogeneous interface and can load more photocatalytic materials to enhance the photocatalytic performance.

[0025] Furthermore, the graphite phase carbon nitride nanosheets of the core-shell material deposited with the heterogeneous interface are mixed with the molybdenum disulfide nanosheets, and ethylene glycol is used as a cross-linking agent to form a mutually crossed or arranged layer structure between the graphite phase carbon nitride nanosheets and the molybdenum disulfide nanosheets. The layer structure can absorb the stress generated by the external force, thereby avoiding the degradation of the photocatalytic performance of the loaded nano-titanium dioxide hollow nanomaterial due to the brittleness of the hollow structure, thereby affecting the performance of the concrete. The loaded nano-titanium dioxide hollow nanomaterial is filled between the graphite phase carbon nitride nanosheets and the molybdenum disulfide nanosheets to form a concave-convex layer structure, thereby increasing the reflection and reflection distance of visible light, thereby increasing the contact area and contact time between the loaded nano-titanium dioxide hollow nanomaterial and the light source, thereby ensuring the stability and durability of the concrete in degrading automobile exhaust.

[0026] Furthermore, the dosage ratio of the loaded nano-titanium dioxide hollow nanomaterial, deionized water, succinic acid, and hydrochloric acid is (1.1-1.3) g: (70-90) mL: (0.05-0.15) g: (0.1-0.2) mL.

[0027] Furthermore, the dosage ratio of solid, deionized water, molybdenum disulfide nanosheets, and ethylene glycol is (2-3) g:(90-110) mL:(1-3) g:(1-3) mL.

[0028] Furthermore, the nano-titanium dioxide-loaded hollow nanomaterial is prepared by mixing the carbon-iron-zinc hollow nanomaterial with tetrabutyl titanate and subjecting it to a hydrothermal treatment;

[0029] Furthermore, the particle size of the carbon-iron-zinc hollow nanomaterial is 220-250nm.

[0030] Furthermore, the hydrothermal treatment temperature is 200-300°C, and the hydrothermal treatment time is 5-7h.

[0031] Furthermore, the nano-titanium dioxide loaded hollow nanomaterial is prepared by the following steps:

[0032] The carbon iron zinc hollow nanomaterial is added to ethanol, stirred evenly, and a concentrated ammonia solution and tetrabutyl titanate with a mass fraction of 28% are added. After stirring and mixing for 15 minutes, the mixture is stirred and reacted at 45°C for 2 hours, treated at 200-300°C for 6 hours, cooled to room temperature, washed with deionized water for 3 times, and dried in an oven at 70°C for 10 minutes to obtain a hollow nanomaterial loaded with nano-titanium dioxide.

[0033] Among them, tetrabutyl titanate undergoes a hydrolysis reaction and can combine with a large number of hydroxyl groups on the surface of the carbon-iron-zinc hollow nanomaterial through chemical bonds, so that the titanium dioxide precursor is coated on the surface of the carbon-iron-zinc hollow nanomaterial. After heat treatment, the in-situ synthesis of nano-titanium dioxide on the surface of the carbon-iron-zinc hollow nanomaterial is achieved to form a core-shell material with a heterogeneous interface, which reduces the chance of photogenerated electron-hole recombination and can promote the separation and transfer of photogenerated carriers, thereby enhancing the photocatalytic activity of the hollow nanomaterial loaded with nano-titanium dioxide and increasing the degradation effect of concrete on pollutants.

[0034] Furthermore, the amount ratio of carbon iron zinc hollow nanomaterial, ethanol, concentrated ammonia solution, and tetrabutyl titanate is (0.2-0.3) g: (80-120) mL: (0.2-0.4) mL: (0.6-0.8) g.

[0035] Furthermore, the carbon-iron-zinc hollow nanomaterial is prepared by the following steps:

[0036] Glucose, zinc acetate dihydrate and ferric chloride hexahydrate were added to deionized water, stirred for 30 minutes, heated to 180°C and maintained for 24 hours, cooled to room temperature, filtered, washed with deionized water three times, dried in an oven at 70°C for 10 minutes, and annealed at 450°C for 4 hours to obtain carbon-iron-zinc hollow nanomaterials.

[0037] Furthermore, the dosage ratio of glucose, zinc acetate dihydrate, ferric chloride hexahydrate, and deionized water is (2-4) g: (0.2-0.4) g: (0.7-0.9) g: (25-35) mL.

