Silane modified polyether resin and application thereof in MS sealant
Sealant was solved by using composite UV absorber of nano-TiO2 and 5-allyl-3-methoxysalicylate in silane-modified polyether sealant and phenylvinyl silicone oil modified calcium carbonate The weather resistance and extrusion performance problems achieve better UV resistance and mechanical properties.
Patent Information
- Application Number
- CN202411315665.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing silane modified polyether sealants are susceptible to UV damage when exposed to external environment for a long time, resulting in insufficient weather resistance and UV resistance. The poor dispersion of nano calcium carbonate fillers in the resin matrix affects the extrusion performance of the sealant.
Using nano-TiO2 and 5-allyl-3-methoxysalicylate composite UV absorber through chemical grafting, combined with phenyl vinyl silicone oil to modify calcium carbonate, to form composite UV absorber and grafted nanofiller , improve the UV resistance and extrusion performance of sealant.
The weather resistance and UV aging resistance of the sealant are significantly improved, the service life is extended, and the dispersion and cross-linking structure of nano calcium carbonate are improved through grafting technology, and the mechanical properties and fluidity of the sealant are improved.
Smart Images

Figure FT_1 
Figure BDA0005052121490000031 
Figure BDA0005052121490000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sealants, and in particular to a silane-modified polyether resin and application of the same in MS sealants. Background Art
[0002] Silane modified polyether sealant (MS sealant for short) has the advantages of both polyurethane sealant and silicone sealant, overcoming the performance deficiencies of both, with excellent mechanical strength, coating properties, and stain resistance, and the product does not contain isocyanates and organic solvents. It is the main development direction of new sealants at home and abroad. At present, MS sealant has been widely used in construction, rail transit, automobile, interior decoration and other industries.
[0003] MS sealants used in the construction industry and vehicles and ships are exposed to the outdoors for a long time and need to withstand the test of climate, such as comprehensive damage caused by light, heat, cold, wind, rain, bacteria, etc., and have high requirements for their weather resistance and UV resistance. Only sealants with good weather resistance and UV resistance can maintain excellent sealing or bonding effects for a long time. In order to improve the UV resistance and weather resistance of MS sealants, most of them will add UV absorbers and antioxidants to the sealants to shield the damage of ultraviolet rays, so as to achieve the purpose of extending the service life of MS sealants. However, since most of the current UV absorbers are small organic molecules, they are easy to volatilize, and it is difficult to achieve a barrier effect, and the purpose of extending the service life cannot be achieved.
[0004] Chinese patent document CN117986564A discloses a silane-modified polyether resin, a silane-modified polyether sealant and a preparation method thereof, which are mainly prepared from the following components according to the following weight ratio: 90-110 parts of silane-modified polyether resin, a plasticizer, 30-50 parts of a filler, 100-130 parts of a thixotropic agent, 1-3 parts of a water remover, 2-3 parts of an anti-aging agent, 1-3 parts of a silane coupling agent, 1-3 parts of a catalyst, and 0.3-0.5 parts. The invention overcomes the shortcomings of existing silane-modified polyether sealants, such as toxicity to humans, long curing time, and easy stickiness on the surface for a long time. The invention adopts a silane-modified polyether resin with a special structure, cooperates with a preferred type of catalyst, and synergizes with the preferred types of components in the system and their dosage ratios, and has the advantages of being green and environmentally friendly, fast curing speed, non-sticky surface, and excellent resistance to ultraviolet aging and heat aging. The filler used in the invention is nano calcium carbonate, which has the defects of high surface energy and easy agglomeration, and poor dispersion in the resin matrix, thereby affecting the fluidity of the sealant and affecting the extrusion performance of the sealant. Summary of the invention
[0005] The main purpose of the invention is to provide a MS sealant which is resistant to aging and has good extrusion performance.
[0006] To achieve the above object, the present invention provides a silane-modified polyether resin, and a preparation method thereof comprises the following steps:
[0007] (1) mixing nano-TiO2 and ethanol aqueous solution and stirring them uniformly, adding vinyl triethoxysilane, heating for reaction, cooling and filtering, collecting solids, washing and drying the solids to obtain vinyl TiO2, dispersing the vinyl TiO2 in xylene, adding 5-allyl-3-methoxy salicylic acid methyl ester and benzoyl peroxide, reacting at 80-120° C., cooling and filtering, collecting solids, and drying the solids to obtain a composite ultraviolet absorber;
[0008] (2) mixing a polyether having a hydroxyl group endcapped at one end and a carbon-carbon double bond endcapped at the other end and xylene, adding a composite ultraviolet absorber, adjusting the pH to 8-11 with an aqueous NaOH solution, heating for reaction, and removing the solvent under reduced pressure after the reaction is completed to obtain a composite ultraviolet absorber grafted modified polyether;
[0009] (3) dispersing the composite ultraviolet absorber grafted modified polyether in N,N-dimethylformamide, adding vinyl trimethoxysilane, heating, adding an initiator to react, and after the reaction is completed, evaporating the solvent under reduced pressure to obtain a silane-modified polyether resin.
