Wide-temperature-range stable sodium bismuth titanate-based ceramic capacitor dielectric material and preparation method thereof

CN118955123AActive Publication Date: 2024-11-15CHENGDU UNIV OF INFORMATION TECH

Patent Information

Application Number
CN202411060790.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-15
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

[0005]本发明的目的是提供一种宽温区稳定的钛酸铋钠基陶瓷电容器介质材料及其制备方法,解决现有的钛酸铋钠基压电陶瓷介电稳定性差、低介电常数以及高损耗,制备工艺条件苛刻的问题

Benefits of technology

[0023] The advantages and positive effects of a wide temperature range stable sodium bismuth titanate-based ceramic capacitor dielectric material and its preparation method according to the present invention are:

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955123A_ABST
    Figure CN118955123A_ABST
Patent Text Reader

Abstract

The invention discloses a wide-temperature-range stable sodium bismuth titanate-based ceramic capacitor dielectric material and a preparation method thereof, and belongs to the technical field of piezoelectric ceramic materials. The wide-temperature-range stable sodium bismuth titanate-based ceramic capacitor dielectric material has a chemical general formula of (Na < 0.3 + x > Bi < 0.38-0.2 > x Sr < 0.28-0.7 x >) (Ti < 1-x > Nbx) O3, and x is greater than or equal to 0 and less than or equal to 0.1. The preparation method comprises the following steps: performing primary ball milling, pre-sintering at 900 DEG C, performing secondary ball milling, granulating, screening, performing dry pressing molding on fine powder under 8MPa, performing high-temperature glue discharging at 550 DEG C, and burying coarse powder in an air atmosphere and sintering at 1100-1130 DEG C to obtain the ceramic capacitor dielectric material. By adopting the sodium bismuth titanate-based ceramic capacitor dielectric material with the stable wide temperature range and the preparation method of the sodium bismuth titanate-based ceramic capacitor dielectric material, the problems of poor dielectric stability, low dielectric constant, high loss and harsh preparation process conditions of the existing sodium bismuth titanate-based piezoelectric ceramic can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of piezoelectric ceramic materials, and in particular to a sodium bismuth titanate-based ceramic capacitor dielectric material that is stable over a wide temperature range and a preparation method thereof. Background Art

[0002] As a new type of lead-free relaxor ferroelectric material, sodium bismuth titanate-based ceramics have attracted much attention due to their excellent dielectric properties and wide temperature range stability. In modern electronic devices, capacitors, as key passive devices, undertake multiple functions such as voltage smoothing, pulse discharge, and filtering. With the rapid development of science and technology, especially in high-end application fields such as 5G communications, electric vehicles, and aerospace, the performance requirements for capacitors are getting higher and higher, especially the stable performance at high temperatures and wide temperature ranges. Although traditional ceramic capacitor dielectric materials, such as BaTiO3 and its modified systems, can meet the performance requirements within a certain temperature range, at higher temperatures, the temperature stability of their dielectric properties deteriorates sharply, limiting their application in extreme environments. In addition, these materials may contain harmful elements such as lead, which pose a threat to the environment and human health. Therefore, it is particularly important to develop environmentally friendly and high-performance alternative materials.

[0003] Sodium bismuth titanate-based ceramics have become a hot topic of research due to their high Curie temperature, low dielectric loss and excellent dielectric temperature stability. This material is occupied by Na and Bi at the A site and Ti at the B site, forming a unique perovskite structure that enables it to exhibit stable dielectric properties over a wide temperature range. In particular, through doping modification, such as adding Sr 0.53 Ba 0.47 Nb2O6 can further improve its dielectric constant and temperature stability, and achieve stable operation in the temperature range from room temperature to 400°C or even higher. However, the preparation process of sodium bismuth titanate-based ceramics is relatively complicated, requiring precise control of multiple factors such as chemical composition, sintering temperature and time to achieve optimal performance. In addition, the microstructure of the material has an important influence on its macroscopic dielectric properties, so basic research on the material's grain growth, phase change behavior, etc. is also crucial.

