Preparation method of self-repairing coating, photovoltaic panel, preparation method of photovoltaic panel and photovoltaic module

By applying polyurethane elastomer-organic fluororesin composite coating on photovoltaic panels, the problem of prone to cracking and damage of photovoltaic panels is solved, self-repair and weather resistance are achieved, the life of photovoltaic modules is extended and the power generation efficiency is improved.

CN118956249APending Publication Date: 2024-11-15SHENZHEN HELLO TECH ENERGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411041164.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Photovoltaic panels are prone to cracking and damage during long-term use, resulting in a decrease in output power and may cause damage to the internal part of the solar cell. In severe cases, the entire component may be scrapped.

Method used

By using the preparation method of self-healing coating, the polyol and isocyanate curing agent are cross-linked under the action of chain extender to form polyurethane elastomer and compound with organic fluororesin to prepare weather resistance, mechanical strength and flexibility A composite coating of polyurethane elastomer-organic fluororesin for protecting photovoltaic panels.

Benefits of technology

This composite coating not only has self-healing function, it can withstand the influence of physical damage and environmental factors, extend the service life of photovoltaic modules, and improve power generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956249A_ABST
    Figure CN118956249A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a self-repairing coating, a photovoltaic panel, a preparation method of the photovoltaic panel and a photovoltaic module, relates to the technical field of photovoltaics, and aims to solve the problems that the photovoltaic panel is easy to crack and damage and the like. The preparation method of the self-repairing coating comprises the following steps: preparing the self-repairing coating through preparation raw materials; wherein the preparation raw materials comprise polyhydric alcohols, and the mass percent of the polyhydric alcohols in the preparation raw materials is greater than or equal to 45% and less than or equal to 70%; the isocyanate curing agent accounts for more than or equal to 4.5% and less than or equal to 10% of the preparation raw materials in percentage by mass; the chain extender accounts for more than or equal to 2% and less than or equal to 5% of the preparation raw materials in percentage by mass; the organic fluorine resin accounts for more than or equal to 3% and less than or equal to 5% by mass of the preparation raw materials; and the solvent accounts for more than or equal to 20% and less than or equal to 40% by mass of the preparation raw materials. The prepared coating can resist ultraviolet radiation, and the service life of the photovoltaic module is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of photovoltaic technology, and in particular to a method for preparing a self-repairing coating, a photovoltaic panel and a method for preparing the same, and a photovoltaic module. Background Art

[0002] With the development of solar cell technology and the continuous improvement of solar cell working efficiency, solar panels tend to be light, compact and efficient. The reform of solar energy technology and the continuous optimization of packaging materials have promoted the development of lightweight photovoltaic panels. The use of lightweight photovoltaic panels in color steel roof tiles, photovoltaic roofs, balconies, courtyards, RVs, yachts and other scenes has been increasingly promoted.

[0003] However, with long-term use, in scenes with more human contact such as RVs, yachts and courtyards, it is easy to cause surface scratches, cracks, breakage, etc., resulting in a decrease in output power and the appearance of hot spots. If the defects caused by the damage penetrate the front panel protective layer, water vapor in the air may penetrate into the interior of the solar cell through the defects, directly causing damage to the interior of the solar cell. In severe cases, it may even cause the entire solar cell module to be scrapped. Summary of the invention

[0004] The present invention aims to solve or improve the problems of photovoltaic panels being prone to cracking and damage in the prior art.

[0005] A first aspect of the present invention is to provide a method for preparing a self-repairing coating.

[0006] A second aspect of the present invention is to provide a photovoltaic panel.

[0007] A third aspect of the present invention is to provide a photovoltaic module.

[0008] A fourth aspect of the present invention is to provide a method for preparing a photovoltaic panel.

[0009] The present invention provides a method for preparing a self-repairing coating, which is applied to a photovoltaic module. The method for preparing the self-repairing coating comprises: preparing the self-repairing coating by preparing raw materials; wherein the raw materials comprise: a polyol, the mass percentage of the polyol in the preparation raw materials is greater than or equal to 45%, and less than or equal to 70%; an isocyanate curing agent, the mass percentage of the isocyanate curing agent in the preparation raw materials is greater than or equal to 4.5%, and less than or equal to 10%; a chain extender, the mass percentage of the chain extender in the preparation raw materials is greater than or equal to 2%, and less than or equal to 5%; an organic fluorine resin, the mass percentage of the organic fluorine resin in the preparation raw materials is greater than or equal to 3%, and less than or equal to 5%; and a solvent, the mass percentage of the solvent in the preparation raw materials is greater than or equal to 20%, and less than or equal to 40%.

[0010] The present invention obtains a polyurethane elastomer by cross-linking a polyol and an isocyanate curing agent under the action of a chain extender, and then the polyurethane elastomer can be compounded with an organic fluorine resin to obtain a polyurethane elastomer-organic fluorine resin composite coating. Since the organic fluorine resin coating has extremely high weather resistance, it can resist the influence of ultraviolet radiation, extreme temperature changes, humidity, weathering and other natural environmental factors, protect photovoltaic panels from external damage, and extend the service life of photovoltaic modules. In addition, organic fluorine resin coatings usually have good mechanical strength and flexibility, and can resist physical damage such as impact and scratches. It can be seen that the composite coating prepared by the present invention not only has a self-repairing function, but is also very suitable for photovoltaic panels, and has better heat resistance, corrosion resistance and impact resistance, which improves the power generation of photovoltaic modules.

[0011] In the above embodiment, optionally, the mass percentage of the polyol in the preparation raw material is greater than or equal to 50% and less than or equal to 65%, for example, 50%, 55% or 60%.

[0012] In the above embodiment, optionally, the mass percentage of the isocyanate curing agent in the preparation raw materials is greater than or equal to 5% and less than or equal to 8%, for example, 6%, 7% or 8%.

[0013] In the above embodiment, optionally, the mass percentage of the chain extender in the preparation raw material is greater than or equal to 3% and less than or equal to 4%, for example, 3% or 4%.

[0014] In the above embodiment, optionally, the mass percentage of the organic fluorine resin in the preparation raw material is greater than or equal to 4% and less than or equal to 5%, for example, 4% or 5%.

[0015] In the above embodiment, optionally, the mass percentage of the solvent in the raw material is greater than or equal to 25% and less than or equal to 35%, for example, 25%, 30% or 35%. Of course, the mass percentage of the solvent is not limited to 20% to 40%. The solvent only plays a dissolving role in the whole process, does not participate in the reaction, and does not affect the performance of the coating. When other components are determined, the total component can be made 100% by the solvent.

[0016] In the above embodiment, optionally, the organic fluorine resin includes one of the following or a combination thereof: polytetrafluoroethylene, fluorinated ethylene propylene copolymer, polyperfluoroalkoxy resin, polyvinylidene fluoride and ethylene-tetrafluoroethylene polymer.