[0038] Furthermore, the reinforcing material is prepared by depositing fish scale powder on the surface of carbon fiber and then reacting with acrylamide and acrylic acid, and is specifically prepared by the following steps:

[0039] A1. Add carbon fiber to a 36% sodium hydroxide aqueous solution by mass, stir at 40°C for 1.5h, filter, wash with deionized water 3 times, dry in an oven at 70°C for 10min, place in ethanol, stir evenly, add fish scale powder, heat to 85°C, stir until the organic solvent evaporates, collect the solid, wash the solid with deionized water 3 times, and dry in an oven at 80°C for 10min to obtain modified carbon fiber.

[0040] Among them, after the carbon fiber is treated with an alkaline solution, the impurities on the surface of the carbon fiber are decomposed and removed, so that the carbon fiber exposes more oxygen-containing functional groups, and then contains a large number of hydroxyl functional groups, which can be combined with the hydroxyl and carboxyl groups in the fish scale powder through chemical bonds, so that the fish scale powder is deposited on the surface of the carbon fiber, blocking the pore structure of the carbon fiber, reducing the hygroscopicity of the carbon fiber, and avoiding the performance degradation of the concrete due to the easy moisture absorption of the carbon fiber. The carbon fiber can enhance the compressive strength, deformation and toughness of the concrete, and can also bridge the internal cracks of the concrete.

[0041] Furthermore, the usage ratio of carbon fiber, sodium hydroxide aqueous solution, ethanol and fish scale powder is (0.1-0.3) g:(15-25) mL:(25-35) mL:(2-3) g.

[0042] A2. Add acrylamide and acrylic acid to deionized water, stir evenly, add methylenebisacrylamide and modified carbon fiber, stir evenly, add ammonium persulfate, stir and react at 60°C for 2h to obtain a gel-like substance, take out the gel-like substance, and place it in 30mL of deionized water to obtain a reinforced material.

[0043] Among them, acrylamide and acrylic acid are polymerized under the action of the initiator ammonium persulfate to form a polymer with good hydrophilicity and flexibility. The hydroxyl and carboxyl groups contained in the fish scale powder in the modified carbon fiber can be combined with the polyacrylamide-acrylic acid polymer through chemical bonds to form a cross-linked structure, which increases the mechanical strength and toughness of the concrete and makes the carbon fiber have better dispersibility.

[0044] Furthermore, the usage ratio of acrylamide, acrylic acid, deionized water, methylenebisacrylamide, modified carbon fiber, and ammonium persulfate is (5-7) g:(1-2) g:(45-55) mL:(0.01-0.03) g:(0.3-0.7) g:(0.05-0.07) g.

[0045] Furthermore, the hydroxyapatite-loaded kapok fiber is prepared by treating the kapok fiber with a sodium hypochlorite solution and then mixing it with hydroxyapatite.

[0046] Furthermore, the sodium hypochlorite solution is prepared by mixing sodium hypochlorite, ethanol, and deionized water in a dosage ratio of (1-3) g: (8-12) mL: (170-190) mL.

[0047] Furthermore, compared with the prior art, the present invention has the following beneficial effects:

[0048] (1) In the technical solution of the present invention, the carbon-iron-zinc hollow nanomaterial, as a hollow nanomaterial, has a large specific surface area, can expand the light absorption range and reduce the photogenerated charge recombination, and has good photocatalytic performance. Nano-titanium dioxide is in situ synthesized on the surface of the carbon-iron-zinc hollow nanomaterial to form a core-shell material with a heterogeneous interface, which reduces the chance of photogenerated electron-hole recombination and can promote the separation and transfer of photogenerated carriers, thereby enhancing the photocatalytic activity of the hollow nanomaterial loaded with nano-titanium dioxide and increasing the degradation effect of concrete on pollutants.

[0049] (2) In the technical solution of the present invention, the nano-titanium dioxide loaded hollow nanomaterial is deposited on the surface of the graphite phase carbon nitride nanosheet in the form of chemical bonds, and then mixed with the molybdenum disulfide nanosheet to form a cross-linked or arranged lamellar structure. The lamellar structure can absorb the stress generated by external force, thereby avoiding the brittleness of the hollow nanomaterial of the nano-titanium dioxide loaded, which leads to a decrease in the photocatalytic performance and affects the performance of the concrete. The nano-titanium dioxide loaded hollow nanomaterial is filled between the graphite phase carbon nitride nanosheet and the molybdenum disulfide nanosheet to form a concave-convex layer structure, which increases the reflection and reflection distance of visible light, thereby increasing the contact area and contact time between the nano-titanium dioxide loaded hollow nanomaterial and the light source, thereby ensuring the stability and durability of the concrete in degrading automobile exhaust.

