Long-process ferrous metallurgy production method for producing iron and steel products by consuming iron-containing materials through electro-hydrogen circulation
By using a green electricity and green hydrogen recycling system in the reduction furnace and smelting furnace, the problems of high carbon emissions and tail gas treatment in the blast furnace ironmaking process have been solved, realizing an efficient and low-cost carbon-free metallurgical process, and improving the reducibility of iron and the sustainability of green metallurgy.
Patent Information
- Application Number
- CN202411020448.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
Existing technologies for blast furnace ironmaking involve high carbon emissions, irreplaceable use of coke, scarcity of high-quality iron ore resources, and challenges in heat absorption and tail gas treatment during pure hydrogen ironmaking, leading to environmental pollution and high production costs.
The all-hydrogen method utilizes green electricity and green hydrogen in reduction furnaces and smelting furnaces, and processes iron-containing materials through an electric-hydrogen circulation system to achieve a carbon-free metallurgical process. This includes improved rotary kilns, vertical shaft furnaces, blast furnaces, and other equipment for electric heating and hydrogen reduction, combined with a flue gas circulation system for tail gas treatment, to achieve efficient utilization of green hydrogen.
It has enabled a carbon-free metallurgical process, reduced production costs, improved the reducibility of iron, reduced carbon emissions, solved the problems of high cost and low efficiency in tail gas treatment, and supported the sustainable development of green metallurgy.
Smart Images

Figure CN118957190A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a long-process iron and steel metallurgical production method for producing iron and steel products by consuming iron-containing materials through electric hydrogen circulation, and belongs to the technical field of green metallurgy. Background Art
[0002] The steel industry is an important pillar industry of the national economy and plays a huge supporting role in economic and social development. The steel industry produces molten iron with a long process mainly based on blast furnaces, and blast furnace ironmaking accounts for about 90%. In the production process of blast furnace ironmaking, iron ore, coke and slag-making solvents should be added to control the blast furnace coke ratio to 450-550 kg / ton of pig iron. It can be found from the blast furnace production process that energy has high carbonity, and the input of highly carbonized coal coke is close to 90%. At the same time, due to the addition of coke in the blast furnace ironmaking process, a large amount of carbon-containing (such as CO2, CO, etc.) flue gas will be formed.
[0003] Green metallurgy refers to a metallurgical method that achieves resource conservation, environmental friendliness and sustainable economic benefits in the metal smelting process by adopting environmentally friendly, efficient and energy-saving technologies and processes. Green metallurgy emphasizes the recycling of resources, reducing waste emissions, reducing energy consumption and reducing environmental pollution. It also pays attention to technological innovation and industrial upgrading, and plays a very important role in promoting the sustainable development of metallurgy.
[0004] Green electricity refers to electricity produced in a way that its carbon dioxide emissions are zero or close to zero, because it has a lower impact on the environment than electricity produced by other methods (such as thermal power generation). The main sources of green electricity are solar energy, wind power, biomass energy, geothermal energy, etc. China mainly relies on green electricity generated by solar energy and wind power. At present, the price of green electricity is cheaper than conventional electricity, and there is no effective way to store green electricity.
[0005] Hydrogen energy is mainly divided into gray hydrogen, blue hydrogen, and green hydrogen according to the production method and carbon emissions. Gray hydrogen is hydrogen produced by burning fossil fuels (such as oil, natural gas, coal, etc.), and there will be emissions of carbon dioxide during the production process. Blue hydrogen is made by steam methane reforming or autothermal steam reforming of natural gas. Only green hydrogen is hydrogen produced by using renewable energy (such as solar energy, wind energy, nuclear energy, etc.), and basically no greenhouse gases are produced during the production process. How to effectively utilize the produced green hydrogen is a technical problem.
[0006] Currently, the application of hydrogen in iron-making mainly includes hydrogen-rich blast furnace smelting method, hydrogen-based vertical furnace direct reduction method, and hydrogen-based direct reduction method based on fluidized bed.
[0007] The hydrogen-rich blast furnace smelting method is to inject coke oven gas, natural gas or hydrogen to replace the heat source and reducing agent of coal powder and part of coke, thereby reducing the carbon emission of the blast furnace. However, due to the irreplaceable role of coke skeleton in the blast furnace, the replacement ratio of hydrogen-rich blast furnace to coke is only about 0.3, which is still insufficient in terms of economy and reducing process energy consumption.
[0008] The hydrogen-based shaft furnace direct reduction method uses reducing gas containing 50% to 70% hydrogen to produce sponge iron, but this technology requires the use of high-grade iron ore resources as raw materials, and the world is facing the problem of a shortage of high-quality and high-grade iron ore resources. At the same time, due to heat supply, it is difficult to solve the problem of full hydrogen ironmaking.