[0017] In this embodiment, the above-mentioned organic fluorine resins have the advantages of good weather resistance, chemical stability, electrical insulation, high mechanical strength, flexibility and high flame retardancy. After compounding with polyurethane elastomer, they can greatly improve the strength and heat resistance of photovoltaic panels and extend the service life of photovoltaic modules.

[0018] In the above embodiment, optionally, the polyol includes aliphatic polyether, or the polyol includes aliphatic polyether, and the aliphatic polyether includes polytetramethylene ether diol. And / or the polyol includes polyester polyol, or the polyol includes polyester polyol, and the polyester polyol includes polycaprolactone diol and / or adipic acid polyester polyol. And / or the isocyanate curing agent includes isophorone diisocyanate curing agent and / or hexamethylene diisocyanate curing agent.

[0019] In this embodiment, the hydroxyl groups in the aliphatic polyether and polyester polyol can react with the isocyanate groups in the isocyanate to form urethane bonds, thereby polymerizing to obtain a polyurethane prepolymer.

[0020] In the above embodiment, optionally, the polyol includes a polyol having a hydroxyl value greater than or equal to 150 mgKOH / g and less than or equal to 350 mgKOH / g.

[0021] In this embodiment, the hydroxyl value of the polyol is greater than or equal to 150 mgKOH / g and less than or equal to 350 mgKOH / g; for example, it can be 200 mgKOH / g or 250 mgKOH / g. Polyols with higher hydroxyl values ​​will form more crosslinking points, resulting in an increase in the crosslinking density of the coating, thereby improving the hardness, wear resistance and chemical resistance of the coating. However, too high a crosslinking density may make the coating brittle and hard, so it can be controlled within 200 mgKOH / g to 250 mgKOH / g.

[0022] In the above embodiment, optionally, in the isocyanate curing agent, the mass percentage of the isocyanate group in the isocyanate curing agent is greater than or equal to 15% and less than or equal to 35%.

[0023] In this embodiment, the isocyanate group also affects the degree of crosslinking. A high proportion of isocyanate groups will result in a higher crosslinking density. The denser the crosslinking network, the higher the hardness, chemical resistance and mechanical strength of the coating will generally be, but the flexibility and elongation will be relatively lower. Therefore, it is most appropriate to control the mass proportion of isocyanate groups to 15% to 35%, and can also be controlled to 20% to 25%, for example, 20%, 22% or 25%.

[0024] In the above embodiment, optionally, the preparation raw material further includes a leveling agent, and the mass percentage of the leveling agent in the preparation raw material is greater than or equal to 0.05% and less than or equal to 0.1%.

[0025] In this embodiment, the leveling agent can improve the surface flatness, help the coating to be evenly distributed on the substrate, reduce the orange peel effect, improve the flatness and smoothness of the coating, and make the coating surface smoother. In addition, it also helps to quickly release the air and solvent in the coating, prevent the formation of pinholes and bubbles, and improve the density of the coating. Optionally, the mass percentage of the leveling agent in the preparation raw material is 0.05%, 0.08% or 0.1%.

[0026] In the above embodiment, optionally, the preparation raw material further includes a dispersant, and the mass percentage of the dispersant in the preparation raw material is greater than or equal to 0.02% and less than or equal to 0.05%.

[0027] In this embodiment, the dispersant can effectively reduce the attraction between particles, prevent the particles from agglomerating, and ensure that the components are evenly distributed in the coating, which has a direct impact on the color consistency, hiding power and glossiness of the coating. The dispersant can also improve the rheological properties of the coating, so that the coating has better fluidity during construction, which is convenient for spraying, brushing or roller coating, while reducing splashing and dripping, and improving construction efficiency. Optionally, the mass percentage of the dispersant in the prepared raw materials is equal to 0.02%, 0.03%, 0.04% or 0.05%.

[0028] In the above embodiment, optionally, the raw material for preparation further includes an antioxidant, and the weight percentage of the antioxidant in the raw material for preparation is greater than or equal to 0.1% and less than or equal to 0.3%.

[0029] In this embodiment, the antioxidant can prevent or slow down the oxidative aging of the coating caused by environmental factors such as ultraviolet rays, heat, oxygen, etc., thereby helping to maintain the original mechanical properties of the coating and extend the service life of the coating. Optionally, the antioxidant accounts for 0.1%, 0.2% or 0.3% by mass of the raw material.

[0030] In the above embodiment, optionally, the raw material further comprises an ultraviolet absorber, and the mass percentage of the ultraviolet absorber in the raw material is greater than or equal to 0.5% and less than or equal to 1.5%.

[0031] In this embodiment, the ultraviolet absorber can significantly improve the resistance of the coating to ultraviolet rays and reduce the aging of the coating caused by ultraviolet radiation, such as powdering, cracking, discoloration and performance degradation. Optionally, the mass percentage of the ultraviolet absorber in the raw material is equal to 0.5%, 1% or 1.5%.

[0032] The second aspect of the present invention provides a photovoltaic panel, comprising: a self-repairing coating, wherein the self-repairing coating is prepared by the method for preparing the self-repairing coating provided by any technical solution of the first aspect of the present invention. Since the photovoltaic panel provided by the present invention comprises the self-repairing coating prepared by the method for preparing the self-repairing coating provided by any technical solution of the first aspect of the present invention, it has all the beneficial effects of the method for preparing the self-repairing coating provided by any technical solution of the first aspect of the present invention.

[0033] The third aspect of the present invention provides a photovoltaic module, comprising: a self-repairing coating, which is prepared by the method for preparing a self-repairing coating as provided by any technical solution of the first aspect of the present invention; a panel, wherein the self-repairing coating is arranged on one side of the panel; a battery, which is arranged on the side of the panel away from the self-repairing coating; a reinforcing plate, which is arranged on the side of the battery away from the panel; a back plate, which is arranged on the side of the reinforcing plate away from the battery, and a self-repairing coating is arranged on the side of the back plate away from the reinforcing plate. Since the photovoltaic module provided by the present invention includes a self-repairing coating prepared by the method for preparing a self-repairing coating provided by any technical solution of the first aspect of the present invention, it has all the beneficial effects of the method for preparing a self-repairing coating provided by any technical solution of the first aspect of the present invention.

[0034] In addition, the present invention also designs a reinforcing plate for the battery, so that the battery can be protected, and the self-repairing coating is arranged on the outside of the entire photovoltaic module, so that all internal structures can be protected.

[0035] In the above embodiments, the panel (also called the front panel) includes one of the following or a combination thereof: PET (Polyethylene Terephthalate) board, CPC (Continuous Polymer Composite) board or HPC (High Performance Composite) board.