[0010] Preferably, in step (1), the mass ratio of nano-titanium dioxide, 3-aminopropyltriethoxysilane, and 5-allyl-3-methoxysalicylic acid methyl ester is 20-30:1-2:15-18.
[0011] Preferably, the polyether terminated with a hydroxyl group at one end and a carbon-carbon double bond at the other end in step (2) has a structure as shown in formula (I):
[0012]
[0013] Preferably, in the formula (I), R1 is one of -H, -CH2CH3, and CH3.
[0014] Preferably, in the formula (I), x is 100-500; further preferably, x is 100-200.
[0015] Preferably, in step (2), the mass ratio of the polyether capped with a hydroxyl group at one end and a carbon-carbon double bond at the other end to the composite ultraviolet absorber is 10-20:2-3.
[0016] Preferably, in step (3), the mass ratio of the composite ultraviolet absorber grafted modified polyether to vinyltrimethoxysilane is 40-60:3-5.
[0017] Preferably, the initiator in step (3) is one of ammonium persulfate, potassium persulfate, azobisisobutyronitrile and dibenzoyl peroxide.
[0018] The silane-modified polyether of the present invention is a polyether with a hydroxyl group at one end and a carbon-carbon double bond at the other end, and a UV absorber composed of TiO2 and 5-allyl-3-methoxysalicylic acid methyl ester is grafted on the polyether, thereby avoiding the defect that a single UV absorber is easy to migrate out and thus affects the UV aging resistance. The composite UV absorber of the present invention combines the advantages of an inorganic UV absorber and an organic absorber, and effectively avoids the agglomeration of nano titanium dioxide through chemical grafting, so that the nano titanium dioxide is evenly dispersed in the matrix resin, and the MS sealant is endowed with excellent UV resistance in a wider range of UV light absorption, thereby improving the overall UV protection effect, reducing degradation under light, and extending the service life of the MS sealant.
[0019] The present invention also provides application of the silane-modified polyether resin in MS sealant.
[0020] Preferably, the MS sealant comprises the following components in parts by weight: 80-120 parts of silane-modified polyether resin, 200-300 parts of phenyl vinyl silicone oil-modified calcium carbonate, 50-150 parts of plasticizer, 1-2 parts of water absorbent, and 0.2-0.5 parts of catalyst.
[0021] Preferably, the preparation method of the phenyl vinyl silicone oil modified calcium carbonate is as follows:
[0022] The calcium carbonate powder and ethanol aqueous solution are mixed and stirred evenly, 3-mercaptopropyltrimethoxysilane is added, heated for reaction, cooled and filtered, the solid is collected, and the solid is washed and dried to obtain silane-coupled calcium carbonate; the silane-coupled calcium carbonate is dispersed in N,N-dimethylformamide, phenyl vinyl silicone oil is added, irradiated under ultraviolet light for reaction, filtered after the reaction is completed, washed, and dried to obtain phenyl vinyl silicone oil-modified calcium carbonate.
[0023] Preferably, the mass ratio of the calcium carbonate powder, 3-mercaptopropyltrimethoxysilane and phenyl vinyl silicone oil is 20-30:1-2:5-8.
[0024] Calcium carbonate is an inorganic nanofiller. Due to its unique nano effect and large specific surface area, inorganic nanofiller can greatly improve the mechanical properties of MS sealant. However, it has poor compatibility with the matrix resin and is difficult to disperse evenly in the matrix resin. By grafting phenyl vinyl silicone oil with good weather resistance on calcium carbonate, phenyl vinyl silicone oil is similar to rolling bearings and can play a lubricating role to prevent mutual friction between fillers that affects fluidity, thereby improving the dispersion effect and extrusion performance; grafting is more conducive to the cross-linking between calcium carbonate and other components, producing a more complex and dense cross-linking structure, thereby improving the mechanical properties of MS.
[0025] Preferably, the plasticizer may be diisodecyl phthalate and / or diisononyl phthalate.
[0026] Preferably, the water absorbent is a mixture of one or more water removing agents selected from vinyl trimethoxy silane, 3-isocyanate propyl trimethoxy silane, anhydrous calcium chloride and calcium oxide.
[0027] Preferably, the catalyst is a mixture of one or more of dibutyltin dilaurate, monobutyltin triisooctoate, dihydroxybutyltin chloride, and stannous octoate.
