Manganese tetrachloride pyridine quaternary ammonium salt, fiber film and preparation method thereof

By designing the combination of tetrachloromanganese pyridine quaternary ammonium salt and polylactic fiber film, the problem of poor effect of existing antibacterial materials is solved, and the luminescence under ultraviolet light and effective inhibition of bacteria is achieved, which demonstrates the high efficiency of green and environmental protection Antibacterial material, suitable for a variety of applications.

CN118955361APending Publication Date: 2024-11-15SOUTH CHINA AGRICULTURAL UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411031652.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-07-09
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing antibacterial materials have limitations in their bactericidal effects and environmental protection, and lack new organic-inorganic antibacterial materials with luminescence functions.

Method used

Design a quaternary ammonium tetrachloro-manganese pyridine salt, combined with polylactic fiber film, and prepare a material with luminescence and antibacterial activity through specific synthetic methods. This material emits green light under 365nm ultraviolet light and is used to treat E. coli and Staphylococcus aureus has good antibacterial activity.

Benefits of technology

The green light emission of the material under ultraviolet light irradiation and effective inhibition of a variety of bacteria is achieved. The preparation method is simple to operate and low cost, suitable for industrial production, and has green and environmentally friendly characteristics. It is suitable for future antibacterial agents and photodynamic bactericidal research.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955361A_ABST
    Figure CN118955361A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of nanofiber films, and particularly relates to a manganese tetrachloride pyridine quaternary ammonium salt, manganese tetrachloride is used as an anion, benzyl pyridine quaternary ammonium salt is used as a cation, and the manganese tetrachloride pyridine quaternary ammonium salt and a base material are subjected to near-field direct writing to prepare an ordered fiber film material. The manganese tetrachloride pyridine quaternary ammonium salt material shows a good green fluorescence effect under 365 nm ultraviolet irradiation, shows good antibacterial activity on staphylococcus aureus and escherichia coli, is a light-emitting and antibacterial bifunctional material, and can maintain green fluorescence and increase the antibacterial effect after being spun into a film. The preparation method is simple and convenient to operate and high in yield; required instruments and equipment are simple and easy to operate; and the method has the advantages of low solvent consumption, cost saving, wide application range and facilitation of industrial popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nanofiber films, and in particular relates to a quaternary ammonium tetrachloromanganese pyridinium salt with luminescence and antibacterial functions, a fiber film and a preparation method thereof. Background Art

[0002] As people's high standards for living hygiene are increasing, the limitations of existing antibacterial materials are becoming more and more obvious, and the development of new organic-inorganic antibacterial materials is imminent. Pyridine quaternary ammonium salts not only have excellent bactericidal and hydrophilic properties, but also have more active chemical properties and richer reactivity due to their conjugated aromatic pyridine ring structure and the electron-withdrawing effect of pyridine nitrogen atoms. They are good hydrogen bond acceptors and can be coordinated with metal halides to form organic-inorganic hybrid materials with excellent catalytic, antibacterial, magnetic and optical properties. Transition metal Mn is an emerging class of luminescent materials due to its rich valence states and special electronic structures, with a variety of coordination structures and interesting photophysical properties.

[0003] Polylactic acid (PLA) is a new type of biodegradable material, made from starch raw materials extracted from renewable plant resources (such as corn). It has excellent biocompatibility, glossiness, transparency and heat resistance. After use, it can be degraded by microorganisms in nature, eventually generating carbon dioxide and water, without causing pollution to the environment. Summary of the invention

[0004] One of the purposes of the present invention is to prepare a quaternary ammonium tetrachloromanganese pyridinium salt having luminescence and antibacterial activity, and to prepare a composite PLA fiber film, which can emit strong green light under 365nm ultraviolet light irradiation, and is achieved by the following technical scheme:

[0005] A tetrachloromanganese pyridinium quaternary ammonium salt is designed, with tetrachloromanganese as the anion and benzyl pyridinium quaternary ammonium salt as the cation, and the chemical structure is shown in the following formula:

[0006]

[0007] Preferably, the tetrachloromanganese pyridinium quaternary ammonium salt is a yellow-green blocky single crystal, belongs to the orthorhombic system, P212121 space group; the unit cell parameters are: α=90°, β=90°, γ=90°.