[0036] In this embodiment, the PET board has good optical transparency, allowing light to fully penetrate into the photovoltaic cell sheet, and the PET board has certain mechanical strength and flexibility, which is suitable for light or flexible photovoltaic modules, and has good weather resistance and chemical stability, and can withstand ultraviolet radiation and temperature changes in outdoor environments. The CPC board has high strength and rigidity, which is suitable for large photovoltaic modules, and has good weather resistance and corrosion resistance, which is suitable for long-term outdoor use. The CPC board also has excellent thermal stability and dimensional stability, and is not easy to deform under temperature changes. The HPC board has extremely high mechanical strength and rigidity, which is suitable for photovoltaic systems that require high load capacity, and the HPC board has excellent chemical resistance and weather resistance, which can withstand harsh outdoor conditions. The HPC board also has excellent thermal stability and dimensional stability, and can maintain structural integrity even under extreme temperatures.

[0037] In the above embodiments, the battery includes one of the following or a combination thereof: XBC (eXtreme Base Contact) battery (cross back contact solar cell), MWT (Metal Wrap Through) battery (metal perforated wrap battery), PERC (Passivated Emitter and Rear Cell) battery (back passivated emitter battery), TOPCON (Tunnel Oxide Passivated Contact) battery (tunnel oxide passivated contact battery) and HJT (Heterojunction with Intrinsic Thin Layer) battery (intrinsic thin film heterojunction battery).

[0038] In this embodiment, the XBC cell can achieve higher photoelectric conversion efficiency and better performance. Compared with the traditional front-contact cell, the XBC cell places all the contact points on the back of the cell, which can reduce the shading of the front side, thereby increasing the light capture and conversion efficiency. The MWT cell collects current through the metal conductor on the back, and there is no grid line on the front side, which reduces the shading loss and improves the photoelectric conversion efficiency of the cell. The PERC cell uses a passivation layer on the back to reduce electron-hole recombination and improve power generation efficiency. The technology is mature, the cost is relatively low, and there is rich experience in large-scale production. TOPCon cells have efficient carrier selective transmission, reduce interface recombination, have higher photoelectric conversion efficiency and lower cost. HJT cells have very low contact resistance, very low temperature coefficient, less efficiency loss at high temperature, and extremely high photoelectric conversion efficiency, which can theoretically exceed 26%.

[0039] In the above-mentioned embodiment, the reinforcing plate includes a glass fiber-resin composite plate.

[0040] In this embodiment, glass fibers have high specific strength and specific modulus, which means that they are lighter in weight but can bear greater loads, which makes photovoltaic modules lighter while maintaining sufficient strength. In addition, glass fiber-resin composite panels have excellent corrosion resistance and can resist corrosion from the atmosphere, seawater, weak acids, alkalis and salts, and are suitable for various harsh environments, including coastal areas and industrial pollution areas.

[0041] In the above embodiments, the backboard includes one of the following or a combination thereof: PET (Polyethylene Terephthalate) board, CPC (Composite Polymeric Coating) board and HPC (High Performance Composite) board.

[0042] In this embodiment, the PET board, CPC board and HPC board all have high weather resistance, excellent resistance to ultraviolet rays, temperature difference changes and chemical resistance, and are suitable for long-term outdoor use. They also have high mechanical strength, enhance the structural stability of the photovoltaic module, and can effectively prevent the intrusion of moisture and dust to protect the interior of the module.

[0043] In the above embodiment, the photovoltaic module also includes: a first adhesive layer, arranged between the panel and the battery; a second adhesive layer, arranged between the battery and the reinforcing plate; a third adhesive layer, arranged between the reinforcing plate and the back plate; the first adhesive layer, the second adhesive layer and the third adhesive layer all include one of the following or a combination thereof: EVA (Ethylene-Vinyl Acetate, ethylene-vinyl acetate copolymer) adhesive layer, POE (Polyolefin Elastomer, polyolefin elastomer) adhesive layer and EPE (Encapsulant Polyolefin Elastomer, encapsulation polyolefin elastomer) adhesive layer.

[0044] In this embodiment, the EVA adhesive layer, the POE adhesive layer and the EPE adhesive layer all have good bonding properties. In addition, they also have high transparency, allowing sunlight to fully penetrate, thereby improving the photoelectric conversion efficiency of the photovoltaic module.

[0045] The fourth aspect of the present invention provides a method for preparing a photovoltaic panel, comprising: mixing a solvent, a polyol, and an organic fluorine resin to obtain a prepolymer; adding an isocyanate curing agent to the prepolymer, reacting at a first preset temperature for a first preset time, and then adding a chain extender, reacting for a second preset time to obtain a self-repairing coating slurry; applying the self-repairing coating slurry to the surface of a substrate, and keeping it warm at a second preset temperature for a third preset time to obtain a photovoltaic panel.

[0046] The preparation method of the photovoltaic panel provided by the present invention is that the polyol and the isocyanate curing agent undergo a cross-linking reaction under the action of a chain extender to obtain a polyurethane elastomer, and then the polyurethane elastomer can be compounded with an organic fluorine resin to obtain a polyurethane elastomer-organic fluorine resin composite coating. Since the organic fluorine resin coating has extremely high weather resistance, it can resist the influence of ultraviolet radiation, extreme temperature changes, humidity, weathering and other natural environmental factors, protect the photovoltaic panel from external damage, and extend the service life of the photovoltaic module. In addition, the organic fluorine resin coating usually has good mechanical strength and flexibility, and can resist physical damage such as impact and scratching. It can be seen that the composite coating prepared by the present invention not only has the function of self-repair, but is also very suitable for photovoltaic panels, and has better heat resistance, corrosion resistance and impact resistance, which improves the power generation of photovoltaic modules.

[0047] The reaction mechanism of this process is that the hydroxyl group in the polyol reacts with the isocyanate group in the isocyanate to form a carbamate bond (-NH-CO-O-) to generate a polyurethane prepolymer, while the chain extender can react with the remaining -NCO group in the polyurethane prepolymer to form more carbamate bonds, thereby producing longer polymer chains. This process will significantly improve the crosslinking density and mechanical strength of the coating.

[0048] In the above embodiment, optionally, before the step of adding the isocyanate curing agent to the prepolymer, the step further includes: adding a leveling agent, an antioxidant, and a UV (Ultraviolet) additive to the prepolymer, and adding a dispersant after stirring.

[0049] In this embodiment, the leveling agent, antioxidant, and UV additive do not participate in the cross-linking reaction, but can be mixed into the prepolymer to form a self-repairing coating slurry, thereby improving the surface smoothness, helping the coating to be evenly distributed on the substrate, reducing the orange peel effect, and improving the oxidation resistance of the photovoltaic panel.

[0050] In the above embodiment, optionally, the first preset temperature is greater than or equal to 60°C and less than or equal to 85°C; the first preset temperature is also the reaction temperature of the polyol and the isocyanate curing agent, for example, 60°C, 70°C or 80°C.