[0050] (3) In the technical solution of the present invention, acrylamide and acrylic acid are copolymerized to form a polymer with good hydrophilicity and flexibility. The modified carbon fiber is combined with the polyacrylamide-acrylic acid polymer through chemical bonds to form a cross-linked structure, which increases the mechanical strength and toughness of the concrete, and the carbon fiber has good dispersibility; the fish scale powder in the modified carbon fiber contains collagen, lecithin, vitamins, and a large amount of hydroxyl structure, which can be combined with the recycled aggregate through hydrogen bonds and can connect the recycled aggregate to form a more effective stress transfer network, thereby preventing the concrete from being affected by environmental factors, wear, rain erosion, etc., which causes the nano-photocatalytic material to fall off easily, affecting the concrete's degradation performance for atmospheric pollutants.

[0051] (4) In the technical solution of the present invention, the porous structure contained in the recycled aggregate can adsorb the composite photocatalytic material on the surface of the recycled aggregate, and the carboxyl group carried by the polyacrylic acid in the reinforcing material is negatively charged, and can adhere to the surface of the recycled aggregate with positive charge through electrostatic action, and then through the action of physical adsorption and chemical bonds, the composite photocatalytic material is more firmly adhered to the surface of the recycled aggregate, thereby increasing the bonding force between the composite photocatalytic material and concrete and preventing the composite photocatalytic material from falling off;

[0052] After the waste concrete is made into recycled aggregate, it is given photocatalytic properties by soaking it in a solution of composite nano-titanium dioxide photocatalytic material. It can be used to replace natural aggregate, which can not only save natural aggregate, but also significantly increase the light-receiving area of ​​the composite nano-titanium dioxide photocatalytic material in the concrete, ensuring the stability and durability of the concrete in degrading automobile exhaust, which is conducive to the large-scale promotion and application of recycled permeable concrete in concrete.

[0053] (5) In the technical solution of the present invention, porous recycled aggregate is directly used as a carrier for loading composite nano-titanium dioxide photocatalyst material. Because of its high water absorption rate, large specific surface area and other characteristics, the pores contained therein are conducive to the attachment of composite nano-titanium dioxide photocatalyst material, which greatly increases the number of active sites of composite nano-titanium dioxide photocatalyst material, thereby increasing the specific surface area of ​​composite nano-titanium dioxide photocatalyst material in contact with the light source and improving its photocatalytic performance.

[0054] (6) In the technical solution of the present invention, recycled aggregate is selected as the direct carrier of the composite nano-titanium dioxide photocatalytic material, which reduces the influence of cement hydration products on the photocatalytic performance of the composite nano-titanium dioxide photocatalytic material, is conducive to improving the photocatalytic durability of concrete, and ensures the long-term effect of degrading pollutants. Through the dispersion method combining physical and chemical combination, the stability of the composite nano-titanium dioxide photocatalytic material is increased, which is conducive to increasing the loading amount of recycled aggregate of the composite nano-titanium dioxide photocatalytic material and increasing the photocatalytic reaction active sites of the composite nano-titanium dioxide photocatalytic material. DETAILED DESCRIPTION

[0055] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0056] The particle size of the carbon-iron-zinc hollow nanomaterial is 220-250nm.

[0057] The carbon-iron-zinc hollow nanomaterial is specifically prepared by the following steps:

[0058] 3 g of glucose, 0.3 g of zinc acetate dihydrate and 0.8 g of ferric chloride hexahydrate were added to 30 mL of deionized water, stirred for 30 min, heated to 180 ° C and maintained for 24 h, cooled to room temperature, filtered, washed with deionized water three times, dried in an oven at 70 ° C for 10 min, and annealed at 450 ° C for 4 h to obtain carbon-iron-zinc hollow nanomaterials.