[0008] The present invention also provides a method for preparing tetrachloromanganese pyridinium quaternary ammonium salt, which has high yield, saves cost, is easy to operate, and is conducive to industrial production. The method comprises the following steps:

[0009] (1) placing a certain amount of benzyl bromide and pyridine in a container (the molar ratio is preferably 1:0.8-1.2), adding an appropriate amount of solvent (preferably acetone) to dissolve, and reacting at 65-70°C (stirring and refluxing for 18-24 hours); after the reaction (pour into a beaker while hot), standing to separate the layers, washing the lower layer of liquid with acetone and ether in turn, and volatilizing naturally to obtain a light yellow oily quaternary ammonium salt;

[0010] (2) placing a certain amount of the quaternary ammonium salt and manganese chloride tetrahydrate in a container (the molar ratio is preferably 1.8-2.2:1), using an appropriate amount of methanol as a solvent, and adding an appropriate amount of concentrated hydrochloric acid, reacting at 65-70° C. (stirring and reflux for 0.5-1.5 hours); after the reaction is completed (pour into a beaker while hot and heat), concentrating part of the solvent, cooling (in a fume hood) and crystallizing to obtain the tetrachloromanganese pyridinium quaternary ammonium salt of the present invention.

[0011] The tetrachloromanganese pyridinium quaternary ammonium salt of the present invention is further used to prepare a fiber film material, comprising the following steps:

[0012] A certain amount of substrate (polylactic acid PLA, polyvinyl chloride PVC or thermoplastic biodegradable plastic PBAT) and tetrachloromanganese pyridinium ammonium salt are added to a solvent (preferably, the mass ratio of the polylactic acid to the tetrachloromanganese pyridinium ammonium salt is 3-5:1, and the solvent is a mixed solvent of DMF and CHCl3, and the volume ratio of the two is preferably 1:8-10), and heated at 50-70°C for reaction for 1.5-2.5h; after the reaction, the material is allowed to stand for defoaming and near-field direct writing is performed to obtain a tetrachloromanganese pyridinium ammonium salt fiber film material.

[0013] Optimal near-field direct writing conditions: high voltage power supply voltage of 2.0-2.5 kV, receiving distance of 3.5-3.8 mm, liquid supply rate of 1.2-1.8 mL·h -1 , speed is 110-130mm·s -1 , acceleration is 500-700 mm·s -1 , ambient temperature 24-30℃, film width 50mm×50mm.

[0014] The present invention has the following positive and beneficial effects:

[0015] (1) The tetrachloromanganese pyridinium quaternary ammonium salt material of the present invention exhibits a good green fluorescence effect under 365nm ultraviolet light irradiation, and exhibits good antibacterial activity against Escherichia coli and Staphylococcus aureus, and is an excellent optical and antibacterial dual-energy material. After being spun into a film, it also has excellent luminescence properties and improved antibacterial effect. The preparation method of the present invention is simple to operate and has a high yield; the required instruments and equipment are simple and easy to operate; the required solvent consumption is small, cost-saving, and the application range is wide, which is conducive to industrial promotion.

[0016] (2) The Mn-based metal complex of the present invention is more environmentally friendly than the Cu-based metal complex. The transition metal Mn is an important component of photoluminescent materials because of its rich valence states and special electronic structure, and has the characteristics of diverse structures and excellent performance. The photoluminescent materials are combined with antibacterial materials to further explore the specific identification of induced emission light sources and explore photodynamic sterilization. It is of great significance in the future development of antibacterial agents, membrane sensors, pesticide detection, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 : is the crystal structure diagram of the tetrachloromanganese pyridinium quaternary ammonium salt of the present invention (hydrogen atoms are omitted);

[0018] Figure 2 This is a picture of the tetrachloromanganese pyridinium quaternary ammonium salt fiber film of the present invention under natural light (left: blank PLA film; right: tetrachloromanganese pyridinium quaternary ammonium salt fiber film);

[0019] Figure 3 This is a picture of the tetrachloromanganese pyridinium quaternary ammonium salt fiber film of the present invention under ultraviolet light irradiation (left: blank PLA film; right: tetrachloromanganese pyridinium quaternary ammonium salt fiber film);

