Polyester type polymer chelating dispersant as well as preparation method and application thereof
Through the use of polyester polymer chelating dispersants, the problems of poor heat resistance and insufficient affinity of dispersants in the prior art have been solved, and the stability of high-temperature and high-pressure dyeing and the improvement of soap washing performance are achieved, and the process is simplified. Reduced environmental impact.
Patent Information
- Application Number
- CN202411258719.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-15
AI Technical Summary
The existing dispersants have poor heat resistance and stability, complex process and high cost during high temperature and high pressure dyeing, and have insufficient affinity for polyester oligomers and dispersed dyes, resulting in poor dyeing effect and poor environmental protection.
Polyester polymer chelating dispersant is used. The combination of polyester links and polycarboxylic acid links in its molecular structure provides strong affinity and chelation, forming a "core-shell" structure for dispersing dye dyeing and soap Wash, simplify the process.
It has achieved the improvement of dyeing stability and soap washing performance under high temperature and high pressure conditions, simplified the process, reduced environmental impact and production costs, and expanded the scope of application.
Smart Images

Figure BDA0005034865700000121 
Figure BDA0005034865700000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textiles, and in particular to a polyester type polymer chelating dispersant and a preparation method and application thereof. Background Art
[0002] At present, in the process of dyeing polyester fibers with disperse dyes in a high-temperature and high-pressure dye bath, in order to inhibit the melting and aggregation of disperse dyes and their crystal transformation under the action of alternating cold and hot, and to ensure the thermal stability of the dye bath and the stability of the dye aggregation state, a high-temperature leveling agent based on a composite system of nonionic surfactants and anionic surfactants or a dispersant such as lignin, cardanol, polycarboxylic acid, and naphthalenesulfonic acid formaldehyde condensate is often added to the dye bath. Among them, the heat stability of naphthalenesulfonic acid formaldehyde condensate dispersant is not high, and the raw material cost is high; the reaction conditions of polycarboxylic acid dispersants are harsh, the process is complex, and the industrialization cost is high. In addition, the weakly hydrophilic polyester oligomers produced in the high-temperature and high-pressure dyeing process of polyester fibers also need to be relatively effectively removed under high temperature and alkaline conditions with the help of surfactants (or dispersants). At the same time, in order to fully remove the floating color after dyeing, the non-water-soluble disperse dyes have to be reduced and soaped under alkaline and reducing conditions. The above process technologies not only have high energy consumption, complicated process, and poor environmental protection, but also their process effects are not satisfactory. Theoretically, the above confusion is due to the fact that traditional dispersants, leveling agents, and soaping agents have significantly insufficient affinity for polyester oligomers and disperse dyes, and their hydrophilicity / water solubility is sensitive to hard water and high temperature, and even fail at high temperature.
[0003] Specifically, the common dispersants and leveling agents related to polyester fibers or disperse dyes mainly include the following:
[0004] 1. Cardanol-based dispersants and high-temperature leveling agents for disperse dyes, mainly including cardanol sulfonates, cardanol sulfates, cardanol ethoxylates, cardanol carboxylates, cardanol quaternary ammonium salts and gemini surfactants.
[0005] For example, in "Preparation and Dyeing Properties of Highly Dispersible Hard Water Resistant High Temperature Leveling Agents" (Volume 37, No. 8, 2020) written by Zhang Shenggang, Liu Yuqing, etc., the complex of cardanol polyoxyethylene ether TF-n (EOn=3, 5, 7, 9, 10) and cardanol polyoxyethylene ether ammonium sulfonate was used for high temperature and high pressure dyeing with disperse dyes. The dispersion, slow dyeing, migration and dyeing effects (color yield, dyeing fastness, etc.) showed that the cardanol-based disperse dye high temperature leveling agent has better slow dyeing properties for disperse dyes than the traditional AB type high temperature leveling agent composed of glycerol polyoxyethylene ether oleate and styrylphenol polyoxyethylene ether sulfonate, and the difference in dyeing performance between the two under hard water conditions is more obvious; at the same time, the two are relatively close in migration performance.
[0006] For example, the book "Synthesis of Biomass Cardanol-Based High-Temperature Leveling Agents" written by Li Haonan and Wang Shugen (Journal of Xi'an Polytechnic University, Vol. 29, No. 6, 2015) discloses a high-temperature leveling agent of cardanol polyoxyethylene ether sulfate generated by sulfonation of biomass cardanol polyoxyethylene ether with aminosulfonic acid. It was found that cardanol polyoxyethylene ether sulfate has good dispersing ability for disperse dyes, and has good leveling and migration properties for high-temperature dyeing of polyester fabrics. Its leveling and migration properties for disperse dye-dyed polyester fabrics are roughly the same as those of commercially available high-temperature leveling agents.
[0007] However, although the highly dispersible, hard water resistant and high temperature leveling agents in the literature contain aromatic ring structures with good affinity for polyester and disperse dyes, such composite surfactant dispersants or high temperature leveling agents composed of "hydrophilic + hydrophobic" and "non-ionic + anionic" structures still have problems such as poor hard water resistance, poor high temperature resistance, and weak dispersion and chelation ability due to weak ionicity, lack of common structure with the dispersed objects (dispersed dyes, polyester oligomers), lack of effective chelating structure, and serious deterioration of hydrophilicity of the polyether chain segments on them that are important for dispersing power at high temperatures.