[0028] The present invention also discloses a method for preparing the MS sealant, comprising the following steps:
[0029] Under N2 atmosphere, phenyl vinyl silicone oil modified calcium carbonate, plasticizer and water absorbent are mixed evenly and heated to 90-100°C, vacuum dried for 1-3h, then cooled to 40-50°C, silane modified polyether resin is added and stirred evenly, and then a catalyst is added and mixed evenly to obtain the MS sealant.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1. The present invention synthesizes a silane-modified polyether grafted with a composite ultraviolet absorber, and uses the silane-modified polyether to prepare MS sealant, thereby enhancing the weather resistance and ultraviolet resistance of the sealant. The composite ultraviolet absorber prepared by the present invention is grafted onto the polyether molecule through a chemical bond, which can prevent the ultraviolet absorber from migrating and precipitating from the resin matrix, thereby improving the ultraviolet aging resistance of the MS sealant;
[0032] 2. The present invention has the advantages of mild reaction conditions, easy availability of reaction raw materials, easy separation and purification of products, and easy operation of the reaction process;
[0033] 3. The present invention grafts phenyl vinyl silicone oil with good weather resistance onto nano calcium carbonate. The phenyl vinyl silicone oil is similar to a rolling bearing and can play a lubricating role to prevent the friction between fillers from affecting fluidity, thereby improving the dispersion effect and extrusion performance; grafting is more conducive to the cross-linking between calcium carbonate and other components, producing a more complex and dense cross-linking structure, thereby improving the mechanical properties of the MS sealant. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0035] Figure 1 The following is the reaction formula for preparing the silane-modified polyether resin of the present invention. DETAILED DESCRIPTION
[0036] The sources of some raw materials in the examples of the present invention are as follows. Unless otherwise specified, the raw materials used in the examples can be obtained from conventional commercial channels or can be prepared by conventional methods.
[0037] The sources of some raw materials used in the present invention are as follows:
[0038] Calcium carbonate, mesh number 1250, was purchased from Lingshou County Chengming Mineral Products Processing Plant.
[0039] Nano-TiO2, rutile type, with a particle size of 5 nm, was purchased from Hebei Jipin New Materials Co., Ltd.
[0040] Taking Example 1 as an example, a polyether having a hydroxyl group at one end and a carbon-carbon double bond at the other end can be prepared by a conventional method, and the preparation method is as follows:
[0041] 50.3g of allyl alcohol and 1.4g of metal Na were mixed and stirred at room temperature for 1h, heated to 110°C, 300g of propylene oxide was added, and the mixture was reacted at 110°C for 2h. After the reaction was completed, the propylene oxide was evaporated under reduced pressure, 6.5g of phosphoric acid and 100g of water were added to the residue, stirred for 30min, and then allowed to stand. The oil phase was collected and vacuum dried to obtain an allyl alcohol polyether with a molecular weight of 400. 0.03g of DMC bimetallic catalyst was added to 30g of the dried allyl polyether, the temperature was raised to 110°C, 340g of propylene oxide was added, and the reaction was continued for 2h. After the reaction was completed, the unreacted propylene oxide was evaporated under reduced pressure to obtain a polyether with a number average molecular weight of 5000 and a number average molecular weight of 5000, which was terminated at one end by hydroxyl and terminated at the other end by carbon-carbon double bond, with a degree of polymerization of 85, a PDI of 1.10, a degree of unsaturation of 0.19mmol / g, and a structure of:
[0042]
[0043] Example 1
[0044] A method for preparing MS sealant comprises the following steps:
[0045] Under N2 atmosphere, 250g of phenyl vinyl silicone oil modified calcium carbonate, 120g of diisodecyl phthalate, and 1.6g of 3-isocyanate propyltrimethoxysilane were mixed evenly, heated to 100°C, vacuum dried for 2h, and then cooled to 45°C. 100g of silane modified polyether resin was added and stirred evenly, and then 0.3g of dibutyltin dilaurate was added and mixed evenly to obtain the MS sealant.
[0046] The preparation method of the phenyl vinyl silicone oil modified calcium carbonate is as follows:
[0047] 250g of calcium carbonate powder and 1000mL of 50wt% ethanol aqueous solution were mixed and stirred evenly, 15g of 3-mercaptopropyltrimethoxysilane was added, and the mixture was reacted at 50°C for 4h, cooled and filtered, and the solid was collected. The solid was washed with anhydrous ethanol and dried to obtain silane-coupled calcium carbonate; the silane-coupled calcium carbonate was dispersed in 1000mL of N,N-dimethylformamide, 62g of phenyl vinyl silicone oil was added, and the mixture was irradiated under 100W, 365nm ultraviolet light for reaction for 15min. After the reaction was completed, the mixture was filtered, washed, and dried to obtain phenyl vinyl silicone oil-modified calcium carbonate.
