Silicate blue-red double-light light conversion agent, preparation method thereof and light conversion film containing light conversion agent
By developing the silicate blue-red double-light conversion agent Ba1-xEuxSrMg1-yMnySi2O7, the existing conversion agents have been solved in terms of cost, stability and light energy utilization efficiency, and the matching with the plant photosynthesis spectrum has been achieved, which has improved the Plant photosynthesis efficiency and the service life and dispersion of the phototransformation film are improved through the multi-layer coextrusion blown film process.
Patent Information
- Application Number
- CN202411040077.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
Smart Images

Figure CN118956397A_ABST
Abstract
Description
Technical field:
[0001] The invention relates to inorganic optical functional materials, in particular to a silicate blue-red dual light conversion agent and a preparation method thereof and a light conversion film containing the light conversion agent. Background technology:
[0002] With the rapid development of modern agricultural technology, agricultural films with light-conversion function (light-conversion films) are playing an increasingly important role in modern agricultural production. Solar radiation is an indispensable source of plant photosynthesis. Plant photosynthesis is mainly completed by chlorophyll absorbing sunlight. The absorption bands of chlorophyll a and chlorophyll b are concentrated in blue-violet light (400-480nm) and red-orange light (600-700nm). Chlorophyll has the largest absorption ratio of blue-violet light and the greatest impact on photosynthesis. Blue-violet light can promote the growth of plant roots and stems and the expansion of branches and leaves, and red-orange light can promote the elongation growth and flowering process of plants. Therefore, blue-violet light and red-orange light are the most important for plant photosynthesis. The short-wave ultraviolet rays of 200-280nm in sunlight will be absorbed by the ozone layer when passing through the stratosphere on the earth's surface, so only the ultraviolet rays with a wavelength of 290-380nm can reach the ground. The ultraviolet rays with a wavelength range of 290-315nm will promote the aging and decay of plant branches and trunks, which is not conducive to plant growth, and will cause the aging of agricultural films. The near-ultraviolet rays with a wavelength range of 315-400nm, except for the light near 360nm that is beneficial to promoting the coloring of plant fruits, will make individual plants shorter and thicker, restricting the normal growth of plants. Therefore, the development of a light-converting film that can convert the ultraviolet light of 280-400nm in sunlight into blue-violet light and red-orange light can not only reduce the disadvantages of ultraviolet rays in sunlight to plants, but more importantly, it can improve the light quality, effectively improve the utilization rate of light energy of crops, benefit crop growth and promote early maturity and increase yield of crops.
[0003] Light conversion agents are the core material of light conversion films and are the key to achieving light energy conversion and improving the quality of light transmitted through the film. At present, light conversion agents on the market are mainly divided into three categories: rare earth complex light conversion agents, organic dye light conversion agents and inorganic salt light conversion agents. Rare earth complex light conversion agents and organic dye light conversion agents have good compatibility with the base resin of agricultural films, but their emission spectra have poor matching with the absorption wavelength of plant chlorophyll. They are easily oxidized and decomposed under long-term exposure to sunlight, and their decay rate is fast, resulting in a short service life that cannot be synchronized with the life of the greenhouse film. In addition, the production cost is high, which limits their widespread promotion. Inorganic salt light conversion agents have the advantages of good high temperature resistance, easy preparation, strong weather resistance, and long service life, but Eu 2+ The doped alkaline earth metal sulfides are easily deliquesced in the air and release H2S gas to pollute the environment. 2+ The production cost of doped nitride is high, Mn 4+The photoconversion efficiency of doped inorganic compounds is low, Eu 3+ The emission spectrum of the doped inorganic compound has a poor match with the absorption wavelength of plant chlorophyll, and most of the research focuses on red light conversion agents. Therefore, the existing light conversion agents and light conversion films still have deficiencies in production cost, stability, and efficient use of light energy. The dispersibility of the light conversion agent in the film matrix needs to be further improved, and new low-cost and efficient light conversion agents and light conversion films are urgently needed. Summary of the invention:
[0004] The purpose of the present invention is to provide a silicate blue-red dual-light conversion agent and a preparation method thereof, and a light conversion film containing the light conversion agent.