[0004] In summary, the research background of sodium bismuth titanate-based ceramics focuses on the development of high-performance capacitor dielectric materials with wide temperature stability to meet the application requirements of high-end electronic equipment in harsh environments and promote the development of lead-free and environmentally friendly materials. Future research will continue to optimize the preparation process and deeply understand the physical mechanism of the material to achieve higher performance sodium bismuth titanate-based ceramic capacitor dielectric materials. Summary of the invention

[0005] The purpose of the present invention is to provide a sodium bismuth titanate-based ceramic capacitor dielectric material that is stable in a wide temperature range and a preparation method thereof, so as to solve the problems of poor dielectric stability, low dielectric constant, high loss and harsh preparation process conditions of existing sodium bismuth titanate-based piezoelectric ceramics.

[0006] To achieve the above object, the present invention provides a sodium bismuth titanate-based ceramic capacitor dielectric material that is stable over a wide temperature range. The chemical formula of the ceramic capacitor dielectric material is: (Na 0.3 Bi 0.38 Sr 0.28 )TiO3.

[0007] A sodium bismuth titanate-based ceramic capacitor dielectric material that is stable over a wide temperature range, the chemical formula of the ceramic capacitor dielectric material being: (Na 0.3+x Bi 0.38-0.2x Sr 0.28-0.7x )(Ti 1-x Nb x )O3,0 <x≤0.1。

[0008] The method for preparing the above-mentioned wide temperature range stable sodium bismuth titanate-based ceramic capacitor dielectric material comprises the following steps:

[0009] S1. Batching and primary ball milling: weigh and analyze the pure raw materials according to molar percentage, the raw materials include bismuth oxide Bi2O3, sodium carbonate Na2CO3, titanium dioxide TiO2, strontium carbonate SrCO3, and niobium pentoxide Nb2O5, mix the raw materials and pass them through a planetary ball mill to obtain a uniformly mixed primary slurry by wet ball milling;

[0010] S2, pre-burning: After drying the primary slurry, pre-burn it;

[0011] S3, secondary ball milling: the pre-sintered powder is subjected to secondary ball milling using a planetary ball mill to obtain a uniformly mixed secondary slurry;

[0012] S4, granulation: drying the secondary slurry to obtain dry powder, granulating the dry powder, and sieving to obtain fine powder and coarse powder;

[0013] S5, dry pressing: using a tablet press to press the fine powder into thin discs;

[0014] S6, debinding: debinding the formed thin disc at high temperature to obtain a ceramic body;

[0015] S7. Sintering: The ceramic body is buried with coarse powder and sintered at high temperature in an air atmosphere using a muffle furnace to obtain a ceramic capacitor dielectric material.

[0016] Preferably, in S1, the ball milling medium is anhydrous ethanol, the ball milling jar is a nylon jar, the grinding balls are zirconium balls, the ball milling speed is 400 r / min, and the ball milling time is 12 hours to 16 hours.

[0017] Preferably, in S2, the primary slurry is pre-fired in a corundum crucible at a pre-fired temperature of 900° C. for 4 hours.

[0018] Preferably, in S3, the secondary ball milling medium is anhydrous ethanol, and the ball milling time is 8 hours to 12 hours.

[0019] Preferably, in S4, a polyvinyl alcohol aqueous solution with a mass percentage of 6wt% to 8wt% is added to the dry powder, and the powder is dried and then ground for 5 minutes to 15 minutes. The ground powder is sieved with a 120-mesh sieve to obtain fine powder and coarse powder.

[0020] Preferably, in S5, the pressure of the tablet press is 8 MPa and the holding time is 1 second.

[0021] Preferably, in S6, the debinding temperature is 530°C-580°C, the heating rate is 1°C / min, the temperature is raised to 120°C and kept for 1 hour, and then the temperature is raised to 530°C-580°C at the same heating rate and kept for 3 hours.

[0022] Preferably, in S7, the ceramic green body is buried in a small crucible with coarse powder, the sintering temperature is 1100° C.-1130° C., the sintering time is 6 hours-8 hours, and the cooling rate is 2° C. / min.

