Transparent aluminum nitride textured along c axis and preparation method thereof
Through strong magnetic field orientation technology and pressure-free sintering process, the limitation of the grain size of aluminum nitride ceramics on optical transmittance is solved, and transparent ceramics with high texture and excellent performance are prepared, which solves the problem of decreasing thermal conductivity and realizes the The feasibility of industrial production.
Patent Information
- Application Number
- CN202411189346.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-15
AI Technical Summary
The research on the optical properties of aluminum nitride ceramics, especially optical linear transmittance, has progressed slowly, mainly due to the birefringence phenomenon caused by the anisotropy of its grain refractive index, which leads to a decrease in thermal conductivity, limiting its application field.
Using strong magnetic field orientation technology to texture aluminum nitride ceramics in the c-axis direction, transparent ceramics with high texture, good thermal conductivity and linear optical transmittance were prepared through pressure-free sintering process, and treated using surface wrapping process. The aluminum nitride powder, sintering aid and dispersant are prepared by ball milling, grouting and molding under magnetic field, pretreatment and sintering.
It significantly improves the optical linear transmittance of aluminum nitride ceramics, maintains high thermal conductivity and mechanical properties, simplifies process operations, reduces production costs, widens the application range, and is suitable for industrial production.
Smart Images

Figure CN118955147A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a highly textured, non-cubic, non-oxide transparent ceramic material and a preparation method thereof, in particular to an aluminum nitride transparent ceramic and a preparation method thereof, and also to a preparation method of textured ceramics under a strong magnetic field, which is applied to transparent ceramics, textured ceramics, low-symmetry non-oxide ceramics and high thermal conductivity nitride ceramic technologies. Background Art
[0002] Aluminum nitride ceramics are emerging thermal conductive, mechanical structural and optical materials in the past 20 years. They have high thermal conductivity (320W / (m·K)), low thermal expansion coefficient, good mechanical properties, outstanding thermal shock resistance, wide bandgap (6.2eV), low optical absorption coefficient, low dielectric constant, low dielectric loss and good chemical stability. Aluminum nitride materials with the above excellent properties can be made into thermal conductive materials, high-temperature structural components, windows, fairings, and laser dielectric materials, becoming the most promising structural functional ceramic materials in the fields of large-scale integrated circuits, high-power semiconductor modules, high-temperature windows and aerospace.
[0003] In recent years, with the continuous attention and research of scientific researchers and engineering technicians on aluminum nitride ceramics, its thermal and mechanical properties have been significantly improved. However, since N. Kuramoto prepared a piece of translucent aluminum nitride ceramic in 1984, the research on transparent aluminum nitride ceramics has also received continuous attention. However, the research progress of the optical properties of aluminum nitride ceramics, especially the optical linear transmittance performance, is quite slow. The fundamental reason lies in the birefringence phenomenon inside aluminum nitride ceramics. Due to the anisotropy of the refractive index of aluminum nitride grains, birefringence is generated when light is transmitted in aluminum nitride grains, thereby reducing the linear optical transmittance of aluminum nitride ceramics. According to the RGD theory, the scattering caused by birefringence is usually positively correlated with the grain size of the ceramic. Therefore, previous research work mainly focused on how to obtain highly dense aluminum nitride transparent ceramics on the basis of reducing the grain size of aluminum nitride. A series of ceramic sintering technologies that require pressure-assisted systems, such as hot pressing, SPS, and ultra-high pressure, are widely used in the research and production of transparent aluminum nitride ceramics. However, the processes of these technologies are often complicated and have certain limitations on the size of the sample. What is more fatal is that as the grain size of the sample decreases, the grain boundaries of the sample increase, which increases the probability of phonon scattering in aluminum nitride ceramics, causing the thermal conductivity of aluminum nitride ceramics to drop sharply, seriously restricting the application field of aluminum nitride ceramics.
[0004] Ceramic texturing technology refers to the technology that, during the ceramic forming process, anisotropic external fields are used to make the anisotropic grains in the microstructure of ceramic materials arrange regularly along certain specific directions, or increase the probability of orientation in these directions, so that they grow preferentially. Ceramics with directional arrangement of crystal axes are called textured ceramics. Ceramic texturing technology, using the anisotropy of ceramic grains themselves, can not only maintain all the original traditional characteristics of the material, but also significantly improve the necessary performance in specific directions. It has become a unique method to improve the performance of traditional structural ceramics and has attracted widespread attention from ceramic manufacturers and researchers.
