Peanut coat extract / chitosan blend solution with antibacterial function and high mechanical property and application of peanut coat extract / chitosan blend solution in fibers and membranes
By ionic crosslinking with peanut clothing extract on chitosan, a peanut clothing extract/chitosan blend solution with high mechanical properties and antibacterial functions was prepared, which solved the problem of insufficient performance of chitosan film and achieved the The performance of fibers and membranes has expanded their application range.
Patent Information
- Application Number
- CN202411093223.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Peanut Clothing Extract is not used in the chitosan system, resulting in insufficient mechanical properties, antioxidant and antibacterial abilities of the chitosan film, limiting its application.
Peanut Clothing Extract is prepared by solvent extraction method, and peanut Clothing Extract/chitosan blend solution is prepared by ionic crosslinking between the amino group on chitosan and the phenolic hydroxyl group on peanut Clothing Extract, and by spinning or Cast and prepare fibers and membranes to improve their mechanical properties, hydrophobic properties and antibacterial properties.
It significantly improves the mechanical properties, hydrophobic properties and antibacterial properties of fibers and membranes, enhances the mechanical properties and antibacterial properties of chitosan, and expands its application potential in the field of textile materials.
Smart Images

Figure CN118955957A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a peanut skin extract / chitosan blended liquid with antibacterial function and high mechanical performance and application thereof in fibers and films, belonging to the technical field of functional textile materials. Background Art
[0002] With the increasing awareness of environmental protection, the development of environmentally friendly and degradable materials has become an important direction of scientific research and industrial application. Chitosan, as a natural polymer, has great application potential in the fields of clothing, medicine and food packaging due to its good biocompatibility and biodegradability. However, the traditional chitosan film is too hydrophilic, has poor mechanical properties, and its antioxidant and antibacterial capabilities still need to be improved, which limits its application.
[0003] Peanut skins are widely available and inexpensive, and as a byproduct, most of them are treated as animal feed or waste. However, peanut skins are rich in polyphenolic compounds, which have significant antioxidant and antibacterial activities and have not been fully utilized.
[0004] Some researchers have studied the application of peanut skin extract as an additional material in composite films. For example, Qingyin Dai et al. (Dai, Qingyin; Huang, Xi; Jia, Ruijing; Fang, Yanyuan; Qin, Zhiyong. Development of antibacterial film based on alginate fiber, and peanutred skin extract for food packaging [J]. Journal of Food Engineering, 2022, Vol. 330: 111106) used sodium alginate / cellulose nanofibers as the base material and added peanut skin extract. 2+An antibacterial composite film for fruit preservation was prepared by cross-linking, and the effect of the concentration of added peanut skin extract on the structural properties of the composite film was studied; Wenbo Meng et al. (Wenbo Meng; Jingying Shi; Xiaoyan Zhang; Huan Lian; Qingguo Wang; Yong Peng. Effects of peanut shell and skin extracts on the antioxidantability, physical and structure properties of starch-chitosan active packaging films [J]. International Journal of Biological Macromolecules, 2020, Vol. 152: 137-146) studied the antioxidant capacity of peanut shell and peanut skin extracts and their effects on the physical and structural properties of starch-chitosan films. The results showed that the antioxidant capacity of peanut skin extract was significantly higher than that of peanut shell and would increase the tensile strength of the composite film; Ahreum et al. (Ju, A.; Song, KB. Active biodegradable films based on water soluble polysaccharides from white jelly mushroom (Tremella fuciformis) containing roasted peanut skin extract(Article)[J].LWT,2020,Vol.126:109293) used water-soluble polysaccharides in Tremella fuciformis as the main raw material and added peanut skin extract of different concentrations to prepare biodegradable Tremella fuciformis polysaccharide film. The study found that the addition of peanut skin extract can improve the surface hydrophobicity and antioxidant capacity of the polysaccharide film.
[0005] However, chitosan is the product of chitin deacetylation and is the only alkaline polysaccharide among natural polysaccharides. The C2 position of chitosan is -NH2, which makes its chemical structure tighter and has stronger intramolecular hydrogen bonding. At present, some natural polyphenols are routinely added to the chitosan system, such as: CN 111234324A discloses a multifunctional chitosan / gallic tannin blended film and its preparation method, which uses gallic tannin to improve the performance of chitosan film. Peanut skin extract modified chitosan not only improves the mechanical properties of chitosan, but also improves its antibacterial properties; and the rich active ingredients in peanut skin extract, such as resveratrol, tannic acid, proanthocyanidins, etc., and rich sterol esters and glycerides, have the function of improving platelet quality and have good therapeutic effects on various hemorrhagic diseases; the combination of the two is expected to be applied in the field of medical textiles. Summary of the invention
[0006] [Technical issues]
[0007] Peanut skin extract was not used in the chitosan system.
[0008] [Technical solution]
[0009] In order to solve the above problems, the present invention firstly prepares peanut skin extract by solvent extraction, and then combines the amino groups on chitosan and the phenolic hydroxyl groups on the peanut skin extract by ionic crosslinking to prepare a peanut skin extract / chitosan blend. Finally, the peanut skin extract / chitosan blend is spun to prepare fibers, or cast to prepare membranes, so as to improve the mechanical properties, hydrophobic properties, antibacterial properties, etc. of the fibers and membranes.
[0010] The first object of the present invention is to provide a method for preparing a peanut skin extract / chitosan blend, comprising the following steps:
[0011] (1) adding peanut skin powder to an ethanol solution with a mass concentration of 0-100% for extraction, allowing the solution to stand after extraction, filtering, evaporating the filtrate, and drying to obtain a peanut skin extract;
[0012] (2) Dissolving the peanut skin extract in water, adding chitosan and acetic acid and mixing evenly to obtain a peanut skin extract / chitosan blend solution.
[0013] In one embodiment of the present invention, the ratio of peanut skin powder to ethanol solution in step (1) is 1 g: 25-35 mL.
[0014] In one embodiment of the present invention, the extraction in step (1) is performed at 45-55° C. for 50-70 min.