[0009] The hydrogen-based direct reduction method based on fluidized bed uses iron ore powder as raw material, and no longer needs to be agglomerated. However, this technology has the disadvantages of requiring the use of high-grade iron ore, high metallization rate of the product, which is prone to cause adhesion and loss of flow, and higher energy consumption per unit product than hydrogen-based vertical furnace.
[0010] The gas-based direct reduction process in the prior art uses reducing gas as a reducing agent. The heat in the reduction furnace (gas-based vertical furnace) mainly comes from the physical heat of the reducing gas. The reduction process is from iron ore directly to metallic iron, that is, heat must be provided by the reducing agent during the reduction process, and carbon-containing materials must be added during the iron reduction process. The reducing agent must provide heat by combustion, so it relies on an oxygen atmosphere. There is no pure hydrogen iron ore ironmaking method in the prior art. There is no good way to solve the endothermic effect of the full hydrogen reduction of pure green hydrogen when pure hydrogen is used for ironmaking. Moreover, when carbon-containing materials are added during the iron reduction process, carbon-containing gas will be produced in an oxygen atmosphere. There is no low-cost recycling method for the tail gas mainly composed of carbon-containing gas and water vapor, which will further affect carbon emissions to the environment. Summary of the invention
[0011] In view of the problems and shortcomings of the above-mentioned prior art, the present invention provides a long-process iron and steel metallurgical production method for consuming iron-containing materials by electric hydrogen circulation to produce iron and steel products. In order to realize the smooth conversion of industrial blast furnace ironmaking into a full hydrogen ironmaking method, the smelting furnace and the reduction furnace of the present invention are all improved existing industrial equipment. The smelting furnace and the reduction furnace are used to reduce and smelt the iron ore by a full hydrogen method without adding any coke, completely replacing the technical shortcomings of industrial blast furnace ironmaking that requires coke to generate carbon emissions and there is no way to effectively treat the tail gas.
[0012] The present invention includes a reduction furnace, a smelting furnace and a flue gas circulation system. The reducing atmosphere and the reducing gas introduced in the reduction furnace and the smelting furnace are all green hydrogen. Green electricity provides electricity and heat for the reduction furnace and the smelting furnace. The iron ore is treated in the reduction furnace and the smelting furnace to obtain green iron. The tail gas generated in the reduction furnace and the smelting furnace is treated by the flue gas circulation system to obtain industrial pure hydrogen, and then returned to the reduction furnace for smelting reduction. The present invention uses green hydrogen reducing gas in the entire reduction and smelting process, and the electricity used is green electricity. In the metallurgical production process, the carbon required for the traditional process is replaced by the combination of green electricity and green hydrogen, realizing the four principles of no addition of carbon, no circulation of carbon, no emission of carbon, and no involvement of carbon. The present invention is implemented by the following technical solutions.
[0013] like Figure 1 As shown, the long process of iron and steel metallurgical production technology for producing iron and steel products from iron-containing materials covers eight links: mineral processing, reduction, smelting, pretreatment, steelmaking, refining, casting and rolling.
[0014] A long-process iron and steel metallurgical production method for consuming iron-containing materials to produce iron and steel products by utilizing electric hydrogen circulation, comprising a reduction furnace, a smelting furnace, a flue gas circulation system and a steelmaking furnace.
[0015] (1) The reduction furnace is electrically heated by green electricity, and a mixture of green hydrogen, smelting furnace tail gas and industrial hydrogen is continuously introduced into the reduction furnace to reduce the iron ore in the reduction furnace into reduced iron;
[0016] (2) adding the reduced iron in step (1) into a smelting furnace, electrically heating the smelting furnace using green electricity, continuously introducing green hydrogen into the smelting furnace, melting and slagging the reduced iron, and smelting into green iron;
[0017] (3) The tail gas in the reduction furnace of step (1) and the smelting furnace of step (2) is collected. A portion of the tail gas in the smelting furnace is introduced into the reduction furnace to participate in the heating and reduction of the iron ore. A portion of the tail gas is collected and enters the flue gas circulation system for cooling to obtain cooling water and industrial hydrogen with high chemical heat. A portion of the tail gas is used to preheat the green hydrogen. The industrial hydrogen is returned to the smelting furnace or the reduction furnace to achieve hydrogen recycling.
[0018] The reduction furnace in step (1) is an improved rotary kiln, vertical furnace, mixed iron furnace, rotary hearth furnace or fluidized bed; the rotary kiln, vertical furnace, mixed iron furnace, rotary hearth furnace or fluidized bed is improved by adding electromagnetic induction, electric arc, resistor or electrode, providing green electricity to the electromagnetic induction, electric arc, resistor or electrode for heating, thereby increasing the physical heat in the furnace, and the hydrogen reducing gas entering the reduction furnace provides chemical energy for the reduction of the iron ore.
[0019] An example of an improved rotary kiln is Figure 5As shown, it comprises a segmented movable electromagnetic coil 9, a rotary kiln shell 10, a hydrogen blowing inlet 11 and a gas outlet 12. The rotary kiln shell 10 is respectively provided with a segmented movable electromagnetic coil 9, a hydrogen blowing inlet 11 and a gas outlet 12.