[0005] The present invention is achieved through the following technical solutions:
[0006] A silicate blue-red dual-light conversion agent, the chemical formula is as follows: Ba 1-x Eu x SrMg 1-y Mn y SiO 7, Among them, 0.005≤x≤0.035,0.1≤y≤0.4.
[0007] Preferably, 0.015≤x≤0.025, 0.15≤y≤0.25.
[0008] The preparation method of the above-mentioned silicate blue-red dual light conversion agent comprises the following steps:
[0009] 1) Using barium carbonate, strontium carbonate, magnesium oxide, silicon dioxide, europium trioxide and manganese carbonate as raw materials, according to Ba 1-x Eu x SrMg 1-y Mn y The raw materials are accurately weighed in the stoichiometric ratio of Si2O7, and all the raw materials are ball-milled and mixed to obtain a mixture;
[0010] 2) placing the mixture obtained in step 1) in a corundum crucible, sintering at 1200-1300° C. for 6-10 hours in an air atmosphere, and crushing the mixture after natural cooling to obtain a powder material;
[0011] 3) Sintering the powder material obtained in step 2) at 1150-1250° C. for 4-6 hours in a reducing atmosphere;
[0012] 4) crushing, ball-milling and sieving the sintered product obtained in step 3), placing the water-powder mixture into a vacuum drying oven and drying it at 100-200° C., crushing and sieving the dried product to obtain the silicate blue-red dual-light conversion agent.
[0013] Preferably, the reducing atmosphere in step 3) is a mixture of nitrogen and hydrogen.
[0014] A light-converting film containing the above-mentioned silicate blue-red dual-light-converting agent is prepared from the following components in parts by weight:
[0015] Film substrate: 100 parts;
[0016] Masterbatch matrix: 20-40 parts;
[0017] Blue-red dual-light conversion agent: 1-2 parts;
[0018] Additives: 1-3 parts.
[0019] The film matrix is at least one of low-density polyethylene, linear low-density polyethylene, ethylene-vinyl acetate copolymer, and metallocene polyethylene.
[0020] The masterbatch matrix is at least one of low-density polyethylene, linear low-density polyethylene, ethylene-vinyl acetate copolymer, and metallocene polyethylene.
[0021] The auxiliary agent is at least one of polyethylene wax, zinc stearate, paraffin, hindered amine light stabilizer, salicylate light stabilizer, hindered phenol antioxidant, and phosphite antioxidant.
[0022] The preparation method of the light-converting film containing the above-mentioned silicate blue-red dual light-converting agent comprises the following steps:
[0023] 1) mixing the silicate blue-red dual-light conversion agent and the masterbatch matrix uniformly, and then subjecting the mixture to thermoplasticization extrusion granulation by a twin-screw extruder to obtain a light conversion masterbatch;
[0024] 2) After the masterbatch matrix and the additive are uniformly mixed, they are extruded and granulated by a twin-screw extruder to obtain the additive masterbatch;
[0025] 3) Evenly mixing the light conversion agent masterbatch with the film matrix, evenly mixing the auxiliary agent masterbatch with the film matrix, and obtaining at least three layers of light conversion film by multi-layer co-extrusion blown film, wherein the light conversion agent is located in the middle layer.
[0026] Preferably, in step 1), the mass ratio of the silicate blue-red dual-light conversion agent to the masterbatch matrix is 1-2:10.
[0027] Preferably, in step 2), the mass ratio of the auxiliary agent to the masterbatch matrix is 1-3:10.
[0028] Preferably, in step 3), the mass ratio of the transfer agent masterbatch to the film matrix is 950-990:10-50; the mass ratio of the auxiliary agent masterbatch to the film matrix is 950-990:10-50.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1) The silicate blue-red dual light conversion agent provided by the present invention has broadband absorption at 200-400nm, and simultaneously emits blue-violet light at 400-480nm and red-orange light at 600-700nm, which matches the photosynthesis spectrum of plants. The light conversion film prepared using the silicate light conversion agent provided by the present invention can effectively absorb ultraviolet light in sunlight that is harmful to plant growth, and convert it into blue-violet light and red-orange light that can promote plant photosynthesis, thereby improving the photosynthesis efficiency of plants.
