Low-dielectric low-loss LTCC (Low Temperature Co-Fired Ceramic) material suitable for high frequency and preparation method thereof

By adjusting the glass components and process flow, the problems of high dielectric constant and high process risks in the existing LTCC materials were solved, and low dielectric low loss LTCC with dielectric constants of 4 to 6 and dielectric loss of 0.0003 to 0.0015 were prepared. Porcelain material, suitable for high-frequency microwave components.

CN118955103APending Publication Date: 2024-11-15BEIJING YUAN LIU HONG YUAN ELECTRONIC TECHNOLOGY CO LTD +1

Patent Information

Application Number
CN202411015209.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing LTCC materials have a large dielectric constant, which cannot meet the demand for lower dielectric constants for high frequency and diversified development. At the same time, the melting temperature and low loss performance of glass powder are difficult to take into account, resulting in high process risks.

Method used

By adjusting the glass components, introducing alkali metals and alkaline earth metals, reducing the melting temperature of the glass, and through ball milling and sintering processes, low dielectric and low loss with dielectric constants of 4 to 6 and dielectric loss of 0.0003 to 0.0015 was prepared. LTCC porcelain material.

Benefits of technology

The preparation of LTCC materials with low dielectric constant and low dielectric loss at lower melting temperatures is achieved, which improves process operability and is suitable for high-frequency microwave components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955103A_ABST
    Figure CN118955103A_ABST
Patent Text Reader

Abstract

The invention discloses a low-dielectric low-loss LTCC (Low Temperature Co-Fired Ceramic) material suitable for high frequency and a preparation method thereof, and particularly relates to the field of electronic components. The method comprises the following steps: uniformly mixing raw materials by using a dry method, screening out the materials after ball-milling and mixing, melting at high temperature, performing cold quenching on glass slag in deionized water in a high-temperature state, drying, grinding, drying and screening to obtain glass powder; then carrying out ball milling treatment on glass powder and aluminum oxide, and drying and sieving after ball milling to obtain the LTCC ceramic material; finally, carrying out granulation on the LTCC ceramic material and the pre-dissolved PVB colloid, and pressing into a wafer; and sintering the pressed wafer to obtain the low-dielectric low-loss LTCC ceramic body. The material is prepared by mixing 50 wt% of glass powder and 50 wt% of alumina powder, the glass is a SiO2-B2O3-Al2O3-MgO-ZnO-Li2O-K2O system, the glass powder has good stability, the glass is softened during sintering, and the sintering temperature of the material is reduced through liquid phase mass transfer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electronic components, and in particular to a low-dielectric and low-loss LTCC ceramic material suitable for high frequencies and a preparation method thereof. Background Art

[0002] In recent years, with the rapid development of microelectronic information technology, the demand for miniaturization, digitization, multi-function, high reliability and high performance of electronic equipment has further promoted the development of electronic components towards miniaturization, integration and high frequency. Dielectric antennas, high-frequency substrates, high-precision capacitors and micro-integrated millimeter-wave components require microwave dielectric ceramics to have lower dielectric constants and smaller dielectric losses. Among them, low dielectric constant silicate microwave dielectric ceramics have a small dielectric constant, low dielectric loss and near-zero temperature drift coefficient, which can ensure the stability of device use, thus attracting great attention in the research field. Low-temperature co-fired ceramics (LTCC) are an effective and practical sintering ceramic technology, which has become an important technology in the field of complex miniaturized circuits. Low-temperature (≤950℃) co-fired ceramics with Ag and Cu as electrodes have good chemical compatibility, low dielectric constant and low dielectric loss, and show excellent performance in practical applications. At present, the commercialized LTCC products are represented by Ferro-A6M, Dupont-951 and Dupont-9K7 from the United States. Heraeus from Germany and Murata from Japan also have independent supporting system products. Europe, the United States, Japan and South Korea occupy most of the LTCC market, and the key formula and process parameters of LTCC materials are strictly kept confidential. The domestic military, aviation, aerospace and other key fields have a large demand for LTCC materials and basically rely on imports. Based on the current tense international situation, it is urgent to develop and master LTCC system materials with independent intellectual property rights.

