Polyacrylamide for oil displacement as well as preparation method and application thereof

By preparing five-membered polymer polyacrylamide with high interfacial activity and shear resistance, the problems of poor hydrolysis stability and high interfacial tension under high temperature and high mineralization conditions are solved, and the oil field oil production efficiency is improved.

CN118955818AInactive Publication Date: 2024-11-15SHENGLI OIL FIELD FANGYUAN CHEM IND

Patent Information

Application Number
CN202411441614.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing polyacrylamide has poor hydrolysis stability under high temperature and high mineralization conditions, and lacks surfactant groups, which cannot reduce the oil-water interface tension, affecting the recovery rate.

Method used

Five-membered polymers are used, including acrylamide, 4-trifluoromethylcinnamic acid, 4,4'-diaminodisyl-2,2'-disulfonic acid, (3-acryloyloxypropyl) Tris(trimethylsiloxy)silane and allyl alcohol polyoxyethylene ether are prepared by specific monomer reaction sequence and initiator dropping process to prepare polyacrylamides with high interfacial activity and shear resistance.

Benefits of technology

The high interfacial activity, high viscosity and good shear resistance of polyacrylamide are achieved, the oil-water interface tension is reduced, and the crude oil recovery rate is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the technical field of tertiary oil recovery, and particularly relates to polyacrylamide for oil displacement and a preparation method and application thereof. The preparation method comprises the following steps: introducing nitrogen into a reactor, sequentially adding acrylamide, 4-trifluoromethylcinnamic acid, 4, 4 '-diaminostilbene-2, 2'-disulfonic acid, (3-acryloyloxypropyl) tri (trimethylsiloxy) silane, allyl alcohol polyoxyethylene ether, buffer salt, a dispersing agent and deionized water, stirring, and adjusting the pH value to 7-8; adding an initiator into a high-position dropwise adding tank, dropwise adding the initiator into the reactor, in the dropwise adding process, automatically heating the solution, continuously reacting for 1-2 hours, heating to 60-70 DEG C, carrying out heat preservation reaction for 2-8 hours, cooling to 40 DEG C or below, and adjusting the pH value to 7-8; and drying and granulating the mixed solution to obtain the polyacrylamide for oil displacement. The polyacrylamide for oil displacement has the characteristics of high interfacial activity, high viscosity and shear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tertiary oil recovery, and specifically relates to polyacrylamide for oil recovery and a preparation method and application thereof. Background Art

[0002] Polymer flooding is achieved by adding a certain amount of high molecular weight polyacrylamide to the injected water to increase the viscosity of the injected water, improve the oil-water mobility ratio, increase the seepage resistance of the injected water, increase the water absorption of the low permeability layer or the low but not flooded layer, expand the contact area of ​​the injected water on the plane of the oil layer and the flooding thickness of the oil layer in the vertical direction, and then expand the swept volume to displace the unused crude oil during water flooding, thereby achieving the purpose of improving crude oil recovery.

[0003] There are amide active groups in the molecular structure of polyacrylamide, which can be easily obtained through grafting or cross-linking to obtain a variety of modified products with branched or network structures. Polyacrylamide molecules can introduce various ionic groups to obtain specific properties and are widely used in increasing oil field production.

[0004] The quality of polyacrylamide determines the effect of improving oil recovery to a considerable extent. Many scientific researchers are committed to structural modification of polyacrylamide to make it have significant viscosity-increasing effect, shear resistance and high activity, thereby effectively increasing the viscosity of the displacement fluid, improving the sweep coefficient and increasing the swept volume.

[0005] CN104448129B discloses a high temperature resistant hydrolysis copolymer for oil fields, a preparation method and its application in oil production, which mainly solves the problem of poor hydrolysis stability of polyacrylamide under high temperature and high mineralization conditions in the previous technology. The invention adopts a high temperature resistant hydrolysis copolymer for oil fields shown in the general formula, R1 and R2 are taken from C1~C16 hydrocarbon groups; M is taken from any one of alkali metal ions or ammonium ions; x, y, m, n are respectively the molar number of structural units of acrylamide, hydrolyzed acrylamide, N, N-dialkyl substituted acrylamide, and N-vinyl pyrrolidone, and the technical scheme of x:y:m:n=100:(1~85):(1~100):(1~80) solves the problem well and can be used in oil production in oil fields. However, there is no surfactant group in the molecular structure of the invention, and it only has the function of ordinary polymer flooding, which cannot reduce the oil-water interfacial tension, cannot emulsify and reduce viscosity, and affects the recovery rate.