[0020] An example of an improved vertical furnace is Figure 6 As shown, it includes a material inlet 13, a hydrogen blowing port A14, a vertical furnace electromagnetic coil 15, a vertical furnace shell 16, a base 17 and a hydrogen blowing port B18. The vertical furnace shell 16 is respectively provided with a material inlet 13, a hydrogen blowing port A14, a vertical furnace electromagnetic coil 15 base 17 and a hydrogen blowing port B18.
[0021] An example of an improved mixing furnace is Figure 7 As shown, it includes a resistance wire A19, molten iron 20, a hydrogen blowing port 21 and an iron outlet 22. The resistance wire A19, the hydrogen blowing port 21 and the iron outlet 22 are arranged outside the mixing furnace.
[0022] An example of an improved rotary hearth furnace is Figure 8 As shown, the rotary hearth furnace includes a material inlet 23, a running direction 24, a rotary hearth furnace shell 25, a rotary hearth furnace electromagnetic coil 26, a material outlet 27, a lower hydrogen blowing port 28, an upper hydrogen blowing port 29 and a resistance wire B30. The rotary hearth furnace is provided with a material inlet 23, a rotary hearth furnace shell 25, a rotary hearth furnace electromagnetic coil 26, a material outlet 27, a lower hydrogen blowing port 28, an upper hydrogen blowing port 29 and a resistance wire B30.
[0023] In step (2), the smelting furnace is an electromagnetic induction furnace or an electric arc furnace. The electromagnetic induction furnace or the electric arc furnace uses green electricity to heat up, increase the physical heat in the furnace, and provide physical conditions for the melting of direct reduced iron. The hydrogen reducing gas entering the smelting furnace provides chemical energy for the further reduction of direct reduced iron and oxygen-containing molten iron. The flux added to the furnace provides slag-forming conditions in the furnace to generate slag and molten iron. Figure 4 As shown, the electromagnetic induction furnace includes an upper hydrogen blowing port 1, an electrode 2, an oblique hydrogen blowing port 3, a side hydrogen blowing port 4, molten iron 5, a furnace shell 6, a bottom hydrogen blowing port 7 and an electromagnetic coil 8. The electromagnetic coil 8 is provided outside the furnace shell 6 of the electromagnetic induction furnace, and the upper hydrogen blowing port 1, the electrode 2, the oblique hydrogen blowing port 3 and the side hydrogen blowing port 4 are inserted from the furnace shell 6.
[0024] In the step (1) and the step (2), the green hydrogen is introduced through a hydrogen blowing port, more than one hydrogen blowing port is provided, and the orientation of the hydrogen blowing port is arranged to enter the furnace in a top blowing, bottom blowing, oblique blowing, or side blowing manner.
[0025] The green hydrogen reduction in the reduction furnace in step (1) includes preheating, drying, pre-reduction and deep reduction processes.
[0026] The step (1) of preheating, drying and pre-reduction is as follows: the iron ore is placed in a reduction furnace and preheated to a temperature of 25-1245° C. During this process, a mixture of green hydrogen at a temperature of 435-1600° C., reduction furnace tail gas and industrial hydrogen is introduced, and preheating is performed for 15-120 minutes to fill the reduction furnace with a hydrogen atmosphere.
[0027] The deep reduction in step (1) is as follows: the ore is further heated to a temperature of 780-1150°C, green hydrogen at a temperature of 20-1700°C is introduced, and reduction smelting is performed for 0.2-4h, and reduced iron liquid and slag are discharged from the iron mouth, and high-temperature hydrogen is discharged from the furnace top for reuse.
[0028] The specific process of full green hydrogen smelting in the smelting furnace in step (2) is as follows:
[0029] 2.1. Add reduced iron and calcium-magnesium flux into the smelting furnace, and continuously spray green hydrogen at a temperature of 20-1700°C into the smelting furnace to fill the smelting furnace with a green hydrogen atmosphere;
[0030] 2.2. The ore is heated to a temperature of 1435-1650°C, and green hydrogen at a temperature of 20-1700°C is sprayed into the melt by top blowing and bottom blowing. The top blowing pipe is inserted into the melt to a depth of 8-30mm. The smelting is performed for 0.2-4h, and green iron is obtained after slag removal.
[0031] In the above step 2.1, the smelting furnace is filled with green hydrogen atmosphere by spraying green hydrogen from top blowing, oblique blowing, side blowing or a combination of methods. In step 2.2, the top blowing pipe is inserted into the molten liquid to a depth of 8-30 mm, and the bottom blowing method is used to directly spray green hydrogen into the molten liquid, thereby solving the problem of the change of gas flow when spraying hydrogen, making the smelting process more effective and solving the problem of needing a large amount of hydrogen spraying.