[0031] 2) The silicate light conversion agent provided by the present invention adjusts the activation ion Eu 2+ and Mn 2+ The content can adjust the ratio of blue-violet light and red-orange light, and the required blue-red light ratio can be designed according to the light-loving characteristics of crops.
[0032] 3) The silicate light conversion agent provided by the present invention also has the advantages of stable physical and chemical properties, good weather resistance, long service life, simple synthesis process, low production cost, and can be directly prepared into light conversion masterbatch and light conversion film without surface treatment. Its body color is white and has little effect on the light transmittance of the film.
[0033] 4) The present invention first prepares a silicate light conversion agent and an auxiliary agent into a master batch, and then prepares a light conversion film, so that the light conversion agent and the auxiliary agent can be pre-dispersed to improve the dispersibility of the light conversion agent and the auxiliary agent in the film matrix. In addition, adding the light conversion agent and the auxiliary agent to different film layers can avoid the reaction between the light conversion agent and the auxiliary agent to affect the light conversion efficiency. Finally, placing the light conversion agent in the middle layer can effectively reduce the influence of water, oxygen, ultraviolet rays, etc. on the light conversion agent, thereby improving the light conversion efficiency and service life of the light conversion film, and reducing the cost of crop planting. Description of the drawings:
[0034] Figure 1 is the XRD pattern of the silicate blue-red dual light conversion agent in Example 1;
[0035] Figure 2 The excitation and emission spectra of the silicate blue-red dual-light conversion agent in Example 1;
[0036] Figure 3 It is the normalized emission spectrum of the silicate blue-red dual-light conversion agent in Example 1-5. Specific implementation method:
[0037] The following is a further description of the present invention, rather than a limitation of the present invention.
[0038] Example 1: Ba 0.98 Eu 0.02 SrMg 0.8 Mn 0.2Si2O7 light conversion agent
[0039] Barium carbonate, strontium carbonate, magnesium oxide, silicon dioxide, europium trioxide and manganese carbonate are used as raw materials. The raw materials are accurately weighed according to the stoichiometric ratio, ball-milled and mixed evenly, and then the raw materials are placed in a corundum crucible and placed in a high-temperature kiln. They are sintered at 1250°C for 10 hours in an air atmosphere, and crushed to obtain a powder material after natural cooling. The crushed material is then placed in a corundum crucible and placed in a high-temperature kiln. It is sintered at 1200°C for 6 hours in an atmosphere of 25% N2 + 75% H2 to obtain a sintered product. The sintered product is crushed, ball-milled, and sieved. The water-powder mixture is placed in a vacuum drying oven and dried at 200°C. The dried product is ball-milled and sieved to obtain a silicate blue-red dual-light conversion agent. The XRD pattern of the light conversion agent is shown as follows: Figure 1 The excitation and emission spectra of the light conversion agent are shown in Figure 2 As shown, the light conversion agent has broadband absorption at 200-400nm, and broadband emission of blue-violet light and red-orange light at 400-480nm and 600-700nm. The light conversion agent can effectively absorb ultraviolet light that is harmful to plant growth, and emit blue-violet light and red-orange light that can promote plant photosynthesis.
[0040] Example 2: Ba 0.98 Eu 0.02 SrMg 0.9 Mn 0.1 Si2O7 light conversion agent
[0041] Barium carbonate, strontium carbonate, magnesium oxide, silicon dioxide, europium trioxide and manganese carbonate are used as raw materials, and the raw materials are accurately weighed according to the stoichiometric ratio. After ball milling and mixing evenly, the raw materials are loaded into a corundum crucible, put into a high-temperature kiln, sintered at 1250°C for 10 hours in an air atmosphere, and crushed to obtain a powder material after natural cooling. The crushed material is then loaded into a corundum crucible, put into a high-temperature kiln, sintered at 1200°C for 6 hours in a 25% N2+75% H2 atmosphere to obtain a sintered product. The sintered product is crushed, ball milled, and sieved, and the water-powder mixture is placed in a vacuum drying oven and dried at 200°C. The dried product is ball milled and sieved to obtain a silicate blue-red dual-light conversion agent.