[0003] The dielectric constant of the LTCC product materials currently on the market is relatively large, and cannot meet the demand for lower dielectric constant LTCC materials for the high-frequency and diversified development of components.

[0004] The glass powder of LTCC ceramic components usually does not take into account both the melting temperature and low loss performance. When the dielectric loss is low, the glass network structure is complete, but the melting temperature is high (up to 1500℃-1600℃), the equipment requirements are high, and the process risks are high. Adding alkali metals such as Na and K can effectively reduce the melting temperature, but it usually has an adverse effect on the dielectric loss. Summary of the invention

[0005] To this end, the present invention provides a low-dielectric and low-loss LTCC ceramic material suitable for high frequency and a preparation method thereof, so as to achieve a low dielectric constant by changing the glass component; and to achieve low dielectric loss of the material by finely adjusting the glass component and preparing glass powder at a lower melting temperature.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] According to one aspect of the present invention, a method for preparing a low-dielectric and low-loss LTCC ceramic material suitable for high frequency is provided, the method comprising:

[0008] Step 1: Preparation of glass powder

[0009] The raw materials are mixed evenly by dry method, the materials are sieved out after ball milling, melted at high temperature, quenched in deionized water at high temperature, dried, ground and dried again, and sieved to obtain glass powder;

[0010] Step 2: Preparation of LTCC ceramics

[0011] The glass powder and alumina are ball-milled, and then dried and sieved to obtain LTCC ceramic material;

[0012] Step 3: Granulation, tableting and sintering

[0013] The LTCC ceramic material and the pre-dissolved PVB colloid are granulated and pressed into discs; the pressed discs are sintered to obtain a low-dielectric and low-loss LTCC ceramic body.

[0014] Furthermore, in step 1, the raw materials include silicon dioxide, boron-containing compounds, aluminum-containing compounds, zinc oxide, magnesium-containing compounds, lithium carbonate, and potassium carbonate.

[0015] Furthermore, the porcelain raw material comprises 50-70wt% silicon dioxide, 10-15wt% boron-containing compound, 5-15wt% aluminum-containing compound, 0.1-5wt% zinc oxide, 0.1-10wt% magnesium-containing compound, 0.1-10wt% lithium carbonate, and 0.1-20wt% potassium carbonate.

[0016] Furthermore, in the step 1, the ball milling mixing conditions are a rotation speed of 200-400 r / min and a time of 0.5-2 h; the melting conditions are a melting temperature of 1450±50°C and a holding time of 1-3 h; and the drying conditions are a drying temperature of 60-80°C and a drying time of 4-8 h.

[0017] Furthermore, in the step 1, the ball-to-material ratio of the re-grinding is (3-5):1, the ball milling speed is 200-400 r / min, and the ball milling time is 4-8 h.

[0018] Furthermore, in the step 2, the glass powder and alumina are 50wt% of glass powder with a particle size of 1.0-2.0μm and 50wt% of alumina powder with a particle size of 1.0-2.0μm; the ball-water-to-material ratio is (3-5):(1-3):1, the ball milling speed is 200-400r / min, and the ball milling time is 4-8h; the drying temperature is 60-80°C, and the drying time is 12-24h.

[0019] Furthermore, in step three, the PVB colloid contains 0.4 to 0.6 g of PVB.

[0020] Furthermore, in the step three, the sintering conditions are sintering at 850-950° C. and keeping the temperature for 0.5-2 hours.

[0021] According to another aspect of the present invention, a low-dielectric and low-loss LTCC ceramic material suitable for high frequency is provided and is prepared by the above method. The dielectric constant of the ceramic material is 4-6 and the dielectric loss is 0.0003-0.0015.