[0059] Example 1

[0060] The composite nano titanium dioxide photocatalytic material is specifically prepared by the following steps:

[0061] A1. Add 0.25g of carbon iron zinc hollow nanomaterial into 100mL of ethanol, stir evenly, add 0.3mL of 28% concentrated ammonia solution and 0.7g of tetrabutyl titanate, stir and mix for 15min, stir and react at 45℃ for 2h, treat at 200-300℃ for 6h, cool to room temperature, wash with deionized water 3 times, and dry in an oven at 70℃ for 10min to obtain a hollow nanomaterial loaded with nano-titanium dioxide.

[0062] A2. Add 1.2g of loaded nano-titanium dioxide hollow nanomaterials to 80mL of deionized water, stir evenly, add 0.1g of succinic acid and 0.2mL of 36% hydrochloric acid, react at 60°C for 1h, add graphite phase carbon nitride nanosheets, continue to react for 10min, collect the precipitate by centrifugation at 3000rpm, dry the precipitate in an oven at 70°C for 10min to obtain a solid, place 2.5g of the solid in 100mL of deionized water, add 2g of molybdenum disulfide nanosheets and 2mL of ethylene glycol, stir and react at 70°C for 10min, filter, wash with deionized water 3 times, and dry in an oven at 70°C for 10min to obtain a composite nano-titanium dioxide photocatalytic material.

[0063] Comparative Example 1

[0064] The difference between this comparative example and Example 1 is that the nano-titanium dioxide-loaded hollow nanomaterial is replaced by nano-titanium dioxide, and the remaining steps and raw materials are the same as those of Example 1.

[0065] 1.2 g of nano titanium dioxide was added to 80 mL of deionized water, stirred evenly, 0.1 g of succinic acid and 0.2 mL of 36% hydrochloric acid were added, the mixture was reacted at 60°C for 1 h, graphite phase carbon nitride nanosheets were added, the reaction was continued for 10 min, the precipitate was collected by centrifugation at 3000 rpm, the precipitate was dried in an oven at 70°C for 10 min to obtain a solid, 2.5 g of the solid was placed in 100 mL of deionized water, 2 g of molybdenum disulfide nanosheets and 2 mL of ethylene glycol were added, the mixture was stirred and reacted at 70°C for 10 min, the mixture was filtered, washed with deionized water 3 times, and dried in an oven at 70°C for 10 min to obtain a composite nano titanium dioxide photocatalytic material.

[0066] Comparative Example 2

[0067] The difference between this comparative example and Example 1 is that no graphite phase carbon nitride nanosheets and molybdenum disulfide nanosheets are added, and the remaining steps and raw materials are the same as Example 1.

[0068] Add 0.25g of carbon iron zinc hollow nanomaterial into 100mL of ethanol, stir evenly, add 0.3mL of 28% concentrated ammonia solution and 0.7g of tetrabutyl titanate, stir and mix for 15min, stir and react at 45°C for 2h, treat at 200-300°C for 6h, cool to room temperature, wash with deionized water 3 times, and dry in an oven at 70°C for 10min to obtain a composite nano titanium dioxide photocatalytic material.

[0069] Example 2

[0070] The reinforcement material is specifically prepared by the following steps:

[0071] B1. Add 0.2g of carbon fiber to 20mL of 36% sodium hydroxide aqueous solution, stir at 40°C for 1.5h, filter, wash with deionized water three times, dry in an oven at 70°C for 10min, place in 30mL of ethanol, stir evenly, add 2.5g of fish scale powder, heat to 85°C, stir until the organic solvent evaporates, collect the solid, wash the solid with deionized water three times, and dry in an oven at 80°C for 10min to obtain modified carbon fiber.

[0072] B2. Add 6 g acrylamide and 1.5 g acrylic acid to 50 mL deionized water, stir evenly, add 0.02 g methylene bisacrylamide and 0.5 g modified carbon fiber, stir evenly, add 0.06 g ammonium persulfate, stir and react at 60 ° C for 2 h to obtain a gel-like substance, take out the gel-like substance, and place it in 30 mL deionized water to obtain a reinforced material.

[0073] Comparative Example 3

[0074] The difference between this comparative example and Example 2 is that the modified carbon fiber is replaced by carbon fiber, and the remaining steps and raw materials are the same as Example 2.

[0075] Add 6 g acrylamide and 1.5 g acrylic acid into 50 mL deionized water, stir evenly, add 0.02 g methylenebisacrylamide and 0.5 g carbon fiber, stir evenly, add 0.06 g ammonium persulfate, stir and react at 60°C for 2 h to obtain a gel-like substance, take out the gel-like substance, and place it in 30 mL deionized water to obtain a reinforced material.