[0042] Example 3: Ba 0.98 Eu 0.02 SrMg 0.85 Mn 0.15 Si2O7 light conversion agent
[0043] Barium carbonate, strontium carbonate, magnesium oxide, silicon dioxide, europium trioxide and manganese carbonate are used as raw materials, and the raw materials are accurately weighed according to the stoichiometric ratio. After ball milling and mixing evenly, the raw materials are loaded into a corundum crucible, put into a high-temperature kiln, sintered at 1250°C for 10 hours in an air atmosphere, and crushed to obtain a powder material after natural cooling. The crushed material is then loaded into a corundum crucible, put into a high-temperature kiln, sintered at 1200°C for 6 hours in a 25% N2+75% H2 atmosphere to obtain a sintered product. The sintered product is crushed, ball milled, and sieved, and the water-powder mixture is placed in a vacuum drying oven and dried at 200°C. The dried product is ball milled and sieved to obtain a silicate blue-red dual-light conversion agent.
[0044] Example 4: Ba 0.995 Eu 0.005 SrMg 0.8 Mn 0.2 Si2O7 light conversion agent
[0045] Barium carbonate, strontium carbonate, magnesium oxide, silicon dioxide, europium trioxide and manganese carbonate are used as raw materials, and the raw materials are accurately weighed according to the stoichiometric ratio. After ball milling and mixing evenly, the raw materials are loaded into a corundum crucible, put into a high-temperature kiln, sintered at 1300°C for 6 hours in an air atmosphere, and crushed to obtain a powder material after natural cooling. The crushed raw materials are then loaded into a corundum crucible, sintered at 1150°C for 4 hours in a 50% N2+50% H2 atmosphere to obtain a sintered product. The sintered product is crushed, ball milled, and sieved, and the water-powder mixture is placed in a vacuum drying oven and dried at 100°C. The dried product is ball milled and sieved to obtain a silicate blue-red dual-light conversion agent.
[0046] Example 5: Ba 0.965 Eu 0.035 SrMg 0.6 Mn 0.4 Si2O7 light conversion agent
[0047] Barium carbonate, strontium carbonate, magnesium oxide, silicon dioxide, europium trioxide and manganese carbonate are used as raw materials, and the raw materials are accurately weighed according to the stoichiometric ratio. After ball milling and mixing evenly, the raw materials are loaded into a corundum crucible, put into a high-temperature kiln, sintered at 1250°C for 6 hours in an air atmosphere, and crushed to obtain a powder material after natural cooling. The crushed raw materials are then loaded into a corundum crucible, sintered at 1250°C for 6 hours in an atmosphere of 75% N2+75% H2 to obtain a sintered product. The sintered product is crushed, ball milled, and sieved, and the water-powder mixture is placed in a vacuum drying oven and dried at 150°C. The dried product is ball milled and sieved to obtain a silicate blue-red dual-light conversion agent.
[0048] Example 6: Preparation of light-converting film
[0049] Take 1 kg of the silicate light conversion agent prepared in Example 1 of the present invention and 10 kg of low-density polyethylene, add the above materials to a high-speed mixer and mix them evenly, then add them to a twin-screw extruder for heating and plasticization, and then cut into pellets after drawing and water cooling to obtain light conversion masterbatch.
[0050] Take 0.2 kg of polyethylene wax, 0.5 kg of hindered amine light stabilizer, 0.4 kg of phosphite antioxidant, and 10 kg of low-density polyethylene, add the above materials to a high-speed mixer and mix evenly, then add them to a twin-screw extruder for heating and plasticization, and then cut into pellets after drawing and water cooling to obtain the additive masterbatch.
[0051] Take 990 kg of low-density polyethylene and 10 kg of the light-converting masterbatch prepared above; take 990 kg of low-density polyethylene and 10 kg of the auxiliary agent masterbatch prepared above, mix them evenly, and then put the mixed raw materials into an extruder for multi-layer co-extrusion blown film to obtain a light-converting film.