[0023] The advantages and positive effects of the sodium bismuth titanate-based ceramic capacitor dielectric material with wide temperature range stability and the preparation method thereof described in the present invention are:

[0024] 1. The present invention uses A and B position composite doping in sodium bismuth titanate to form defects, which helps to improve the dielectric temperature stability and dielectric loss of the material. 0.3+x Bi 0.38-0.2x Sr 0.28-0.7x )(Ti 1-x Nb x )O3 ceramics in the A position (Na + 、Bi 3 + , Sr 2+ ) and B position (Ti 4+ , Nb 5+ ) is occupied by composite ions, forming polar nanoregions (PNRs) of various structural types inside the material, and the wide dielectric response with diffusion phase transition characteristics weakens the dielectric anomaly peak, thereby maintaining the stability of dielectric properties over a wide temperature range. + and Nb 5+As the content increases, a small amount of the second phase Bi2Ti2O7 appears in the crystal structure of the ceramic, which can reduce the sintering temperature, reduce the volatilization loss of the material at high temperature, and help reduce the dielectric loss. The ceramic capacitor dielectric material has a high and stable dielectric constant (~2350±15%) and low dielectric loss (<5%) in a wide high temperature range (22°C~316°C), which improves the performance of the ceramic capacitor dielectric material. In addition, the ceramic capacitor dielectric material is non-toxic, highly safe, and reduces pollution to the environment. The dielectric constant ε of the ceramic capacitor dielectric material prepared by the present invention under 1kHz conditions is r =2350(150℃), loss tanδ=0.032%(150℃), TCC 150℃ ≤15% temperature range is 22℃-316℃.

[0025] 2. The present invention can obtain ceramic capacitor dielectric materials by dry pressing under a pressure of 8 MPa and burying powder and sintering in an air atmosphere. The preparation method is simple, easy to operate, and easy to realize industrialization.

[0026] 3. The ceramic capacitor dielectric material of the present invention is sintered at a relatively low sintering temperature, which is beneficial to saving energy and reducing preparation costs.

[0027] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a flow chart of an embodiment of the present invention;

[0029] Figure 2 X-ray diffraction analysis diagram of the ceramic capacitor dielectric material obtained in Examples 1-4 of the present invention;

[0030] Figure 3 Schematic diagram of the change of relative dielectric constant and dielectric loss of the ceramic capacitor dielectric material obtained in Examples 1-4 of the present invention at 1 kHz with temperature;

[0031] Figure 4 This is a graph showing the change in capacitance-temperature change rate (based on 150° C.) of the ceramic capacitor dielectric material obtained in Examples 1-4 of the present invention at a frequency of 1 kHz as a function of temperature. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0033] A sodium bismuth titanate-based ceramic capacitor dielectric material that is stable over a wide temperature range, the general chemical formula of which is: (Na 0.3+ x Bi 0.38-0.2x Sr 0.28-0.7x )(Ti1-x Nb x )O3, 0≤x≤0.1.

[0034] The method for preparing the above-mentioned wide temperature range stable sodium bismuth titanate-based ceramic capacitor dielectric material comprises the following steps:

[0035] S1. Ingredients and primary ball milling: According to molar percentage, weigh and analyze the pure raw materials, which include bismuth oxide Bi2O3, sodium carbonate Na2CO3, titanium dioxide TiO2, strontium carbonate SrCO3, and niobium pentoxide Nb2O5. Mix the raw materials and pass them through a planetary ball mill to obtain a uniformly mixed primary slurry by wet ball milling.

[0036] The raw materials include Na2CO3 with a purity of 99.8%, TiO2 with a purity of 98%, Nb2O5 with a purity of 99.5%, SrCO3 with a purity of 99%, and Bi2O3 with a purity of 99%.

[0037] The ball milling medium is anhydrous ethanol, the ball milling jar is a nylon jar, the grinding balls are zirconium balls, the ball milling speed is 400 r / min, and the ball milling time is 12 hours to 16 hours.

[0038] S2, pre-calcination: drying the primary slurry to obtain a uniformly mixed powder, and pre-calcining the powder in a corundum crucible.

[0039] The pre-firing temperature is 900°C and the pre-firing time is 4 hours.