[0015] In one embodiment of the present invention, the evaporation in step (1) is carried out at 35-45° C. for 20-30 h.
[0016] In one embodiment of the present invention, the mass concentration of chitosan in water in step (2) is 2-3%.
[0017] In one embodiment of the present invention, the mass concentration of acetic acid in water in step (2) is 1.5-2.5%.
[0018] In one embodiment of the present invention, the amount of peanut skin extract used in step (2) is 3-15% of the mass of chitosan.
[0019] In one embodiment of the present invention, the peanut skin extract is dissolved in water in step (2) by mechanical stirring at a speed of 300 rpm for 2-5 hours.
[0020] In one embodiment of the present invention, the uniform mixing in step (2) is performed by stirring at 50-60° C. and 500-1000 rpm for 4-12 hours.
[0021] In one embodiment of the present invention, if the reaction temperature is not specifically specified in step (1) and step (2), the reaction is carried out at room temperature, which refers to 20-30°C.
[0022] The second object of the present invention is the peanut skin extract / chitosan blend prepared by the method of the present invention.
[0023] The third object of the present invention is to provide a method for preparing peanut skin extract / chitosan blended fibers, which uses the peanut skin extract / chitosan blended liquid of the present invention.
[0024] In one embodiment of the present invention, the method comprises the following steps:
[0025] The peanut skin extract / chitosan blended liquid is degassed and placed in a spinning solution injection container. The fibers are pushed through a coagulation bath at a certain speed. The fibers are then appropriately drawn and wound on a winding device for collection, and washed until the fibers are neutral. The neutral fibers are then immersed in a glycerol solution, taken out, and dried to obtain peanut skin extract / chitosan blended fibers.
[0026] In one embodiment of the present invention, the degassing is static degassing.
[0027] In one embodiment of the present invention, the advancing speed is 0.4-0.6 mL / min.
[0028] In one embodiment of the present invention, the coagulation bath is a mixed solution of NaOH solution and ethanol, wherein the mass concentration of the NaOH solution is 4-6%, the solvent is water, and the mass ratio of the NaOH solution to the ethanol is 2:1.
[0029] In one embodiment of the present invention, the winding temperature is 20-30° C., and the winding speed is 40-60 r / min.
[0030] In one embodiment of the present invention, washing is performed with water at a temperature of 20-30°C.
[0031] In one embodiment of the present invention, the volume concentration of the glycerol solution is 0.5-1.5%, and the solvent is water.
[0032] In one embodiment of the present invention, the immersion is carried out at 20-30° C. (normal temperature) for 1-3 hours.
[0033] In one embodiment of the present invention, the drying is air drying.
[0034] In one embodiment of the present invention, when the peanut skin extract / chitosan blend is used for spinning, the preparation method of the peanut skin extract / chitosan blend is as follows:
[0035] (1) adding peanut skin powder to an ethanol solution with a mass concentration of 0-100% for extraction, allowing the solution to stand after extraction, filtering, evaporating the filtrate, and drying to obtain a peanut skin extract;
[0036] (2) Dissolve the peanut skin extract in the extraction solvent, stir at 300 rpm for 2 hours, then add chitosan and acetic acid and mix evenly to obtain a peanut skin extract / chitosan blend; wherein the mixing is carried out by stirring at 60°C and 600 rpm for 12 hours; the amount of peanut skin extract used is 3-15% of the mass of chitosan, and the mass concentration of chitosan in water is 2.5%.
[0037] The fourth objective of the present invention is the peanut skin extract / chitosan blended fiber prepared by the method of the present invention.
[0038] The fifth object of the present invention is to provide a method for preparing a peanut skin extract / chitosan blend film, which uses the peanut skin extract / chitosan blend solution of the present invention.
[0039] In one embodiment of the present invention, the method comprises the following steps:
[0040] The peanut skin extract / chitosan blend liquid is poured into a mold and dried to obtain a peanut skin extract / chitosan blend film.
[0041] In one embodiment of the present invention, the drying is natural air drying.
[0042] In one embodiment of the present invention, when the peanut skin extract / chitosan blend is used to prepare a film, the preparation method of the peanut skin extract / chitosan blend is as follows:
[0043] (1) adding peanut skin powder to an ethanol solution with a mass concentration of 0-100% for extraction, allowing the solution to stand after extraction, filtering, evaporating the filtrate, and drying to obtain a peanut skin extract;
[0044] (2) Dissolve the peanut skin extract in the extraction solvent, stir at 300 rpm for 2 hours, then add chitosan and acetic acid and mix evenly to obtain a peanut skin extract / chitosan blend; wherein the mixing is carried out by stirring at 50°C and 600 rpm for 6 hours; the amount of peanut skin extract used is 5-15% of the mass of chitosan, and the mass concentration of chitosan in water is 2%.
[0045] The sixth objective of the present invention is the peanut skin extract / chitosan blended film prepared by the method of the present invention.
[0046] The seventh objective of the present invention is to use the peanut skin extract / chitosan blended liquid, peanut skin extract / chitosan blended fiber, and peanut skin extract / chitosan blended film described in the present invention in the field of antibacterial composite materials.
[0047] The eighth object of the present invention is to provide a method for simultaneously improving the mechanical properties, hydrophobic properties and antibacterial properties of composite materials, which adopts the peanut skin extract / chitosan blended liquid, peanut skin extract / chitosan blended fiber, and peanut skin extract / chitosan blended film described in the present invention.
[0048] [Beneficial Effects]
[0049] (1) The chitosan and peanut skin extract in the peanut skin extract / chitosan blend of the present invention have good compatibility.
[0050] (2) When the peanut skin extract / chitosan blend of the present invention is used as a spinning solution to prepare fibers, the apparent viscosity and tensile rheological properties of the spinning solution are improved compared with those of pure chitosan spinning solution, and the preparation method is simpler.
[0051] (3) Compared with pure chitosan fiber, the initial thermal decomposition temperature of peanut skin extract / chitosan blended fiber is increased, and the temperature corresponding to the maximum thermal decomposition rate is increased by about 10°C; the dry strength, wet strength and wet elongation at break are all increased; and the antibacterial property is enhanced.