[0052] Example 7: Preparation of light-converting film
[0053] Take 1 kg of the silicate light conversion agent prepared in Example 1 of the present invention and 10 kg of linear low-density polyethylene, add the above materials to a high-speed mixer and mix them evenly, then add them to a twin-screw extruder for heating and plasticization, and then cut into pellets after drawing and water cooling to obtain light conversion masterbatch.
[0054] Take 0.3 kg of polyethylene wax, 0.8 kg of hindered amine light stabilizer, 0.5 kg of phosphite antioxidant, and 10 kg of linear low-density polyethylene, add the above materials to a high-speed mixer and mix evenly, then add them to a twin-screw extruder for heating and plasticization, and then cut into pellets after drawing and water cooling to obtain the additive masterbatch.
[0055] Take 990 kg of linear low-density polyethylene and 10 kg of the light-converting masterbatch prepared above; take 990 kg of linear low-density polyethylene and 10 kg of the auxiliary agent masterbatch prepared above, mix them evenly, and then put the mixed raw materials into an extruder for multi-layer co-extrusion blown film to obtain a light-converting film.
[0056] Example 8: Preparation of light-converting film
[0057] Take 1.5 kg of the silicate light conversion agent prepared in Example 1 of the present invention and 10 kg of ethylene-vinyl acetate copolymer, add the above materials into a high-speed mixer and mix them evenly, then add them into a twin-screw extruder for heating and plasticization, extrude them, and then cut them into pellets after drawing and water cooling to obtain light conversion masterbatch.
[0058] Take 0.3 kg of paraffin wax, 0.5 kg of hindered amine light stabilizer, 1.0 kg of phosphite antioxidant, and 10 kg of ethylene-vinyl acetate copolymer, add the above materials into a high-speed mixer and mix evenly, then add them into a twin-screw extruder for heating and plasticization, and then cut into pellets after drawing and water cooling to obtain the additive masterbatch.
[0059] Take 990 kg of ethylene-vinyl acetate copolymer and 10 kg of the light conversion masterbatch prepared above, take 990 kg of ethylene-vinyl acetate copolymer and 10 kg of the light conversion auxiliary agent masterbatch prepared above, mix them evenly, and then put the mixed raw materials into an extruder for multi-layer co-extrusion blown film to obtain a light conversion film.
[0060] Example 9: Preparation of light-converting film
[0061] Take 1.5 kg of the silicate light conversion agent prepared in Example 1 of the present invention and 10 kg of metallocene polyethylene, add the above materials into a high-speed mixer and mix them evenly, then add them into a twin-screw extruder for heating and plasticization, extrude them, and then cut them into pellets after drawing and water cooling to obtain light conversion masterbatch.
[0062] Take 0.2 kg paraffin, 0.8 kg hindered amine light stabilizer, 1.0 kg phosphite antioxidant, and 10 kg metallocene polyethylene, add the above materials into a high-speed mixer and mix evenly, then add them into a twin-screw extruder for heating and plasticization, extrude them, and then cut into pellets after drawing and water cooling to obtain the additive masterbatch.
[0063] Take 990 kg of metallocene polyethylene and 10 kg of the light conversion masterbatch prepared above, take 990 kg of metal polyethylene and 10 kg of the additive masterbatch prepared above, mix them evenly, and then put the mixed raw materials into an extruder for multi-layer co-extrusion blown film to obtain a light conversion film.
[0064] Example 10: Preparation of light-converting film
[0065] Take 1 kg of the silicate light conversion agent prepared in Example 1 of the present invention and 10 kg of low-density polyethylene, add the above materials to a high-speed mixer and mix them evenly, then add them to a twin-screw extruder for heating and plasticization, and then cut into pellets after drawing and water cooling to obtain light conversion masterbatch.
[0066] Take 0.1 kg polyethylene wax, 0.5 kg hindered amine light stabilizer, 0.4 kg phosphite antioxidant, and 10 kg low-density polyethylene, add the above materials to a high-speed mixer and mix evenly, then add them to a twin-screw extruder for heating and plasticization, and then cut into pellets after drawing and water cooling to obtain the additive masterbatch.