[0040] S3. Secondary ball milling: The pre-sintered powder is subjected to secondary ball milling using a planetary ball mill to obtain a uniformly mixed secondary slurry.

[0041] The secondary ball milling medium is anhydrous ethanol, and the ball milling time is 8 hours to 12 hours.

[0042] S4. Granulation: Dry the secondary slurry to obtain dry powder, granulate the dry powder, and sieve to obtain fine powder and coarse powder.

[0043] Add 6wt% to 8wt% of polyvinyl alcohol aqueous solution to the dry powder, dry and grind for 5 to 15 minutes, sieve the ground powder with a 120-mesh sieve to obtain fine powder and coarse powder, and package the fine powder and coarse powder separately.

[0044] S5. Dry pressing: Use a tablet press to press the fine powder into thin round tablets.

[0045] The tablet press pressure was 8 MPa and the holding time was 1 second.

[0046] S6, debinding: debinding the formed thin disc at high temperature to obtain a ceramic body.

[0047] The debinding temperature is 530℃-580℃, the heating rate is 1℃ / min, the temperature is raised to 120℃ and kept for 1h, and then the temperature is raised to 530℃-580℃ at the same heating rate and kept for 3h.

[0048] S7. Sintering: The ceramic body is buried with coarse powder and sintered at high temperature in an air atmosphere using a muffle furnace to obtain a ceramic capacitor dielectric material.

[0049] The ceramic body is buried in a small crucible with coarse powder, the sintering temperature is 1100°C-1130°C, the sintering time is 6 hours-8 hours, and the cooling rate is 2°C / min.

[0050] Example 1

[0051] x=0, the general chemical formula of ceramic capacitor dielectric material is: (Na 0.3 Bi 0.38 Sr 0.28 )TiO3.

[0052] The method for preparing a sodium bismuth titanate-based ceramic capacitor dielectric material that is stable over a wide temperature range comprises the following steps:

[0053] S1. Ingredients and primary ball milling: According to molar percentage, weigh and analyze the pure raw materials, which include bismuth oxide Bi2O3, sodium carbonate Na2CO3, titanium dioxide TiO2, strontium carbonate SrCO3, and niobium pentoxide Nb2O5. Mix the raw materials and pass them through a planetary ball mill to obtain a uniformly mixed primary slurry by wet ball milling.

[0054] The raw materials include Na2CO3 with a purity of 99.8%, TiO2 with a purity of 98%, Nb2O5 with a purity of 99.5%, SrCO3 with a purity of 99%, and Bi2O3 with a purity of 99%.

[0055] The ball milling medium is anhydrous ethanol, the ball milling jar is a nylon jar, the grinding balls are zirconium balls, the ball milling speed is 400 r / min, and the ball milling time is 14 hours.

[0056] S2, pre-calcination: drying the primary slurry to obtain a uniformly mixed powder, and pre-calcining the powder in a corundum crucible.

[0057] The pre-firing temperature is 900°C and the pre-firing time is 4 hours.

[0058] S3. Secondary ball milling: The pre-sintered powder is subjected to secondary ball milling using a planetary ball mill to obtain a uniformly mixed secondary slurry.

[0059] The secondary ball milling medium was anhydrous ethanol, and the ball milling time was 10 hours.

[0060] S4. Granulation: Dry the secondary slurry to obtain dry powder, granulate the dry powder, and sieve to obtain fine powder and coarse powder.

[0061] A 7 wt % polyvinyl alcohol aqueous solution was added to the dry powder, and the powder was dried and ground for 10 minutes. The ground powder was sieved with a 120-mesh sieve to obtain fine powder and coarse powder, which were then packaged separately.

[0062] S5. Dry pressing: Use a tablet press to press the fine powder into thin round tablets.

[0063] The tablet press pressure was 8 MPa and the holding time was 1 second.

[0064] S6, debinding: debinding the formed thin disc at high temperature to obtain a ceramic body.

[0065] The debinding temperature was 550°C, the heating rate was 1°C / min, the temperature was raised to 120°C and kept for 1 hour, and then the temperature was raised to 550°C at the same heating rate and kept for 3 hours.