[0052] (4) Compared with pure chitosan film, the modulus and hardness of the peanut skin extract / chitosan blend film increased; the roughness increased, and the surface hydrophobicity improved; the initial thermal decomposition temperature increased; the dry strength, wet strength and wet elongation at break all increased; in terms of color, the L value decreased significantly, and the a*, b*, and c* values increased significantly. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 These are the viscosity test results of peanut skin extract / chitosan blend and pure chitosan solution.
[0054] Figure 2 These are the test results of tensile rheological properties of peanut skin extract / chitosan blend and pure chitosan solution; among them, (a) is CS / PS-W series fiber; (b) is CS / PS-M series fiber; (c) is CS / PS-E series fiber; (d) is CS, CS / PS-W-15%, CS / PS-M-15%, CS / PS-E-15% fiber.
[0055] Figure 3 SEM images of the longitudinal surface of the fibers, where (a) is CS fiber (300 μm); (b) is CS fiber (10 μm); (c) is CS / PS-W-9% blended fiber (300 μm); (d) is CS / PS-W-9% blended fiber (10 μm); (e) is CS / PS-M-9% blended fiber (300 μm); (f) is CS / PS-M-9% blended fiber (10 μm); (g) CS / PS-E-9% blended fiber (300 μm); (h) CS / PS-E-9% blended fiber (10 μm).
[0056] Figure 4 These are SEM images of the fiber fracture surfaces, where (a) is CS fiber (300 μm); (b) is CS fiber (10 μm); (c) is CS / PS-W-9% blended fiber (300 μm); (d) is CS / PS-W-9% blended fiber (10 μm); (e) is CS / PS-M-9% blended fiber (300 μm); (f) is CS / PS-M-9% blended fiber (10 μm); (g) CS / PS-E-9% blended fiber (300 μm); and (h) CS / PS-E-9% blended fiber (10 μm).
[0057] Figure 5 These are the infrared spectra of CS fiber, CS / PS-W-9% blended fiber, CS / PS-M-9% blended fiber, and CS / PS-E-9% blended fiber.
[0058] Figure 6These are the test results of thermal stability of CS fiber, CS / PS-W-9% blended fiber, CS / PS-M-9% blended fiber, and CS / PS-E-9% blended fiber, where (a) is the mass residual rate; (b) is the mass loss rate.
[0059] Figure 7 The mechanical properties test results of peanut skin extract / chitosan blended fibers, where (a) is the breaking strength and (b) is the breaking elongation.
[0060] Figure 8 These are the test results of wet breaking strength and wet breaking elongation of peanut skin extract / chitosan blended fibers, where (a) is wet breaking strength; (b) is wet breaking elongation.
[0061] Fig. 9 SEM images of the surfaces of (a) CS film, (b) CS / PS-W-10% film, (c) CS / PS-M-10% film, and (d) CS / PS-E-10% film.
[0062] Fig.10 SEM images of the fracture surfaces of (a) CS film, (b) CS / PS-W-10% film, (c) CS / PS-M-10% film, and (d) CS / PS-E-10% film.
[0063] Fig.11 FT-IR spectra of CS film, CS / PS-W-15% film, CS / PS-M-15% film, and CS / PS-E-15% film.
[0064] Fig.12 The pressure-displacement relationship diagram of CS membrane and CS / PS-W-10% membrane, CS / PS-M-10% membrane, and CS / PS-E-10% blend membrane.
[0065] Fig.13 The hydrophilicity and hydrophobicity of CS membrane, CS / PS-W-10% membrane, CS / PS-M-10% membrane and CS / PS-E-10% blended membrane.
[0066] Fig.14 (a) Thermogravimetric and (b) mass loss rate curves of CS film and CS / PS-W-10% film, CS / PS-M-10% film, and CS / PS-E-10% blend film.
[0067] Fig.15 (a) Breaking strength and (b) Breaking elongation of CS film and CS / PS-W-10% film, CS / PS-M-10% film, and CS / PS-E-10% blend film.
[0068] Fig.16(a) Wet breaking strength and (b) wet breaking elongation of CS film and CS / PS-W-10% film, CS / PS-M-10% film, and CS / PS-E-10% blend film.
[0069] Fig.17 This is a physical picture of the film prepared in Comparative Example 3.
[0070] Fig.18 This is a physical picture of the film prepared in Comparative Example 4.
[0071] Fig.19 This is a physical picture of the film prepared in Comparative Example 5.
[0072] Fig. 20 This is a physical picture of the film prepared in Comparative Example 6. DETAILED DESCRIPTION
[0073] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explaining the present invention and are not used to limit the present invention.
[0074] Test method:
[0075] 1. Apparent viscosity
[0076] The apparent viscosity of different spinning solutions was measured using a NDJ-79 rotational viscometer at 25° C. The rotor used was No. 2 or No. 3, and the speed was 750 r / min.
[0077] 2. Extensional rheological properties
[0078] The rheological properties of the spinning solution under tension were tested using a HAAKE CaBER 1 extensional rheometer (Thermo Fisher Scientific, USA). A small amount of sample (<1 mL) was placed between two round flat plates, and the upper plate was rapidly separated from the lower plate at a set strain rate to form an unstable fluid filament. A laser micrometer monitored the change in the midpoint diameter of the gradually thinning fluid filament over time.
[0079] 3. Microstructure
[0080] The samples were scanned and photographed using a field emission electron microscope at an accelerating voltage of 5 kV to observe the morphological structures of the surfaces and fracture surfaces of the fibers and membranes; the fracture surfaces were obtained by tensile fracture.
[0081] 4. Fourier transform infrared spectroscopy
[0082] The FTIR spectra of the fibers and membranes were measured using a Fourier transform infrared spectrometer. The fibers and membranes were dried in a vacuum oven at 50 °C for 12 h and then -1 The resolution recorded is 4000 to 500 cm -1 spectrum.