[0048] The silane-modified polyether resin has a reaction formula as follows: Figure 1 As shown, the specific preparation method comprises the following steps:
[0049] (1) 25.6 g of nano-TiO2 and 300 mL of 50 wt% ethanol aqueous solution were mixed and stirred uniformly, 1.58 g of vinyl triethoxysilane was added, the mixture was reacted at 50° C. for 3 h, cooled and filtered, and solid matter was collected. The solid matter was washed and dried to obtain vinyl TiO2. The vinyl TiO2 was dispersed in 300 mL of xylene, 16.5 g of 5-allyl-3-methoxy salicylic acid methyl ester and 2.8 g of benzoyl peroxide were added, the mixture was reacted at 100° C. for 6 h, cooled and filtered, and solid matter was collected. The composite ultraviolet absorber was obtained after the solid matter was dried;
[0050] (2) 157 g of a polyether having one end capped with a hydroxyl group and the other end capped with a carbon-carbon double bond and 500 mL of xylene were mixed, and 24.6 g of a composite ultraviolet absorber was added. The pH was adjusted to 10 with a 1 mol / L NaOH aqueous solution, and the mixture was heated at 60° C. for 4 h. After the reaction was completed, the solvent was evaporated under reduced pressure to obtain a composite ultraviolet absorber grafted modified polyether;
[0051] (3) Disperse 50 g of the composite UV absorber grafted modified polyether in 500 mL of N,N-dimethylformamide, add 4.6 g of vinyltrimethoxysilane and 1.3 g of benzoyl peroxide, and react at 100 °C for 6 h. After the reaction is completed, evaporate the solvent under reduced pressure to obtain a silane-modified polyether resin.
[0052] Example 2
[0053] A method for preparing MS sealant comprises the following steps:
[0054] Under N2 atmosphere, 300g of phenyl vinyl silicone oil modified calcium carbonate, 150g of diisodecyl phthalate, and 2g of 3-isocyanate propyltrimethoxysilane were mixed evenly, heated to 90°C, vacuum dried for 3h, and then cooled to 50°C. 120g of the silane-modified polyether resin prepared in Example 2 was added and stirred evenly, and then 0.5g of dibutyltin dilaurate was added and mixed evenly to obtain the MS sealant.
[0055] The preparation method of the phenyl vinyl silicone oil modified calcium carbonate is as follows:
[0056] 300 g of calcium carbonate powder and 1000 mL of 50 wt% ethanol aqueous solution were mixed and stirred evenly, 20 g of 3-mercaptopropyltrimethoxysilane was added, the mixture was reacted at 50° C. for 4 h, cooled and filtered, the solid was collected, and the solid was washed with anhydrous ethanol and dried to obtain silane-coupled calcium carbonate; the silane-coupled calcium carbonate was dispersed in 1000 mL of N,N-dimethylformamide, 80 g of phenyl vinyl silicone oil was added, and the mixture was irradiated under 120 W, 365 nm ultraviolet light for reaction for 20 min. After the reaction was completed, the mixture was filtered, washed, and dried to obtain phenyl vinyl silicone oil-modified calcium carbonate.
[0057] The silane-modified polyether resin and its preparation method include the following steps:
[0058] (1) 25.6 g of nano-TiO2 and 300 mL of 50 wt% ethanol aqueous solution were mixed and stirred uniformly, 1.58 g of vinyl triethoxysilane was added, the mixture was reacted at 50° C. for 3 h, cooled and filtered, and solid matter was collected. The solid matter was washed and dried to obtain vinyl TiO2. The vinyl TiO2 was dispersed in 300 mL of xylene, 16.5 g of 5-allyl-3-methoxy salicylic acid methyl ester and 2.8 g of benzoyl peroxide were added, the mixture was reacted at 100° C. for 6 h, cooled and filtered, and solid matter was collected. The composite ultraviolet absorber was obtained after the solid matter was dried;
[0059] (2) 157 g of a polyether having one end capped with a hydroxyl group and the other end capped with a carbon-carbon double bond and 500 mL of xylene were mixed, and 24.6 g of a composite ultraviolet absorber was added. The pH was adjusted to 10 with a 1 mol / L NaOH aqueous solution, and the mixture was heated at 60° C. for 4 h. After the reaction was completed, the solvent was evaporated under reduced pressure to obtain a composite ultraviolet absorber grafted modified polyether;
[0060] (3) Disperse 50 g of the composite UV absorber grafted modified polyether in 500 mL of N,N-dimethylformamide, add 4.6 g of vinyltrimethoxysilane and 1.3 g of benzoyl peroxide, and react at 100 °C for 6 h. After the reaction is completed, evaporate the solvent under reduced pressure to obtain a silane-modified polyether resin.