[0076] Comparative Example 4

[0077] The difference between this comparative example and Example 2 is that acrylamide and acrylic acid are not added, and the remaining steps and raw materials are the same as those of Example 2.

[0078] Add 0.2 g of carbon fiber to 20 mL of 36% sodium hydroxide aqueous solution, stir at 40 ° C for 1.5 h, filter, wash with deionized water three times, dry in an oven at 70 ° C for 10 min, place in 30 mL of ethanol, stir evenly, add 2.5 g of fish scale powder, heat to 85 ° C, stir until the organic solvent evaporates, collect the solid, wash the solid with deionized water three times, and dry in an oven at 80 ° C for 10 min to obtain modified carbon fiber.

[0079] Example 3

[0080] A permeable concrete based on recycled aggregate loaded with nano-TiO2 comprises the following components by mass: 350 parts of natural aggregate, 200 parts of recycled aggregate, 210 parts of cement, 240 parts of spun yarn, 60 parts of mineral powder, 12 parts of reinforcing material, 10 parts of composite nano-titanium dioxide photocatalytic material, 0.8 parts of sodium tripolyphosphate, 5 parts of water reducer and 250 parts of water.

[0081] A method for preparing permeable concrete based on recycled aggregate loaded with nano-TiO2 comprises the following steps:

[0082] S1. The composite nano-titanium dioxide photocatalytic material and 1 / 3 water were mixed, stirred evenly, sodium tripolyphosphate was added, and stirred at a speed of 9000r / min for 20min to obtain a suspension;

[0083] S2. The suspension was mixed with the recycled aggregate and soaked for 24 h, and dried in an oven at 80 ° C for 30 min to obtain a recycled aggregate loaded with composite nano-titanium dioxide photocatalytic material;

[0084] S3. Mix the recycled aggregate loaded with composite nano-titanium dioxide photocatalytic material, natural aggregate, reinforcing material and 1 / 3 part of water, stir for 30 seconds, add cement, fine yarn, mineral powder and water reducing agent, stir for 60 seconds to obtain a solid mixture, and finally add the remaining water and stir for 2 minutes to obtain permeable concrete.

[0085] Example 4

[0086] A permeable concrete based on recycled aggregate loaded with nano-TiO2 comprises the following components by mass: 380 parts of natural aggregate, 230 parts of recycled aggregate, 220 parts of cement, 250 parts of spun yarn, 80 parts of mineral powder, 13 parts of reinforcing material, 15 parts of composite nano-titanium dioxide photocatalytic material, 0.9 parts of sodium tripolyphosphate, 7 parts of HPWR-Q8011 polycarboxylic acid series high-efficiency water reducing agent, and 260 parts of water.

[0087] A method for preparing permeable concrete based on recycled aggregate loaded with nano-TiO2 comprises the following steps:

[0088] S1. The composite nano-titanium dioxide photocatalytic material and 1 / 3 water were mixed, stirred evenly, sodium tripolyphosphate was added, and stirred at a speed of 9000r / min for 20min to obtain a suspension;

[0089] S2. The suspension was mixed with the recycled aggregate and soaked for 24 h, and dried in an oven at 80 ° C for 30 min to obtain a recycled aggregate loaded with composite nano-titanium dioxide photocatalytic material;

[0090] S3. Mix the recycled aggregate loaded with composite nano-titanium dioxide photocatalytic material, natural aggregate, reinforcing material and 1 / 3 part of water, stir for 30 seconds, add cement, fine yarn, mineral powder and HPWR-Q8011 polycarboxylic acid high-efficiency water reducing agent, stir for 60 seconds to obtain a solid mixture, and finally add the remaining water and stir for 2 minutes to obtain permeable concrete.

[0091] Example 5

[0092] A permeable concrete based on recycled aggregate loaded with nano-TiO2 comprises the following components by mass: 400 parts of natural aggregate, 250 parts of recycled aggregate, 230 parts of cement, 260 parts of spun yarn, 90 parts of mineral powder, 15 parts of reinforcing material, 20 parts of composite nano-titanium dioxide photocatalytic material, 1 part of sodium tripolyphosphate, 10 parts of HPWR-Q8011 polycarboxylic acid series high-efficiency water reducing agent, and 270 parts of water.