[0032] In the step (3), the flue gas circulation system realizes heat exchange heating of the newly produced green hydrogen. After the industrial tail gas is cooled, cooling water and industrial hydrogen with high chemical heat are generated for recycling and reuse, including dust removal and cooling to obtain cooling water and industrial hydrogen. The industrial hydrogen is returned to the reduction furnace after secondary dust removal.
[0033] The above green molten iron contains hydrogen and can be used to cast green iron or to make steel.
[0034] The green iron is pretreated with molten iron to remove silicon, phosphorus and sulfur, and then enters the steelmaking furnace to obtain molten steel. The heat for steelmaking comes from hydrogen-oxygen reaction, silicon-oxygen reaction and electric heating. The electric heating includes electromagnetic induction, electrode discharge and resistance heating. The hydrogen and silicon elements in the molten iron entering the furnace react with the blown oxygen to release heat, achieving four removals and two removals and two reductions. The molten steel is formed through a casting process, and the required steel is produced through hot rolling, cold rolling and other rolling methods.
[0035] When the entire metallurgical system of the present invention is in normal production operation, carbon-free equipment, materials or electrodes should be used. This is because carbon plays a negative role in the entire metallurgical system and will accumulate in a cycle. For example, in a gas circulation system, water is condensed from the tail gas by using heat exchange and tail gas cooling methods to increase the proportion of tail gas hydrogen. It should be noted that in the long-process iron and steel metallurgical system in which the electric hydrogen cycle consumes iron-containing materials to produce iron and steel products, carbon often appears in a harmful form, and the entire system production shows a carbon-averse form. This is because the tail gas cooling cannot remove carbon dioxide and carbon monoxide, resulting in a gradual increase in the proportion of carbon dioxide and carbon monoxide in the metallurgical system, changing the gas phase composition of the entire metallurgical system, resulting in changes in production efficiency. To remove this part of carbon monoxide or carbon dioxide, an additional gas purification or modification device is required. However, when the entire metallurgical system is in the maintenance stage or debugging mode, in order to adjust the use status of the system or part of the equipment, carbon-containing raw materials, coke coal powder, graphite electrodes, carbon-containing gases, etc. can be used.
[0036] The beneficial effects of the present invention are:
[0037] (1) The present invention adopts green hydrogen reduction gas in the entire reduction and smelting process, and uses green electricity. In the metallurgical production process, the carbon required by the traditional process is replaced by the combination of green electricity and green hydrogen, realizing the four principles of no carbon addition, no carbon circulation, no carbon emission, and no carbon involvement, thus realizing the entire process of green metallurgy.
[0038] (2) The reduction furnace of the present invention is obtained by improving existing ironmaking equipment such as rotary kilns, vertical furnaces, iron-mixing furnaces, rotary hearth furnaces, and fluidized beds. The green hydrogen reduction technology in the reduction furnace and the smelting furnace can directly replace the blast furnace ironmaking technology, thereby reducing the production cost during the improved process and contributing to the industrialization of the full green hydrogen reduction technology.
[0039] (3) The flue gas circulation system of the present invention can cool down the water in the tail gas generated in the reduction furnace and the smelting furnace only by heat exchange (or cooling), thereby realizing the efficient separation of water and hydrogen, and the formed industrial hydrogen is returned to the reduction furnace; compared with the existing blast furnace carbon smelting flue gas treatment, the method of the present invention does not require the effective separation of CO2, CO and hydrogen, that is, does not require any separation method of carbon-containing gas and hydrogen, and effectively solves the problems of high production cost, insufficient chemical heat and physical heat utilization of tail gas, and poor treatment effect of the existing blast furnace carbon smelting flue gas treatment.
[0040] (4) The green hydrogen of the present invention is heated to a specified temperature by heat exchange with part of the tail gas generated from the reduction furnace and the smelting furnace, and then introduced into the reduction furnace and the smelting furnace for reduction. The green hydrogen preheating process does not require other electric energy to provide heat, thereby reducing production and operation costs.
[0041] (5) The traditional blast furnace ironmaking process or other hydrogen reduction process requires a partial oxygen atmosphere environment so that heat can be provided by the combustion of the reducing agent during the reduction process; however, the present method generates heat by providing green electricity to the reduction furnace and the smelting furnace, and does not require any oxygen atmosphere environment, nor does it require any heat to be provided by the reducing agent.
[0042] (6) The present invention can process iron ore of any iron grade. In the process of green hydrogen reduction of iron ore, in order to improve the reduction rate of green hydrogen reduction of iron ore, the reduction furnace first preheats the iron ore by green electricity in the reduction furnace. During the preheating process, green hydrogen at 435-1600°C is continuously provided to completely fill the reduction furnace with green hydrogen. The green electricity is then continued to heat to 780°C-1150°C, and green hydrogen at 20-1700°C is introduced. Through the specific green hydrogen reduction method of the present invention, the reduction degree of iron exceeds 85%, which lays a good foundation for the subsequent smelting with a good reduction effect.