[0083] 5. Fiber mechanical properties test
[0084] The samples were cut into strips of a specific size of 20 cm, placed under conditions of 25°C and 60% relative humidity for 48 hours, and the dry strength and elongation at break of the fibers were tested on a tensile testing machine. After being fully soaked in water, the surface water was wiped off, and the wet strength and wet elongation at break of the fibers were tested on a tensile testing machine.
[0085] Test parameters: clamping distance is 50mm, tensile speed is 100mm / min, at least 20 specimens for each sample. Use a thickness gauge to test the diameter of the fiber within the clamping distance, and the measured thickness value is accurate to 0.001mm.
[0086] 6. Membrane mechanical properties test
[0087] The sample was cut into strips of a specific size of 10×0.5 cm, placed at 25°C and a relative humidity of 60% for equilibration for 48 hours, and the dry strength and elongation at break of the membrane were tested on a tensile testing machine. After being fully soaked in water, the surface water was wiped off, and the wet strength and wet elongation at break of the membrane were tested on a tensile testing machine.
[0088] Test parameters: 1.3.3 The clamping distance is 50mm, the tensile speed is 100mm / min, and at least 10 specimens are required for each sample. The thickness of the inner film of the clamping distance is tested with a thickness meter, and the measured thickness value is accurate to 0.001mm.
[0089] 7. Antibacterial properties
[0090] The antibacterial properties of the fibers were determined according to GB / T 20944.3-2008 “Evaluation of antibacterial properties of textiles Part 3: Oscillation method”, the bacterial growth of the fibers was observed, and the bacterial reduction rate (%) of Staphylococcus aureus and Escherichia coli in the sample fibers was calculated according to the formula.
[0091]
[0092] Where: Y is the antibacterial rate of the sample (%); W is the average number of colonies of 3 control samples (pieces); Q is the average number of colonies of 3 samples (pieces).
[0093] 8. Thermal stability test
[0094] The thermal stability of the fibers and membranes was analyzed using a thermogravimetric analyzer. The samples were heated from 30°C to 800°C at a heating rate of 20°C / min in a nitrogen environment with a flow rate of 50 mL / min.
[0095] 9. Micromechanical properties test of membrane
[0096] The surface roughness and micromechanical properties of the membrane were detected using a nanoindenter, and the pressure applied by the probe was 1000 μN.
[0097] 10. Surface hydrophilicity and hydrophobicity test
[0098] The contact angle of the film was measured by a contact angle meter for 3 minutes, with a photo taken every 30 seconds. Five points of each sample were measured and the average value was taken. The size of the water droplet was 5 μL.
[0099] 11. Color feature value test
[0100] After pretreatment for 24 hours under standard conditions of temperature of 20±2°C and humidity of 65±3%, the color characteristic values of the fabric, L*, a*, b*, c*, h and K / S value, were measured using D65 light source and 10° viewing field.
[0101] The color characteristic value of each sample is the average value of 5 test points.
[0102] The raw materials used in the embodiments and comparative examples are:
[0103] Peanut skins: purchased from Anhui Shengshi Biotechnology Co., Ltd.
[0104] Peanut skin powder: Peanut skin is dried and crushed to obtain a particle size of 7 μm;
[0105] Chitosan: deacetylation degree 95%, viscosity 1250 mPa·s, purchased from Huaifang Haizhiyuan Biological Products Co., Ltd.;
[0106] Acetic acid, anhydrous ethanol, and sodium hydroxide were all of analytical grade and purchased from Sinopharm Chemical Reagent Co., Ltd.
[0107] In the examples, the % without specific content is mass percentage, the solution without specific solvent is water as solvent, and the reaction temperature without specific reaction temperature is carried out at room temperature, which means 20-30°C.
[0108] Example 1
[0109] A method for preparing a peanut skin extract / chitosan blend liquid comprises the following steps:
[0110] (1) 10 g of peanut skin powder was added to 300 mL of 50% ethanol solution, and the mixture was extracted at 50° C. for 60 min. After the extraction, the mixture was allowed to stand, filtered, and the filtrate was evaporated at 40° C. for 24 h and dried to obtain a peanut skin extract;
[0111] (2) Dissolve the peanut skin extract in water, stir at 300 rpm for 2 h to allow the peanut extract to be fully dissolved in the water, then add chitosan and acetic acid, stir at 600 rpm and 60° C. in a water bath for 12 h to mix evenly, and obtain a peanut skin extract / chitosan blend (CS / PS-M-12%); wherein the mass concentration of chitosan in water is 2.5%, the mass concentration of acetic acid in water is 2%, and the amount of peanut skin extract is 12% of the mass of chitosan.
[0112] Example 2
[0113] The amount of peanut skin extract in step (2) of Example 1 was adjusted to 3%, 6%, 9%, and 15% of the mass of chitosan, and the rest was consistent with Example 1 to obtain peanut skin extract / chitosan blends (CS / PS-M-3%, CS / PS-M-6%, CS / PS-M-9%, CS / PS-M-15%).
[0114] Example 3
[0115] The ethanol solution with a mass concentration of 50% in step (1) of Example 1 was adjusted to water, and the rest was kept consistent with Example 1 to obtain a peanut skin extract / chitosan blend (CS / PS-W-12%).
[0116] Example 4
[0117] The amount of peanut skin extract in step (2) of Example 3 was adjusted to 3%, 6%, 9%, and 15% of the mass of chitosan, and the rest was consistent with Example 3 to obtain peanut skin extract / chitosan blends (CS / PS-W-3%, CS / PS-W-6%, CS / PS-W-9%, CS / PS-W-15%).
[0118] Example 5
[0119] The ethanol solution with a mass concentration of 50% in step (1) of Example 1 was adjusted to anhydrous ethanol, and the rest was kept consistent with Example 1 to obtain a peanut skin extract / chitosan blend (CS / PS-E-12%).
[0120] Example 6
[0121] The amount of peanut skin extract in step (2) of Example 3 was adjusted to 3%, 6%, 9%, and 15% of the mass of chitosan, and the rest was consistent with Example 3 to obtain peanut skin extract / chitosan blends (CS / PS-E-3%, CS / PS-E-6%, CS / PS-E-9%, CS / PS-E-15%).