[0061] Example 3
[0062] A method for preparing MS sealant comprises the following steps:
[0063] Under N2 atmosphere, 200g of phenyl vinyl silicone oil modified calcium carbonate, 50g of diisodecyl phthalate, and 1.1g of 3-isocyanate propyltrimethoxysilane were mixed evenly and heated to 100°C, vacuum dried for 3h, and then cooled to 50°C, 100g of the silane-modified polyether resin prepared in Example 1 was added, stirred evenly, and then 0.2g of dibutyltin dilaurate was added and mixed evenly to obtain the MS sealant.
[0064] The preparation method of the phenyl vinyl silicone oil modified calcium carbonate is as follows:
[0065] 200 g of calcium carbonate powder and 1000 mL of 50 wt% ethanol aqueous solution were mixed and stirred evenly, 10 g of 3-mercaptopropyltrimethoxysilane was added, the mixture was reacted at 50° C. for 4 h, cooled and filtered, the solid was collected, and the solid was washed with anhydrous ethanol and dried to obtain silane-coupled calcium carbonate; the silane-coupled calcium carbonate was dispersed in 1000 mL of N,N-dimethylformamide, 50 g of phenyl vinyl silicone oil was added, the mixture was irradiated under 80 W, 365 nm ultraviolet light for reaction for 10 min, and after the reaction was completed, the mixture was filtered, washed, and dried to obtain phenyl vinyl silicone oil-modified calcium carbonate.
[0066] The silane-modified polyether resin and its preparation method include the following steps:
[0067] (1) 25.6 g of nano-TiO2 and 300 mL of 50 wt% ethanol aqueous solution were mixed and stirred uniformly, 1.58 g of vinyl triethoxysilane was added, the mixture was reacted at 50° C. for 3 h, cooled and filtered, and solid matter was collected. The solid matter was washed and dried to obtain vinyl TiO2. The vinyl TiO2 was dispersed in 300 mL of xylene, 16.5 g of 5-allyl-3-methoxy salicylic acid methyl ester and 2.8 g of benzoyl peroxide were added, the mixture was reacted at 100° C. for 6 h, cooled and filtered, and solid matter was collected. The composite ultraviolet absorber was obtained after the solid matter was dried;
[0068] (2) 157 g of a polyether having one end capped with a hydroxyl group and the other end capped with a carbon-carbon double bond and 500 mL of xylene were mixed, and 24.6 g of a composite ultraviolet absorber was added. The pH was adjusted to 10 with a 1 mol / L NaOH aqueous solution, and the mixture was heated at 60° C. for 4 h. After the reaction was completed, the solvent was evaporated under reduced pressure to obtain a composite ultraviolet absorber grafted modified polyether;
[0069] (3) Disperse 50 g of the composite UV absorber grafted modified polyether in 500 mL of N,N-dimethylformamide, add 4.6 g of vinyltrimethoxysilane and 1.3 g of benzoyl peroxide, and react at 100 °C for 6 h. After the reaction is completed, evaporate the solvent under reduced pressure to obtain a silane-modified polyether resin.
[0070] Comparative Example 1
[0071] A method for preparing MS sealant is similar to Example 1, except that nano-TiO2 is not added to the silane-modified polyether resin, and specifically comprises the following steps:
[0072] Under N2 atmosphere, 250g of phenyl vinyl silicone oil modified calcium carbonate, 120g of diisodecyl phthalate, and 1.6g of 3-isocyanate propyltrimethoxysilane were mixed evenly, heated to 100°C, vacuum dried for 2h, and then cooled to 45°C. 100g of silane modified polyether resin was added and stirred evenly, and then 0.3g of dibutyltin dilaurate was added and mixed evenly to obtain the MS sealant.
[0073] The preparation method of the phenyl vinyl silicone oil modified calcium carbonate is as follows:
[0074] 250g of calcium carbonate powder and 1000mL of 50wt% ethanol aqueous solution were mixed and stirred evenly, 15g of 3-mercaptopropyltrimethoxysilane was added, and the mixture was reacted at 50°C for 4h, cooled and filtered, and the solid was collected. The solid was washed with anhydrous ethanol and dried to obtain silane-coupled calcium carbonate; the silane-coupled calcium carbonate was dispersed in 1000mL of N,N-dimethylformamide, 62g of phenyl vinyl silicone oil was added, and the mixture was irradiated under 100W, 365nm ultraviolet light for reaction for 15min. After the reaction was completed, the mixture was filtered, washed, and dried to obtain phenyl vinyl silicone oil-modified calcium carbonate.