[0093] A method for preparing permeable concrete based on recycled aggregate loaded with nano-TiO2 comprises the following steps:

[0094] S1. The composite nano-titanium dioxide photocatalytic material and 1 / 3 water were mixed, stirred evenly, sodium tripolyphosphate was added, and stirred at a speed of 9000r / min for 20min to obtain a suspension;

[0095] S2. The suspension was mixed with the recycled aggregate and soaked for 24 h, and dried in an oven at 80 ° C for 30 min to obtain a recycled aggregate loaded with composite nano-titanium dioxide photocatalytic material;

[0096] S3. Mix the recycled aggregate loaded with composite nano-titanium dioxide photocatalytic material, natural aggregate, reinforcing material and 1 / 3 part of water, stir for 30 seconds, add cement, fine yarn, mineral powder and HPWR-Q8011 polycarboxylic acid high-efficiency water reducing agent, stir for 60 seconds to obtain a solid mixture, and finally add the remaining water and stir for 2 minutes to obtain permeable concrete.

[0097] Comparative Example 5

[0098] The difference between this comparative example and Example 4 is that the composite nano-titanium dioxide photocatalytic material is replaced by the material prepared in Comparative Example 1.

[0099] Comparative Example 6

[0100] The difference between this comparative example and Example 4 is that the composite nano-titanium dioxide photocatalytic material is replaced by the material prepared in Comparative Example 2.

[0101] Comparative Example 7

[0102] The difference between this comparative example and Example 4 is that the reinforcing material is replaced by the material prepared in Comparative Example 3.

[0103] Comparative Example 8

[0104] The difference between this comparative example and Example 4 is that the reinforcing material is replaced by the material prepared in Comparative Example 4.

[0105] The performance of the permeable concrete prepared in Examples 3-5 and Comparative Examples 5-8 is now tested;

[0106] Concrete specimens were prepared according to the methods of Examples 1-3 and Comparative Examples 5-8. The specimens had a size of 100 mm×100 mm×100 mm and were cured for 28 days at a temperature of 20±2° C. and a relative humidity of more than 95%.

[0107] Mechanical properties and water permeability test:

[0108] The permeable concrete prepared above was tested for 28-day permeability coefficient and connected porosity of the concrete test block according to CJJ / T253-2016 "Technical Code for Application of Recycled Aggregate Permeable Concrete" and CJJ / T135-2009 "Technical Code for Permeable Cement Concrete Pavement".

[0109] The compressive strength is tested according to the method in the Standard for Test Methods of Physical and Mechanical Properties of Concrete (GB / T50081-2019) using a WAW-2000KN electro-hydraulic servo universal press;

[0110] Photocatalytic degradation rate using test model GP-203-NO X Portable nitrogen oxide detector measures NO X Concentration. The test was conducted in a sealed, light-transmitting plexiglass test container for 60 minutes. Three concrete pieces were selected from each group to test the compressive strength of the specimens, and the test results were averaged;

[0111] Freeze-thaw cycle test and photocatalytic efficiency test: freeze-thaw cycle refers to the method in the standard "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete" (GB / T50082-2009), and 20, 40, 60, and 80 freeze-thaw cycles are carried out using a NELD-FC810 concrete rapid freeze-thaw test machine;

[0112] The engineering plastics prepared above were subjected to wear testing using a wear testing device to observe the wear marks on the surface of the engineering plastics. The results are shown in Table 1 below.

[0113] Table 1

[0114] project Compressive strength / MPa Photodegradation rate / % Porosity / % Water permeability mm / s Example 4 22.32 34.35 20.2 2.5 Example 5 22.58 34.62 20.3 2.6 Example 6 22.47 34.11 20.1 2.5 Comparative Example 5 21.68 29.63 19.6 2.4 Comparative Example 6 16.56 28.38 19.9 2.4 Comparative Example 7 18.36 26.36 20.1 2.5 Comparative Example 8 18.53 25.89 19.8 2.4

[0115] Table 2

[0116]

[0117]