[0066] S7. Sintering: The ceramic body is buried with coarse powder and sintered at high temperature in an air atmosphere using a muffle furnace to obtain a ceramic capacitor dielectric material.

[0067] The ceramic body was buried in a small crucible with coarse powder, the sintering temperature was 1120°C, the sintering time was 7 hours, and the cooling rate was 2°C / min.

[0068] Example 2

[0069] x = 0.025, the general chemical formula of ceramic capacitor dielectric material is: (Na 0.325 Bi 0.375 Sr 0.2625 )(Ti 0.975 Nb 0.025 )O3.

[0070] The method for preparing a sodium bismuth titanate-based ceramic capacitor dielectric material that is stable over a wide temperature range comprises the following steps:

[0071] S1. Ingredients and primary ball milling: According to molar percentage, weigh and analyze the pure raw materials, which include bismuth oxide Bi2O3, sodium carbonate Na2CO3, titanium dioxide TiO2, strontium carbonate SrCO3, and niobium pentoxide Nb2O5. Mix the raw materials and pass them through a planetary ball mill to obtain a uniformly mixed primary slurry by wet ball milling.

[0072] The raw materials include Na2CO3 with a purity of 99.8%, TiO2 with a purity of 98%, Nb2O5 with a purity of 99.5%, SrCO3 with a purity of 99%, and Bi2O3 with a purity of 99%.

[0073] The ball milling medium is anhydrous ethanol, the ball milling jar is a nylon jar, the grinding balls are zirconium balls, the ball milling speed is 400 r / min, and the ball milling time is 14 hours.

[0074] S2, pre-calcination: drying the primary slurry to obtain a uniformly mixed powder, and pre-calcining the powder in a corundum crucible.

[0075] The pre-firing temperature is 900°C and the pre-firing time is 4 hours.

[0076] S3. Secondary ball milling: The pre-sintered powder is subjected to secondary ball milling using a planetary ball mill to obtain a uniformly mixed secondary slurry.

[0077] The secondary ball milling medium was anhydrous ethanol, and the ball milling time was 10 hours.

[0078] S4. Granulation: Dry the secondary slurry to obtain dry powder, granulate the dry powder, and sieve to obtain fine powder and coarse powder.

[0079] A 7 wt % polyvinyl alcohol aqueous solution was added to the dry powder, and the powder was dried and ground for 10 minutes. The ground powder was sieved with a 120-mesh sieve to obtain fine powder and coarse powder, which were then packaged separately.

[0080] S5. Dry pressing: Use a tablet press to press the fine powder into thin round tablets.

[0081] The tablet press pressure was 8 MPa and the holding time was 1 second.

[0082] S6, debinding: debinding the formed thin disc at high temperature to obtain a ceramic body.

[0083] The debinding temperature was 550°C, the heating rate was 1°C / min, the temperature was raised to 120°C and kept for 1 hour, and then the temperature was raised to 550°C at the same heating rate and kept for 3 hours.

[0084] S7. Sintering: The ceramic body is buried with coarse powder and sintered at high temperature in an air atmosphere using a muffle furnace to obtain a ceramic capacitor dielectric material.

[0085] The ceramic body was buried in a small crucible with coarse powder, the sintering temperature was 1120°C, the sintering time was 7 hours, and the cooling rate was 2°C / min.

[0086] Example 3

[0087] x = 0.05, the general chemical formula of ceramic capacitor dielectric material is: (Na 0.35 Bi 0.37 Sr 0.245 )(Ti 0.95 Nb 0.05 )O3.

[0088] The method for preparing a sodium bismuth titanate-based ceramic capacitor dielectric material that is stable over a wide temperature range comprises the following steps:

[0089] S1. Ingredients and primary ball milling: According to molar percentage, weigh and analyze the pure raw materials, which include bismuth oxide Bi2O3, sodium carbonate Na2CO3, titanium dioxide TiO2, strontium carbonate SrCO3, and niobium pentoxide Nb2O5. Mix the raw materials and pass them through a planetary ball mill to obtain a uniformly mixed primary slurry by wet ball milling.