[0006] CN105542073B discloses a method for preparing polyacrylamide for polymer flooding oil recovery, belonging to the field of polymer technology. Steps: evenly mix cationic monomer, acrylamide, trimethylolmethylamine, surfactant and water, and then introduce nitrogen into the mixed solution; add initiator, heat up, keep reacting, cool down, add hydroxyethyl acrylate and dimethylchlorosilane to the mixture, adjust the pH of the reaction system, heat up, keep reacting, take out the obtained colloidal product after the end, cut, dry, granulate and screen to obtain the polyacrylamide product. The invention adjusts the monomer reaction sequence of the modified polyacrylamide during polymerization, first partially polymerizes the cationic monomer and acrylamide, and then continues the polymerization reaction by hydroxyethyl acrylate and dimethylchlorosilane, so that the prepared modified polyacrylamide has the effect of increasing viscosity in a solution with a high ion concentration. However, the viscosity of the invention when the concentration is 1500mg / L is only about 30mPa•s, which is low as a polymer flooding viscosity. The increase in sweep coefficient and swept volume is limited. Summary of the invention

[0007] The present invention provides a polyacrylamide for oil displacement and a preparation method and application thereof. The polyacrylamide for oil displacement of the present invention has the characteristics of high interfacial activity, high viscosity and shear resistance.

[0008] In order to achieve the above-mentioned object, one of the objects of the present invention is to disclose a polyacrylamide for oil displacement, wherein the molecular structure of the polyacrylamide is as follows:

[0009] in: a=100000-1000000; b = 5000-100000; c = 2000-50000; d = 5000-100000; e=2000-50000; n=5-20.

[0010] Preferably, the viscosity average molecular weight of the polyacrylamide is 30,000,000-40,000,000.

[0011] Another object of the present invention is to disclose a method for preparing the above-mentioned polyacrylamide, and the specific steps of the preparation method are as follows: (1) nitrogen is introduced into the reactor to replace the air therein, and the nitrogen is kept introduced. In the later process, the materials in the reactor are always kept away from air; acrylamide, 4-trifluoromethylcinnamic acid, 4,4'-diaminobenzylbenzene-2,2'-disulfonic acid, (3-acryloxypropyl) tris(trimethylsiloxy)silane, allyl alcohol polyoxyethylene ether, buffer salt, dispersant, and deionized water are added in sequence, stirred, and the pH is adjusted to 7-8; (2) Add the initiator to the high-position drop tank and drip it into the reactor. During the dripping process, the solution automatically heats up and continues to react for 1-2 hours. Heat to 60-70°C and keep the temperature for 2-8 hours. Cool down to below 40°C and adjust the pH to 7-8. (3) Drying and granulating the mixed solution to obtain polyacrylamide for oil displacement.

[0012] In the present invention, preferably, the molar ratio of 4-trifluoromethylcinnamic acid, 4,4'-diaminostilbene-2,2'-disulfonic acid, (3-acryloxypropyl)tris(trimethylsiloxy)silane, allyl alcohol polyoxyethylene ether and acrylamide is 0.05-0.1:0.02-0.05:0.05-0.1:0.02-0.05:1.

[0013] In the present invention, preferably, in step (1), the buffer salt is one of sodium dihydrogen phosphate, potassium dihydrogen phosphate and ammonium dihydrogen phosphate, and the weight ratio of the buffer salt to acrylamide is 0.02-0.04:1.

[0014] In the present invention, preferably, in step (1), the dispersant is one of hydroxypropyl methylcellulose, hydroxyethyl cellulose and carboxymethyl cellulose, and the weight ratio of the dispersant to acrylamide is 0.02-0.04:1.

[0015] In the present invention, preferably, in step (1), the weight ratio of deionized water to acrylamide is 6-8:1.