[0075] The silane-modified polyether resin and its preparation method include the following steps:
[0076] (1) 157 g of a polyether having a hydroxyl group at one end and a carbon-carbon double bond at the other end and 500 mL of xylene were mixed, and 24.6 g of methyl 5-allyl-3-methoxysalicylate was added. The pH was adjusted to 10 with a 1 mol / L NaOH aqueous solution, and the mixture was heated at 60° C. for 4 h. After the reaction was completed, the solvent was evaporated under reduced pressure to obtain a UV absorber grafted modified polyether;
[0077] (2) Disperse 50 g of the UV absorber grafted modified polyether in 500 mL of N,N-dimethylformamide, add 4.6 g of vinyltrimethoxysilane and 1.3 g of benzoyl peroxide, and react at 100° C. for 6 h. After the reaction is completed, evaporate the solvent under reduced pressure to obtain a silane-modified polyether resin.
[0078] Comparative Example 2
[0079] A method for preparing MS sealant is similar to that of Example 1, except that nano-TiO2 is directly added to the silane-modified polyether resin, and specifically comprises the following steps:
[0080] Under N2 atmosphere, 250g of phenyl vinyl silicone oil modified calcium carbonate, 120g of diisodecyl phthalate, and 1.6g of 3-isocyanate propyltrimethoxysilane were mixed evenly, heated to 100°C, vacuum dried for 2h, and then cooled to 45°C. 100g of silane modified polyether resin was added and stirred evenly, and then 0.3g of dibutyltin dilaurate was added and mixed evenly to obtain the MS sealant.
[0081] The preparation method of the phenyl vinyl silicone oil modified calcium carbonate is as follows:
[0082] 250g of calcium carbonate powder and 1000mL of 50wt% ethanol aqueous solution were mixed and stirred evenly, 15g of 3-mercaptopropyltrimethoxysilane was added, and the mixture was reacted at 50°C for 4h, cooled and filtered, and the solid was collected. The solid was washed with anhydrous ethanol and dried to obtain silane-coupled calcium carbonate; the silane-coupled calcium carbonate was dispersed in 1000mL of N,N-dimethylformamide, 62g of phenyl vinyl silicone oil was added, and the mixture was irradiated under 100W, 365nm ultraviolet light for reaction for 15min. After the reaction was completed, the mixture was filtered, washed, and dried to obtain phenyl vinyl silicone oil-modified calcium carbonate.
[0083] The silane-modified polyether resin and its preparation method include the following steps:
[0084] (1) 157 g of a polyether having a hydroxyl group at one end and a carbon-carbon double bond at the other end and 500 mL of xylene were mixed, 12.3 g of nano-TiO2 and 12.3 g of 5-allyl-3-methoxysalicylic acid methyl ester were added, the pH was adjusted to 10 with a 1 mol / L NaOH aqueous solution, and the mixture was heated at 60° C. for 4 h. After the reaction was completed, the solvent was evaporated under reduced pressure to obtain a composite ultraviolet absorber modified polyether;
[0085] (2) Disperse 50 g of the composite UV absorber-modified polyether in 500 mL of N,N-dimethylformamide, add 4.6 g of vinyltrimethoxysilane and 1.3 g of benzoyl peroxide, and react at 100 °C for 6 h. After the reaction is completed, evaporate the solvent under reduced pressure to obtain a silane-modified polyether resin.
[0086] Comparative Example 3
[0087] A method for preparing MS sealant is similar to that of Example 1, except that calcium carbonate and phenyl vinyl silicone oil are added separately, and specifically comprises the following steps:
[0088] Under N2 atmosphere, 218g of calcium carbonate, 41.2g of phenyl vinyl silicone oil, 120g of diisodecyl phthalate and 1.6g of 3-isocyanatepropyltrimethoxysilane were mixed and heated to 100°C, vacuum dried for 2h, and then cooled to 45°C. 100g of silane-modified polyether resin was added and stirred evenly, and then 0.3g of dibutyltin dilaurate was added and mixed evenly to obtain the MS sealant.
[0089] The silane-modified polyether resin and its preparation method include the following steps:
[0090] (1) 25.6 g of nano-TiO2 and 300 mL of 50 wt% ethanol aqueous solution were mixed and stirred uniformly, 1.58 g of vinyl triethoxysilane was added, the mixture was reacted at 50° C. for 3 h, cooled and filtered, and solid matter was collected. The solid matter was washed and dried to obtain vinyl TiO2. The vinyl TiO2 was dispersed in 300 mL of xylene, 16.5 g of 5-allyl-3-methoxy salicylic acid methyl ester and 2.8 g of benzoyl peroxide were added, the mixture was reacted at 100° C. for 6 h, cooled and filtered, and solid matter was collected. The composite ultraviolet absorber was obtained after the solid matter was dried;
[0091] (2) 157 g of a polyether having one end capped with a hydroxyl group and the other end capped with a carbon-carbon double bond and 500 mL of xylene were mixed, and 24.6 g of a composite ultraviolet absorber was added. The pH was adjusted to 10 with a 1 mol / L NaOH aqueous solution, and the mixture was heated at 60° C. for 4 h. After the reaction was completed, the solvent was evaporated under reduced pressure to obtain a composite ultraviolet absorber grafted modified polyether;
[0092] (3) Disperse 50 g of the composite UV absorber grafted modified polyether in 500 mL of N,N-dimethylformamide, add 4.6 g of vinyltrimethoxysilane and 1.3 g of benzoyl peroxide, and react at 100 °C for 6 h. After the reaction is completed, evaporate the solvent under reduced pressure to obtain a silane-modified polyether resin.