[0020] Figure 4 The antibacterial zone diagram of the tetrachloromanganese pyridinium quaternary ammonium salt of the present invention against Staphylococcus aureus and Escherichia coli;

[0021] Figure 5 It is a graph showing the minimum inhibitory concentration of the tetrachloromanganese pyridinium quaternary ammonium salt and the tetrachloromanganese pyridinium quaternary ammonium salt fiber film against Escherichia coli and Staphylococcus aureus;

[0022] Figure 6 is the cation mass spectrum of [BzPy]2[MnCl4] of the present invention;

[0023] Figure 7 is the infrared spectrum of [BzPy]2[MnCl4] of the present invention;

[0024] Figure 8 The UV-visible diffuse reflectance spectrum and band gap diagram of [BzPy]2[MnCl4] of the present invention;

[0025] Fig. 9 This is the liquid fluorescence spectrum of [BzPy]2[MnCl4] of the present invention;

[0026] Fig.10 This is the solid fluorescence spectrum of [BzPy]2[MnCl4] of the present invention;

[0027] Fig.11 The luminescence effect diagram of the tetrachloromanganese pyridinium quaternary ammonium salt of the present invention (the left is powder and the right is crystal); DETAILED DESCRIPTION

[0028] In order to better understand the present invention, the technical solution of the present invention is described below through specific embodiments.

[0029] Example 1

[0030] A method for preparing a tetrachloromanganese pyridinium quaternary ammonium salt fiber film material comprises the following steps:

[0031] (1) Preparation of quaternary ammonium salt [BzPy]Cl: 5.13 g (0.03 mol) of benzyl bromide and 2.37 g (0.03 mol) of pyridine were weighed into a 100 mL ground-mouth conical flask, 30 mL of acetone was added to dissolve, and the mixture was stirred and refluxed at 65-70°C for 24 h. After the reaction, the mixture was poured into a beaker while hot, and allowed to stand for stratification. The upper layer of liquid was removed with a dropper, and then a small amount of acetone was added for washing. The upper layer of liquid was removed with a dropper, and the operation was repeated three times. The mixture was washed with ether three times according to the same steps as before, and then sealed with plastic wrap, pierced with a syringe, and evaporated naturally in a dark place to obtain a light yellow oily substance [BzPy]Cl.

[0032] (2) Preparation of tetrachloromanganese pyridinium ammonium salt [BzPy]2[MnCl4]: Take 10mmol [BzPy]Cl and 5mmol manganese chloride tetrahydrate in a conical flask, add 20mL methanol to dissolve, add 1mL concentrated hydrochloric acid (12mol / L), stir and reflux at 65-70℃ for 1h; after the reaction, pour into a beaker while hot, heat and concentrate, and let stand to cool; seal with plastic wrap, poke a hole with a needle, put it under a fume hood, and obtain crystals in about a week. Finally, yellow-green granular crystals of tetrachloromanganese pyridinium ammonium salt are obtained. The main crystallographic data are shown in Table 1, and the crystal structure is shown in Figure 1 .

[0033] Table 1 Main crystallographic data of tetrachloromanganese pyridinium quaternary ammonium salt of Example 1

[0034]

[0035] (3) Preparation of tetrachloromanganese pyridine quaternary ammonium salt fiber film material: PLA was added to a mixed solvent of DMF and CHCl3 (the volume ratio of DMF and CHCl3 was 1:9) with ten times its weight, and the above crystals with a weight of 20% of PLA were weighed and added to the bottle, the lid was covered, and the bottle was placed in a water bath at a constant temperature of 60°C and stirred for 2 hours; after ultrasonic defoaming, near-field direct writing was performed to obtain a milky white tetrachloromanganese pyridine quaternary ammonium salt fiber film material, which emitted green fluorescence under ultraviolet light. Near-field direct writing conditions: The voltage of the high-voltage power supply of the instrument was adjusted to 2.3 kV, the receiving distance was 3.6 mm, and the liquid supply rate was 1.5 mL·h -1 , speed is 120 mm·s -1 , acceleration is 600 mm·s-1 , ambient temperature 25℃, film width 50mm×50mm. The obtained fiber film has uniform fiber distribution and no obvious agglomeration, indicating that the near-field direct writing is relatively successful. The macroscopic image and the image under UV light are shown in Figure 2 and Figure 3 .