[0122] Comparative Example 1
[0123] The peanut skin extract in Example 1 was omitted, and the other steps were the same as in Example 1 to obtain a pure chitosan solution (CS).
[0124] The products obtained in Examples 1-6 and Comparative Example 1 were subjected to performance tests, and the test results are as follows:
[0125] Figure 1 The viscosity test results of peanut skin extract / chitosan blend and pure chitosan solution are shown in Figure 2. Figure 1 It can be seen that the viscosity of pure chitosan spinning solution is the lowest, and the viscosity of peanut skin extract / chitosan blend solution increases with the increase of peanut skin extract content, among which CS / PS-M-15% has the highest viscosity. When the viscosity of the blend is high, the primary fibrils are not easy to break and show good spinnability.
[0126] Figure 2 The results of tensile rheological properties test of peanut skin extract / chitosan blend and pure chitosan solution; (a) is CS / PS-W series fiber; (b) is CS / PS-M series fiber; (c) is CS / PS-E series fiber; (d) is CS, CS / PS-W-15%, CS / PS-M-15%, CS / PS-E-15% fiber. Figure 2 It can be seen that the rupture time from the beginning of stretching to the rupture of CS / PS-W, CS / PS-M, and CS / PS-E blends increased significantly compared with the pure chitosan solution, and it was less likely to break as the content of peanut skin extract increased. Compared with the pure chitosan solution, it took longer for the three blends of CS / PS-W, CS / PS-M, and CS / PS-E to stretch the CS / PS blend to the same diameter. The longer rupture time indicates that the ductility of the blend becomes better after the addition of peanut skin extract, which may make the blend have better spinnability. Good spinnability can improve the mechanical properties of the fiber. With the improvement of spinnability, the molecular chains in the fiber can be better arranged to eliminate the defects of the fiber, thereby improving its mechanical properties.
[0127] Example 7
[0128] A method for preparing peanut skin extract / chitosan blended fiber comprises the following steps:
[0129] The pure chitosan solution prepared in Comparative Example 1 and the peanut skin extract / chitosan blended solution prepared in Examples 1-6 were allowed to stand for degassing, placed in a microinjection pump, and propelled at a flow rate of 0.5 mL / min, so that the fiber passed through a coagulation bath (a mixed solution of NaOH solution and ethanol in a mass ratio of 2:1, and a mass concentration of NaOH solution of 5%) at a certain speed, and then at room temperature, the fiber was appropriately stretched and the fiber was wound on a winding device at a speed of 50 r / min for collection, and washed with water at 25°C until the fiber was neutral; thereafter, the neutral fiber was immersed in a glycerol solution with a volume fraction of 1% at room temperature for 2 hours, taken out, and naturally dried to obtain peanut skin extract / chitosan blended fibers (CS fibers, CS / PS blended fibers).
[0130] The obtained peanut skin extract / chitosan blended fiber was subjected to performance testing, and the test results are as follows:
[0131] Figure 3 SEM images of the longitudinal surface of the fibers, where (a) is CS fiber (300 μm); (b) is CS fiber (10 μm); (c) is CS / PS-W-9% blended fiber (300 μm); (d) is CS / PS-W-9% blended fiber (10 μm); (e) is CS / PS-M-9% blended fiber (300 μm); (f) is CS / PS-M-9% blended fiber (10 μm); (g) CS / PS-E-9% blended fiber (300 μm); (h) CS / PS-E-9% blended fiber (10 μm).
[0132] Figure 4 These are SEM images of the fiber fracture surfaces, where (a) is CS fiber (300 μm); (b) is CS fiber (10 μm); (c) is CS / PS-W-9% blended fiber (300 μm); (d) is CS / PS-W-9% blended fiber (10 μm); (e) is CS / PS-M-9% blended fiber (300 μm); (f) is CS / PS-M-9% blended fiber (10 μm); (g) CS / PS-E-9% blended fiber (300 μm); and (h) CS / PS-E-9% blended fiber (10 μm).
[0133] from Figure 3 and Figure 4 It can be seen that the surface of chitosan CS fiber is smooth and flat. After adding peanut skin extract, smaller particles begin to appear on the surface of the blended fiber. The addition of peanut skin extract will make the cross section present a tough fracture state, the fracture end face is rough, and there are no obvious large particles in the cross section, which shows that the compatibility between peanut skin extract and chitosan is very good.
[0134] Figure 5The infrared spectra of CS fiber, CS / PS-W-9% blended fiber, CS / PS-M-9% blended fiber, and CS / PS-E-9% blended fiber. Figure 5 It can be seen that CS fiber is at 3352cm -1 The wide absorption peak is shown at the bottom, which is caused by the overlap of multiple absorption peaks of stretching vibration of O—H and N—H. In the infrared spectrum of the blended fiber, after the peanut skin extract is added, no new peak appears in the FT-IR image, indicating that the overlapping peaks of multiple absorption of O—H and N—H stretching vibration of chitosan move to the low wave number region. This phenomenon is mainly attributed to the intermolecular interaction between the phenolic hydroxyl groups of the peanut skin extract and the hydroxyl groups of chitosan, which reduces the chemical bond force constant of the participating hydroxyl groups, causing their absorption frequency to move to the low wave number direction.
[0135] Figure 6 The test results of thermal stability of CS fiber, CS / PS-W-9% blended fiber, CS / PS-M-9% blended fiber, and CS / PS-E-9% blended fiber, where (a) is the mass residual rate and (b) is the mass loss rate. Figure 6 It can be seen that the initial thermal decomposition temperature of CS / PS blended fibers is higher than that of CS films, and the temperature corresponding to the maximum thermal decomposition rate of CS / PS blended films increases by about 10°C. These results indicate that the addition of PS can improve the thermal stability of CS / PS blended fibers, which is mainly attributed to the intermolecular forces between chitosan molecules and peanut skin extracts.