[0008] 2. Lignin-based disperse dye dispersants and high-temperature leveling agents, mainly including lignin sulfonates, a by-product of acid pulping, and alkali lignin sulfonates, a by-product of alkaline pulping.
[0009] For example, the book "Preparation and Performance of High-temperature Sulfonmethylated Alkali Lignin Dye Dispersant" written by Zhang Zhiming, Zhou Mingsong, Yang Dongjie, etc. (Fine Chemicals, Vol. 31, No. 12, 2014) discloses the preparation of sulfomethylated alkali lignin by sulfomethylation reaction of formaldehyde and sodium bisulfite at high temperature using acid-precipitated alkali lignin as raw material. It was found that the sulfonate content of sulfomethylated alkali lignin was 1.2-1.4 mmol / g, which had better comprehensive performance, especially its high-temperature stability was significantly better than that of traditional commercial dye dispersants, but it still had a certain staining property on the fiber.
[0010] For example, the book "Study on the Preparation and Application of Lignin-based Dye Dispersants" written by Liu Zhipeng and Liu Minghua (Volume 23, Issue 3, 2015) discloses that lignin-based dye dispersants are prepared by using lignin as raw material, carboxylating it, and then performing hydroxymethylation and sulfonation reactions with formaldehyde and sodium bisulfite. It is found that the dispersion grade of disperse dyes can reach 5.0, which has reached the commercial requirements in terms of dispersion performance, and the product can maintain good dispersion performance at 150°C.
[0011] However, although the higher the sulfonic acid content of lignin, the lower the staining rate of polyester fibers, even so, its staining is still higher than that of traditional commercial dye dispersants; at the same time, the sulfonation modification of lignin usually requires the assistance of formaldehyde, resulting in poor environmental protection of the product. Similarly, since lignin sulfonate lacks the common structure and effective chelating structure with the dispersed object (polyester oligomer, disperse dye), it still cannot meet the requirements of effectively cleaning the floating color of dyed polyester in the absence of the support of a reducing and alkaline environment.
[0012] 3. Polycarboxylic acid dispersants and soaping agents, mainly copolymers of maleic acid and acrylic acid or complexes based thereon.
[0013] For example, the copolymer of maleic anhydride and acrylic acid (acidic soaping agent) disclosed in "Acidic Soaping of Maleic Anhydride Acrylic Acid Polymer" written by Song Qingshuang, Zheng Qingkang and Du Gaomin ("Knitting Industry" 2013 Issue 1) has a higher K / S value, color saturation and various color fastnesses after the dyed fabric is washed with an acidic soaping agent; compared with the traditional soaping process based on surfactants, the K / S value and color saturation of the fabric after washing with an acidic soaping agent are higher, the dye hydrolysis is less, the various color fastnesses are improved or remain the same, and it has a significant water-saving effect.
[0014] As disclosed in the book "Development and Application of New Acidic Soaping Agent" written by Yan Zi (Journal of Xi'an Polytechnic University, Vol. 25, No. 6, 2011), maleic anhydride, acrylic acid, and N-vinyl pyrrolidone are copolymerized, and then compounded with carboxyethyl thiosuccinic acid and hydroxyethylidene diphosphonic acid to prepare a new acidic soaping agent. The study found that the color of the fabric washed with the new acidic soaping agent is brighter and has higher color fastness than that of the fabric washed with ordinary soaping agents; at the same time, because of its extremely strong acidity, it can be used to replace acetic acid for neutralization, and the soaping process is simpler.
[0015] However, although polycarboxylic acid acid soaping agents have good dispersibility, no foaming, and low preparation cost, their anti-staining properties are not ideal. Similarly, since polycarboxylic acid acid soaping agents lack the common structure with polyester oligomers and disperse dyes, they cannot be used in the dyeing and soaping process of disperse dyes on polyester fibers, and cannot meet the requirements of effectively cleaning the floating color of dyed polyester in the absence of a reducing and alkaline environment. Summary of the invention
[0016] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art and provide a polyester-type polymer chelating dispersant and its preparation method and application. The polyester-type polymer chelating dispersant can be used as a high-temperature leveling agent and a reduction-free soaping agent for disperse dye dyeing, and can also be used for aqueous dispersion of polyester material micropowders, surface hydrophilic modification, and inhibition of aggregation tendency of water-based disperse dyes. In the present invention, the polyester chain segments in the molecular structure of the product have good affinity for polyester oligomers and disperse dyes; at the same time, the numerous "ortho-carboxyl groups + isolated carboxyl groups" on the polycarboxylic acid chain segments and the "isolated sulfonic acid groups" on the polyester macromolecules in the molecular structure of the product give it excellent "chelating + dispersing" power; in addition, the "core-shell" structure of the product composed of the polyester "core" and the polycarboxylic acid "shell" enables it to provide excellent thermodynamic stabilization for polyester oligomers and disperse dyes, thereby giving it excellent leveling and soaping properties for disperse dyes, greatly expanding its application range.