[0022] The present invention has the following advantages:

[0023] The glass powder of the present invention has good stability after formula optimization. By introducing alkali metal and alkaline earth metal into traditional Si-B-Al glass, the glass powder is successfully prepared at 1400℃~1500℃ and ground to a certain particle size. The glass powder is mixed with alumina powder and ground to make porcelain powder. After granulation and tableting, it is co-fired with metal slurry at 850℃~950℃ to finally obtain low dielectric and low loss LTCC material. The technical effect of the present invention is: by adjusting the content of glass components, a low dielectric constant ε=4~6 (1MHz) is achieved, the dielectric loss is as low as tanδ=0.0003 (1MHz), and the Q value is as high as 3000~4000, which has the characteristics of low dielectric and low loss.

[0024] The material of the present invention is prepared by mixing 50wt% glass powder and 50wt% alumina powder, wherein the glass is SiO 2 -B 2 O 3 -Al 2 O 3 -MgO-ZnO-Li 2 OK 2 O system, the glass powder has good stability, the glass softens during sintering, and the sintering temperature of the material is reduced through liquid phase mass transfer. Adjust the MgO / ZnO / Li 2 O / K 2 The content of O is finally obtained, and the low dielectric and low loss LTCC material is obtained, with a dielectric constant of 4 to 6 and a dielectric loss of 0.0003 to 0.0015. It can be matched and co-fired with metal paste at 850 to 950 ° C, and is suitable for microwave components such as filters, couplers, and LTCC substrates.

[0025] The present invention successfully prepares a low dielectric constant and low dielectric loss porcelain body by adjusting the glass components; introduces alkali metals and alkaline earth metals into traditional Si-B-Al glass, reduces the melting temperature of the glass and increases the process operability; introduces two alkali metals Li and K at the same time to produce a "mutual resistance effect", which reduces the activity of alkali metal ions compared to a single alkali metal, thereby reducing the dielectric loss of the material; introduces alkaline earth metals Mg and Zn to tighten the glass network, Mg 2+ and Zn 2+ There is a "mutual resistance effect" and a "suppression effect" on alkali metal ions, making Li + and K + It is not easy to move, which reduces the activity of alkali metal ions and thus reduces dielectric loss. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. Obviously, the drawings in the following description are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.

[0027] The structures, proportions, sizes, etc. illustrated in this specification are only used to match the contents disclosed in the specification so as to facilitate understanding and reading by persons familiar with the technology. They are not used to limit the conditions under which the present invention can be implemented, and therefore have no substantial technical significance. Any structural modification, change in proportion or adjustment of size shall still fall within the scope of the technical contents disclosed in the present invention without affecting the effects and purposes that can be achieved by the present invention.

[0028] Figure 1 This is a scanning electron microscope image of a cross section of a sintered sample obtained in Example 1-4 provided in the present invention 1, wherein A is Example 1, B is Example 2, C is Example 3, and D is Example 4. DETAILED DESCRIPTION

[0029] The following is a description of the implementation of the present invention by specific embodiments. People familiar with the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] A method for preparing a low-dielectric and low-loss LTCC ceramic material suitable for high frequency:

[0031] This material is a mixed powder of ceramic powder and glass powder, which is prepared by mixing ceramic powder and glass powder in a certain ratio. The specific preparation process is as follows:

[0032] 1. Glass Powder Preparation

[0033] The preparation process of glass powder includes: batching, mixing, melting, water quenching, drying, grinding and screening;

[0034] (1) Ingredients: The proportions of the glass components are shown in Table 1. The effective component content is calculated in turn according to the proportions and the amount of chemical raw materials corresponding to each component is weighed. The raw materials include silicon dioxide, boron-containing compounds (boric acid or boron oxide), aluminum-containing compounds (aluminum oxide or aluminum hydroxide), zinc oxide, magnesium-containing compounds (magnesium oxide or magnesium hydroxide, magnesium carbonate, basic magnesium carbonate), lithium carbonate, and potassium carbonate;

[0035] Table 1

[0036]

[0037] (2) Mixing: Pour the ingredients prepared in step 1) into a ball mill containing grinding balls, place the ball mill in a ball mill, and mix them evenly using a dry method at a speed of 200 to 400 r / min for 0.5 to 2 h. After mixing, sieve out the materials and prepare for the next step;