[0005] At present, the research on aluminum nitride textured ceramics at home and abroad is still in its infancy, and there is a lack of methods for producing aluminum nitride ceramics with high optical transmittance. Summary of the invention
[0006] In order to solve or partially solve the above technical problems, the present invention provides a method for preparing transparent aluminum nitride textured along the c-axis, comprising the following steps: adding the selected aluminum nitride powder treated by the surface coating process, the sintering aid and the dispersant into the dispersion medium respectively, and preparing the aluminum nitride slurry by ball milling process;
[0007] Performing slip casting molding on the aluminum nitride slurry under a magnetic field to prepare a ceramic blank with texture along the c-axis;
[0008] Pre-treating the ceramic embryo;
[0009] The pretreated ceramic blank is sintered to prepare transparent aluminum nitride ceramics.
[0010] Optionally,
[0011] The particle size of the aluminum nitride powder is 50nm-10um, the powder purity is greater than or equal to 99%, and the powder has good hydrolysis resistance after surface coating treatment (can be stable in water for more than one month).
[0012] Optionally, the sintering aid includes at least one or more of an alkali metal compound, an alkaline earth metal compound, a rare earth metal compound and an aluminum-containing compound, and the content of the sintering aid in the aluminum nitride slurry is between 0.1wt% and 7wt%.
[0013] Optionally, the dispersant is polyvinylpyrrolidone (PVP), the molecular weight of the dispersant is between 3000-30000, and the content of the dispersant in the aluminum nitride slurry is between 0.1wt% and 7wt%.
[0014] Optionally, the dispersion medium is deionized water or anhydrous ethanol;
[0015] The aluminum nitride slurry has a solid content higher than 30 vol% and a viscosity between 20 and 20000 mPa·s.
[0016] Optionally, the magnetic field type is any one of a static vertical magnetic field, a static horizontal magnetic field and a rotating magnetic field, and the intensity of the magnetic field is in the range of 1 to 20T.
[0017] Optionally, in the step of preparing the ceramic blank:
[0018] The magnetic field is a static magnetic field, and the ceramic embryo rotates in the magnetic field; or,
[0019] The ceramic embryo remains stationary, and the magnetic field rotates relative to the ceramic embryo; or,
[0020] The ceramic green body and the magnetic field rotate simultaneously, and the rotation directions of the ceramic green body and the magnetic field are parallel or perpendicular to each other.
[0021] Optionally, in the step of pre-treating the ceramic green blank, the ceramic green blank is subjected to debinding and isostatic pressing treatments.
[0022] The debinding is carried out in air atmosphere or vacuum atmosphere, the debinding temperature is 450℃~800℃, and the debinding time is 12h~72h;
[0023] The isostatic pressing temperature is 25°C to 80°C, the pressure is 20MPa to 300MPa, and the holding time is 2min to 30min.
[0024] Optionally, in the sintering step,
[0025] The sintering process adopts pressureless sintering, the sintering temperature is between 1600°C and 2000°C, the holding time is between 2 and 70 hours, and the sintering atmosphere is nitrogen or argon.
[0026] The present invention also provides a transparent aluminum nitride, which is prepared by any one of the preparation methods mentioned above.
[0027] The transparent aluminum nitride of the present invention uses a strong magnetic field orientation technology to achieve the texture of the aluminum nitride embryo, and prepares aluminum nitride transparent ceramics with high texture, good thermal conductivity, mechanical properties and linear optical transmittance through a pressureless sintering technology.
[0028] Compared with the prior art, the present invention has the following obvious outstanding substantive features and significant advantages:
[0029] (1) The transparent aluminum nitride ceramics textured along the c-axis prepared by the present invention have good optical linear transmittance compared with previous technical solutions, especially in the visible light range, the optical linear transmittance is significantly higher than the data provided by previous technical solutions.
[0030] (2) The transparent aluminum nitride ceramics textured along the c-axis prepared by the present invention not only have excellent linear optical transmittance, but also have high texture degree, excellent thermal conductivity and good mechanical properties, which effectively broadens the application range of aluminum nitride.