[0016] In the present invention, preferably, in step (2), the initiator is a mixed solution of persulfate and sodium bisulfite, wherein the concentration of persulfate is 10-12wt%, the concentration of sodium bisulfite is 3-5wt%, and the weight ratio of initiator to acrylamide is 0.2-0.5:1.

[0017] Preferably, the persulfate is one of potassium persulfate, ammonium persulfate and sodium persulfate.

[0018] The synthetic reaction equation of polyacrylamide for oil displacement of the present invention is as follows:

[0019]

[0020] The third object of the present invention is to disclose the application of the above polyacrylamide in polymer flooding.

[0021] The polyacrylamide for oil displacement of the present invention is a five-membered high molecular polymer with acrylamide, 4-trifluoromethylcinnamic acid, 4,4'-diaminostilbene-2,2'-disulfonic acid, (3-acryloxypropyl)tris(trimethylsiloxy)silane, and allyl alcohol polyoxyethylene ether as monomers. Trifluoromethylcinnamic acid and (3-acryloxypropyl)tris(trimethylsiloxy)silane are special surfactant lipophilic monomers, which have lower interfacial tension than conventional surfactants and can better strip crude oil; the molecule contains a benzene ring structure and has a strong shear resistance; the molecule contains a carboxyl group and a sulfonic acid anion, which can reduce the oil-water interfacial tension, emulsify crude oil and reduce crude oil viscosity; allyl alcohol polyoxyethylene ether contains a long-chain hydrophilic group, which can transfer the stripped crude oil to the water phase and improve the crude oil recovery rate.

[0022] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) The polyacrylamide for oil displacement of the present invention has good interfacial activity, and the interfacial tension at a concentration of 500 mg / L reaches 0.12×10 -3 Below mN / m; (2) The polyacrylamide for oil displacement of the present invention has a relatively high surface viscosity. At 60°C, the viscosity at a concentration of 2000 mg / L reaches 88 mPa•s or above; (3) The polyacrylamide for oil displacement of the present invention has shear resistance. After 2 hours of shearing, the viscosity retention rate reaches more than 92%. DETAILED DESCRIPTION

[0023] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0024] The technical solution of the present invention is further described below in conjunction with specific embodiments:

[0025] Example 1 (1) nitrogen was introduced into the reactor to replace the air therein, and the nitrogen was kept introduced. During the later process, the materials in the reactor were always kept away from air. 0.5 mol acrylamide, 0.025 mol 4-trifluoromethylcinnamic acid, 0.025 mol 4,4'-diaminobenzylbenzene-2,2'-disulfonic acid, 0.025 mol (3-acryloxypropyl) tris(trimethylsiloxy)silane, 0.025 mol allyl alcohol polyoxyethylene ether, 0.71 g sodium dihydrogen phosphate, 0.9 g hydroxypropyl methylcellulose, and 213 g deionized water were added in sequence, stirred, and the pH was adjusted to 7-8 with sodium hydroxide solution. (2) Add 7.1 g of initiator containing 12 wt% potassium persulfate and 4 wt% sodium bisulfite to the high-position drop tank and drip it into the reactor. During the dripping process, the solution automatically heats up and continues to react for 1 hour. The temperature is then raised to 70°C and kept at this temperature for 2 hours. The temperature is then lowered to below 40°C and the pH is adjusted to 7-8 with sodium hydroxide. (3) Drying and granulating the mixed solution to obtain polyacrylamide for oil displacement.

[0026] Example 2 (1) nitrogen was introduced into the reactor to replace the air therein, and the nitrogen was kept introduced. During the later stage, the materials in the reactor were always kept away from air. 0.5 mol acrylamide, 0.03 mol 4-trifluoromethylcinnamic acid, 0.015 mol 4,4'-diaminobenzylbenzene-2,2'-disulfonic acid, 0.03 mol (3-acryloxypropyl) tris(trimethylsiloxy)silane, 0.02 mol allyl alcohol polyoxyethylene ether, 0.88 g sodium dihydrogen phosphate, 0.95 g hydroxypropyl methylcellulose, and 247 g deionized water were added in sequence, stirred, and the pH was adjusted to 7-8 with sodium hydroxide solution. (2) 8.9 g of initiator containing 12 wt% potassium persulfate and 5 wt% sodium bisulfite was added to the high-position dropping tank and dripped into the reactor. During the dripping process, the solution automatically heated up and continued to react for 2 h. The temperature was heated to 60 ° C and kept for 8 h. The temperature was lowered to below 40 ° C and the pH was adjusted to 7-8 with sodium hydroxide. (3) Drying and granulating the mixed solution to obtain polyacrylamide for oil displacement.