[0038] (3) Melting: Place the mixture into a quartz crucible and place it in a high-temperature electric furnace for melting at a melting temperature of 1450±50°C for 1 to 3 hours;

[0039] (4) Water quenching: Prepare sufficient deionized water and quickly pour the molten glass into the deionized water at high temperature to obtain cold-quenched glass slag;

[0040] (5) Drying: drying the obtained glass slag in an oven at a temperature of 60 to 80° C. for 4 to 8 hours;

[0041] (6) Grinding: Add the water-quenched and dried glass slag into a ball mill, add a certain amount of grinding balls and anhydrous ethanol, grind in a planetary ball mill and then dry, the ball-to-material ratio is (3-5):1, the ball mill speed is 200-400 r / min, and the ball milling time is 4-8 h;

[0042] (7) Sieving: The powder obtained by grinding is passed through a 200-mesh sieve and bagged for later use;

[0043] 2. Preparation of LTCC ceramic materials

[0044] The process of preparing porcelain materials includes: batching, ball milling, drying, and screening;

[0045] 1) Ingredients: According to the proportion of the ceramic material components, the corresponding raw materials are weighed in sequence: 50wt% of glass powder with a particle size of 1.0-2.0μm, and 50wt% of alumina powder with a particle size of 1.0-2.0μm;

[0046] 2) Ball milling: Use a ball mill, load grinding balls, pour the ingredients in step 1) into the ball mill, add deionized water, and place the ball mill in a ball mill to mix well. The ball-water-material ratio is (3-5):(1-3):1, the ball mill speed is 200-400r / min, and the ball milling time is 4-8h;

[0047] 3) Drying: Place the ground porcelain slurry in an oven for drying at a temperature of 60 to 80°C for 12 to 24 hours;

[0048] 4) Sieving: The dried powder is sieved through a 200-mesh sieve to complete the preparation of the LTCC ceramic material;

[0049] 3. Granulation, tableting and sintering

[0050] 1) Granulation and tableting: Take 5g of porcelain powder, add pre-dissolved PVB colloid (containing PVB 0.4-0.6g) to granulate, and press into φ13mm round tablets;

[0051] 2) Sintering: Sinter the wafer at 850-950°C and keep it warm for 0.5-2h to obtain a low-dielectric and low-loss LTCC ceramic body.

[0052] Example

[0053] A low dielectric and low loss LTCC ceramic material formula suitable for high frequency is shown in Table 2.

[0054] Table 2

[0055] Glass components <![CDATA[SiO 2 ]]> <![CDATA[B 2 THE 3 ]]> <![CDATA[Al 2 THE 3 ]]> ZnO MgO <![CDATA[Li 2 The]]> <![CDATA[K 2 The]]> Content (wt%) 50~70 10~15 5~15 0.1~5 0.1~10 0.1~10 0.1~20 Example 1 50 15 15 0.1 0.1 0.1 20 Example 2 60 10 10 0.1 0.1 10 10 Example 3 60 10 10 0.1 10 5 5 Example 4 70 10 5 5 5 2.5 2.5 Comparative Example 1 50 15 15 0.1 0.1 10 10 Comparative Example 2 60 10 10 5 5 5 5

[0056] Preparation method:

[0057] Step 1: Preparation of glass powder

[0058] Mixing: Pour the ingredients of silicon dioxide, boric acid (or boron oxide), aluminum oxide (or aluminum hydroxide), zinc oxide, magnesium oxide (or magnesium hydroxide, magnesium carbonate, basic magnesium carbonate), lithium carbonate, and potassium carbonate into a ball mill with grinding balls, place the ball mill in a ball mill, and mix them evenly using a dry method at a speed of 200-400r / min for 0.5-2h. After mixing, sieve out the materials and prepare for the next step;

[0059] Melting: put the mixed material into a quartz crucible and place it in a high-temperature electric furnace for melting at a melting temperature of 1450±50℃ and a holding time of 1 to 3 hours;

[0060] Water quenching: prepare enough deionized water, and quickly pour the molten glass liquid into the deionized water at high temperature to obtain cold quenched glass slag;