[0031] (3) The method of the present invention does not require the use of a pressure-assisted sintering system, has simple process operation, low production cost, a wide range of applications, is easy for industrial production, has significant industrial application value, and is conducive to the large-scale industrial application of aluminum nitride. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The aluminum nitride embryo ( Figure 1 a) and aluminum nitride ceramics ( Figure 1 b) XRD diffraction pattern.
[0033] Figure 2 The untextured aluminum nitride ceramic ( Figure 2 a) and aluminum nitride ceramics textured along the c-axis ( Figure 2 b) Comparison picture of the actual object 5mm away from the paper.
[0034] Figure 3 This is the test result of the linear optical transmittance of the aluminum nitride ceramic according to the first embodiment of the present invention. DETAILED DESCRIPTION
[0035] In order to solve the scientific problem of incompatibility of optical, thermal and mechanical properties of aluminum nitride ceramics, and to improve the technical problem of complex preparation process of aluminum nitride transparent ceramics, the purpose of the present invention is to overcome the shortcomings of the existing technology, realize the texturing of aluminum nitride ceramic grains along the c-axis through strong magnetic field orientation technology, solve the limitation of aluminum nitride grain size on optical transmittance, and prepare aluminum nitride ceramic materials with high texture, good thermal conductivity, mechanical properties and linear optical transmittance.
[0036] In the implementation manner of the present application, the manufacturing process of the aluminum nitride ceramic material is given as follows:
[0037] (1) Material selection: Aluminum nitride powder with a particle size of 50 nm to 10 μm and a purity of 99% is selected as the raw material;
[0038] (2) Pretreatment: The aluminum nitride powder is subjected to surface coating treatment so that it can be stably present in water for more than one month;
[0039] (3) Slurry preparation: adding a sintering aid and a dispersant to the above-mentioned aluminum nitride powder in sequence, and preparing an aluminum nitride slurry by ball milling;
[0040] (4) Preparation of textured blank: introducing the above aluminum nitride slurry into a mold and placing it under a strong magnetic field for molding;
[0041] (5) Texturing blank treatment: the aluminum nitride blank is subjected to debinding and isostatic pressing treatment;
[0042] (6) Preparation of transparent aluminum nitride ceramics with texture along the c-axis: placing the above-mentioned pre-nitrided aluminum blank in an atmosphere furnace, introducing a protective atmosphere for pressureless sintering, and obtaining transparent aluminum nitride ceramics with texture along the c-axis after cooling in the furnace;
[0043] Furthermore, the sintering aid added in step (3) is one or more of an alkali metal compound, an alkaline earth metal compound, a rare earth metal oxide and an aluminum-containing compound as a sintering aid, and the content is between 0.1wt% and 7wt%, and the dispersant is PVP with a molecular weight of 3000-30000, and the content is between 0.1wt% and 7wt%;
[0044] Furthermore, the ball milling process used in step (3) is planetary ball milling, the rotation speed is 100 to 250 r / min, and the ball milling time is 2 to 48 h;
[0045] Furthermore, the aluminum nitride slurry prepared in step (3) is a water-based or alcohol-based slurry, and has the following characteristics: a solid content higher than 30 vols%, a viscosity between 20 and 20000 mPa·s, and can be stably present for 1 week without sedimentation;
[0046] Furthermore, the magnetic field used in step (4) is: a magnetic field strength of 1 to 20 T, the magnetic field types are divided into three types: vertical magnetic field, horizontal magnetic field and rotating magnetic field, and the magnetic field types are steady-state magnetic field and pulsed magnetic field;
[0047] Furthermore, the textured blank obtained in step (4) is characterized by: grains are textured along the c-axis, the relative density is not less than 50%, and the texturing degree is not less than 5%;
[0048] Furthermore, the debinding process in step (5) is as follows: the debinding temperature is 300-600° C., the time is 4-72 hours, and the isostatic pressing process is as follows: the temperature is 25-80° C., the pressure is 20 MPa-300 MPa, and the holding time is 2 min-30 min;
[0049] Furthermore, the pressureless sintering process in step (6) is as follows: the sintering temperature is 1600° C. to 2000° C., the holding time is within 2 to 70 hours, and the protective atmosphere is nitrogen or argon;
[0050] The above scheme is further described below in conjunction with specific embodiments. The preferred embodiments of the present invention are described in detail as follows:
[0051] Embodiment 1:
[0052] In this example, a method for preparing transparent aluminum nitride textured along the c-axis comprises the following steps:
[0053] (1) Weigh a certain amount of aluminum nitride powder with a particle size of 1 μm, a sintering aid and a dispersant, and place them in anhydrous ethanol to prepare aluminum nitride slurry.