[0027] Example 3 (1) nitrogen was introduced into the reactor to replace the air therein, and the nitrogen was kept introduced. During the later process, the materials in the reactor were always kept away from air. 0.5 mol acrylamide, 0.035 mol 4-trifluoromethylcinnamic acid, 0.02 mol 4,4'-diaminobenzylbenzene-2,2'-disulfonic acid, 0.04 mol (3-acryloxypropyl) tris(trimethylsiloxy)silane, 0.015 mol allyl alcohol polyoxyethylene ether, 1.42 g potassium dihydrogen phosphate, 0.71 g hydroxyethyl cellulose, and 236 g deionized water were added in sequence, stirred, and the pH was adjusted to 7-8 with sodium hydroxide solution. (2) 14.7 g of initiator containing 11 wt% potassium persulfate and 3 wt% sodium bisulfite was added to the high-position dropping tank and dripped into the reactor. During the dripping process, the solution automatically heated up and continued to react for 2 h. The temperature was raised to 70 ° C and kept for 2 h. The temperature was lowered to below 40 ° C and the pH was adjusted to 7-8 with sodium hydroxide. (3) Drying and granulating the mixed solution to obtain polyacrylamide for oil displacement.

[0028] Example 4 (1) nitrogen was introduced into the reactor to replace the air therein, and the nitrogen was kept introduced. During the later stage, the materials in the reactor were always kept away from air. 0.5 mol acrylamide, 0.04 mol 4-trifluoromethylcinnamic acid, 0.02 mol 4,4'-diaminobenzylbenzene-2,2'-disulfonic acid, 0.05 mol (3-acryloxypropyl) tris(trimethylsiloxy)silane, 0.01 mol allyl alcohol polyoxyethylene ether, 1.08 g potassium dihydrogen phosphate, 1.33 g hydroxyethyl cellulose, and 284 g deionized water were added in sequence, stirred, and the pH was adjusted to 7-8 with sodium hydroxide solution. (2) 16.7 g of initiator containing 10 wt% potassium persulfate and 3 wt% sodium bisulfite was added to the high-position drop tank and dripped into the reactor. During the dripping process, the solution automatically heated up and continued to react for 1.5 h. The temperature was heated to 65 ° C and kept for 6 h. The temperature was lowered to below 40 ° C and the pH was adjusted to 7-8 with sodium hydroxide. (3) Drying and granulating the mixed solution to obtain polyacrylamide for oil displacement.

[0029] Example 5 (1) nitrogen was introduced into the reactor to replace the air therein, and the nitrogen was kept introduced. During the later stage, the materials in the reactor were always kept away from air. 0.5 mol acrylamide, 0.045 mol 4-trifluoromethylcinnamic acid, 0.01 mol 4,4'-diaminobenzylbenzene-2,2'-disulfonic acid, 0.045 mol (3-acryloxypropyl) tris(trimethylsiloxy)silane, 0.02 mol allyl alcohol polyoxyethylene ether, 1.21 g ammonium dihydrogen phosphate, 1.42 g carboxymethyl cellulose, and 255 g deionized water were added in sequence, stirred, and the pH was adjusted to 7-8 with sodium hydroxide solution. (2) 17.75 g of initiator containing 10 wt% ammonium persulfate and 4 wt% sodium bisulfite was added to the high-position dropping tank and dripped into the reactor. During the dropping process, the solution automatically heated up and continued to react for 1.8 h. The temperature was heated to 68 ° C and kept for 4 h. The temperature was lowered to below 40 ° C and the pH was adjusted to 7-8 with sodium hydroxide. (3) Drying and granulating the mixed solution to obtain polyacrylamide for oil displacement.