[0017] In order to achieve the above object, the present invention provides a method for preparing a polyester polymer chelating dispersant, which method comprises the following steps:
[0018] (1) Raw material preparation: The raw materials include an ester exchange catalyst, an aromatic dimethyl ester, a diol, a diisocyanate, an unsaturated hydroxyalkyl ester, an unsaturated anionic monomer, an initiator, water, and an optional organic solvent;
[0019] Wherein, the transesterification catalyst is zinc acetate;
[0020] The aromatic dimethyl esters are dimethyl 5-sulfonate sodium isophthalate, dimethyl terephthalate and dimethyl phthalate;
[0021] The diol is selected from one or more of ethylene glycol, 1,4-butanediol, 1,6-hexanediol and diethylene glycol;
[0022] The diisocyanate is toluene diisocyanate or isophorone diisocyanate;
[0023] The unsaturated hydroxyalkyl ester is hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate or hydroxypropyl methacrylate;
[0024] The unsaturated anionic monomers are maleic anhydride and acrylic acid;
[0025] The initiator is potassium persulfate or ammonium persulfate;
[0026] The organic solvent is propylene glycol methyl ether acetate;
[0027] The molar fractions of the components in the raw materials are: 5 for aromatic dimethyl ester, 6 to 10 for diol, the molar fraction of diisocyanate = 2×(the molar fraction of diol-the molar fraction of aromatic dimethyl ester), and the molar fraction of unsaturated hydroxyalkyl ester is 1 to 1.1 times the molar fraction of diisocyanate;
[0028] The weight of the unsaturated anionic monomer is 0.5 to 1.5 times the total weight of the aromatic dimethyl ester and the diol;
[0029] Based on the total molar amount of the aromatic dimethyl ester, the molar proportion of dimethyl isophthalate-5-sodium sulfonate is 10-30%, the molar proportion of dimethyl terephthalate is 30-60%, and the molar proportion of dimethyl phthalate is 30-60%;
[0030] Based on the total weight of the unsaturated anionic monomer, the content of maleic anhydride is 30 to 70 wt %;
[0031] (2) Transesterification: reacting a transesterification catalyst, an aromatic dimethyl ester and a diol to obtain a polyester-type polymer chelating dispersant primary polymer;
[0032] (3) End-capping: reacting a polyester-type polymer chelating dispersant prepolymer, a diisocyanate, an unsaturated hydroxyalkyl ester and an organic solvent to obtain a polyester-type polymer chelating dispersant intermediate;
[0033] (4) Polymerization: The polyester type polymer chelating dispersant intermediate, unsaturated anionic monomer, initiator and water are reacted to prepare the polyester type polymer chelating dispersant.
[0034] Preferably, the amount of the transesterification catalyst used is 0.4-0.8 wt % of the total weight of the aromatic dimethyl ester and the diol.
[0035] Preferably, the amount of the initiator used is 0.5-1 wt % of the total weight of the unsaturated hydroxyalkyl ester and the unsaturated anionic monomer.
[0036] Preferably, the amount of the organic solvent used is 0 to 1 times the total weight of the aromatic dimethyl ester, diol, diisocyanate and unsaturated hydroxyalkyl ester.
[0037] Preferably, the amount of water used is 1 to 2 times the total weight of the aromatic dimethyl ester, diol, diisocyanate, unsaturated hydroxyalkyl ester and unsaturated anionic monomer.
[0038] Preferably, the specific process of step (2) includes:
[0039] (2.1) Adding an ester exchange catalyst, an aromatic dimethyl ester and a diol into a reactor, heating the reaction system to 150 to 200° C. within 10 to 30 minutes, and keeping the temperature under nitrogen protection, condensation reflux and stirring for 50 to 100 minutes;
[0040] (2.2) The reaction system in step (2.1) is heated to 200-250° C. within 10-30 minutes, and the reaction is kept warm for 50-100 minutes under nitrogen protection, condensation reflux and stirring to obtain a polyester-type polymer chelating dispersant prepolymer.
[0041] Preferably, the specific process of step (3) includes:
[0042] (3.1) cooling the reaction system in step (2) to 150-200° C., adding an organic solvent and a diisocyanate, and then reacting at 150-200° C. under nitrogen protection, condensation reflux and stirring for 20-40 minutes;
[0043] (3.2) Add unsaturated hydroxyalkyl ester to the reaction system in step (3.1), and continue the reaction for 20 to 40 minutes to obtain a polyester-type polymer chelating dispersant intermediate.
[0044] Preferably, the specific process of step (4) includes:
[0045] (4.1) cooling the reaction system in step (3) to 80-110° C., removing the reflux device, adding unsaturated anionic monomers and 40-60 wt % of water in total, and shearing and dispersing at 60-80° C. to obtain a dispersion, and then taking out 70-90 wt % of the dispersion for later use;
[0046] (4.2) adding 35-45 wt% of water and 20-40 wt% of initiator to the remaining dispersion in step (4.1) under stirring, and maintaining stirring reaction at 70-90° C. for 20-60 min; controlling the temperature of the reaction system to 70-90° C. and adding 5-15 wt% of water, the remaining initiator and 70-90 wt% of the dispersion taken out in step (4.1) within 40-90 min; and then continuing the reaction at 70-90° C. for 30-60 min;
[0047] (4.3) While stirring, the reaction system in step (4.2) is cooled to below 50° C. to obtain a polyester-type polymer chelating dispersant.