[0067] Take 490 kg of low-density polyethylene, 500 kg of linear low-density polyethylene, and 10 kg of the light-converting masterbatch prepared above; take 490 kg of low-density polyethylene, 500 kg of linear low-density polyethylene, and 10 kg of the additive masterbatch prepared above, mix them respectively and then put the mixed raw materials into an extruder for multi-layer co-extrusion blown film to obtain a light-converting film.
[0068] Example 11: Preparation of light-converting film
[0069] Take 2 kg of the silicate light conversion agent prepared in Example 1 of the present invention and 10 kg of low-density polyethylene, add the above materials to a high-speed mixer and mix them evenly, then add them to a twin-screw extruder for heating and plasticization, and then cut into pellets after drawing and water cooling to obtain light conversion masterbatch.
[0070] Take 0.3 kg of polyethylene wax, 1.5 kg of hindered amine light stabilizer, 1.2 kg of phosphite antioxidant, and 10 kg of low-density polyethylene, add the above materials to a high-speed mixer and mix evenly, then add them to a twin-screw extruder for heating and plasticization, and then cut into pellets after drawing and water cooling to obtain the additive masterbatch.
[0071] Take 390Kg of low-density polyethylene, 400Kg of linear low-density polyethylene, 200Kg of ethylene-vinyl acetate copolymer, and 10Kg of the light-converting masterbatch prepared above; take 390Kg of low-density polyethylene, 500Kg of linear low-density polyethylene, and 10Kg of the additive masterbatch prepared above, mix them respectively and then put the mixed raw materials into an extruder for multi-layer co-extrusion blown film to obtain a light-converting film.
[0072] Example 12: Preparation of light-converting film
[0073] Take 1.5 kg of the silicate light conversion agent prepared in Example 1 of the present invention and 10 kg of low-density polyethylene, add the above materials to a high-speed mixer and mix them evenly, then add them to a twin-screw extruder for heating, plasticization and extrusion, and then cut into pellets after drawing and water cooling to obtain light conversion masterbatch.
[0074] Take 0.2 kg of paraffin, 1.0 kg of hindered amine light stabilizer, 1.2 kg of phosphite antioxidant, and 10 kg of low-density polyethylene, add the above materials into a high-speed mixer and mix evenly, then add them into a twin-screw extruder for heating and plasticization, and then cut into pellets after drawing and water cooling to obtain the additive masterbatch.
[0075] Take 440Kg of low-density polyethylene, 450Kg of linear low-density polyethylene, 100Kg of metallocene polyethylene, and 10Kg of the light-converting masterbatch prepared above; take 440Kg of low-density polyethylene, 450Kg of linear low-density polyethylene, 100Kg of metallocene polyethylene, and 10Kg of the additive masterbatch prepared above, mix them respectively and then put the mixed raw materials into an extruder for multi-layer co-extrusion blown film to obtain a light-converting film.
[0076] Example 13: Preparation of light-converting film
[0077] Take 1.5 kg of the silicate light conversion agent prepared in Example 1 of the present invention and 10 kg of low-density polyethylene, add the above materials to a high-speed mixer and mix them evenly, then add them to a twin-screw extruder for heating, plasticization and extrusion, and then cut into pellets after drawing and water cooling to obtain light conversion masterbatch.
[0078] Take 0.2 kg of paraffin, 0.8 kg of hindered amine light stabilizer, 1.0 kg of phosphite antioxidant, and 10 kg of low-density polyethylene, add the above materials into a high-speed mixer and mix evenly, then add them into a twin-screw extruder for heating and plasticization, and then cut into pellets after drawing and water cooling to obtain the additive masterbatch.
[0079] Take 240Kg of low-density polyethylene, 250Kg of linear low-density polyethylene, 250Kg of metallocene polyethylene, 250Kg of ethylene-vinyl acetate copolymer, and 10Kg of the light-converting masterbatch prepared above; take 240Kg of low-density polyethylene, 250Kg of linear low-density polyethylene, 250Kg of metallocene polyethylene, 250Kg of ethylene-vinyl acetate copolymer, and 10Kg of the auxiliary agent masterbatch prepared above, mix them respectively and then put the mixed raw materials into an extruder for multi-layer co-extrusion blown film to obtain a light-converting film.