[0030] Example 6 (1) nitrogen was introduced into the reactor to replace the air therein, and the nitrogen was kept introduced. During the later stage, the materials in the reactor were always kept away from air. 0.5 mol acrylamide, 0.05 mol 4-trifluoromethylcinnamic acid, 0.01 mol 4,4'-diaminobenzylbenzene-2,2'-disulfonic acid, 0.03 mol (3-acryloxypropyl) tris(trimethylsiloxy)silane, 0.015 mol allyl alcohol polyoxyethylene ether, 0.91 g ammonium dihydrogen phosphate, 1.26 g carboxymethyl cellulose, and 273 g deionized water were added in sequence, stirred, and the pH was adjusted to 7-8 with sodium hydroxide solution. (2) 15.1 g of initiator containing 11 wt% ammonium persulfate and 5 wt% sodium bisulfite was added to the high-position drop tank and dripped into the reactor. During the dripping process, the solution automatically heated up and continued to react for 1.8 h. The temperature was heated to 66 ° C and kept at this temperature for 7 h. The temperature was then lowered to below 40 ° C and the pH was adjusted to 7-8 with sodium hydroxide. (3) Drying and granulating the mixed solution to obtain polyacrylamide for oil displacement.

[0031] Example 7 Test of interfacial tension The polyacrylamide for oil recovery (Examples 1-6) of the present invention was prepared into a solution with a concentration of 500 mg / L with tap water, and the interfacial tension was tested at 60°C according to the method in SY / T 5370-2018 "Surface and interfacial tension determination method". The oil phase was crude oil from Xianhe Oil Production Plant of Shengli Oilfield, and the viscosity at 60°C was 150 mPa•s. The PAM for oil recovery produced by Shandong Dongying Baomo Environmental Engineering Co., Ltd. was used as a comparative sample, and the test results are shown in Table 1.

[0032] It can be seen from Table 1 that the interfacial tension of the polyacrylamide for oil displacement (Examples 1-6) of the present invention at a concentration of 500 mg / L is 0.12×10 -3 Below mN / m, the lowest is 0.072×10 -3 mN / m (Example 5); while the interfacial tension of the PAM for oil recovery produced by Shandong Dongying Baomo Environmental Engineering Co., Ltd. in the comparative example is 18mN / m, which is significantly higher than that of the present invention.

[0033] Example 8 Test of apparent viscosity The polyacrylamide for oil displacement (Examples 1-6) of the present invention was prepared into a solution with a concentration of 2000 mg / L with tap water, and the apparent viscosity was tested using a Haake rheometer at 60° C. The PAM for oil displacement produced by Shandong Dongying Baomo Environmental Engineering Co., Ltd. was used as a comparative sample, and the test results are shown in Table 1.

[0034] It can be seen from Table 1 that the apparent viscosity of the polyacrylamide for oil recovery of the present invention (Examples 1-6) at a concentration of 2000 mg / L at 60°C is 88 mPa•s or above, and the highest is 96 mPa•s (Example 4); while the apparent viscosity of the PAM for oil recovery of the comparative example Shandong Dongying Baomo Environmental Engineering Co., Ltd. is 30 mPa•s, which is significantly lower than that of the present invention.

[0035] Example 9 Shear resistance test The sample in Example 8 was heated at 60°C for 170 seconds. -1 The apparent viscosity was tested and the viscosity retention rate was calculated by continuous shearing for 2 hours under the condition of . The PAM for oil displacement produced by Shandong Dongying Baomo Environmental Engineering Co., Ltd. was used as a comparative sample. The test results are shown in Table 1.

[0036] Table 1 Test results of surface tension, interfacial tension, apparent viscosity and shear resistance

[0037] It can be seen from Table 1 that the polyacrylamide for oil displacement of the present invention (Examples 1-6) is heated to 60°C and 170s -1 Under the conditions of continuous shearing for 2 hours, the viscosity retention rate reached more than 92%, with the highest reaching 95.8% (Example 6); while the viscosity retention rate of PAM for oil recovery produced by Shandong Dongying Baomo Environmental Engineering Co., Ltd. in the comparative example was 81%, which was significantly lower than that of the present invention.