[0054] (2) placing the material in step (1) in a ball mill, and using a planetary ball mill to prepare an aluminum nitride slurry having a solid content of 48 vol% and a viscosity of 60 mPa·s for slip casting;
[0055] (3) placing the aluminum nitride slurry in step (2) in a gypsum mold, placing the gypsum mold in a horizontal magnetic field with a magnetic field strength of 12 T and rotating it for 1 hour at a speed of 60 r / min to prepare an aluminum nitride blank with a texture along the c-axis, wherein the relative density of the blank is 56% and the texture degree is 32%;
[0056] (4) Debinding the raw material in step (3) to remove residual organic matter at a temperature of 600° C. for 6 h; then isostatic pressing at a pressure of 200 MPa for 5 min;
[0057] (5) placing the green blank in step (4) in an atmosphere furnace for sintering at a sintering temperature of 1800° C. for a holding time of 2 h; after cooling in the furnace, a transparent aluminum nitride ceramic with a c-axis texture is obtained;
[0058] The main properties of the c-axis textured transparent aluminum nitride ceramics prepared by the present invention are as follows:
[0059] Density:3.26g / cm 3
[0060] Phase (XRD, EBSD, EDS, EPMA characterization): Aluminum nitride
[0061] Texture: 79%
[0062] Thermal conductivity: 195W / (m·K)
[0063] Hardness: 12GPa
[0064] Fracture toughness: 3.1MPa·m 1 / 2
[0065] Bending strength: 350MPa
[0066] Optical linear transmittance: 22% at 800nm, 70% at 5200nm
[0067] The phase and texture of the transparent aluminum nitride ceramic textured along the c-axis prepared in this embodiment are as follows: Figure 1 As shown in Figure 1, the grains of the aluminum nitride embryo formed in the magnetic field are textured along the c-axis, and the texture is further improved after sintering. The actual image and linear optical transmittance of the sample are shown in Figure 1. Figure 2 and Figure 3 As shown, it can be seen that when the grains in the sample are textured along the c-axis, the birefringence phenomenon in the sample is improved and the linear transmittance of the sample is significantly improved.
[0068] The transparent aluminum nitride ceramics textured along the c-axis prepared in this embodiment are obtained by rotary grouting and pressureless sintering in a horizontal strong magnetic field. Experiments have shown that as the grains in the sample are textured along the c-axis, the linear optical transmittance of the sample increases significantly, while maintaining good thermal conductivity and mechanical properties. The present invention solves the birefringence phenomenon caused by the anisotropy of the refractive index of aluminum nitride grains, and effectively improves the optical linear transmittance of aluminum nitride ceramics. In addition, since this embodiment does not need to introduce a pressure-assisted sintering process, it has the advantages of simple method and process, low production cost, wide range of use, and easy industrial production. It has significant industrial application value and is conducive to the large-scale industrial application of aluminum nitride transparent ceramics.
[0069] Embodiment 2:
[0070] This embodiment is basically the same as the first embodiment, except that:
[0071] (1) The particle size of the aluminum nitride powder used is 50 nm
[0072] (2) The solid content of the prepared aluminum nitride slurry is 32 vol% and the viscosity is 20 mPa·s
[0073] (3) The sintering temperature of the transparent aluminum nitride sample with c-axis texture is 1600℃ and the holding time is 24h.
[0074] The main properties of the c-axis textured transparent aluminum nitride ceramics prepared by the present invention are as follows:
[0075] Density:3.26g / cm 3
[0076] Phase (XRD, EBSD, EDS, EPMA characterization): Aluminum nitride
[0077] Texture: 67%
[0078] Thermal conductivity: 182W / (m·K)
[0079] Hardness: 9.3GPa
[0080] Fracture toughness: 2.5MPa·m 1 / 2
[0081] Bending strength: 310MPa
[0082] Optical linear transmittance: 14% at 800nm, 62% at 5200nm
[0083] The method of this embodiment has simple process operation, low production cost, wide application range, and is easy for industrial production. It has significant industrial application value and is conducive to the large-scale industrial application of aluminum nitride transparent ceramics.