[0048] The second aspect of the present invention provides a polyester polymer chelating dispersant prepared according to the method described above.
[0049] The third aspect of the present invention provides the use of the polyester polymer chelating dispersant described above in the disperse dye dyeing process.
[0050] Compared with the prior art, the present invention has the following beneficial effects:
[0051] 1. In the present invention, the polyester chain segments in the product molecular structure have a universal affinity for disperse dyes and polyester molecules (i.e., affinity under any process environment), and this affinity is simple, direct, and clear. This affinity based on the principle of "like is compatible" enables it to have excellent dye bath stabilization and leveling effects in the dyeing system of disperse dyes on polyester fibers, thereby making a simple, direct and efficient dyeing heating process possible. In particular, the polyester-type polymer chelating dispersant described in the present invention has a strong affinity for disperse dyes and polyester oligomers, and the good chelating and dispersing ability of the polycarboxylic acid network thereon enables it to achieve effective cleaning of disperse dye-dyed fabrics without the assistance of reducing agents and alkali agents, and the post-dyeing cleaning process is simple and environmentally friendly.
[0052] 2. In the present invention, the numerous "vicinal carboxyl groups + isolated carboxyl groups" on the polycarboxylic acid network chain links and the "isolated sulfonic acid groups" on the polyester macromolecules in the product molecular structure give it excellent "chelating + dispersing" power. These two characteristic chemical structures provide excellent complementarity for the chelating and dispersing properties of the product, thereby further enhancing its dispersing, chelating, cleaning and other properties.
[0053] 3. In the present invention, the "core" formed by the polyester segments and the "shell" formed by the polycarboxylic acid network together constitute the "core-shell" structure of the product. This special physical and chemical structure enables the product of the present invention to provide excellent thermodynamic stabilization for polyester oligomers and disperse dyes, thereby giving it excellent leveling and soaping properties for disperse dyes, greatly enhancing its performance characteristics and expanding its application range.
[0054] 4. The polyester-type polymer chelate dispersant of the present invention has excellent water dispersibility and hard water chelate / softening ability, and has good affinity for polyester oligomers and disperse dyes. Therefore, it can be used as a leveling agent for dyeing polyester fibers with disperse dyes in a high-temperature and high-pressure dye bath, or as a reduction-free soaping agent in the soaping process after dyeing, so as to simplify the process and enhance the process effect. DETAILED DESCRIPTION
[0055] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0056] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0057] On the one hand, the present invention provides a method for preparing a polyester-type polymer chelating dispersant. The method comprises the following steps:
[0058] (1) Raw material preparation: The raw materials include an ester exchange catalyst, an aromatic dimethyl ester, a diol, a diisocyanate, an unsaturated hydroxyalkyl ester, an unsaturated anionic monomer, an initiator, water, and an optional organic solvent;
[0059] Wherein, the transesterification catalyst is zinc acetate;
[0060] The aromatic dimethyl esters are dimethyl 5-sulfonate sodium isophthalate, dimethyl terephthalate and dimethyl phthalate;
[0061] The diol is selected from one or more of ethylene glycol, 1,4-butanediol, 1,6-hexanediol and diethylene glycol;
[0062] The diisocyanate is toluene diisocyanate or isophorone diisocyanate;
[0063] The unsaturated hydroxyalkyl ester is hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate or hydroxypropyl methacrylate;
[0064] The unsaturated anionic monomers are maleic anhydride and acrylic acid;
[0065] The initiator is potassium persulfate or ammonium persulfate;
[0066] The organic solvent is propylene glycol methyl ether acetate;
[0067] The molar fractions of the components in the raw materials are: 5 for aromatic dimethyl ester, 6 to 10 for diol, the molar fraction of diisocyanate = 2×(the molar fraction of diol-the molar fraction of aromatic dimethyl ester), and the molar fraction of unsaturated hydroxyalkyl ester is 1 to 1.1 times the molar fraction of diisocyanate;
[0068] The weight of the unsaturated anionic monomer is 0.5 to 1.5 times the total weight of the aromatic dimethyl ester and the diol;
[0069] Based on the total molar amount of the aromatic dimethyl ester, the molar proportion of dimethyl isophthalate-5-sodium sulfonate is 10-30%, the molar proportion of dimethyl terephthalate is 30-60%, and the molar proportion of dimethyl phthalate is 30-60%;
[0070] Based on the weight of the unsaturated anionic monomer, the content of maleic anhydride is 30 to 70 wt %;
[0071] (2) Transesterification: reacting a transesterification catalyst, an aromatic dimethyl ester and a diol to obtain a polyester-type polymer chelating dispersant primary polymer;
[0072] (3) End-capping: reacting a polyester-type polymer chelating dispersant prepolymer, a diisocyanate, an unsaturated hydroxyalkyl ester and an organic solvent to obtain a polyester-type polymer chelating dispersant intermediate;
[0073] (4) Polymerization: The polyester type polymer chelating dispersant intermediate, unsaturated anionic monomer, initiator and water are reacted to prepare the polyester type polymer chelating dispersant.