[0051] In the above embodiment, optionally, the first preset duration is greater than or equal to 2 hours and less than or equal to 4 hours, for example, 2 hours, 3 hours or 4 hours.

[0052] In the above embodiment, optionally, the second preset duration is greater than or equal to 1 hour and less than or equal to 2 hours, for example, 1 hour, 1.5 hours or 2 hours.

[0053] In the above embodiment, optionally, the second preset temperature is greater than or equal to 50° C. and less than or equal to 55° C. For example, 50° C., 52° C. or 55° C.

[0054] In the above embodiment, optionally, the third preset duration is greater than or equal to 20 hours and less than or equal to 28 hours, for example, 20 hours, 24 hours or 28 hours.

[0055] Additional aspects and advantages of the present invention will become apparent in the following description or may be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] The above and / or additional aspects and advantages of the embodiments of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0057] Figure 1 One of the flow charts of the method for preparing the self-repairing coating provided by an embodiment of the present invention is shown;

[0058] Figure 2 The second flowchart of the method for preparing the self-repairing coating provided by the embodiment of the present invention is shown;

[0059] Figure 3 The third flowchart of the method for preparing the self-repairing coating provided by the embodiment of the present invention is shown;

[0060] Figure 4 A schematic diagram of the structure of a self-repairing coating provided by an embodiment of the present invention is shown;

[0061] Figure 5 One of the structural schematic diagrams of the photovoltaic assembly provided by the embodiment of the present invention is shown;

[0062] Figure 6 A second schematic diagram of the structure of a photovoltaic assembly provided by an embodiment of the present invention is shown;

[0063] Figure 7 A fourth flow chart of the method for preparing a self-repairing coating provided in an embodiment of the present invention is shown.

[0064] in, Figures 4 to 6 The corresponding relationship between the reference numerals and component names in the figure is:

[0065] 1 photovoltaic module, 100 self-repairing coating, 200 panel, 300 first adhesive layer, 400 battery, 500 second adhesive layer, 600 reinforcement plate, 700 third adhesive layer, 800 backplane. DETAILED DESCRIPTION

[0066] In order to more clearly understand the above aspects, features and advantages of the embodiments of the present invention, the embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings and specific implementation methods. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0067] In the following description, many specific details are set forth to facilitate a full understanding of the embodiments according to the present invention. However, the embodiments according to the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the embodiments according to the present invention is not limited to the specific embodiments disclosed below.

[0068] Embodiment 1:

[0069] like Figure 1 As shown, this embodiment provides a method for preparing a self-repairing coating, comprising the following steps:

[0070] S102: After the solvent, polyester polyol, fluororesin, leveling agent, antioxidant and UV additive are fully stirred and mixed, a dispersant is added, and after stirring and dispersing, a semi-finished prepolymer is obtained;

[0071] S104: Add diisocyanate curing agent to the semi-finished prepolymer, fully react for 2 hours, the reaction temperature is 60°C, then add chain extender, react at room temperature for 1 hour, and prepare slurry, wherein the components are calculated by weight percentage: 60 parts of polycaprolactone diol, 10 parts of isophorone diisocyanate, 5 parts of chain extender, 5 parts of polytetrafluoroethylene, 0.1 parts of leveling agent, 0.05 parts of dispersant, 0.30 parts of antioxidant, 1.5 parts of UV additive, a total of 100 parts, and the balance is solvent;

[0072] S106: Apply the slurry to the surface of the transparent front plate coated with corona treatment by slit extrusion or micro-concave coating, heat and bake, and perform constant temperature curing for 24 hours to obtain a self-repairing coating.

[0073] Comparative Example 1

[0074] The preparation methods of this comparative example 1 are basically the same as those of the embodiment 1, the only difference being that no fluororesin is added in this comparative example, and the content of fluororesin is supplemented to 100 parts by a solvent.

[0075] Comparative Example 2

[0076] The preparation method of this comparative example 2 is basically the same as that of the example 1, the only difference being that the amount of the fluororesin in this comparative example is 10 parts, which is still supplemented to 100 parts by the solvent.

[0077] Comparative Example 3

[0078] The preparation method of this comparative example 3 is basically the same as that of the example 1, the only difference being that the amount of the fluororesin in this comparative example is 1 part, which is still supplemented to 100 parts by the solvent.

[0079] The mechanical strength and weather resistance of the coatings prepared in the above-mentioned embodiment 1 and comparative examples 1 to 3 were tested. The test standards were ASTM B117: evaluating the corrosion resistance of the coating in a salt spray environment and ASTMD2794: evaluating the ability of the coating to withstand impact without cracking or peeling. The experiment showed that the present invention not only has excellent impact resistance but also has good corrosion resistance by adding organic fluorine resin to the raw materials and controlling the content of the organic fluorine resin, thus achieving the goal of having both fish and bear's paw. No fluorine resin was added in comparative example 1, and the fluorine resin content in comparative example 3 was low, so the self-repairing coating had poor aging resistance, which affected the life of the self-repairing coating. In comparative example 2, the fluorine resin content was too much, the components were unevenly dispersed, and agglomeration occurred, which affected the film-forming effect of the coating.

[0080] like Figure 2 As shown, another embodiment of the present invention provides a method for preparing a self-repairing coating, the self-repairing coating is applied to a photovoltaic module, and the method for preparing the self-repairing coating includes:

[0081] S202: Prepare a self-healing coating by preparing raw materials; wherein the prepared raw materials include: polyols, the mass percentage of the polyols in the prepared raw materials is greater than or equal to 45%, and less than or equal to 70%; isocyanate curing agent, the mass percentage of the isocyanate curing agent in the prepared raw materials is greater than or equal to 4.5%, and less than or equal to 10%; chain extender, the mass percentage of the chain extender in the prepared raw materials is greater than or equal to 2%, and less than or equal to 5%; organic fluorine resin, the mass percentage of the organic fluorine resin in the prepared raw materials is greater than or equal to 3%, and less than or equal to 5%; solvent, the mass percentage of the solvent in the prepared raw materials is greater than or equal to 20%, and less than or equal to 40%.

[0082] The present invention obtains a polyurethane elastomer by cross-linking a polyol and an isocyanate curing agent under the action of a chain extender, and then the polyurethane elastomer can be compounded with an organic fluorine resin to obtain a polyurethane elastomer-organic fluorine resin composite coating. Since the organic fluorine resin coating has extremely high weather resistance, it can resist the influence of ultraviolet radiation, extreme temperature changes, humidity, weathering and other natural environmental factors, protect photovoltaic panels from external damage, and extend the service life of photovoltaic modules. In addition, organic fluorine resin coatings usually have good mechanical strength and flexibility, and can resist physical damage such as impact and scratches. It can be seen that the composite coating prepared by the present invention not only has a self-repairing function, but is also very suitable for photovoltaic panels, and has better heat resistance, corrosion resistance and impact resistance, which improves the power generation of photovoltaic modules.