[0093] Comparative Example 4
[0094] A method for preparing MS sealant is similar to Example 1, except that calcium carbonate is not modified, and specifically comprises the following steps:
[0095] Under N2 atmosphere, 250g of calcium carbonate, 120g of diisodecyl phthalate and 1.6g of 3-isocyanatepropyltrimethoxysilane were mixed evenly, heated to 100°C, vacuum dried for 2h, then cooled to 45°C, 100g of silane-modified polyether resin was added and stirred evenly, and then 0.3g of dibutyltin dilaurate was added and mixed evenly to obtain the MS sealant.
[0096] The silane-modified polyether resin and its preparation method include the following steps:
[0097] (1) 25.6 g of nano-TiO2 and 300 mL of 50 wt% ethanol aqueous solution were mixed and stirred uniformly, 1.58 g of vinyl triethoxysilane was added, the mixture was reacted at 50° C. for 3 h, cooled and filtered, and solid matter was collected. The solid matter was washed and dried to obtain vinyl TiO2. The vinyl TiO2 was dispersed in 300 mL of xylene, 16.5 g of 5-allyl-3-methoxy salicylic acid methyl ester and 2.8 g of benzoyl peroxide were added, the mixture was reacted at 100° C. for 6 h, cooled and filtered, and solid matter was collected. The composite ultraviolet absorber was obtained after the solid matter was dried;
[0098] (2) 157 g of a polyether having one end capped with a hydroxyl group and the other end capped with a carbon-carbon double bond and 500 mL of xylene were mixed, and 24.6 g of a composite ultraviolet absorber was added. The pH was adjusted to 10 with a 1 mol / L NaOH aqueous solution, and the mixture was heated at 60° C. for 4 h. After the reaction was completed, the solvent was evaporated under reduced pressure to obtain a composite ultraviolet absorber grafted modified polyether;
[0099] (3) Disperse 50 g of the composite UV absorber grafted modified polyether in 500 mL of N,N-dimethylformamide, add 4.6 g of vinyltrimethoxysilane and 1.3 g of benzoyl peroxide, and react at 100 °C for 6 h. After the reaction is completed, evaporate the solvent under reduced pressure to obtain a silane-modified polyether resin.
[0100] Test Case
[0101] The performance tests were performed on the MS sealants prepared in Examples 1-3 and Comparative Examples 1-4 respectively, and the test methods were as follows:
[0102] 1. Anti-ultraviolet aging test:
[0103] The MS sealants prepared in Examples 1-3 and Comparative Examples 1-2 were subjected to UV aging treatment according to the method of GB / T16776-2005 "Silicone structural sealants for construction";
[0104] Shear strength: Tested with reference to JC / T 2186-2013 Nail-free adhesive for lightweight decorative panels on indoor walls;
[0105] The test results are shown in Table 1:
[0106] Table 1 Results of UV aging test of MS sealant
[0107]
[0108] It can be seen from the experimental results in Table 1 that the MS sealant prepared in the embodiment of the present invention still maintains a relatively high shear strength value after UV oxidation treatment, and its performance is significantly better than that of the MS sealant directly added with the blended UV absorber.
[0109] 2. Heat aging test: The MS sealants prepared in Examples 1-3 and Comparative Examples 3-4 were cured for 7 days under standard conditions and then placed in a 150°C oven for heat treatment for 30 days. The shear strength was tested with reference to JC / T2186-2013 nail-free glue for lightweight decorative panels on indoor walls. The test results are shown in Table 2:
[0110] Table 2 Thermal aging test results of MS sealant
[0111]
[0112] It can be seen from the experimental results in Table 2 that the MS sealant prepared in the embodiment of the present invention still maintains a relatively high shear strength value after being heat treated at 150°C.
[0113] 3. Extrusion performance test: The mass extrusion rate of the MS sealant prepared in Example 1 and Comparative Examples 3-4 was measured with reference to GB / T13477.3-2017 "Test methods for building sealing materials Part 3: Determination of basic properties of sealing materials using standard instruments". The test results are shown in Table 3:
[0114] <![CDATA[Mass extrusion rate (g·min -1 )]]> Example 1 1856.3 Comparative Example 3 1365.4 Comparative Example 4 1128.7
[0115] It can be seen from the experimental data in Table 3 that the mass extrusion rate of the MS sealant prepared in Example 1 of the present invention is the highest, and thus its fluidity is better.