Claims
1. A silicate blue-red dual-light conversion agent, It is characterized in that The general chemical formula is as follows: Ba 1-x Eu x SrMg 1-y Mn y Si 2 O 7 , where 0.005≤x≤0.035,0.1≤y≤0.
4.
2. The silicate blue-red dual light conversion agent according to claim 1, It is characterized in that 0.015≤x≤0.025,0.15≤y≤0.
25.
3. A method for preparing the silicate blue-red dual light conversion agent according to claim 1, It is characterized in that The following steps are involved: 1) Using barium carbonate, strontium carbonate, magnesium oxide, silicon dioxide, europium trioxide and manganese carbonate as raw materials, according to Ba 1- x Eu x SrMg 1-y Mn y Si 2 O 7 The raw materials are accurately weighed according to the stoichiometric ratio, and all the raw materials are ball-milled and mixed to obtain a mixture; 2) placing the mixture obtained in step 1) in a corundum crucible, sintering at 1200-1300° C. for 6-10 hours in an air atmosphere, and crushing the mixture after natural cooling to obtain a powder material; 3) Sintering the powder material obtained in step 2) at 1150-1250° C. for 4-6 hours in a reducing atmosphere; 4) crushing, ball-milling and sieving the sintered product obtained in step 3), placing the water-powder mixture into a vacuum drying oven and drying it at 100-200° C., crushing and sieving the dried product to obtain the silicate blue-red dual-light conversion agent.
4. The preparation method of the silicate blue-red dual light conversion agent according to claim 3, It is characterized in that The reducing atmosphere in step 3) is a mixture of nitrogen and hydrogen.
5. A light-converting film containing the silicate blue-red dual-light-converting agent according to claim 1, It is characterized in that It is prepared from the following components in parts by weight: Film substrate: 100 parts; Masterbatch matrix: 20-40 parts; Blue-red dual-light conversion agent: 1-2 parts; Additives: 1-3 parts.
6. The light-converting film according to claim 5, It is characterized in that The film matrix is at least one of low-density polyethylene, linear low-density polyethylene, ethylene-vinyl acetate copolymer, and metallocene polyethylene.
7. The light-converting film according to claim 5, It is characterized in that The masterbatch matrix is at least one of low-density polyethylene, linear low-density polyethylene, ethylene-vinyl acetate copolymer, and metallocene polyethylene.
8. The light-converting film according to claim 5, It is characterized in that The auxiliary agent is at least one of polyethylene wax, zinc stearate, paraffin, hindered amine light stabilizer, salicylate light stabilizer, hindered phenol antioxidant, and phosphite antioxidant.
9. The method for preparing the light-converting film according to claim 5, It is characterized in that The following steps are involved: 1) mixing the silicate blue-red dual-light conversion agent and the masterbatch matrix uniformly, and then subjecting the mixture to thermoplasticization extrusion granulation by a twin-screw extruder to obtain a light conversion masterbatch; 2) After the masterbatch matrix and the additive are uniformly mixed, they are extruded and granulated by a twin-screw extruder to obtain the additive masterbatch; 3) Evenly mixing the light conversion agent masterbatch with the film matrix, evenly mixing the auxiliary agent masterbatch with the film matrix, and obtaining at least three layers of light conversion film by multi-layer co-extrusion blown film, wherein the light conversion agent is located in the middle layer.
10. The method for preparing the light-converting film according to claim 9, It is characterized in that In step 1), the mass ratio of the silicate blue-red dual light conversion agent to the masterbatch matrix is 1-2:10; in step 2), the mass ratio of the auxiliary agent to the masterbatch matrix is 1-3:10; in step 3), the mass ratio of the light conversion agent masterbatch to the film matrix is 950-990:10-50; the mass ratio of the auxiliary agent masterbatch to the film matrix is 950-990:10-50.
Citation Information
Patent Citations
Light conversion agricultural film, and making method and application thereof
CN105385014A