[0083] In the above embodiment, optionally, the mass percentage of the polyol in the preparation raw material is greater than or equal to 50% and less than or equal to 65%, for example, 50%, 55% or 60%.

[0084] In the above embodiment, optionally, the mass percentage of the isocyanate curing agent in the preparation raw materials is greater than or equal to 5% and less than or equal to 8%, for example, 6%, 7% or 8%.

[0085] In the above embodiment, optionally, the mass percentage of the chain extender in the preparation raw material is greater than or equal to 3% and less than or equal to 4%, for example, 3% or 4%.

[0086] In the above embodiment, optionally, the mass percentage of the organic fluorine resin in the preparation raw material is greater than or equal to 4% and less than or equal to 5%, for example, 4% or 5%.

[0087] In the above embodiment, optionally, the mass percentage of the solvent in the raw material is greater than or equal to 25% and less than or equal to 35%, for example, 25%, 30% or 35%. Of course, the mass percentage of the solvent is not limited to 20% to 40%. The solvent only plays a dissolving role in the whole process, does not participate in the reaction, and does not affect the performance of the coating. When other components are determined, the total component can be made 100% by the solvent.

[0088] In the above embodiment, optionally, the organic fluorine resin includes one of the following or a combination thereof: polytetrafluoroethylene, fluorinated ethylene propylene copolymer, polyperfluoroalkoxy resin, polyvinylidene fluoride and ethylene-tetrafluoroethylene polymer.

[0089] In this embodiment, the above-mentioned organic fluorine resins have the advantages of good weather resistance, chemical stability, electrical insulation, high mechanical strength, flexibility and high flame retardancy. After compounding with polyurethane elastomer, they can greatly improve the strength and heat resistance of photovoltaic panels and extend the service life of photovoltaic modules.

[0090] In the above embodiment, optionally, the polyol includes aliphatic polyether, or the polyol includes aliphatic polyether, and the aliphatic polyether includes polytetramethylene ether diol. And / or the polyol includes polyester polyol, or the polyol includes polyester polyol, and the polyester polyol includes polycaprolactone diol and / or adipic acid polyester polyol. And / or the isocyanate curing agent includes isophorone diisocyanate curing agent and / or hexamethylene diisocyanate curing agent.

[0091] In this embodiment, the hydroxyl groups in the aliphatic polyether and polyester polyol can react with the isocyanate groups in the isocyanate to form urethane bonds, thereby polymerizing to obtain a polyurethane prepolymer.

[0092] In the above embodiment, optionally, the polyol includes a polyol having a hydroxyl value greater than or equal to 150 mgKOH / g and less than or equal to 350 mgKOH / g.

[0093] In this embodiment, the hydroxyl value of the polyol is greater than or equal to 150 mgKOH / g and less than or equal to 350 mgKOH / g; for example, it can be 200 mgKOH / g or 250 mgKOH / g. Polyols with higher hydroxyl values ​​will form more crosslinking points, resulting in an increase in the crosslinking density of the coating, thereby improving the hardness, wear resistance and chemical resistance of the coating. However, too high a crosslinking density may make the coating brittle and hard, so it can be controlled within 200 mgKOH / g to 250 mgKOH / g.

[0094] In the above embodiment, optionally, in the isocyanate curing agent, the mass percentage of the isocyanate group in the isocyanate curing agent is greater than or equal to 15% and less than or equal to 35%.

[0095] In this embodiment, the isocyanate group also affects the degree of crosslinking. A high proportion of isocyanate groups will result in a higher crosslinking density. The denser the crosslinking network, the higher the hardness, chemical resistance and mechanical strength of the coating will generally be, but the flexibility and elongation will be relatively lower. Therefore, it is most appropriate to control the mass proportion of isocyanate groups to 15% to 35%, and can also be controlled to 20% to 25%, for example, 20%, 22% or 25%.

[0096] In the above embodiment, optionally, the preparation raw material further includes a leveling agent, and the mass percentage of the leveling agent in the preparation raw material is greater than or equal to 0.05% and less than or equal to 0.1%.

[0097] In this embodiment, the leveling agent can improve the surface flatness, help the coating to be evenly distributed on the substrate, reduce the orange peel effect, improve the flatness and smoothness of the coating, and make the coating surface smoother. In addition, it also helps to quickly release the air and solvent in the coating, prevent the formation of pinholes and bubbles, and improve the density of the coating. Optionally, the mass percentage of the leveling agent in the preparation raw material is 0.05%, 0.08% or 0.1%.

[0098] In the above embodiment, optionally, the preparation raw material further includes a dispersant, and the mass percentage of the dispersant in the preparation raw material is greater than or equal to 0.02% and less than or equal to 0.05%.

[0099] In this embodiment, the dispersant can effectively reduce the attraction between particles, prevent the particles from agglomerating, and ensure that the components are evenly distributed in the coating, which has a direct impact on the color consistency, hiding power and glossiness of the coating. The dispersant can also improve the rheological properties of the coating, so that the coating has better fluidity during construction, which is convenient for spraying, brushing or roller coating, while reducing splashing and dripping, and improving construction efficiency. Optionally, the mass percentage of the dispersant in the prepared raw materials is equal to 0.02%, 0.03%, 0.04% or 0.05%.

[0100] In the above embodiment, optionally, the raw material for preparation further includes an antioxidant, and the weight percentage of the antioxidant in the raw material for preparation is greater than or equal to 0.1% and less than or equal to 0.3%.

[0101] In this embodiment, the antioxidant can prevent or slow down the oxidative aging of the coating caused by environmental factors such as ultraviolet rays, heat, oxygen, etc., thereby helping to maintain the original mechanical properties of the coating and extend the service life of the coating. Optionally, the antioxidant accounts for 0.1%, 0.2% or 0.3% by mass of the raw material.

[0102] In the above embodiment, optionally, the raw material further comprises an ultraviolet absorber, and the mass percentage of the ultraviolet absorber in the raw material is greater than or equal to 0.5% and less than or equal to 1.5%.

[0103] In this embodiment, the ultraviolet absorber can significantly improve the resistance of the coating to ultraviolet rays and reduce the aging of the coating caused by ultraviolet radiation, such as powdering, cracking, discoloration and performance degradation. Optionally, the mass percentage of the ultraviolet absorber in the raw material is equal to 0.5%, 1% or 1.5%.

[0104] In the above embodiments, optionally, the leveling agent can be one of terminal modified silicone or polyester modified silicone. The dispersant can be polyether modified polysiloxane or polyacrylate dispersant. The antioxidant can be antioxidant 1010 (a highly efficient macromolecular hindered phenol antioxidant). The ultraviolet absorber can be one of UV326 or UV531. The solvent can be one of N,N-dimethylformamide, tetrahydrofuran and 1,4-dioxane.