[0136] Figure 7 The mechanical properties test results of peanut skin extract / chitosan blended fibers, where (a) is the breaking strength and (b) is the breaking elongation. Figure 8 The test results of wet breaking strength and wet breaking elongation of peanut skin extract / chitosan blended fibers are shown in Figure 2, where (a) is wet breaking strength and (b) is wet breaking elongation. Figure 7 and Figure 8It can be seen that: except for the wet CS / PS-E blended fiber, the breaking strength increases with the increase of peanut skin content, the breaking strength of other blended fibers at different humidity levels shows a trend of increasing first and then decreasing. When the PS dosage is 6%, the dry breaking strength of the blended fiber is improved most significantly; when the PS dosage is 12%, the wet breaking strength of the blended fiber is improved most significantly. In particular, the dry strength of the CS / PS-M blended fiber is increased by 160% and the wet strength is increased by 115% compared with the CS fiber. Under dry conditions, the elongation at break is reduced compared with pure chitosan; under completely wet conditions, the elongation at break of the blended fiber shows a trend of increasing first and then decreasing. When the PS dosage of the CS / PS-W blended fiber is 3%, the elongation at break is increased by 19% compared with the CS fiber; when the PS dosage of the CS / PS-M blended fiber is 3%, the elongation at break is increased by 4% compared with the CS fiber; when the PS dosage of the CS / PS-E blended fiber is 12%, the elongation at break is increased by 39% compared with the CS fiber. This is mainly attributed to the ionic cross-linking formed between peanut skin extract and chitosan.
[0137] Table 1 shows the antibacterial rate of CS fiber and CS / PS blended fiber. It can be seen from Table 1 that the bacterial reduction rate of CS / PS blended fiber is significantly higher than that of CS fiber, especially for E. coli. The bactericidal rate of CS fiber against E. coli is 76.28%, and the bactericidal rate against Staphylococcus aureus is only 46.07%, which is difficult to meet the requirements of the antibacterial textile standard. However, the bactericidal rate of CS / PS-M-6% blended fiber against E. coli is as high as 95.03%, and the bactericidal rate against Staphylococcus aureus is 71.20%, which can meet the requirements of some antibacterial textiles.
[0138] Table 1 Antibacterial rate of CS fiber and CS / PS blended fiber
[0139]
[0140] Example 8
[0141] A method for preparing a peanut skin extract / chitosan blend liquid comprises the following steps:
[0142] (1) 10 g of peanut skin powder was added to 300 mL of 50% ethanol solution, and the mixture was extracted at 50° C. for 60 min. After the extraction, the mixture was allowed to stand, filtered, and the filtrate was evaporated at 40° C. for 24 h and dried to obtain a peanut skin extract;
[0143] (2) Dissolve the peanut skin extract in the extraction solvent, stir at 300 rpm for 2 h to allow the peanut extract to be fully dissolved in the water, then add chitosan and acetic acid, stir at 600 rpm and 50° C. in a water bath for 6 h to mix evenly, and obtain a peanut skin extract / chitosan blend (CS / PS-M-15%); wherein the mass concentration of chitosan in water is 2%, the mass concentration of acetic acid in water is 2%, and the amount of peanut skin extract is 15% of the mass of chitosan.
[0144] Example 9
[0145] The amount of peanut skin extract in step (2) of Example 8 was adjusted to 5% and 10% of the mass of chitosan; the rest was kept consistent with Example 8 to obtain peanut skin extract / chitosan blends (CS / PS-M-5%, CS / PS-M-10%).
[0146] Example 10
[0147] The ethanol solution with a mass concentration of 50% in step (1) of Example 8 was adjusted to water, and the rest was kept consistent with Example 8 to obtain a peanut skin extract / chitosan blend (CS / PS-W-15%).
[0148] Embodiment 11
[0149] The amount of peanut skin extract in step (2) of Example 10 was adjusted to 5% and 10% of the mass of chitosan, and the rest was kept consistent with Example 11 to obtain peanut skin extract / chitosan blends (CS / PS-W-5%, CS / PS-W-10%).
[0150] Example 12
[0151] The ethanol solution with a mass concentration of 50% in step (1) of Example 8 was adjusted to anhydrous ethanol, and the rest was kept consistent with Example 8 to obtain a peanut skin extract / chitosan blend (CS / PS-E-15%).
[0152] Example 13
[0153] The amount of peanut skin extract in step (2) of Example 12 was adjusted to 5% and 10% of the mass of chitosan, and the rest was kept consistent with Example 12 to obtain peanut skin extract / chitosan blends (CS / PS-E-5%, CS / PS-E-10%).
[0154] Comparative Example 2
[0155] The peanut skin extract in Example 8 was omitted, and the other steps were the same as in Example 8 to obtain a pure chitosan solution (CS).
[0156] Embodiment 14
[0157] A method for preparing a peanut skin extract / chitosan blended film comprises the following steps:
[0158] 40 g of pure chitosan solution prepared in Comparative Example 2 and 40 g of peanut skin extract / chitosan blended solution prepared in Examples 9-13 were poured into a disc with a diameter of 15 cm and dried naturally to obtain chitosan film and peanut skin extract / chitosan blended film.
[0159] The obtained membrane was subjected to performance test, and the test results are as follows:
[0160] Fig. 9 SEM images of the surfaces of (a) CS film, (b) CS / PS-W-10% film, (c) CS / PS-M-10% film, and (d) CS / PS-E-10% film. Fig.10 SEM images of the fracture surfaces of (a) CS film, (b) CS / PS-W-10% film, (c) CS / PS-M-10% film, and (d) CS / PS-E10% film. Fig. 9 and Fig.10 It can be seen that the surface of the chitosan film is smooth and flat, and after adding the peanut skin extract, smaller particles begin to appear on the film surface; the chitosan film shows a brittle fracture trend, and the addition of the peanut skin extract will make the cross section show a tough fracture state, with a rough fracture end surface. There are no obvious large particles in the cross section, which shows that the peanut skin extract and chitosan are very compatible.