[0074] In a preferred embodiment, the amount of the transesterification catalyst is 0.4-0.8 wt% of the total weight of the aromatic dimethyl ester and the diol; specifically, it can be 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt% or 0.8 wt%.
[0075] In a preferred embodiment, the amount of the initiator is 0.5-1 wt% of the total weight of the unsaturated hydroxyalkyl ester and the unsaturated anionic monomer; specifically, it can be 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt% or 1 wt%.
[0076] In a preferred embodiment, the amount of the organic solvent used is 0 to 1 times the total weight of the aromatic dimethyl ester, diol, diisocyanate and unsaturated hydroxyalkyl ester.
[0077] In a preferred embodiment, the amount of water used is 1 to 2 times the total weight of the aromatic dimethyl ester, diol, diisocyanate, unsaturated hydroxyalkyl ester and unsaturated anionic monomer. Further, in steps (4.1)-(4.2), water is added three times.
[0078] Preferably, the water is soft water having a total hardness not exceeding 50 ppm CaCO3.
[0079] In a preferred embodiment, the specific process of step (2) includes:
[0080] (2.1) Adding an ester exchange catalyst, an aromatic dimethyl ester and a diol into a reactor, heating the reaction system to 150 to 200° C. within 10 to 30 minutes, and keeping the temperature under nitrogen protection, condensation reflux and stirring for 50 to 100 minutes;
[0081] (2.2) The reaction system in step (2.1) is heated to 200-250° C. within 10-30 minutes, and the reaction is kept warm for 50-100 minutes under nitrogen protection, condensation reflux and stirring to obtain a polyester-type polymer chelating dispersant prepolymer.
[0082] In the method of the present invention, in step (2.1), the distilled by-products can be separated during the heating and insulation period; in step (2.2), the distilled by-products can be separated during the heating and insulation period.
[0083] In a preferred embodiment, the specific process of step (3) includes:
[0084] (3.1) cooling the reaction system in step (2) to 150-200° C., adding an organic solvent and a diisocyanate, and then reacting at 150-200° C. under nitrogen protection, condensation reflux and stirring for 20-40 minutes;
[0085] (3.2) Add unsaturated hydroxyalkyl ester to the reaction system in step (3.1), and continue the reaction for 20 to 40 minutes to obtain a polyester-type polymer chelating dispersant intermediate.
[0086] In the method described in the present invention, in step (3.2), the reaction conditions (temperature, nitrogen protection, condensation reflux and stirring) when continuing the reaction are consistent with the reaction conditions in step (3.1).
[0087] In a preferred embodiment, the specific process of step (4) includes:
[0088] (4.1) cooling the reaction system in step (3) to 80-110° C., removing the reflux device, adding unsaturated anionic monomers and 40-60 wt % of water in total, and shearing and dispersing at 60-80° C. to obtain a dispersion, and then taking out 70-90 wt % of the dispersion for later use;
[0089] (4.2) adding 35-45 wt% of water and 20-40 wt% of initiator to the remaining dispersion in step (4.1) under stirring, and maintaining stirring reaction at 70-90° C. for 20-60 min; controlling the temperature of the reaction system to 70-90° C. and adding 5-15 wt% of water, the remaining initiator and 70-90 wt% of the dispersion taken out in step (4.1) within 40-90 min and controlling the reaction temperature to 70-90° C.; and then continuing the reaction at 70-90° C. for 30-60 min;
[0090] (4.3) While stirring, the reaction system in step (4.2) is cooled to below 50° C. to obtain a polyester-type polymer chelating dispersant.
[0091] In the method of the present invention, in step (4.1), a portion of the obtained dispersion is taken out for use, and the remaining portion is retained in the reactor; that is, the obtained dispersion is divided into two parts, of which the taken out portion accounts for 70-90wt% and the remaining portion accounts for 10-30wt%.
[0092] In the method described in the present invention, in step (4.2), when a total amount of 35-45wt% of water and a total amount of 20-40wt% of initiator are added to the remaining dispersion in step (4.1), the initiator and water can be first mixed to prepare an initiator aqueous solution, and then the initiator aqueous solution is added to the dispersion.
[0093] In the method of the present invention, in step (4.2), when adding a total amount of 5-15wt% of water, the remaining initiator and 70-90wt% of the dispersion liquid taken out in step (4.1) within 40-90min, water and initiator can be first mixed to prepare an initiator aqueous solution, and then the initiator aqueous solution and the dispersion liquid can be simultaneously dripped into the reaction system. Specifically, two dripping devices can be used to respectively contain the initiator aqueous solution and the dispersion liquid, and then simultaneously dripped into the reaction system.
[0094] The second aspect of the present invention provides a polyester polymer chelating dispersant prepared according to the method described above.
[0095] The polyester-type polymer chelating dispersant prepared by the method of the present invention can be used as a high-temperature leveling agent and a reduction-free soaping agent for disperse dye dyeing, and can also be used for aqueous dispersion of polyester material micropowders, surface hydrophilic modification, and inhibition of aggregation tendency of water-based disperse dyes. In the present invention, the polyester-type polymer chelating dispersant has excellent affinity and excellent "chelating + dispersing" power for disperse dyes and polyester oligomers, can provide a significant positive and beneficial thermodynamic stabilization effect on disperse dye dye baths, and further endows it with excellent leveling and soaping properties for disperse dyes, which has significant positive significance for simplifying the disperse dye dyeing process.