[0043] (7) The high metallization sponge iron obtained in the reduction furnace of the present invention enters the smelting furnace, which is filled with green hydrogen atmosphere. After the temperature rises to 1435-1650°C and the furnace enters the molten state, the top blowing pipe is inserted into the molten liquid to a depth of 8-30 mm, and green hydrogen is continuously blown, which solves the problem that the hydrogen molecules are small and the air flow in the vortex zone of the tuyere will change when the hydrogen is blown, until the smelting is completed, and finally green iron is obtained. The smelting effect is good and the production cost is reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is the overall process flow chart of the present invention;
[0045] Figure 2 It is a schematic diagram of the process of the present invention;
[0046] Figure 3 It is a schematic diagram of the structure of the flue gas circulation system of the present invention;
[0047] Figure 4 It is a schematic diagram of an electromagnetic induction furnace of the present invention that can optionally add electrodes for heating;
[0048] Figure 5 It is a schematic structural diagram of the rotary kiln with segmented electric heating function used as a reduction furnace of the present invention;
[0049] Figure 6 It is a schematic structural diagram of the present invention when the segmented electric heating vertical furnace is used as a reduction furnace;
[0050] Figure 7 This is a schematic structural diagram of the iron-mixing furnace of the present invention when used as a reduction furnace;
[0051] Figure 8 It is a schematic structural diagram of the rotary hearth furnace with segmented electric heating used as a reduction furnace according to the present invention.
[0052] In the figure: 1-upper side hydrogen blowing port, 2-electrode, 3-oblique hydrogen blowing port, 4-side hydrogen blowing port, 5-molten iron, 6-furnace shell, 7-bottom hydrogen blowing port, 8-electromagnetic coil, 9-segmented movable electromagnetic coil, 10-rotary kiln shell, 11-hydrogen blowing inlet, 12-gas outlet, 13-material inlet, 14-hydrogen blowing port A, 15-vertical furnace electromagnetic coil, 16-vertical furnace shell, 17-base, 18-hydrogen blowing port B, 19-resistance wire A, 20-molten iron, 21-hydrogen blowing port, 22-iron outlet, 23-feeding port, 24-running direction, 25-rotary hearth furnace shell, 26-rotary hearth furnace electromagnetic coil, 27-feeding port, 28-lower hydrogen blowing port, 29-upper hydrogen blowing port, 30-resistance wire B. DETAILED DESCRIPTION
[0053] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation methods.
[0054] Example 1
[0055] like Figure 1 and 2 As shown, the long-process iron and steel metallurgical production method for consuming iron-containing materials by electric hydrogen circulation to produce iron and steel products comprises a reduction furnace, a smelting furnace, a flue gas circulation system and a steelmaking furnace.
[0056] (1) The reduction furnace is electrically heated by green electricity, and a mixture of green hydrogen, smelting furnace tail gas and industrial hydrogen is continuously introduced into the reduction furnace to reduce the iron ore in the reduction furnace into reduced iron; the full green hydrogen reduction of the reduction furnace includes preheating, drying, pre-reduction and deep reduction processes, and the specific steps are as follows:
[0057] 1.1 Iron ore (including the following mass percentage components: TFe 68%, SiO2 3.5%, S 0.03%) is placed in a reduction furnace and preheated to 700°C. During this process, a mixture of green hydrogen at a temperature of 435°C, smelting furnace tail gas and industrial hydrogen is introduced. The mixed gas is injected by top blowing, oblique blowing and side blowing at the same time. The flow rate of the mixed gas is 40Nm 3 / min, preheat for 15min to make the reduction furnace completely filled with hydrogen atmosphere;
[0058] 1.2 The ore continues to be heated to 1150°C, and green hydrogen at a temperature of 750°C is introduced by top blowing, oblique blowing and side blowing at a flow rate of 40Nm 3 / min, reduction smelting for 2h to obtain reduced iron;
[0059] This reduction furnace uses an improved rotary kiln, such as Figure 5As shown, it includes a segmented movable electromagnetic coil 9, a rotary kiln shell 10, a hydrogen blowing inlet 11 and a gas outlet 12. The rotary kiln shell 10 is respectively provided with a segmented movable electromagnetic coil 9, a hydrogen blowing inlet 11 and a gas outlet 12. The movable electromagnetic coil 9 is mainly added to the rotary kiln, and green electricity is passed through the movable electromagnetic coil 9, so that the rotary kiln heats the iron ore in the rotary kiln to the preheating temperature and the reduction temperature respectively by heating with green electricity.