[0118] It can be seen from the data in Table 1 that in Comparative Example 5, the composite nano-titanium dioxide photocatalytic material prepared by replacing the loaded nano-titanium dioxide hollow nanomaterial with nano-titanium dioxide is added to the concrete, and its degradation rate decreases. This may be because nano-titanium dioxide is synthesized in situ on the surface of the carbon-iron-zinc hollow nanomaterial to form a core-shell material with a heterogeneous interface, which reduces the chance of photogenerated electron-hole recombination; Comparative Example 6 is a composite nano-titanium dioxide photocatalytic material prepared without adding graphite phase carbon nitride nanosheets and molybdenum disulfide nanosheets, and added to the concrete, and its degradation rate and compressive strength decrease. This may be because a mutually crossed or arranged layer structure is formed, and the layer structure can absorb the stress generated by the external force, and the loaded nano-titanium dioxide hollow nanomaterial is filled between the graphite phase carbon nitride nanosheets and the molybdenum disulfide nanosheets to form a concave-convex layer structure, which increases the reflection and reflection distance of visible light, thereby increasing the contact area and contact time between the loaded nano-titanium dioxide hollow nanomaterial and the light source; Comparative Example 7 replaces the modified carbon fiber with When the reinforcing material prepared by replacing carbon fiber is added to concrete, its compressive strength and degradation rate decrease. This may be because the fish scale powder in the modified carbon fiber contains a large amount of hydroxyl structure, which can be combined with the recycled aggregate through hydrogen bonds, can connect the recycled aggregate, and form a more effective stress transfer network, avoiding the concrete from being affected by local environmental factors, wear, rain erosion, etc., causing the nano photocatalytic material to fall off easily, affecting the degradation performance of the concrete for atmospheric pollutants; Comparative Example 8 did not add acrylamide and acrylic acid to prepare the reinforcing material, and added it to concrete, its compressive strength and degradation rate decreased. This may be because the composite photocatalytic material is adsorbed on the surface of the recycled aggregate, and the carboxyl group carried by polyacrylic acid is negatively charged, which can adhere to the surface of the recycled aggregate with positive charge through electrostatic action, and through the action of physical adsorption and chemical bonds, the composite photocatalytic material is more firmly adhered to the surface of the recycled aggregate, increasing the bonding force between the composite photocatalytic material and the concrete, and avoiding the falling off of the composite photocatalytic material.

[0119] It can be seen from the data in Table 2 that the composite photocatalytic material adheres more firmly to the surface of the recycled aggregate through the effects of physical adsorption and chemical bonds. After freeze-thaw cycle treatment, the concrete has a good degradation rate.

[0120] The data in Table 1 and Table 2 indicate that the permeable concrete prepared in Examples 3-5 not only has a good degradation rate and water permeability, but also the photocatalytic material has a good bonding force with the concrete. The composite nano-titanium dioxide photocatalytic material and 1 / 3 of water are mixed, stirred evenly, sodium tripolyphosphate is added, and stirred at a speed of 9000r / min for 20min to obtain a suspension; the suspension is mixed with the recycled aggregate and soaked for 24h, and dried in an oven at 80°C for 30min to obtain a recycled aggregate loaded with the composite nano-titanium dioxide photocatalytic material; the recycled aggregate loaded with the composite nano-titanium dioxide photocatalytic material, the natural aggregate, the reinforcing material, and 1 / 2 part of water are mixed, stirred for 30s, cement, spun yarn, mineral powder, and water reducer are added, stirred for 60s to obtain a solid mixture, and finally the remaining water is added and stirred for 2min to obtain a permeable concrete that meets the test performance requirements, while the permeable concrete prepared in Comparative Examples 5-8 does not meet the performance requirements, indicating that the permeable concrete prepared by the present invention not only has a good degradation rate and water permeability, but also the photocatalytic material has a good bonding force with the concrete.

[0121] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0122] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A permeable concrete based on recycled aggregate loaded with nano-TiO2, characterized in that: It includes the following mass components: 350-400 parts of natural aggregate, 200-250 parts of recycled aggregate, 210-230 parts of cement, 240-260 parts of spun yarn, 60-90 parts of mineral powder, 12-15 parts of reinforcing material, 10-20 parts of composite nano titanium dioxide photocatalytic material, 0.8-1 parts of sodium tripolyphosphate, 5-10 parts of water reducer, and 250-270 parts of water; The composite nano-titanium dioxide photocatalytic material is prepared by depositing a nano-titanium dioxide-loaded hollow nano-material on the surface of a graphite phase carbon nitride nano-sheet and then mixing it with a molybdenum disulfide nano-sheet; The nano-titanium dioxide loaded hollow nano-material is prepared by mixing carbon iron zinc hollow nano-material with tetrabutyl titanate and subjecting the mixture to hydrothermal treatment; The reinforcing material is prepared by depositing fish scale powder on the surface of carbon fiber and then reacting with acrylamide and acrylic acid.