[0096] The polyester type polymer chelating dispersant product of the present invention must be sealed and stored in a cool and dry place.
[0097] The third aspect of the present invention provides the use of the polyester polymer chelating dispersant described above in the disperse dye dyeing process.
[0098] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto.
[0099] Table 1
[0100]
[0101]
[0102] Example 1
[0103] (1) Raw material preparation, the specific selection and dosage of the raw materials are shown in Table 1;
[0104] (2) an ester exchange step, in which an ester exchange catalyst, an aromatic dimethyl ester, and a diol are reacted to obtain a polyester-type polymer chelating dispersant primary polymer;
[0105] (2.1) Add transesterification catalyst, aromatic dimethyl ester and diol into the reactor, heat the reaction system to 175±1°C within 22 minutes, and keep the temperature for 75 minutes under nitrogen protection, condensation reflux and stirring. During the heating and heat preservation period, separate the distilled by-products;
[0106] (2.2) heating the reaction system in step (2.1) to 235±1° C. within 25 min, and keeping the temperature under nitrogen protection, condensation reflux and stirring for 75 min, separating the distilled by-products during the heating and keeping temperature period to obtain a polyester-type polymer chelating dispersant primary polymer;
[0107] (3) an end-capping step, in which the polyester-type polymer chelating dispersant primary polymer is reacted with diisocyanate, unsaturated hydroxyalkyl ester, and organic solvent to obtain a polyester-type polymer chelating dispersant intermediate;
[0108] (3.1) The reaction system in step (2.2) was cooled to 175±1°C, and an organic solvent and diisocyanate were added, and the reaction was carried out at 175±1°C, under nitrogen protection, condensation reflux and stirring for 35 minutes;
[0109] (3.2) adding unsaturated hydroxyalkyl ester to the reaction system in step (3.1), and continuing the reaction for 35 minutes at 175±1° C., under nitrogen protection, condensation reflux and stirring, to obtain a polyester-type polymer chelating dispersant intermediate;
[0110] (4) A step of initiating polymerization, in which the polyester-type polymer chelate dispersant intermediate is reacted with an unsaturated anionic monomer, an initiator and water to obtain a polyester-type polymer chelate dispersant.
[0111] (4.1) The reaction system in step (3.2) is cooled to 95±1°C, the reflux device is removed, unsaturated anionic monomers and 50 wt% of water are added, and the mixture is fully sheared and dispersed at 75±1°C to obtain a dispersion, and 80 wt% of the dispersion is taken out for later use;
[0112] (4.2) under stirring, add 40 wt% of water and 40 wt% of initiator (water and initiator are pre-mixed to prepare an initiator aqueous solution) to the remaining dispersion in step (4.1), and maintain stirring reaction at 80±1°C for 50 min; control the temperature of the reaction system to 80±1°C and uniformly add the initiator aqueous solution (prepared using 10 wt% of water and the remaining initiator) and the dispersion taken out in step (4.1) dropwise within 85 min; then continue the reaction at 80±1°C for 50 min;
[0113] (4.3) While stirring, the reaction system in step (4.2) is cooled to below 50° C. to obtain a polyester-type polymer chelating dispersant.
[0114] Example 2
[0115] (1) Raw material preparation, the specific selection and dosage of the raw materials are shown in Table 1;
[0116] (2) an ester exchange step, in which an ester exchange catalyst, an aromatic dimethyl ester, and a diol are reacted to obtain a polyester-type polymer chelating dispersant primary polymer;
[0117] (2.1) Add transesterification catalyst, aromatic dimethyl ester and diol into the reactor, heat the reaction system to 180±1°C within 18 minutes, stir and keep the temperature under nitrogen protection and condensation reflux for 85 minutes, and separate the distilled by-products during the heating and keeping temperature;
[0118] (2.2) heating the reaction system in step (2.1) to 235±1° C. within 18 minutes, and keeping the temperature under nitrogen protection, condensation reflux and stirring for 85 minutes, separating the distilled by-products during the heating and keeping temperature period to obtain a polyester-type polymer chelating dispersant primary polymer;
[0119] (3) an end-capping step, in which the polyester-type polymer chelating dispersant primary polymer is reacted with diisocyanate, unsaturated hydroxyalkyl ester, and organic solvent to obtain a polyester-type polymer chelating dispersant intermediate;
[0120] (3.1) The reaction system in step (2.2) was cooled to 165±1°C, an organic solvent and a diisocyanate were added, and then the reaction was continued at 165±1°C, under nitrogen protection, condensation reflux and stirring for 30 minutes;
[0121] (3.2) adding unsaturated hydroxyalkyl ester to the reaction system in step (3.1), and continuing the reaction for 30 min at 165±1° C., under nitrogen protection, condensation reflux and stirring, to obtain a polyester-type polymer chelating dispersant intermediate;
[0122] (4) A step of initiating polymerization, in which the polyester-type polymer chelate dispersant intermediate is reacted with an unsaturated anionic monomer, an initiator and water to obtain a polyester-type polymer chelate dispersant.