[0084] Embodiment three:
[0085] This embodiment is basically the same as the above embodiment, with the following features:
[0086] (1) The particle size of the aluminum nitride powder used is 10 nm
[0087] (2) The solid content of the prepared aluminum nitride slurry is 52 vol% and the viscosity is 80 mPa·s
[0088] (3) The sintering temperature of the transparent aluminum nitride sample with c-axis texture is 2000℃ and the holding time is 70h.
[0089] The main properties of the c-axis textured transparent aluminum nitride ceramics prepared by the present invention are as follows:
[0090] Density:3.26g / cm 3
[0091] Phase (XRD, EBSD, EDS, EPMA characterization): Aluminum nitride
[0092] Texture: 73%
[0093] Thermal conductivity: 201W / (m·K)
[0094] Hardness: 14GPa
[0095] Fracture toughness: 3.7MPa·m 1 / 2
[0096] Bending strength: 380MPa
[0097] Optical linear transmittance: 15.32% at 800nm, 68% at 5200nm
[0098] The method of this embodiment has simple process operation, low production cost, wide application range, and is easy for industrial production. It has significant industrial application value and is conducive to the large-scale industrial application of aluminum nitride transparent ceramics.
[0099] Embodiment 4:
[0100] This embodiment is basically the same as the above embodiment, with the following features:
[0101] (1) The magnetic field used for aluminum nitride grouting is a vertical magnetic field
[0102] (2) The prepared aluminum nitride ceramic needs to be cut to expose the surface parallel to the magnetic field.
[0103] The main properties of the c-axis textured transparent aluminum nitride ceramics prepared by the present invention are as follows:
[0104] Density:3.26g / cm 3
[0105] Phase (XRD, EBSD, EDS, EPMA characterization): Aluminum nitride
[0106] Texture: 42%
[0107] Thermal conductivity: 193W / (m·K)
[0108] Hardness: 14GPa
[0109] Fracture toughness: 3.3MPa·m 1 / 2
[0110] Flexural strength: 410MPa
[0111] Optical linear transmittance: 7.32% at 800nm, 52% at 5200nm
[0112] The method of this embodiment has simple process operation, low production cost, wide application range, and is easy for industrial production. It has significant industrial application value and is conducive to the large-scale industrial application of aluminum nitride transparent ceramics.
[0113] Embodiment five:
[0114] This embodiment is basically the same as the above embodiment, with the following features:
[0115] (1) The magnetic field used in aluminum nitride grouting is a pulsed magnetic field
[0116] (2) During the grouting process, the sample is stationary and the magnetic field rotates
[0117] The main properties of the c-axis textured transparent aluminum nitride ceramics prepared by the present invention are as follows:
[0118] Density:3.26g / cm 3
[0119] Phase (XRD, EBSD, EDS, EPMA characterization): Aluminum nitride
[0120] Texture: 33%
[0121] Thermal conductivity: 173W / (m·K)
[0122] Hardness: 10GPa
[0123] Fracture toughness: 2.3MPa·m 1 / 2
[0124] Flexural strength: 320MPa
[0125] Optical linear transmittance: 5.73% at 800nm, 56% at 5200nm
[0126] The method of this embodiment has simple process operation, low production cost, wide application range, and is easy for industrial production. It has significant industrial application value and is conducive to the large-scale industrial application of aluminum nitride transparent ceramics.
[0127] Embodiment six:
[0128] This embodiment is basically the same as the above embodiment, with the following features:
[0129] (1) The magnetic field used in aluminum nitride grouting is a pulsed magnetic field;
[0130] (2) During the grouting process, the sample and the magnetic field rotate simultaneously;
[0131] The main properties of the transparent aluminum nitride ceramics textured along the c-axis prepared by the present invention are as follows:
[0132] Density:3.26g / cm 3
[0133] Phase (XRD, EBSD, EDS, EPMA characterization): Aluminum nitride
[0134] Texture: 65%
[0135] Thermal conductivity: 188W / (m·K)
[0136] Hardness: 9.6GPa
[0137] Fracture toughness: 2.9MPa·m 1 / 2
[0138] Bending strength: 370MPa
[0139] Optical linear transmittance: 15.73% at 800nm, 64% at 5200nm;
[0140] The method of this embodiment has simple process operation, low production cost, wide application range, and is easy for industrial production. It has significant industrial application value and is conducive to the large-scale industrial application of aluminum nitride transparent ceramics.