[0161] Fig.11 FT-IR spectra of CS film, CS / PS-W-15% film, CS / PS-M-15% film, and CS / PS-E-15% film. Fig.11 It can be seen that the CS film is at 3223cm -1 The wide absorption peak is shown at 40°, which is caused by the overlap of multiple absorption peaks of stretching vibration of O—H and N—H. In the infrared spectrum of the blended film, when the peanut skin extract is added to the film, no new peak appears in the FT-IR image, indicating that the overlapping peaks of multiple absorption of O—H and N—H stretching vibration of chitosan move to the low wave number region. This phenomenon is mainly attributed to the intermolecular interaction between the phenolic hydroxyl groups of the peanut skin extract and the hydroxyl groups of chitosan, which reduces the chemical bond force constant of the participating hydroxyl groups, causing their absorption frequency to move to the low wave number direction.
[0162] Fig.12 Table 2 shows the relationship between pressure and displacement of CS membrane and CS / PS-W-10% membrane, CS / PS-M-10% membrane, and CS / PS-E-10% blend membrane. Table 3 shows the micromechanical properties of CS membrane and CS / PS blend membrane. Fig.12As can be seen from Table 2, after adding peanut skin extract, the modulus, hardness and roughness of the three CS / PS blend films increased, especially the CS / PS-M film, which had a more significant effect and a smaller roughness than the other two blend films. The blend films were not easily deformed after being subjected to force, and were easier to recover after deformation, and the CS / PS-M film was also more effective. In summary, this is all attributed to the intermolecular effect between CS and PS, which changes the structure of chitosan and makes it more compact.
[0163] Table 2 Micromechanical properties of CS membrane and CS / PS blend membrane
[0164]
[0165] Fig.13 The hydrophilicity and hydrophobicity of CS membrane, CS / PS-W-10% membrane, CS / PS-M-10% membrane and CS / PS-E-10% blend membrane. Fig.13 It can be seen that the surface hydrophobicity of the three CS / PS blend films has been improved, especially after 3 minutes, the contact angles of the three CS / PS blend films have decreased by less than 13%. Compared with the CS film, the contact angles have increased by 104%-116%, among which the effect of the blend film CS / PS-E is more significant, with the contact angle increased by 116%.
[0166] Fig.14 (a) Thermogravimetric and (b) mass loss rate curves of CS film and CS / PS-W-10% film, CS / PS-M-10% film, and CS / PS-E-10% blend film. Fig.14 It can be seen that the initial thermal decomposition temperature of the CS / PS blend film is higher than that of the CS film, and the temperature corresponding to the maximum thermal decomposition rate of the CS / PS blend film increases by about 10°C. These results show that the addition of PS can improve the thermal stability of the CS / PS blend film, which is mainly attributed to the intermolecular force between the chitosan molecules and the peanut skin extract.
[0167] Fig.15 (a) Breaking strength and (b) Breaking elongation of CS film and CS / PS-W-10% film, CS / PS-M-10% film, and CS / PS-E-10% blend film. Fig.16 (a) Wet breaking strength and (b) wet breaking elongation of CS film and CS / PS-W-10% film, CS / PS-M-10% film, CS / PS-E-10% blend film. Fig.15 and Fig.16It can be seen that: with the increase of peanut skin content, the breaking strength of the blended film at different humidity shows a trend of increasing first and then decreasing. When the PS dosage is 5%, the breaking strength of the blended film is most significantly improved, especially the blended film CS / PS-M, compared with the CS film, the dry strength is increased by 67%, and the wet strength is increased by 155%. Under dry conditions, the elongation at break is lower than that of pure chitosan; under completely wet conditions, the elongation at break is higher than that of pure chitosan. When the PS dosage is 5%, the elongation at break of the blended film CS / PS-E is increased by 410% compared with the CS film.
[0168] Table 3 shows the color characteristic values of CS film and CS / PS blend film. It can be seen from Table 3 that after adding peanut skin extract, the brightness of the chitosan film is significantly reduced, and the a*, b*, and c* values are significantly increased. With the increase in the amount of peanut skin extract, the color of the CS / PS blend film tends to be more red and yellow, and the color becomes more saturated.
[0169] Table 3 Color characteristic values of CS film and CS / PS blend film
[0170]
[0171] Comparative Example 3
[0172] A method for preparing a peanut skin extract / chitosan blended film comprises the following steps:
[0173] (1) 10 g of peanut skin powder was added to 300 mL of 50% ethanol solution, and the mixture was extracted at 50° C. for 60 min. After the extraction, the mixture was allowed to stand, filtered, and the filtrate was evaporated at 40° C. for 24 h and dried to obtain a peanut skin extract;
[0174] (2) Dissolve chitosan in an aqueous solution of acetic acid, then add peanut skin extract, stir at 600 rpm and 50°C in a water bath for 4 h to mix evenly, and obtain a peanut skin extract / chitosan blend (CS / PS-M-15%); wherein the mass concentration of chitosan in water is 2%, the mass concentration of acetic acid in water is 2%, and the amount of peanut skin extract is 15% of the mass of chitosan.
[0175] (3) Pour 40 g of the peanut skin extract / chitosan blend into a disc with a diameter of 15 cm and dry it naturally to obtain a peanut skin extract / chitosan blend film.
[0176] The obtained peanut skin extract / chitosan blended film was subjected to performance testing, and the test results are as follows:
[0177] Fig.17 This is a physical picture of the film prepared in Comparative Example 3. Fig.17 It can be seen that there are large particles on the surface of the membrane and the uniformity is very poor.
[0178] Comparative Example 4
[0179] A method for preparing a peanut skin extract / chitosan blended film comprises the following steps:
[0180] (1) 10 g of peanut skin powder was added to 300 mL of 50% ethanol solution, and the mixture was extracted at 50° C. for 60 min. After the extraction, the mixture was allowed to stand, filtered, and the filtrate was evaporated at 40° C. for 24 h and dried to obtain a peanut skin extract;
[0181] (2) Dissolve the peanut skin extract in water, stir at 300 rpm for 2 h to allow the peanut extract to be fully dissolved in the water, then add chitosan and acetic acid, stir at 600 rpm and 50° C. in a water bath for 4 h to mix evenly, and obtain a peanut skin extract / chitosan blend (CS / PS-M-15%); wherein the mass concentration of chitosan in water is 2%, the mass concentration of acetic acid in water is 2%, and the amount of peanut skin extract is 15% of the mass of chitosan.