[0123] (4.1) The reaction system in step (3.2) was cooled to 88±1°C, the reflux device was removed, unsaturated anionic monomers and 50 wt% of water were added, and the mixture was fully sheared and dispersed at 67±1°C to obtain a dispersion, and 85 wt% of the dispersion was taken out for later use;
[0124] (4.2) Under stirring, add 40 wt% of water and 30 wt% of initiator (water and initiator are pre-mixed to form an initiator aqueous solution) to the remaining dispersion in step (4.1), and stir the reaction at 84±1°C for 35 min; control the temperature of the reaction system to 84±1°C and evenly drip the initiator solution (obtained by mixing 10 wt% of water and the remaining initiator) and the dispersion taken out in step (4.1) within 75 min, and control the reaction temperature to 84±1°C; then continue the reaction at 84±1°C for 45 min;
[0125] (4.3) While stirring, the reaction system in step (4.2) is cooled to below 50° C. to obtain a polyester-type polymer chelating dispersant.
[0126] Example 3
[0127] (1) Raw material preparation, the specific selection and dosage of the raw materials are shown in Table 1;
[0128] (2) an ester exchange step, in which an ester exchange catalyst, an aromatic dimethyl ester, and a diol are reacted to obtain a polyester-type polymer chelating dispersant primary polymer;
[0129] (2.1) Add transesterification catalyst, aromatic dimethyl ester and diol into the reactor, heat the reaction system to 155±1°C within 17 minutes, and keep the temperature for 60 minutes under nitrogen protection, condensation reflux and stirring. During the heating and heat preservation period, separate the distilled by-products;
[0130] (2.2) heating the reaction system in step (2.1) to 215±1° C. within 15 minutes, and keeping the temperature under nitrogen protection, condensation reflux and stirring for 75 minutes, separating the distilled by-products during the heating and keeping temperature period to obtain a polyester-type polymer chelating dispersant primary polymer;
[0131] (3) an end-capping step, in which the polyester-type polymer chelating dispersant primary polymer is reacted with diisocyanate, unsaturated hydroxyalkyl ester, and organic solvent to obtain a polyester-type polymer chelating dispersant intermediate;
[0132] (3.1) The reaction system in step (3.2) was cooled to 155±1°C, and an organic solvent and diisocyanate were added, and the reaction was carried out at 155±1°C, under nitrogen protection, condensation reflux and stirring for 35 minutes;
[0133] (3.2) adding unsaturated hydroxyalkyl ester to the reaction system in step (3.1), and continuing the reaction for 35 minutes at 155±1°C, under nitrogen protection, condensation reflux and stirring to obtain a polyester-type polymer chelating dispersant intermediate;
[0134] (4) A step of initiating polymerization, in which the polyester-type polymer chelate dispersant intermediate is reacted with an unsaturated anionic monomer, an initiator and water to obtain a polyester-type polymer chelate dispersant.
[0135] (4.1) The reaction system in step (3.2) was cooled to 85±1°C, the reflux device was removed, unsaturated anionic monomers and 50 wt% of water were added, and the mixture was fully sheared and dispersed at 65±1°C to obtain a dispersion, and 90 wt% of the dispersion was taken out for later use;
[0136] (4.2) under stirring, add 40 wt% of water and 20 wt% of initiator (water and initiator are pre-mixed to form an initiator aqueous solution) to the remaining dispersion in step (4.1), and stir the reaction at 80±1°C for 45 min; control the temperature of the reaction system to 80±1°C and uniformly add the initiator solution (mixed with 10 wt% of water and the remaining initiator) and the dispersion taken out in step (4.1) dropwise over 65 min; then continue the reaction at 80±1°C for 40 min;
[0137] (4.3) While stirring, the reaction system in step (4.2) is cooled to below 50° C. to obtain a polyester-type polymer chelating dispersant.
[0138] The polyester polymer chelate dispersant prepared by the embodiment of the present invention can be used for the reduction-free cleaning process of disperse dye dyeing. That is, after the disperse dye dyes are used to dye the polyester fiber, it is not necessary to wash off the "floating color" of the disperse dye remaining on the fiber under the action of insurance powder and alkali agent as in the traditional process (process: insurance powder 4-8g / L, sodium carbonate 3-6g / L, 75°C water washing for 10min) to obtain good color fastness. It is only necessary to wash off the "floating color" of the disperse dye remaining on the fiber after the disperse dye dyeing with the polyester polymer chelate dispersant of the present invention (process: polyester polymer chelate dispersant 3-6g / L, 75°C water washing for 10min), and the same color fastness as the traditional post-dyeing cleaning process (various wet treatment fastness 4-5 levels) can be obtained. Since the polyester polymer chelate dispersant described in the present invention is used for the post-disperse dyeing cleaning process without the assistance of alkali agent and insurance powder, it has good environmental protection and convenience of production process implementation.