[0141] From the above embodiments, it can be seen that the transparent aluminum nitride ceramics textured along the c-axis prepared by the present invention have a high degree of densification, good linear optical transmittance, texture, thermal conductivity, and mechanical properties. The present invention effectively solves the difficulty of preparing transparent aluminum nitride ceramics with high thermal conductivity and good mechanical properties, and the preparation process does not require the use of an additional pressure-assisted system, has the advantages of simple process, low production cost, wide range of use, easy industrial production, significant industrial application value, and is conducive to the large-scale industrial application of aluminum nitride transparent ceramics.
[0142] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made according to the purpose of the invention of the present invention. Any changes, modifications, substitutions, combinations or simplifications made according to the spirit and principle of the technical solution of the present invention should be equivalent replacement methods. As long as they meet the purpose of the invention of the present invention and do not deviate from the technical principles and inventive concepts of the transparent aluminum nitride ceramics textured along the c-axis and the preparation method thereof, they belong to the protection scope of the present invention.
Claims
1. A method for preparing transparent aluminum nitride textured along the c-axis, characterized in that: The steps include: The selected aluminum nitride powder treated by the surface coating process, the sintering aid and the dispersant are added into the dispersion medium respectively, and the aluminum nitride slurry is prepared by the ball milling process; Performing slip casting molding on the aluminum nitride slurry under a magnetic field to prepare a ceramic blank with texture along the c-axis; Pre-treating the ceramic embryo; The pretreated ceramic blank is sintered to prepare transparent aluminum nitride ceramics.
2. The preparation method according to claim 1, characterized in that: The particle size of the aluminum nitride powder is 50nm-10um, and the powder purity is greater than or equal to 99%.
3. The preparation method according to claim 1, characterized in that: The sintering aid comprises at least one or more of an alkali metal compound, an alkaline earth metal compound, a rare earth metal compound and an aluminum-containing compound. The content of the sintering aid in the aluminum nitride slurry is between 0.1wt% and 7wt%.
4. The preparation method according to claim 1, characterized in that: The dispersant is polyvinylpyrrolidone (PVP), the molecular weight of the dispersant is between 3000 and 30000, and the content of the dispersant in the aluminum nitride slurry is between 0.1 wt% and 7 wt%.
5. The preparation method according to claim 1, characterized in that: The dispersion medium is deionized water or anhydrous ethanol; The aluminum nitride slurry is characterized in that the solid content of the slurry is higher than 30 vol% and the viscosity is between 20 and 20000 mPa·s.
6. The preparation method according to claim 1, characterized in that: The magnetic field type is any one of a static vertical magnetic field, a static horizontal magnetic field and a rotating magnetic field, and the intensity of the magnetic field is in the range of 1 to 20T.
7. The preparation method according to claim 6, characterized in that: In the preparation steps of the ceramic blank: a. The magnetic field is a static magnetic field, and the ceramic embryo rotates in the magnetic field; or, b. The ceramic embryo remains stationary, and the magnetic field rotates relative to the ceramic embryo; or, c. The ceramic green body and the magnetic field rotate simultaneously, and the rotation directions of the ceramic green body and the magnetic field are parallel or perpendicular to each other.
8. The preparation method according to claim 1, characterized in that: In the step of pre-treating the ceramic green blank, the ceramic green blank is subjected to debinding and isostatic pressing treatments; in, The debinding is carried out in air atmosphere or vacuum atmosphere, the debinding temperature is 450℃~800℃, and the debinding time is: 4h~72h; The isostatic pressing temperature is 25°C to 80°C, the pressure is 20MPa to 300MPa, and the holding time is 2min to 30min.
9. The preparation method according to claim 1, characterized in that: In the step of sintering the pre-treated ceramic green body, The sintering process adopts pressureless sintering, the sintering temperature is between 1600°C and 2000°C, the holding time is between 2 and 70 hours, and the sintering atmosphere is nitrogen or argon.
10. A transparent aluminum nitride, characterized in that: The method is prepared by any one of claims 1 to 9.
Citation Information
Patent Citations
Aluminum nitride ceramic slurry and preparation method thereof
CN107324812A
Transparent aln sintered body, and production method therefor
CN110072826A
Crystal grain woven multiphase ceramic material and preparation method thereof
CN112552051A
Aluminum nitride-based conductive ceramic and preparation method thereof
CN115677353A
Anti-hydration aluminum nitride powder as well as preparation method and application thereof
CN116003137A