[0090] The raw materials include Na2CO3 with a purity of 99.8%, TiO2 with a purity of 98%, Nb2O5 with a purity of 99.5%, SrCO3 with a purity of 99%, and Bi2O3 with a purity of 99%.

[0091] The ball milling medium is anhydrous ethanol, the ball milling jar is a nylon jar, the grinding balls are zirconium balls, the ball milling speed is 400 r / min, and the ball milling time is 16 hours.

[0092] S2, pre-calcination: drying the primary slurry to obtain a uniformly mixed powder, and pre-calcining the powder in a corundum crucible.

[0093] The pre-firing temperature is 900°C and the pre-firing time is 4 hours.

[0094] S3. Secondary ball milling: The pre-sintered powder is subjected to secondary ball milling using a planetary ball mill to obtain a uniformly mixed secondary slurry.

[0095] The secondary ball milling medium was anhydrous ethanol, and the ball milling time was 12 hours.

[0096] S4. Granulation: Dry the secondary slurry to obtain dry powder, granulate the dry powder, and sieve to obtain fine powder and coarse powder.

[0097] A 7 wt % polyvinyl alcohol aqueous solution was added to the dry powder, and the powder was dried and ground for 10 minutes. The ground powder was sieved with a 120-mesh sieve to obtain fine powder and coarse powder, which were then packaged separately.

[0098] S5. Dry pressing: Use a tablet press to press the fine powder into thin round tablets.

[0099] The tablet press pressure was 8 MPa and the holding time was 1 second.

[0100] S6, debinding: debinding the formed thin disc at high temperature to obtain a ceramic body.

[0101] The debinding temperature was 550°C, the heating rate was 1°C / min, the temperature was raised to 120°C and kept for 1 hour, and then the temperature was raised to 550°C at the same heating rate and kept for 3 hours.

[0102] S7. Sintering: The ceramic body is buried with coarse powder and sintered at high temperature in an air atmosphere using a muffle furnace to obtain a ceramic capacitor dielectric material.

[0103] The ceramic body was buried in a small crucible with coarse powder, the sintering temperature was 1100°C, the sintering time was 8 hours, and the cooling rate was 2°C / min.

[0104] Example 4

[0105] x=0.1, the general chemical formula of ceramic capacitor dielectric material is: (Na 0.4 Bi 0.36 Sr 0.21 )(Ti 0.9 Nb 0.1 )O3.

[0106] The method for preparing a sodium bismuth titanate-based ceramic capacitor dielectric material that is stable over a wide temperature range comprises the following steps:

[0107] S1. Ingredients and primary ball milling: According to molar percentage, weigh and analyze the pure raw materials, which include bismuth oxide Bi2O3, sodium carbonate Na2CO3, titanium dioxide TiO2, strontium carbonate SrCO3, and niobium pentoxide Nb2O5. Mix the raw materials and pass them through a planetary ball mill to obtain a uniformly mixed primary slurry by wet ball milling.

[0108] The raw materials include Na2CO3 with a purity of 99.8%, TiO2 with a purity of 98%, Nb2O5 with a purity of 99.5%, SrCO3 with a purity of 99%, and Bi2O3 with a purity of 99%.

[0109] The ball milling medium is anhydrous ethanol, the ball milling jar is a nylon jar, the grinding balls are zirconium balls, the ball milling speed is 400 r / min, and the ball milling time is 12 hours.

[0110] S2, pre-calcination: drying the primary slurry to obtain a uniformly mixed powder, and pre-calcining the powder in a corundum crucible.

[0111] The pre-firing temperature is 900°C and the pre-firing time is 4 hours.

[0112] S3. Secondary ball milling: The pre-sintered powder is subjected to secondary ball milling using a planetary ball mill to obtain a uniformly mixed secondary slurry.

[0113] The secondary ball milling medium was anhydrous ethanol, and the ball milling time was 8 hours.

[0114] S4. Granulation: Dry the secondary slurry to obtain dry powder, granulate the dry powder, and sieve to obtain fine powder and coarse powder.