[0036] The antibacterial test was carried out by taking tetrachloromanganese pyridinium quaternary ammonium salt crystals. The specific implementation method is as follows: taking an appropriate amount of crystals and dissolving them in dimethyl sulfoxide (DMSO) solution to prepare 0.05 g mL -1 Place the sterilized and dried filter paper (6 mm in diameter) in the drug solution. Add 100 μL of 6.0×10 6 CFU·mL -1 Staphylococcus aureus bacterial suspension and 100 μL of 2.0×10 7 CFU·mL -1 Escherichia coli bacterial solution, evenly spread, add filter paper soaked in quaternary ammonium salt solution, seal the culture dish with a sealing strip, culture at 37℃ for 12h, and measure the diameter of the inhibition zone. See Table 2. Figure 4 .

[0037] Table 2 Antibacterial effect of tetrachloromanganese pyridinium quaternary ammonium salt of Example 1

[0038]

[0039] The composite fiber film was subjected to the minimum inhibitory concentration antibacterial test. The specific implementation method was as follows: 5 mm × 5 mm tetrachloromanganese pyridinium quaternary ammonium salt fiber film was cut and dissolved in dimethyl sulfoxide (DMSO) solution to prepare 0.05 g mL -1 Add 100 μL of liquid culture medium to the mixed solution, then use the 2-fold dilution method to dilute the sample in a gradient manner, and finally add the bacterial solution (the concentration of the bacterial solution is consistent with the above-mentioned inhibition zone method) and mix it by pipetting. Seal the 96-plate with a sealing film and place it in a constant temperature and humidity incubator at 37°C for 12 hours; finally, add 100 μL of TTC dye to the 96-plate for observation and calculate the minimum inhibitory concentration. See Table 3. Figure 5 .

[0040] Table 3 Antibacterial effect of tetrachloromanganese pyridinium quaternary ammonium salt fiber film of Example 1

[0041]

[0042]

[0043] The mass spectrum of the experimentally prepared [BzPy]2[MnCl4] is shown in Figure 6 As shown in the figure, it can be seen that the cation [BzPy]+ The measured molecular weight was 170.2, which was consistent with the theoretical value of 170.0.

[0044] The infrared spectrum of tetrachloromanganese pyridinium quaternary ammonium salt is shown in Figure 7 , 3125cm -1 The absorption peak at 3058cm is caused by the C─H stretching vibration of the benzene ring. -1 The absorption peak at 1630 cm-1 belongs to the C─H stretching vibration of the pyridine ring. -1 and 1584cm -1 The absorption peak at 1489 cm belongs to the C═C stretching vibration of the benzene ring and the C═C stretching vibration of the pyridine ring. -1 The absorption peak near 1456 cm belongs to the C═N stretching vibration of the pyridine ring. -1 The absorption peak at 1289 cm-1 belongs to the methylene C─H bending vibration. -1 The C─H in-plane bending vibration of the benzene ring is 1159 cm -1 The absorption peak at 860cm- -1 The absorption peak at 753 cm is the C─H out-of-plane bending vibration of the pyridine ring. -1 、708cm -1 and 678cm -1 The nearby absorption peaks all belong to the C─H out-of-plane bending vibration of the benzene ring.

[0045] The obtained material was tested by UV-visible diffuse reflectance spectroscopy and the optical band gap was calculated. Figure 8 The wavelength corresponding to the highest absorption peak is 330nm, and the optical band gap is 2.44eV. It has a certain absorption capacity for visible light. This band gap value is within the range of typical semiconductor materials and is comparable to the values ​​of other halide metal compounds studied as potential solar absorbers.

[0046] The liquid fluorescence spectrum of the experimentally obtained crystal [BzPy]2[MnCl4] is shown in Fig. 9 Although the solution becomes transparent when the crystals are dissolved in water, the fluorescence intensity of the substance can still be measured, with the highest intensity at 535nm, providing experimental support for subsequent application research.