[0116] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A MS sealant, It is characterized in that The invention comprises the following components in parts by weight: 80-120 parts of silane-modified polyether resin, 200-300 parts of phenyl vinyl silicone oil-modified calcium carbonate, 50-150 parts of plasticizer, 1-2 parts of water absorbent and 0.2-0.5 parts of catalyst.
2. The MS sealant according to claim 1, It is characterized in that The preparation method of the silane-modified polyether resin is characterized by comprising the following steps: (1) Nano-TiO 2 , ethanol and aqueous solution were mixed and stirred evenly, vinyl triethoxysilane was added, heated for reaction, cooled and filtered, and solids were collected. The solids were washed and dried to obtain vinyl TiO 2 , vinyl TiO 2 Disperse in xylene, add 5-allyl-3-methoxysalicylic acid methyl ester and benzoyl peroxide, react at 80-120°C, cool and filter, collect solids, and dry the solids to obtain a composite ultraviolet absorber; (2) mixing a polyether having a hydroxyl group endcapped at one end and a carbon-carbon double bond endcapped at the other end and xylene, adding a composite ultraviolet absorber, adjusting the pH to 8-11 with an aqueous NaOH solution, heating for reaction, and removing the solvent under reduced pressure after the reaction is completed to obtain a composite ultraviolet absorber grafted modified polyether; (3) dispersing the composite ultraviolet absorber grafted modified polyether in N,N-dimethylformamide, adding vinyl trimethoxysilane, heating, adding an initiator to react, and after the reaction is completed, evaporating the solvent under reduced pressure to obtain a silane-modified polyether resin.
3. The preparation method according to claim 2, Features: In the step (1), the mass ratio of nano titanium dioxide, 3-aminopropyltriethoxysilane and 5-allyl-3-methoxysalicylic acid methyl ester is 20-30:1-2:15-18.
4. The preparation method according to claim 2, It is characterized in that The polyether having a hydroxyl group at one end and a carbon-carbon double bond at the other end in step (2) has a structure as shown in formula (I): In the formula (I), R1 is -H, -CH 2 CH 3 , CH 3 One of the following; wherein x is 100-500.
5. The preparation method according to claim 2, Features: In the step (2), the mass ratio of the polyether capped with a hydroxyl group at one end and a carbon-carbon double bond at the other end to the composite ultraviolet absorber is 10-20:2-3.
6. The preparation method according to claim 2, Features: In the step (3), the mass ratio of the composite ultraviolet absorber grafted modified polyether to vinyltrimethoxysilane is 40-60:3-5.
7. A silane-modified polyether resin, Features: The compound is prepared by the preparation method according to any one of claims 2 to 6.
8. The MS sealant according to claim 1, It is characterized in that The preparation method of the phenyl vinyl silicone oil modified calcium carbonate is as follows: The calcium carbonate powder and ethanol aqueous solution are mixed and stirred evenly, 3-mercaptopropyltrimethoxysilane is added, heated for reaction, cooled and filtered, the solid is collected, and the solid is washed and dried to obtain silane-coupled calcium carbonate; the silane-coupled calcium carbonate is dispersed in N,N-dimethylformamide, phenyl vinyl silicone oil is added, irradiated under ultraviolet light for reaction, filtered after the reaction is completed, washed, and dried to obtain phenyl vinyl silicone oil-modified calcium carbonate.
9. The MS sealant according to claim 8, Features: The mass ratio of the calcium carbonate powder, 3-mercaptopropyltrimethoxysilane and phenyl vinyl silicone oil is 20-30:1-2:5-8.
10. A method for preparing the MS sealant according to claim 1, It is characterized in that The steps include: In N 2 Under the atmosphere, phenyl vinyl silicone oil modified calcium carbonate, plasticizer and water absorbent are mixed evenly, heated to 90-100° C., vacuum dried for 1-3 hours, then cooled to 40-50° C., silane modified polyether resin is added, stirred evenly, and then a catalyst is added and mixed evenly to obtain the MS sealant.
Citation Information
Patent Citations
Silane modified polyether resin, silane modified polyether sealant and preparation method thereof
CN117986564A
Electrorheological fluid of nano titanium dioxide grafted vinyl polysiloxane and preparation method
CN106967475A
Silicone sealant for electronic products and preparation method of silicone sealant
CN107254290A
Industrial silane modified polyether elastic sealant and preparation method thereof
CN114231237A
Preparation method of high-transparency silane modified polyether sealant
CN118480330A
Cited By
Acrylic hardening coating, preparation method thereof and acrylic product
CN119799154A
An acrylic hardening coating, its preparation method and an acrylic product
CN119799154B