[0115] Add 8 wt % of polyvinyl alcohol aqueous solution to the dry powder, dry and grind for 10 minutes, sieve the ground powder with a 120-mesh sieve to obtain fine powder and coarse powder, and package the fine powder and coarse powder separately.

[0116] S5. Dry pressing: Use a tablet press to press the fine powder into thin round tablets.

[0117] The tablet press pressure was 8 MPa and the holding time was 1 second.

[0118] S6, debinding: debinding the formed thin disc at high temperature to obtain a ceramic body.

[0119] The debinding temperature was 550°C, the heating rate was 1°C / min, the temperature was raised to 120°C and kept for 1 hour, and then the temperature was raised to 550°C at the same heating rate and kept for 3 hours.

[0120] S7. Sintering: The ceramic body is buried with coarse powder and sintered at high temperature in an air atmosphere using a muffle furnace to obtain a ceramic capacitor dielectric material.

[0121] The ceramic body was buried in a small crucible with coarse powder, the sintering temperature was 1130°C, the sintering time was 7 hours, and the cooling rate was 2°C / min.

[0122] The ceramic capacitor dielectric materials obtained in Examples 1-4 were subjected to X-ray diffraction analysis, and the results were as follows: Figure 2 As shown. There are 7 characteristic peaks between 20° and 80°, which are (100), (110), (111), (200), (211), (220), and (310) as the angle increases, indicating that the ceramic material is a perovskite ceramic. The (111) and (200) diffraction peaks are split, indicating that the sample presents a pseudo-cubic phase structure. There are impurity peaks near the 30°, 50°, and 60° diffraction peaks, indicating that the introduction of Na + and Nb 5+ This results in the appearance of the second phase Bi2Ti2O7.

[0123] Figure 3 Schematic diagram of the relative dielectric constant and dielectric loss of the ceramic capacitor dielectric material described in Examples 1-4 of the present invention at 1 kHz as a function of temperature. Figure 3 As shown, the relative dielectric constant ε r In the temperature-dependent curve, Examples 1-3 have two dielectric anomaly peaks, while Example 4 has only one obvious dielectric anomaly peak. It can be clearly seen in the figure that when x = 0.025, the relative dielectric constant is at a relatively high level, reflecting that the relative dielectric constant is increased to a certain extent after doping, but too much will cause the dielectric constant to decrease. The dielectric loss tanδ decreases with the increase of the doping amount.

[0124] Figure 4 The graph shows the change in capacitance-temperature ratio (based on 150° C.) of the ceramic capacitor dielectric material prepared in Examples 1 to 4 at a frequency of 1 kHz as a function of temperature.

[0125] The temperature variation rate and dielectric loss of the ceramic capacitor dielectric materials prepared in Examples 1-4 were compared, and the results are shown in Table 1.

[0126] Table 1 Properties of dielectric materials of ceramic capacitors prepared in Examples 1-4

[0127]

[0128] It can be seen that the ceramic capacitor dielectric material prepared by the method described in the present invention has a higher relative dielectric constant, lower dielectric loss and a stable capacitance-temperature change rate. If the capacitance-temperature change rate is required to be ≤15%, the temperature range of Example 2 is 22-316°C, which has better comprehensive performance.

[0129] Therefore, the wide temperature range stable sodium bismuth titanate-based ceramic capacitor dielectric material and its preparation method described in the present invention can solve the problems of poor dielectric stability, low dielectric constant and high loss of existing sodium bismuth titanate-based piezoelectric ceramics and harsh preparation process conditions.

[0130] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A sodium bismuth titanate-based ceramic capacitor dielectric material that is stable over a wide temperature range, characterized in that: The general chemical formula of the ceramic capacitor dielectric material is: (Na 0.3 Bi 0.38 Sr 0.28 )TiO3.