[0047] The solid fluorescence emission spectrum of [BzPy]2[MnCl4] is as follows Fig.10 Its emission peak is located near 511nm, which is due to the transition between molecular orbitals caused by the transfer of electrons from the p orbital of nitrogen atoms to the d orbital of metal ions (charge transfer band), and the Mn 2+The wavelength range of green light is between 492 and 577 nm, so from the measured data, we can know that the crystal can emit green fluorescence, which is consistent with the fluorescence color emitted under ultraviolet light. Fig.11 .

Claims

1. A tetrachloromanganese pyridinium quaternary ammonium salt, characterized in that: With tetrachloromanganese as anion and benzylpyridinium quaternary ammonium salt as cation, the chemical structure is shown in the following formula:

2. The tetrachloromanganese pyridinium quaternary ammonium salt according to claim 1, characterized in that: The tetrachloromanganese pyridinium quaternary ammonium salt is a single crystal material, belongs to the orthorhombic system, and has a space group of P212121.

3. The tetrachloromanganese pyridinium quaternary ammonium salt according to claim 2, characterized in that: The unit cell parameters of the tetrachloromanganese pyridinium quaternary ammonium salt are: α=90°, β=90°, γ=90°.

4. The method for preparing the tetrachloromanganese pyridinium quaternary ammonium salt according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) placing a certain amount of benzyl bromide and pyridine in a container, adding an appropriate amount of solvent to dissolve them, and reacting them at 65-70° C.; after the reaction, standing and stratifying, washing the lower layer of liquid with acetone and ether in turn, and volatilizing them naturally to obtain a quaternary ammonium salt; (2) placing a certain amount of the quaternary ammonium salt and manganese chloride tetrahydrate in a container, taking an appropriate amount of methanol as a solvent, adding an appropriate amount of concentrated hydrochloric acid, and reacting at 65-70° C.; after the reaction is completed, concentrating part of the solvent, cooling and crystallizing, to obtain the tetrachloromanganese pyridinium quaternary ammonium salt of the present invention.

5. The preparation method according to claim 4, characterized in that: The molar ratio of benzyl bromide to pyridine used in step (1) is 1:(0.8-1.2); and the molar ratio of the quaternary ammonium salt to manganese chloride tetrahydrate in step (2) is (1.8-2.2):

1.

6. The preparation method according to claim 4, characterized in that: The solvent used in step (1) is acetone; the reaction conditions in step (1) are stirring and reflux for 18-24 hours; the reaction conditions in step (2) are stirring and reflux for 0.5-1.5 hours.

7. A tetrachloromanganese pyridinium quaternary ammonium salt fiber film, characterized in that: The invention is prepared from the tetrachloromanganese pyridinium quaternary ammonium salt according to any one of claims 1 to 3, a substrate and a solvent.

8. The method for preparing the tetrachloromanganese pyridinium quaternary ammonium salt fiber film material according to claim 7, characterized in that: The following steps are involved: A certain amount of substrate and tetrachloromanganese pyridinium quaternary ammonium salt are added to a solvent, and the mixture is heated at 50-70° C. for reaction for 1.5-2.5 hours. After the reaction, the mixture is allowed to stand for defoaming and near-field direct writing is performed to obtain a tetrachloromanganese pyridinium quaternary ammonium salt fiber film material.

9. The preparation method according to claim 8, characterized in that: The mass ratio of the polylactic acid to the tetrachloromanganese pyridinium quaternary ammonium salt is (3-5):1; the solvent is a mixed solvent of DMF and CHCl3, and the volume ratio of the two is 1:(8-10); the substrate is polylactic acid, polyvinyl chloride or thermoplastic biodegradable plastic.

10. The preparation method according to claim 8, characterized in that: The near-field direct writing conditions are: high voltage power supply voltage of 2.0-2.5 kV, receiving distance of 3.5-3.8 mm, liquid supply rate of 1.2-1.8 mL·h -1 , speed is 110-130mm·s -1 , acceleration is 500-700 mm·s -1 , ambient temperature 24-30℃.

Citation Information

Patent Citations

  • Manganese tetrachloride composite quaternary ammonium salt, fiber film material and preparation method thereof

    CN115057812A