[0060] Through this treatment step, reduced iron with a reduction degree of 85% is obtained;
[0061] (2) Add the reduced iron in step (1) into a smelting furnace, electrically heat the smelting furnace using green electricity, and continuously introduce green hydrogen into the smelting furnace to smelt the reduced iron into green iron; the specific process of full green hydrogen smelting in the smelting furnace is as follows:
[0062] 2.1. Add reduced iron and calcium-magnesium flux (0.15t per ton of green iron) into the smelting furnace, and continuously spray green hydrogen at a temperature of 500°C into the smelting furnace by top blowing, oblique blowing and side blowing at the same time. The green hydrogen flow rate is 50Nm 3 / min, so that the smelting furnace is filled with green hydrogen atmosphere;
[0063] 2.2. The ore is heated to 1650°C and the green hydrogen flow rate is 50Nm 3 / min, spraying green hydrogen at a temperature of 1500°C into the melt by top blowing and bottom blowing, controlling the top and bottom blowing pipes to be inserted into the melt to a depth of 30mm, smelting for 4h, and obtaining green iron (including the following percentage components: iron 96%, Si 0.65%, P <0.7%, S <0.6%) after slagging;
[0064] This smelting furnace adopts electromagnetic induction furnace. Figure 4 As shown, it includes an upper hydrogen blowing port 1, an electrode 2, an oblique hydrogen blowing port 3, a side hydrogen blowing port 4, molten iron 5, a furnace shell 6, a bottom hydrogen blowing port 7 and an electromagnetic coil 8. The electromagnetic coil 8 is arranged outside the furnace shell 6 of the electromagnetic induction furnace, and the upper hydrogen blowing port 1, the electrode 2, the oblique hydrogen blowing port 3 and the side hydrogen blowing port are inserted from the furnace shell 6. The present invention heats and melts the reduced iron by adding the electromagnetic coil 8 and the electrode 2 in the electromagnetic induction furnace, and finally obtains green iron;
[0065] (3) collecting tail gas from the reduction furnace in step (1) and the smelting furnace in step (2); a portion of the tail gas from the smelting furnace is introduced into the reduction furnace to participate in the heating and reduction of the iron ore; a portion of the tail gas is collected and enters the flue gas circulation system for cooling to obtain cooling water and industrial hydrogen with high chemical heat; a portion of the tail gas is used to preheat green hydrogen, and the industrial hydrogen is returned to the smelting furnace or the reduction furnace; Figure 3As shown, the flue gas circulation system realizes heat exchange to heat the newly produced green hydrogen. After the industrial exhaust gas is cooled, cooling water and industrial hydrogen with high chemical heat are generated for recycling and reuse, including dust removal and cooling to obtain cooling water and industrial hydrogen. The industrial hydrogen is returned to the reduction furnace after secondary dust removal.
[0066] In this embodiment, the reduced iron with a reduction degree of 85% is obtained by the reduction furnace treatment in step (1). After the treatment in the smelting furnace in step (2) of the present invention, compared with the conventional blast furnace adding 0.3 tons of calcium-magnesium flux per ton of green iron, the present invention can save half of the calcium-magnesium flux. At the same time, the top and bottom blowing pipes are inserted into the molten liquid to a depth of 30 mm, which solves the problem that the hydrogen molecules are small and the air flow in the vortex zone of the tuyere will change when the hydrogen is sprayed, so that the injection amount of green hydrogen is significantly reduced, thereby reducing the production cost.
[0067] Comparative Example 1
[0068] Except that the preheating, drying and pre-reduction processes are not performed in step (1), the other steps are the same as step (1) in Example 1. The processing method includes a reduction furnace, a smelting furnace and a flue gas circulation system.
[0069] The reduction furnace is electrically heated by green electricity, and a mixture of green hydrogen, smelting furnace tail gas and industrial hydrogen is continuously introduced into the reduction furnace to reduce the iron ore in the reduction furnace into reduced iron; the full green hydrogen reduction of the reduction furnace includes a deep reduction process, and the specific steps are as follows:
[0070] The iron ore (including the following mass percentage components: TFe 68%, SiO 2 3.5%, S 0.03%) was placed in a reduction furnace. During this process, the ore was directly heated to 1150°C, and green hydrogen at a temperature of 750°C was introduced by top blowing, oblique blowing and side blowing. The green hydrogen flow rate was 40Nm 3 / min, reduction smelting for 2.25h to obtain reduced iron;
[0071] This reduction furnace uses an improved rotary kiln, such as Figure 5 As shown, it includes a segmented movable electromagnetic coil 9, a rotary kiln shell 10, a hydrogen blowing inlet 11 and a gas outlet 12. The rotary kiln shell 10 is respectively provided with a segmented movable electromagnetic coil 9, a hydrogen blowing inlet 11 and a gas outlet 12. The movable electromagnetic coil 9 is mainly added to the rotary kiln, and green electricity is passed through the movable electromagnetic coil 9, so that the rotary kiln heats the iron ore in the rotary kiln to the preheating temperature and the reduction temperature respectively by heating with green electricity.
[0072] Through this treatment step, only reduced iron with a degree of iron reduction of 75% is obtained.