[0105] Another embodiment of the present invention provides a transparent self-repairing coating, which is mainly a composite coating of polyurethane elastomer and fluororesin, and the formula of the raw materials for its preparation is: 45-60 parts of polyester polyol; 4.5-10 parts of isocyanate curing agent; 2-5 parts of chain extender; 3-5 parts of organic fluororesin; 0.05-0.1 parts of leveling agent; 0.02-0.05 parts of dispersant; 0.1-0.30 parts of antioxidant; 0.5-1.5 parts of UV additive; 20-30 parts of solvent.

[0106] In the coating prepared in this embodiment, the soft segment is selected from aliphatic polyether or polyester polyol, for example, one of tetramethylene glycol or polycaprolactone glycol, and one or more of adipic acid polyester polyols having a hydroxyl value of 150 mgKOH / g to 350 mgKOH / g; the hard segment is selected from diisocyanate curing agent, preferably one or more of isophorone diisocyanate and hexamethylene diisocyanate, and the isocyanate group (-NCO group) content is 15%-35%.

[0107] The second aspect of the present invention provides a photovoltaic panel, comprising: a self-repairing coating, wherein the self-repairing coating is prepared by the method for preparing the self-repairing coating provided by any technical solution of the first aspect of the present invention. Since the photovoltaic panel provided by the present invention comprises the self-repairing coating prepared by the method for preparing the self-repairing coating provided by any technical solution of the first aspect of the present invention, it has all the beneficial effects of the method for preparing the self-repairing coating provided by any technical solution of the first aspect of the present invention.

[0108] like Figure 4 , Figure 5 and Figure 6 As shown, the third aspect of the present invention provides a photovoltaic module 1, comprising a self-repairing coating 100, a panel 200, a battery 400, a reinforcing plate 600 and a back plate 800, wherein the self-repairing coating 100 is prepared by the method for preparing a self-repairing coating provided by any technical solution of the first aspect of the present invention; the self-repairing coating 100 is arranged on one side of the panel 200; the battery 400 is arranged on the side of the panel 200 away from the self-repairing coating 100; the reinforcing plate 600 is arranged on the side of the battery 400 away from the panel 200; the back plate 800 is arranged on the side of the reinforcing plate 600 away from the battery 400, and the side of the back plate 800 away from the reinforcing plate 600 is provided with the self-repairing coating 100. Since the photovoltaic module 1 provided by the present invention comprises the self-repairing coating 100 prepared by the method for preparing a self-repairing coating provided by any technical solution of the first aspect of the present invention, it has all the beneficial effects of the method for preparing a self-repairing coating provided by any technical solution of the first aspect of the present invention.

[0109] In addition, the present invention also designs a reinforcing plate 600 for the battery 400, so as to protect the battery 400, and the self-repairing coating 100 is arranged on the outside of the entire photovoltaic module 1, so as to protect all internal structures.

[0110] In the above embodiments, the panel 200 includes one of the following or a combination thereof: a PET (Polyethylene Terephthalate) board, a CPC (Continuous Polymer Composite) board or an HPC (High Performance Composite) board.

[0111] In this embodiment, the PET board has good optical transparency, allowing light to fully penetrate into the photovoltaic cells 400, and the PET board has certain mechanical strength and flexibility, which is suitable for light or flexible photovoltaic modules 1, and has good weather resistance and chemical stability, and can withstand ultraviolet radiation and temperature changes in outdoor environments. The CPC board has high strength and rigidity, which is suitable for large photovoltaic modules 1, and has good weather resistance and corrosion resistance, which is suitable for long-term outdoor use. The CPC board also has excellent thermal stability and dimensional stability, and is not easy to deform under temperature changes. The HPC board has extremely high mechanical strength and rigidity, which is suitable for photovoltaic systems that require high load capacity, and the HPC board has excellent chemical resistance and weather resistance, which can withstand harsh outdoor conditions. The HPC board also has excellent thermal stability and dimensional stability, and can maintain structural integrity even under extreme temperatures. The thickness of the panel 200 is 0.3mm to 0.6mm.

[0112] In the above embodiments, the battery 400 includes one of the following or a combination thereof: an XBC (eXtreme Base Contact) battery 400 (cross back contact solar cell 400), an MWT (Metal Wrap Through) battery 400 (metal perforated wrap battery 400), a PERC (Passivated Emitter and Rear Cell) battery 400 (back passivated emitter battery 400), a TOPCON (Tunnel Oxide Passivated Contact) battery 400 (tunneling oxide passivated contact battery 400) and an HJT (Heterojunction with Intrinsic Thin Layer) battery 400 (intrinsic thin film heterojunction battery 400).

[0113] In this embodiment, the XBC cell 400 can achieve higher photoelectric conversion efficiency and better performance. Compared with the traditional front contact cell, the XBC cell 400 places all contact points on the back of the cell 400, which can reduce the shading of the front side, thereby increasing the light capture and conversion efficiency. The MWT cell 400 collects current through the metal conductor on the back side, and there is no grid line on the front side, which reduces the shading loss and improves the photoelectric conversion efficiency of the cell 400. The PERC cell 400 uses a passivation layer on the back side to reduce electron-hole recombination and improve power generation efficiency. The technology is mature, the cost is relatively low, and there is rich experience in large-scale production. The TOPCon cell 400 has efficient carrier selective transmission, reduces interface recombination, has high photoelectric conversion efficiency and low cost. The HJT cell 400 has very low contact resistance, a very low temperature coefficient, less efficiency loss at high temperature, and extremely high photoelectric conversion efficiency, which can theoretically exceed 26%.

[0114] In the above-described embodiment, the reinforcing plate 600 includes a glass fiber-resin composite plate.

[0115] In this embodiment, glass fibers have high specific strength and specific modulus, which means that they are lighter in weight but can withstand greater loads, which makes the photovoltaic module 1 lighter while maintaining sufficient strength. In addition, the glass fiber-resin composite board has excellent corrosion resistance and can resist corrosion from the atmosphere, seawater, weak acids, alkalis and salts, and is suitable for various harsh environments, including coastal areas and industrial pollution areas. Optionally, the thickness of the reinforcing plate 600 is 0.3mm to 0.45mm, the proportion of glass fiber is 50% to 65%; the resin can be selected from one of acrylic resin or epoxy resin, and the proportion of resin is 35% to 50%.

[0116] In the above embodiment, the backboard 800 includes one of the following or a combination thereof: PET (Polyethylene Terephthalate) board, CPC (Composite Polymeric Coating) board and HPC (High Performance Composite) board.