[0139] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a polyester-type polymer chelating dispersant, characterized in that: The method comprises the following steps: (1) Raw material preparation: The raw materials include an ester exchange catalyst, an aromatic dimethyl ester, a diol, a diisocyanate, an unsaturated hydroxyalkyl ester, an unsaturated anionic monomer, an initiator, water, and an optional organic solvent; Wherein, the transesterification catalyst is zinc acetate; The aromatic dimethyl esters are dimethyl 5-sulfonate sodium isophthalate, dimethyl terephthalate and dimethyl phthalate; The diol is selected from one or more of ethylene glycol, 1,4-butanediol, 1,6-hexanediol and diethylene glycol; The diisocyanate is toluene diisocyanate or isophorone diisocyanate; The unsaturated hydroxyalkyl ester is hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate or hydroxypropyl methacrylate; The unsaturated anionic monomers are maleic anhydride and acrylic acid; The initiator is potassium persulfate or ammonium persulfate; The organic solvent is propylene glycol methyl ether acetate; The molar fractions of the components in the raw materials are: 5 for aromatic dimethyl ester, 6 to 10 for diol, the molar fraction of diisocyanate = 2×(the molar fraction of diol-the molar fraction of aromatic dimethyl ester), and the molar fraction of unsaturated hydroxyalkyl ester is 1 to 1.1 times the molar fraction of diisocyanate; The weight of the unsaturated anionic monomer is 0.5 to 1.5 times the total weight of the aromatic dimethyl ester and the diol; Based on the total molar amount of the aromatic dimethyl ester, the molar proportion of dimethyl isophthalate-5-sodium sulfonate is 10-30%, the molar proportion of dimethyl terephthalate is 30-60%, and the molar proportion of dimethyl phthalate is 30-60%; Based on the total weight of the unsaturated anionic monomer, the content of maleic anhydride is 30 to 70 wt %; (2) Transesterification: reacting a transesterification catalyst, an aromatic dimethyl ester and a diol to obtain a polyester-type polymer chelating dispersant primary polymer; (3) End-capping: reacting a polyester-type polymer chelating dispersant primary polymer, a diisocyanate, an unsaturated hydroxyalkyl ester and an optional organic solvent to obtain a polyester-type polymer chelating dispersant intermediate; (4) Polymerization: The polyester type polymer chelating dispersant intermediate, unsaturated anionic monomer, initiator and water are reacted to prepare the polyester type polymer chelating dispersant.
2. The method according to claim 1, characterized in that: The amount of the transesterification catalyst used is 0.4-0.8 wt % of the total weight of the aromatic dimethyl ester and the diol.
3. The method according to claim 1 or 2, characterized in that: The amount of the initiator used is 0.5-1 wt % of the total weight of the unsaturated hydroxyalkyl ester and the unsaturated anionic monomer.
4. The method according to claim 1 or 2, characterized in that: The amount of the organic solvent used is 0 to 1 times the total weight of the aromatic dimethyl ester, diol, diisocyanate and unsaturated hydroxyalkyl ester.
5. The method according to claim 1 or 2, characterized in that: The amount of water used is 1 to 2 times the total weight of the aromatic dimethyl ester, diol, diisocyanate, unsaturated hydroxyalkyl ester and unsaturated anionic monomer.
6. The method according to claim 1, characterized in that The specific process of step (2) includes: (2.1) Adding an ester exchange catalyst, an aromatic dimethyl ester and a diol into a reactor, heating the reaction system to 150 to 200° C. within 10 to 30 minutes, and keeping the temperature under nitrogen protection, condensation reflux and stirring for 50 to 100 minutes; (2.2) The reaction system in step (2.1) is heated to 200-250° C. within 10-30 minutes, and the reaction is kept warm for 50-100 minutes under nitrogen protection, condensation reflux and stirring to obtain a polyester-type polymer chelating dispersant prepolymer.
7. The method according to claim 1 or 6, characterized in that: The specific process of step (3) includes: (3.1) cooling the reaction system in step (2) to 150-200° C., adding an organic solvent and a diisocyanate, and then reacting at 150-200° C. under nitrogen protection, condensation reflux and stirring for 20-40 minutes; (3.2) Add unsaturated hydroxyalkyl ester to the reaction system in step (3.1), and continue the reaction for 20 to 40 minutes to obtain a polyester-type polymer chelating dispersant intermediate.
8. The method according to claim 1, characterized in that The specific process of step (4) includes: (4.1) cooling the reaction system in step (3) to 80-110° C., removing the reflux device, adding unsaturated anionic monomers and 40-60 wt % of water in total, and shearing and dispersing at 60-80° C. to obtain a dispersion, and taking out 70-90 wt % of the dispersion for later use; (4.2) adding 35-45 wt% of water and 20-40 wt% of initiator to the remaining dispersion in step (4.1) under stirring, and maintaining stirring reaction at 70-90° C. for 20-60 min; controlling the temperature of the reaction system to 70-90° C. and adding 5-15 wt% of water, the remaining initiator and 70-90 wt% of the dispersion taken out in step (4.1) within 40-90 min; and then continuing the reaction at 70-90° C. for 30-60 min; (4.3) While stirring, the reaction system in step (4.2) is cooled to below 50° C. to obtain a polyester-type polymer chelating dispersant.
9. A polyester type polymer chelating dispersant prepared by the method according to any one of claims 1 to 8.
10. Use of the polyester polymer chelating dispersant according to claim 9 in a disperse dye dyeing process.