[0182] (3) Pour 40 g of the peanut skin extract / chitosan blend into a disc with a diameter of 15 cm and dry it naturally to obtain a peanut skin extract / chitosan blend film.
[0183] The obtained peanut skin extract / chitosan blended film was subjected to performance testing, and the test results are as follows:
[0184] Fig.18 This is a physical picture of the film prepared in Comparative Example 4. Fig.18 It can be seen that there are small particles on the surface of the membrane and the uniformity is very poor.
[0185] Comparative Example 5
[0186] A method for preparing a peanut skin extract / chitosan blended film comprises the following steps:
[0187] (1) 10 g of peanut skin powder was added to 300 mL of 50% ethanol solution, and the mixture was extracted at 50° C. for 60 min. After the extraction, the mixture was allowed to stand, filtered, and the filtrate was evaporated at 40° C. for 24 h and dried to obtain a peanut skin extract;
[0188] (2) Dissolve the peanut skin extract in the extraction solvent, stir at 300 rpm for 2 h to allow the peanut extract to be fully dissolved in the water, then add chitosan and acetic acid, stir at 600 rpm and 50° C. in a water bath for 4 h to mix evenly, and obtain a peanut skin extract / chitosan blend (CS / PS-M-15%); wherein the mass concentration of chitosan in water is 2%, the mass concentration of acetic acid in water is 2%, and the amount of peanut skin extract is 15% of the mass of chitosan.
[0189] (3) Pour 40 g of the peanut skin extract / chitosan blend into a disc with a diameter of 15 cm and dry it naturally to obtain a peanut skin extract / chitosan blend film.
[0190] The obtained peanut skin extract / chitosan blended film was subjected to performance testing, and the test results are as follows:
[0191] Fig.19 This is a physical picture of the film prepared in Comparative Example 5. Fig.19 It can be seen that there are some flocs on the membrane surface and the uniformity is very poor.
[0192] Comparative Example 6
[0193] A method for preparing a peanut skin extract / chitosan blended film comprises the following steps:
[0194] (1) 10 g of peanut skin powder was added to 300 mL of 50% ethanol solution, and the mixture was extracted at 50° C. for 60 min. After the extraction, the mixture was allowed to stand, filtered, and the filtrate was evaporated at 40° C. for 24 h and dried to obtain a peanut skin extract;
[0195] (2) Dissolve the peanut skin extract in the extraction solvent, stir at 300 rpm for 2 h to allow the peanut extract to be fully dissolved in the water, then add chitosan and acetic acid, stir at 600 rpm and 50° C. in a water bath for 6 h to mix evenly, and obtain a peanut skin extract / chitosan blend (CS / PS-M-15%); wherein the mass concentration of chitosan in water is 2%, the mass concentration of acetic acid in water is 2%, and the amount of peanut skin extract is 15% of the mass of chitosan.
[0196] (3) Pour 40 g of peanut skin extract / chitosan blend into a 15 cm diameter disc, dry naturally, and then soak it in a 1% NaOH solution at room temperature for 30 min, wash it with a large amount of deionized water until it is neutral, and then dry it to obtain a peanut skin extract / chitosan blend film.
[0197] The obtained peanut skin extract / chitosan blended film was subjected to performance testing, and the test results are as follows:
[0198] Fig. 20 This is a physical picture of the film prepared in Comparative Example 6. Fig. 20 It can be seen that the film is very wrinkled and brittle.
[0199] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for preparing a peanut skin extract / chitosan blend, characterized in that: The steps include: (1) adding peanut skin powder to an ethanol solution with a mass concentration of 0-100% for extraction, allowing the solution to stand after extraction, filtering, evaporating the filtrate, and drying to obtain a peanut skin extract; (2) Dissolving the peanut skin extract in an extraction solvent, adding chitosan and acetic acid and mixing evenly to obtain a peanut skin extract / chitosan blend solution.
2. The method according to claim 1, characterized in that The amount of peanut skin extract used in step (2) is 3-15% of the mass of chitosan.
3. The peanut skin extract / chitosan blend prepared by the method according to claim 1 or 2.
4. A method for preparing peanut skin extract / chitosan blended fiber, characterized in that: The peanut skin extract / chitosan blended liquid as claimed in claim 3 is used.
5. The method according to claim 4, characterized in that The method comprises the following steps: The peanut skin extract / chitosan blended liquid is degassed and placed in a spinning solution injection container. The fibers are pushed through a coagulation bath at a certain speed. The fibers are then appropriately drawn and wound on a winding device for collection, and washed until the fibers are neutral. The neutral fibers are then immersed in a glycerol solution, taken out, and dried to obtain peanut skin extract / chitosan blended fibers.
6. Peanut skin extract / chitosan blended fiber prepared by the method according to claim 4 or 5.
7. A method for preparing a peanut skin extract / chitosan blend film, characterized in that: The peanut skin extract / chitosan blended liquid as claimed in claim 3 is used.
8. The peanut skin extract / chitosan blended film prepared by the method according to claim 7.
9. Use of the peanut skin extract / chitosan blended fiber according to claim 6 and the peanut skin extract / chitosan blended film according to claim 8 in the field of antibacterial composite materials.
10. A method for simultaneously improving the mechanical properties, hydrophobic properties, and antibacterial properties of a composite material, characterized in that: The peanut skin extract / chitosan blended fiber according to claim 6 or the peanut skin extract / chitosan blended film according to claim 8.
Citation Information
Patent Citations
Multifunctional chitosan / gallnut tannin blended membrane and preparation method thereof
CN111234324A
Method for preparing high-strength chitosan fiber from multi-component coagulated bath lotion
CN102912475A
Preservative film containing peanut coat procyanidine inclusion compound and preparation method thereof
CN112409615A