[0117] In this embodiment, the PET board, CPC board and HPC board all have high weather resistance, excellent resistance to ultraviolet rays, temperature difference changes and chemical resistance, and are suitable for long-term outdoor use. They also have high mechanical strength, enhance the structural stability of the photovoltaic module 1, and can effectively prevent the intrusion of moisture and dust and protect the interior of the module. Optionally, the thickness of the back sheet 800 is 0.3 mm to 0.6 mm.

[0118] In the above embodiment, the photovoltaic module 1 also includes: a first adhesive layer 300, which is arranged between the panel 200 and the battery 400; a second adhesive layer 500, which is arranged between the battery 400 and the reinforcing plate 600; a third adhesive layer 700, which is arranged between the reinforcing plate 600 and the back plate 800; the first adhesive layer 300, the second adhesive layer 500 and the third adhesive layer 700 all include one of the following or a combination thereof: EVA (Ethylene-Vinyl Acetate, ethylene-vinyl acetate copolymer) adhesive layer, POE (Polyolefin Elastomer, polyolefin elastomer) adhesive layer and EPE (Encapsulant Polyolefin Elastomer, encapsulation polyolefin elastomer) adhesive layer.

[0119] In this embodiment, the EVA adhesive layer, the POE adhesive layer and the EPE adhesive layer all have good bonding properties and high transparency, allowing sunlight to fully penetrate, thereby improving the photoelectric conversion efficiency of the photovoltaic module 1. Optionally, the thickness of the first adhesive layer 300 is 0.3mm-0.7mm; the thickness of the second adhesive layer 500 is 0.3mm-0.7mm; and the thickness of the third adhesive layer 700 is 0.3mm-0.7mm.

[0120] like Figure 7 As shown, the fourth aspect of the present invention provides a method for preparing a photovoltaic panel, comprising:

[0121] S702: mixing a solvent, a polyol, and an organic fluorine resin to prepare a prepolymer;

[0122] S704: adding an isocyanate curing agent to the prepolymer, reacting at a first preset temperature for a first preset time, and then adding a chain extender, reacting for a second preset time, to obtain a self-repairing coating slurry;

[0123] S706: Apply the self-repairing coating slurry to the surface of the substrate, and keep it at a second preset temperature for a third preset time to obtain a photovoltaic panel.

[0124] The preparation method of the photovoltaic panel provided by the present invention is that the polyol and the isocyanate curing agent undergo a cross-linking reaction under the action of a chain extender to obtain a polyurethane elastomer, and then the polyurethane elastomer can be compounded with an organic fluorine resin to obtain a polyurethane elastomer-organic fluorine resin composite coating. Since the organic fluorine resin coating has extremely high weather resistance, it can resist the influence of ultraviolet radiation, extreme temperature changes, humidity, weathering and other natural environmental factors, protect the photovoltaic panel from external damage, and extend the service life of the photovoltaic module. In addition, the organic fluorine resin coating usually has good mechanical strength and flexibility, and can resist physical damage such as impact and scratching. It can be seen that the composite coating prepared by the present invention not only has the function of self-repair, but is also very suitable for photovoltaic panels, and has better heat resistance, corrosion resistance and impact resistance, which improves the power generation of photovoltaic modules.

[0125] The reaction mechanism of this process is that the hydroxyl group in the polyol reacts with the isocyanate group in the isocyanate to form a carbamate bond (-NH-CO-O-) to generate a polyurethane prepolymer, while the chain extender can react with the remaining -NCO group in the polyurethane prepolymer to form more carbamate bonds, thereby producing longer polymer chains. This process will significantly improve the crosslinking density and mechanical strength of the coating.

[0126] In the above embodiment, optionally, the first preset temperature is greater than or equal to 60°C and less than or equal to 85°C; the first preset temperature is also the reaction temperature of the polyol and the isocyanate curing agent, for example, 60°C, 70°C or 80°C.

[0127] In the above embodiment, optionally, the first preset duration is greater than or equal to 2 hours and less than or equal to 4 hours, for example, 2 hours, 3 hours or 4 hours.

[0128] In the above embodiment, optionally, the second preset duration is greater than or equal to 1 hour and less than or equal to 2 hours, for example, 1 hour, 1.5 hours or 2 hours.

[0129] In the above embodiment, optionally, the second preset temperature is greater than or equal to 50° C. and less than or equal to 55° C. For example, 50° C., 52° C. or 55° C.

[0130] In the above embodiment, optionally, the third preset duration is greater than or equal to 20 hours and less than or equal to 28 hours, for example, 20 hours, 24 hours or 28 hours.

[0131] like Figure 3 As shown, the present invention further provides a method for preparing a photovoltaic panel, comprising:

[0132] S302: Stir and mix the solvent, polyester polyol, fluororesin, leveling agent, antioxidant and UV additive thoroughly;

[0133] S304: adding a dispersant, stirring and dispersing at high speed to obtain a semi-finished prepolymer;

[0134] S306: Add diisocyanate curing agent to the semi-finished prepolymer and fully react for 2h-4h at a reaction temperature of 60°C-85°C;

[0135] S308: adding a chain extender, reacting at room temperature of 25°C-30°C for 1h-2h to obtain a self-repairing coating product;

[0136] S310: Corona treatment of transparent front / back panels;

[0137] S312: Apply the self-repairing coating product to the transparent front / back panel by slit extrusion / micro-dimpled coating;

[0138] S314: heating, baking, curing and curing to obtain a self-repairing photovoltaic panel.

[0139] The thickness of the polyurethane elastomer and fluororesin composite coating is 50 μm-150 μm.

[0140] The beneficial effects of the present invention are:

[0141] 1. The present invention designs and develops a transparent two-component polyurethane and fluororesin self-healing composite coating for transparent photovoltaic surface / back panel. Through the formula design and synthetic application of the self-healing material, the coating of the transparent surface / back panel has self-healing properties, achieving a significant improvement in the scratch resistance and wear resistance of the surface of the transparent surface / back panel outer layer coating.

[0142] 2. This proposal designs a transparent self-repairing lightweight photovoltaic module. When exposed to sunlight and the heat generated by the photovoltaic module itself (surface temperature 60℃~80℃), the microphase separation structure between the soft segment and the hard segment and the non-directional rearrangement of broken hydrogen bonds can autonomously repair slight cracks, scratches and abrasions on the coating surface caused by external forces, thereby extending the life of the transparent self-repairing lightweight photovoltaic module and improving the power generation of the transparent self-repairing module.

[0143] In the embodiments according to the present invention, the terms "first", "second", and "third" are only used for description and cannot be understood as indicating or implying relative importance; the term "plurality" refers to two or more, unless otherwise clearly defined. The terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; "connected" can be a direct connection or an indirect connection through an intermediate medium. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments according to the present invention can be understood according to specific circumstances.