[0073] It can be seen from Example 1 and Comparative Example 1 that in Example 1, the preheating, drying and pre-reduction processes were carried out, and the reduction degree of iron reached 85%, while in Comparative Example 1 without the pre-reduction process, other parameters and control conditions were compared with those in Example 1, and the reduction degree of iron was only 75%.
[0074] Comparative Example 2
[0075] Step 1 in this comparative example 2 is exactly the same as that in Example 1, except that the top and bottom blowing pipes are not inserted into the molten liquid to a depth of 30 mm during the treatment process of step 2, that is, top blowing, side blowing and oblique blowing are used in step 2.2, and the green hydrogen flow rate is 100 Nm 3 / min, to obtain green iron (including the following percentage components: iron 90%, Si 0.9%, P < 0.7%, S < 0.6%).
[0076] It can be seen from Example 1 and Comparative Example 2 that in Comparative Example 2, there is no step of inserting the top and bottom blowing pipes into the molten liquid to a depth of 30 mm, and the green hydrogen flow rate needs to be introduced more than one times that of Example 1, and the iron content in the obtained green iron is reduced. This shows that injecting hydrogen into the molten liquid can reduce the problem of changes in the air flow in the vortex zone of the tuyere when injecting hydrogen, reduce the injection amount of hydrogen, and obtain a better reduction effect.
[0077] Example 2
[0078] like Figure 1 and 2 As shown, the long-process iron and steel metallurgical production method for consuming iron-containing materials by electric hydrogen circulation to produce iron and steel products comprises a reduction furnace, a smelting furnace, a flue gas circulation system and a steelmaking furnace.
[0079] (1) The reduction furnace is electrically heated by green electricity, and a mixture of green hydrogen, smelting furnace tail gas and industrial hydrogen is continuously introduced into the reduction furnace to reduce the iron ore in the reduction furnace into reduced iron; the full green hydrogen reduction of the reduction furnace includes preheating, drying, pre-reduction and deep reduction processes, and the specific steps are as follows:
[0080] 1.1 Iron ore (including the following mass percentage components: TFe 65%, SiO2 3.2%, S 0.04%) is placed in a reduction furnace and preheated to 800°C. During this process, a mixture of green hydrogen at 800°C, smelting furnace tail gas and industrial hydrogen is introduced, and the mixed gas is injected by top blowing, oblique blowing and side blowing at the same time. The flow rate of the mixed gas is 10Nm 3 / min, preheat for 120min to make the reduction furnace completely filled with hydrogen atmosphere;
[0081] 1.2 The ore is heated to 1000℃, and green hydrogen at 900℃ is introduced by top blowing, oblique blowing and side blowing at a flow rate of 10Nm3 / min, reduction smelting for 1h to obtain reduced iron;
[0082] This reduction furnace adopts an improved vertical furnace, such as Figure 6 As shown, it includes a material inlet 13, a hydrogen blowing port A14, a vertical furnace electromagnetic coil 15, a vertical furnace shell 16, a base 17 and a hydrogen blowing port B18. The vertical furnace shell 16 is provided with a material inlet 13, a hydrogen blowing port A14, a base 17 of the vertical furnace electromagnetic coil 15 and a hydrogen blowing port B18. The vertical furnace electromagnetic coil 15 is mainly added to the vertical furnace, and green electricity is passed through the vertical furnace electromagnetic coil 15, so that the vertical furnace heats the iron ore in the vertical furnace to the preheating temperature and the reduction temperature respectively by heating with green electricity;
[0083] Through this treatment step, reduced iron with a reduction degree of 90% is obtained;
[0084] (2) Add the reduced iron in step (1) into a smelting furnace, electrically heat the smelting furnace using green electricity, and continuously introduce green hydrogen into the smelting furnace to smelt the reduced iron into green iron; the specific process of full green hydrogen smelting in the smelting furnace is as follows:
[0085] 2.1. Add reduced iron and calcium-magnesium flux (0.15t per ton of green iron) into the smelting furnace, and continuously spray green hydrogen at a temperature of 1700°C into the smelting furnace by top blowing, oblique blowing and side blowing at the same time. The green hydrogen flow rate is 60Nm 3 / min, so that the smelting furnace is filled with green hydrogen atmosphere;
[0086] 2.2. The ore is heated to 1435°C and the green hydrogen flow rate is 60Nm 3 / min, spraying green hydrogen at a temperature of 1700°C into the melt by top blowing and bottom blowing, controlling the top and bottom blowing pipes to be inserted into the melt to a depth of 8mm, smelting for 0.2h, and obtaining green iron (including the following percentage components: iron 96%, Si 0.65%, P <0.7%, S <0.6%) after slagging;
[0087] This smelting furnace adopts electromagnetic induction furnace. Figure 4 As shown, it includes an upper hydrogen blowing port 1, an electrode 2, an oblique hydrogen blowing port 3, a side hydrogen blowing port 4, molten iron 5, a furnace shell 6, a bottom hydrogen blowing port 7 and an electromagnetic coil 8. The electromagnetic coil 8 is arranged outside the furnace shell 6 of the electromagnetic induction furnace, and the upper hydrogen blowing port 1, the electrode 2, the oblique hydrogen blowing port 3 and the side hydrogen blowing port are inserted from the furnace shell 6. The present invention heats and melts the reduced iron by adding the electromagnetic coil 8 and the electrode 2 in the electromagnetic induction furnace, and finally obtains green iron;
[0088] (3) collecting tail gas from the reduction furnace in step (1) and the smelting furnace in step (2); a portion of the tail gas from the smelting furnace is introduced into the reduction furnace to participate in the heating and reduction of the iron ore; a portion of the tail gas is collected and enters the flue gas circulation system for cooling to obtain cooling water and industrial hydrogen with high chemical heat; a portion of the tail gas is used to preheat green hydrogen, and the industrial hydrogen is returned to the smelting furnace or the reduction furnace; Figure 3 As shown, the flue gas circulation system realizes heat exchange to heat the newly produced green hydrogen. After the industrial exhaust gas is cooled, cooling water and industrial hydrogen with high chemical heat are generated for recycling and reuse, including dust removal and cooling to obtain cooling water and industrial hydrogen. The industrial hydrogen is returned to the reduction furnace after secondary dust removal.