2. The permeable concrete based on recycled aggregate loaded with nano-TiO2 according to claim 1, characterized in that: The particle size of the molybdenum disulfide nanosheet is 0.8-1.2 μm; the particle size of the graphite phase carbon nitride nanosheet is 0.5-0.8 μm.

3. The permeable concrete based on recycled aggregate loaded with nano-TiO2 according to claim 1, characterized in that: The carbon-iron-zinc hollow nanomaterial is specifically prepared by the following steps: Glucose, zinc acetate dihydrate and ferric chloride hexahydrate were added to deionized water, stirred for 30 minutes, heated to 180°C and maintained for 24 hours, cooled to room temperature, filtered, washed with deionized water three times, dried in an oven at 70°C for 10 minutes, and annealed at 450°C for 4 hours to obtain carbon-iron-zinc hollow nanomaterials.

4. The permeable concrete based on recycled aggregate loaded with nano-TiO2 according to claim 1, characterized in that: The hydrothermal treatment temperature is 200-300° C., and the hydrothermal treatment time is 5-7 hours; the carbon fiber diameter is 50-70 nm, and the length is 1-3 μm.

5. The permeable concrete based on recycled aggregate loaded with nano-TiO2 according to claim 1, characterized in that: The recycled aggregate is specifically prepared by the following steps: the waste concrete is crushed, passed through a 20-25 mesh sieve, washed with deionized water, and crushed by a crusher to obtain the recycled aggregate.

6. The permeable concrete based on recycled aggregate loaded with nano-TiO2 according to claim 1, characterized in that: The natural aggregate has a particle size of 3.1-3.8 mm, a water absorption rate of 0.69-0.81%, and a dry density of 1500-1520 kg / m 3 The particle size of the recycled aggregate is 2.9-3.5 mm, the water absorption rate is 6.65-6.71%, and the apparent density is 2500-2700 kg / m 3 , bulk density is 1500-1600kg / m 3 .

7. The permeable concrete based on recycled aggregate loaded with nano-TiO2 according to claim 1, characterized in that: The cement is silicate cement with a PO4 of 2.5 and a specific surface area of ​​320-350m 2 / kg, 28d compressive strength is 55.3-55.9MPa, initial setting time is 90-100min, and final setting time is 140-150min.

8. The permeable concrete based on recycled aggregate loaded with nano-TiO2 according to claim 1, characterized in that: The apparent density of the fine sand is 2600-2700 kg / m 3 The fineness modulus is 1.6-2.1, the particle size is 0.25-0.1mm, and the mud content is 0.6-1%; the mineral powder is S95 grade slag powder with a density of 2.9-3.5g / cm 3 , with a specific surface area of ​​450-500m 2 / kg, water content is 0.2-1%, and 28d activity index is 95%.

9. The permeable concrete based on recycled aggregate loaded with nano-TiO2 according to claim 1, characterized in that: The water reducing agent is selected from the HPWR-Q8011 polycarboxylic acid high efficiency water reducing agent produced by Shaanxi Qinfen Building Materials Company, and the water reducing rate of the water reducing agent is 25%.

10. A method for preparing a permeable concrete based on recycled aggregate loaded with nano-TiO2 as claimed in any one of claims 1 to 9, characterized in that: The following steps are involved: S1. The composite nano-titanium dioxide photocatalytic material and 1 / 3 water were mixed, stirred evenly, sodium tripolyphosphate was added, and stirred at a speed of 9000r / min for 20min to obtain a suspension; S2. The suspension was mixed with the recycled aggregate and soaked for 24 h, and dried in an oven at 80 ° C for 30 min to obtain a recycled aggregate loaded with composite nano-titanium dioxide photocatalytic material; S3. Mix the recycled aggregate loaded with composite nano-titanium dioxide photocatalytic material, natural aggregate, reinforcing material and 1 / 2 part of water, stir for 30 seconds, add cement, fine yarn, mineral powder and water reducing agent, stir for 60 seconds to obtain a solid mixture, and finally add the remaining water and stir for 2 minutes to obtain permeable concrete.

Citation Information

Cited By

  • Pervious concrete prepared from modified recycled aggregate and nano reinforced material

    CN119591365A