[0144] In addition, although each operation is described in a specific order, this should be understood as requiring such operation to be performed in a specific order or in a sequential order, or requiring that all illustrated operations should be performed to obtain desired results. Under certain circumstances, multitasking and parallel processing may be advantageous. Similarly, although some specific implementation details are included in the above discussion, these should not be interpreted as limiting the scope of the present invention. Some features described in the context of a separate embodiment can also be implemented in a single implementation in combination. On the contrary, the various features described in the context of a single implementation can also be implemented in multiple implementations individually or in any suitable sub-combination mode.

[0145] Although the subject matter has been described in the language of specific structural features and / or method logical actions, it should be understood that the subject matter defined in the appended claims is not necessarily limited to the specific features or actions described above. On the contrary, the specific features and actions described above are merely example forms of implementing the claims.

[0146] The above are only preferred embodiments according to the embodiments of the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, various modifications and changes may be made according to the embodiments of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the embodiments of the present invention shall be included in the protection scope of the embodiments of the present invention.

Claims

1. A method for preparing a self-repairing coating, characterized in that: The self-repairing coating is applied to a photovoltaic module, and the preparation method of the self-repairing coating comprises: Prepare the self-healing coating by preparing raw materials; Wherein, the preparation raw materials include: Polyol, the mass percentage of the polyol in the preparation raw material is greater than or equal to 45% and less than or equal to 70%; An isocyanate curing agent, wherein the mass percentage of the isocyanate curing agent in the preparation raw material is greater than or equal to 4.5% and less than or equal to 10%; A chain extender, wherein the mass percentage of the chain extender in the preparation raw material is greater than or equal to 2% and less than or equal to 5%; An organic fluorine resin, wherein the mass percentage of the organic fluorine resin in the preparation raw material is greater than or equal to 3% and less than or equal to 5%; A solvent, wherein the mass percentage of the solvent in the preparation raw material is greater than or equal to 20% and less than or equal to 40%.

2. The method for preparing the self-repairing coating according to claim 1, characterized in that: The organic fluorine resin includes one or a combination of the following: Polytetrafluoroethylene, fluorinated ethylene propylene copolymers, polyperfluoroalkoxy resins, polyvinylidene fluoride and ethylene-tetrafluoroethylene polymers.

3. The method for preparing the self-repairing coating according to claim 1, characterized in that: The polyol comprises an aliphatic polyether, or the polyol comprises an aliphatic polyether, and the aliphatic polyether comprises polytetramethylene glycol; and / or The polyol comprises polyester polyol, or the polyol comprises polyester polyol, and the polyester polyol comprises polycaprolactone diol and / or adipic acid polyester polyol; and / or The isocyanate curing agent includes isophorone diisocyanate curing agent and / or hexamethylene diisocyanate curing agent.

4. The method for preparing the self-repairing coating according to claim 1, characterized in that: The polyol includes a polyol having a hydroxyl value greater than or equal to 150 mgKOH / g and less than or equal to 350 mgKOH / g; In the isocyanate curing agent, the mass percentage of the isocyanate group in the isocyanate curing agent is greater than or equal to 15% and less than or equal to 35%.

5. The method for preparing the self-repairing coating according to claim 1, characterized in that: The preparation raw materials also include: A leveling agent, wherein the mass percentage of the leveling agent in the preparation raw material is greater than or equal to 0.05% and less than or equal to 0.1%; and / or A dispersant, wherein the mass percentage of the dispersant in the preparation raw material is greater than or equal to 0.02% and less than or equal to 0.05%; and / or An antioxidant, wherein the antioxidant accounts for a mass percentage of the raw material for preparation of greater than or equal to 0.1% and less than or equal to 0.3%; and / or The ultraviolet absorber accounts for a mass percentage of the preparation raw material greater than or equal to 0.5% and less than or equal to 1.5%.

6. A photovoltaic panel, characterized in that: include: A self-repairing coating, wherein the self-repairing coating is prepared by the preparation method of the self-repairing coating according to any one of claims 1 to 5.

7. A photovoltaic module, characterized in that: include: A self-repairing coating, wherein the self-repairing coating is prepared by the preparation method of the self-repairing coating according to any one of claims 1 to 5; A panel, wherein the self-repairing coating is disposed on one side of the panel; A battery, disposed on a side of the panel away from the self-repairing coating; A reinforcing plate, arranged on a side of the battery away from the panel; The back plate is arranged on a side of the reinforcing plate away from the battery, and the self-repairing coating is arranged on the side of the back plate away from the reinforcing plate.

8. The photovoltaic module according to claim 7, characterized in that: The panel comprises one of the following or a combination thereof: a PET board, a CPC board or a HPC board; and / or The battery comprises one of the following or a combination thereof: an XBC battery, an MWT battery, a PERC battery, a TOPCON battery and an HJT battery; and / or The reinforcing plate comprises a glass fiber-resin composite plate; and / or The backboard includes one of the following or a combination thereof: a PET board, a CPC board and a HPC board.

9. The photovoltaic module according to claim 7, characterized in that: Also includes: A first adhesive layer, disposed between the panel and the battery; A second adhesive layer is provided between the battery and the reinforcing plate; A third adhesive layer, disposed between the reinforcing plate and the back plate; The first adhesive layer, the second adhesive layer and the third adhesive layer each include one of the following or a combination thereof: an EVA adhesive layer, a POE adhesive layer and an EPE adhesive layer.

10. A method for preparing a photovoltaic panel, characterized in that: include: The solvent, polyol and organic fluorine resin are mixed to prepare a prepolymer; Adding an isocyanate curing agent to the prepolymer, reacting at a first preset temperature for a first preset time, then adding a chain extender, reacting for a second preset time, to obtain a self-repairing coating slurry; The self-repairing coating slurry is applied to the surface of the substrate, and kept at a second preset temperature for a third preset time to obtain the photovoltaic panel.

11. The method for preparing a photovoltaic panel according to claim 10, characterized in that: The first preset temperature is greater than or equal to 60° C. and less than or equal to 85° C.; The first preset duration is greater than or equal to 2 hours and less than or equal to 4 hours; The second preset duration is greater than or equal to 1 hour and less than or equal to 2 hours; The second preset temperature is greater than or equal to 50° C. and less than or equal to 55° C.; The third preset duration is greater than or equal to 20 hours and less than or equal to 28 hours.

Citation Information

Patent Citations

  • Self-repairing coating composition, self-repairing coating layer, protective film containing coating layer and application of protective film

    CN108239446A

  • Room-temperature self-repairing type polyurethane coating resin and preparation method thereof

    CN113088177A

  • Polyurethane material as well as preparation method and application thereof

    CN113912819A

  • Outer-layer transparent self-repairing coating for photovoltaic transparent backboard and preparation method of outer-layer transparent self-repairing coating

    CN114032022A

  • Solar backboard with self-repairing function and photovoltaic module

    CN218399674U