2. A sodium bismuth titanate-based ceramic capacitor dielectric material that is stable over a wide temperature range, characterized in that: The general chemical formula of the ceramic capacitor dielectric material is: (Na 0.3+x Bi 0.38-0.2x Sr 0.28-0.7x )(Ti 1-x Nb x )O3,0 <x≤0.1。 3. A method for preparing a wide temperature range stable sodium bismuth titanate based ceramic capacitor dielectric material as claimed in claim 1 or 2, characterized in that: The following steps are involved: S1. Batching and primary ball milling: weigh and analyze the pure raw materials according to molar percentage, the raw materials include bismuth oxide Bi2O3, sodium carbonate Na2CO3, titanium dioxide TiO2, strontium carbonate SrCO3, and niobium pentoxide Nb2O5, mix the raw materials and pass them through a planetary ball mill to obtain a uniformly mixed primary slurry by wet ball milling; S2, pre-burning: After drying the primary slurry, pre-burn it; S3, secondary ball milling: the pre-sintered powder is subjected to secondary ball milling using a planetary ball mill to obtain a uniformly mixed secondary slurry; S4, granulation: drying the secondary slurry to obtain dry powder, granulating the dry powder, and sieving to obtain fine powder and coarse powder; S5, dry pressing: using a tablet press to press the fine powder into thin discs; S6, debinding: debinding the formed thin disc at high temperature to obtain a ceramic body; S7. Sintering: The ceramic body is buried with coarse powder and sintered at high temperature in an air atmosphere using a muffle furnace to obtain a ceramic capacitor dielectric material.

4. The method for preparing a wide temperature range stable sodium bismuth titanate-based ceramic capacitor dielectric material according to claim 3, characterized in that: In S1, the ball milling medium is anhydrous ethanol, the ball milling jar is a nylon jar, the grinding balls are zirconium balls, the ball milling speed is 400 r / min, and the ball milling time is 12 hours to 16 hours.

5. The method for preparing a wide temperature range stable sodium bismuth titanate based ceramic capacitor dielectric material according to claim 3, characterized in that: In S2, the primary slurry is pre-fired in a corundum crucible at a temperature of 900° C. for 4 hours.

6. The method for preparing a wide temperature range stable sodium bismuth titanate based ceramic capacitor dielectric material according to claim 3, characterized in that: In S3, the secondary ball milling medium is anhydrous ethanol, and the ball milling time is 8 hours to 12 hours.

7. The method for preparing a wide temperature range stable sodium bismuth titanate-based ceramic capacitor dielectric material according to claim 3, characterized in that: In S4, a polyvinyl alcohol aqueous solution with a mass percentage of 6 wt% to 8 wt% is added to the dry powder, and the powder is dried and ground for 5 to 15 minutes. The ground powder is sieved with a 120-mesh sieve to obtain fine powder and coarse powder.

8. The method for preparing a wide temperature range stable sodium bismuth titanate based ceramic capacitor dielectric material according to claim 3, characterized in that: In S5, the pressure of the tablet press is 8 MPa and the holding time is 1 second.

9. The method for preparing a wide temperature range stable sodium bismuth titanate-based ceramic capacitor dielectric material according to claim 3, characterized in that: In the step S6, the debinding temperature is 530° C.-580° C., and the heating rate is 1° C. / min.

10. The method for preparing a wide temperature range stable sodium bismuth titanate based ceramic capacitor dielectric material according to claim 3, characterized in that: In the above S7, the ceramic green body is buried in a small crucible with coarse powder, the sintering temperature is 1100° C.-1130° C., the sintering time is 6 hours-8 hours, and the cooling rate is 2° C. / min.

Citation Information

Patent Citations

  • Large-strain small-lag sodium bismuth titanate-based ceramic obtained by constructing ion pairs and preparation method of large-strain small-lag sodium bismuth titanate-based ceramic

    CN111620690A

  • High-temperature stable sodium bismuth titanate-strontium titanate-based dielectric energy storage ceramic material as well as preparation and application thereof

    CN114716243A

  • Wide-temperature-spectrum sodium bismuth titanate-barium titanate-based ferroelectric ceramic dielectric material as well as preparation method and application thereof

    CN115340375A

Cited By

  • Sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material with antiferroelectric-like characteristic and preparation method of sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material

    CN118894722A

  • A sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material with antiferroelectric-like properties and a preparation method thereof

    CN118894722B

  • Wide-temperature stable high-dielectric low-loss ceramic capacitor dielectric material and preparation method and application thereof

    CN120058354A