[0061] Drying: Place the obtained glass slag in an oven for drying at a temperature of 60 to 80°C for 4 to 8 hours;

[0062] Grinding: Add the water-quenched and dried glass slag into a ball mill, add a certain amount of grinding balls and anhydrous ethanol, grind in a planetary ball mill and then dry, the ball-to-material ratio is (3-5):1, the ball mill speed is 200-400r / min, and the ball mill time is 4-8h;

[0063] Sieve: Sieve the powder obtained by grinding through a 200-mesh sieve and bag it for later use;

[0064] Step 2: Preparation of LTCC ceramics

[0065] 1) Ingredients: According to the proportion of the ceramic material components, the corresponding raw materials are weighed in sequence: 50wt% of glass powder with a particle size of 1.0-2.0μm, and 50wt% of alumina powder with a particle size of 1.0-2.0μm;

[0066] 2) Ball milling: Use a ball mill, load grinding balls, pour the ingredients in step 1) into the ball mill, add deionized water, and place the ball mill in a ball mill to mix well. The ball-water-material ratio is (3-5):(1-3):1, the ball mill speed is 200-400r / min, and the ball milling time is 4-8h;

[0067] 3) Drying: Place the ground porcelain slurry in an oven for drying at a temperature of 60 to 80°C for 12 to 24 hours;

[0068] 4) Sieving: The dried powder is sieved through a 200-mesh sieve to complete the preparation of the LTCC ceramic material;

[0069] Step 3: Granulation, tableting and sintering

[0070] 1) Granulation and tableting: Take 5g of porcelain powder, add pre-dissolved PVB colloid (containing PVB 0.4-0.6g) to granulate, and press into φ13mm round tablets;

[0071] 2) Sintering: Sinter the wafer at 850-950°C and keep it warm for 0.5-2h to obtain a low-dielectric and low-loss LTCC ceramic body.

[0072] Experimental example

[0073] 1. The properties of the obtained porcelain body were tested, and the results are shown in Table 3.

[0074] Table 3

[0075]

[0076]

[0077] 2. Scanning electron microscopy of the cross-section of the sintered samples obtained in Examples 1-4 Figure 1 shown.

[0078] Example 1, at 1MHz, ε=5.9, tanδ=0.0015, Q=714. K in glass 2 More O, free and mobile K + Many, K + It has high activity and can easily jump between vacancies, so it has a large dielectric constant and large dielectric loss.

[0079] Example 2, at 1 MHz, ε = 5.6, tanδ = 0.0011, Q = 909. Introduction of Li 2 O replaces an equal amount of K 2 O, K + and Li + A "mutual resistance effect" is generated, and the ability of K+ and Li+ to jump between vacancies is hindered, so the dielectric loss is reduced.

[0080] Example 3, at 1MHz, ε=5.0, tanδ=0.0006, Q=1667. After the introduction of MgO, Mg 2+ Attract negative valence structures in the glass network, tighten the glass network, and have a positive effect on K + and Li + Produce a "suppression effect" that makes K + and Li + It is difficult to transition, thus significantly reducing dielectric loss.

[0081] Example 4, at 1MHz, ε=4.3, tanδ=0.0003, Q=3333. Continue to reduce K 2 O and Li 2 O, while introducing ZnO to replace an equal amount of MgO, the positively charged Mg 2+ and Zn 2+ Attract negative valence structures in the glass network, making the glass network more compact; Mg 2+ and Zn 2+ It has a "mutual resistance effect" and Zn 2+ and Mg 2+ K + and Li + Produce a "suppression effect" that makes K + and Li + It is difficult to transition, so the dielectric loss continues to decrease.

[0082] The material of the present invention is prepared by mixing 50wt% glass powder and 50wt% alumina powder, wherein the glass is SiO2 -B 2 O 3 -Al 2 O 3 -MgO-ZnO-Li 2 OK 2 O system, the glass powder has good stability, the glass softens during sintering, and the sintering temperature of the material is reduced through liquid phase mass transfer. Adjust the MgO / ZnO / Li 2 O / K 2 The content of O is finally obtained, and the low dielectric and low loss LTCC material is obtained, with a dielectric constant of 4 to 6 and a dielectric loss of 0.0003 to 0.0015. It can be matched and co-fired with metal paste at 850 to 950 ° C, and is suitable for microwave components such as filters, couplers, and LTCC substrates.