[0038] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing polyacrylamide for oil displacement, characterized in that: The specific steps of the preparation method are as follows: (1) nitrogen is introduced into the reactor to replace the air therein, and the nitrogen is kept introduced. In the later process, the materials in the reactor are always kept away from air; acrylamide, 4-trifluoromethylcinnamic acid, 4,4'-diaminobenzylbenzene-2,2'-disulfonic acid, (3-acryloxypropyl) tris(trimethylsiloxy)silane, allyl alcohol polyoxyethylene ether, buffer salt, dispersant, and deionized water are added in sequence, stirred, and the pH is adjusted to 7-8; (2) Add the initiator to the high-position drop tank and drip it into the reactor. During the dripping process, the solution automatically heats up and continues to react for 1-2 hours. Heat to 60-70°C and keep the temperature for 2-8 hours. Cool down to below 40°C and adjust the pH to 7-8. (3) drying and granulating the mixed solution to obtain polyacrylamide for oil displacement; The molar ratio of 4-trifluoromethylcinnamic acid, 4,4'-diaminostilbene-2,2'-disulfonic acid, (3-acryloxypropyl)tris(trimethylsiloxy)silane, allyl alcohol polyoxyethylene ether and acrylamide is 0.05-0.1: 0.02-0.05: 0.05-0.1: 0.02-0.05: 1; The molecular structure of the oil displacement polyacrylamide is as follows: in: a=100000-1000000; b=5000-100000; c=2000-50000; d=5000-100000; e=2000-50000; n=5-20。 2. The method for preparing a polyacrylamide for oil displacement according to claim 1, characterized in that: In step (1), the buffer salt is one of sodium dihydrogen phosphate, potassium dihydrogen phosphate, and ammonium dihydrogen phosphate, and the weight ratio of the buffer salt to acrylamide is 0.02-0.04:

1.

3. The method for preparing a polyacrylamide for oil displacement according to claim 1, characterized in that: In step (1), the dispersant is one of hydroxypropyl methylcellulose, hydroxyethyl cellulose and carboxymethyl cellulose, and the weight ratio of the dispersant to acrylamide is 0.02-0.04:

1.

4. The method for preparing a polyacrylamide for oil displacement according to claim 1, characterized in that: In step (1), the weight ratio of deionized water to acrylamide is 6-8:

1.

5. The method for preparing a polyacrylamide for oil displacement according to claim 1, characterized in that: In step (2), the initiator is a mixed solution of persulfate and sodium bisulfite, and the weight ratio of the initiator to acrylamide is 0.2-0.5:

1.

6. The method for preparing polyacrylamide for oil displacement according to claim 5, characterized in that: The concentration of the persulfate is 10-12 wt %, and the concentration of the sodium bisulfite is 3-5 wt %.

7. The method for preparing polyacrylamide for oil displacement according to claim 5, characterized in that: The persulfate is one of potassium persulfate, ammonium persulfate and sodium persulfate.

8. A polyacrylamide for oil displacement, characterized in that: The molecular structure of polyacrylamide is as follows: in: a=100000-1000000; b=5000-100000; c=2000-50000; d=5000-100000; e=2000-50000; n=5-20。 9. The polyacrylamide for oil displacement according to claim 8, characterized in that: The viscosity average molecular weight of the polyacrylamide is 30,000,000-40,000,000.

10. Use of the polyacrylamide for oil recovery according to claim 8 or 9 in polymer oil recovery.

Citation Information

Patent Citations

  • Anionic polyacrylamide for oil extraction and preparation method thereof

    CN117229456A

  • Drag reducer for fracturing and preparation method thereof

    CN117510712A

  • Temperature-resistant and salt-resistant polyacrylamide for oil displacement and synthesis method of temperature-resistant and salt-resistant polyacrylamide

    CN117866141A

  • Polyacrylamide for improving recovery ratio and preparation method and application thereof

    CN118184878A

  • Polymer having dispersing function, polycarboxylic acid cement dispersant, preparation method therefor and use thereof

    US20230391941A1

Cited By

  • High-molecular polymer thickening agent as well as synthesis method and application thereof

    CN119161526A

  • Demulsifier for breaking oil-water transition zone for oil-gas gathering and transportation and preparation method thereof

    CN119955031A

  • A demulsifier for breaking the oil-water transition zone in oil and gas gathering and transportation and its preparation method.

    CN119955031B