[0083] Although the present invention has been described in detail above by general description and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements can be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all belong to the scope of protection claimed by the present invention.

Claims

1. A method for preparing a low-dielectric and low-loss LTCC ceramic material suitable for high frequency, characterized in that: The method comprises: Step 1: Preparation of glass powder The raw materials are mixed evenly by dry method, the materials are sieved out after ball milling, melted at high temperature, quenched in deionized water at high temperature, dried, ground and dried again, and sieved to obtain glass powder; Step 2: Preparation of LTCC ceramics The glass powder and alumina are ball-milled, and then dried and sieved to obtain LTCC ceramic material; Step 3: Granulation, tableting and sintering The LTCC ceramic material and the pre-dissolved PVB colloid are granulated and pressed into discs; the pressed discs are sintered to obtain a low-dielectric and low-loss LTCC ceramic body.

2. The method for preparing a low-dielectric and low-loss LTCC ceramic material suitable for high frequency according to claim 1, characterized in that: In the step 1, the raw materials include silicon dioxide, a boron-containing compound, an aluminum-containing compound, zinc oxide, a magnesium-containing compound, lithium carbonate, and potassium carbonate.

3. The method for preparing a low-dielectric and low-loss LTCC ceramic material suitable for high frequency according to claim 2, characterized in that: The ceramic raw material comprises 50-70wt% of silicon dioxide, 10-15wt% of boron-containing compounds, 5-15wt% of aluminum-containing compounds, 0.1-5wt% of zinc oxide, 0.1-10wt% of magnesium-containing compounds, 0.1-10wt% of lithium carbonate, and 0.1-20wt% of potassium carbonate.

4. The method for preparing a low-dielectric and low-loss LTCC ceramic material suitable for high frequency according to claim 1, characterized in that: In the step 1, the ball milling mixing conditions are a rotation speed of 200-400 r / min and a time of 0.5-2 h; the melting conditions are a melting temperature of 1450±50° C. and a holding time of 1-3 h; and the drying conditions are a drying temperature of 60-80° C. and a drying time of 4-8 h.

5. The method for preparing a low-dielectric and low-loss LTCC ceramic material suitable for high frequency according to claim 1, characterized in that: In the step 1, the ball-to-material ratio of the re-grinding is (3-5):1, the ball milling speed is 200-400 r / min, and the ball milling time is 4-8 h.

6. The method for preparing a low-dielectric and low-loss LTCC ceramic material suitable for high frequency according to claim 1, characterized in that: In the step 2, the glass powder and alumina are 50wt% of glass powder with a particle size of 1.0-2.0μm and 50wt% of alumina powder with a particle size of 1.0-2.0μm; the ball-water-to-material ratio is (3-5):(1-3):1, the ball milling speed is 200-400r / min, and the ball milling time is 4-8h; the drying temperature is 60-80°C, and the drying time is 12-24h.

7. The method for preparing a low-dielectric and low-loss LTCC ceramic material suitable for high frequency according to claim 1, characterized in that: In the step 3, the PVB colloid contains 0.4-0.6g of PVB.

8. The method for preparing a low-dielectric and low-loss LTCC ceramic material suitable for high frequency according to claim 1, characterized in that: In the step 3, the sintering conditions are sintering at 850-950° C. and keeping the temperature for 0.5-2 hours.

9. A low dielectric and low loss LTCC ceramic material suitable for high frequency prepared by the method according to any one of claims 1 to 8, characterized in that: The dielectric constant of the porcelain material is 4-6, and the dielectric loss is 0.0003-0.0015.

Citation Information

Patent Citations

  • High-frequency inductive sheet materials and production thereof

    CN1645528A

Cited By

  • LTCC microwave ceramic material and preparation method thereof

    CN121948954A