[0089] In this embodiment, the reduction furnace treatment in step (1) obtains reduced iron with a reduction degree of 85%. After the treatment in the smelting furnace in step (2) of the present invention, compared with the conventional blast furnace adding 0.3 tons of calcium-magnesium flux per ton of green iron, the present invention can save half of the calcium-magnesium flux. At the same time, the top and bottom blowing pipes are inserted into the molten liquid to a depth of 8 mm, which solves the problem that the hydrogen molecules are small and the air flow in the vortex zone of the tuyere will change when spraying hydrogen, so that the injection amount of green hydrogen is significantly reduced, thereby reducing the production cost.
[0090] Example 3
[0091] like Figure 1 and 2 As shown, the long-process iron and steel metallurgical production method for consuming iron-containing materials by electric hydrogen circulation to produce iron and steel products comprises a reduction furnace, a smelting furnace, a flue gas circulation system and a steelmaking furnace.
[0092] (1) The reduction furnace is electrically heated by green electricity, and a mixture of green hydrogen, smelting furnace tail gas and industrial hydrogen is continuously introduced into the reduction furnace to reduce the iron ore in the reduction furnace into reduced iron; the green hydrogen reduction in the reduction furnace includes preheating, drying, pre-reduction and deep reduction processes, and the specific steps are as follows:
[0093] 1.1 Iron ore (including the following mass percentage components: TFe 62%, SiO2 3.0%, S 0.04%) is placed in a reduction furnace and preheated to 900°C. During this process, a mixture of green hydrogen at a temperature of 435°C, smelting furnace tail gas and industrial hydrogen is introduced. The mixed gas is injected by top blowing, oblique blowing and side blowing at the same time. The flow rate of the mixed gas is 60Nm 3 / min, preheat for 100min to make the reduction furnace completely filled with hydrogen atmosphere;
[0094] 1.2 The ore is heated to 1150℃, and green hydrogen at 1700℃ is introduced by top blowing, oblique blowing and side blowing at a flow rate of 60Nm 3 / min, reduction smelting for 0.5h to obtain reduced iron;
[0095] The reduction furnace used in this invention is a mixed iron furnace, for example, Figure 7 As shown, the iron mixing furnace includes a resistance wire A19, molten iron 20, a hydrogen blowing port 21 and an iron outlet 22. The resistance wire A19, the hydrogen blowing port 21 and the iron outlet 22 are arranged outside the iron mixing furnace. The resistance wire A19 is mainly added to the iron mixing furnace, and green electricity is passed through the resistance wire A19, so that the iron mixing furnace heats the iron ore in the iron mixing furnace to the preheating temperature and the reduction temperature respectively by the heating method of the green electricity;
[0096] Through this treatment step, reduced iron with a reduction degree of 88% is obtained;
[0097] (2) Add the reduced iron in step (1) into a smelting furnace, electrically heat the smelting furnace using green electricity, and continuously introduce green hydrogen into the smelting furnace to smelt the reduced iron into green iron; the specific process of full green hydrogen smelting in the smelting furnace is as follows:
[0098] 2.1. Add reduced iron and calcium-magnesium flux (0.15t per ton of green iron) into the smelting furnace, and continuously spray green hydrogen at a temperature of 20°C into the smelting furnace by top blowing, oblique blowing and side blowing at the same time. The green hydrogen flow rate is 60Nm 3 / min, so that the smelting furnace is filled with green hydrogen atmosphere;
[0099] 2.2. The ore is heated to 1650°C and the green hydrogen flow rate is 60Nm 3 / min, spraying green hydrogen at a temperature of 1000°C into the melt by top blowing and bottom blowing, controlling the top and bottom blowing pipes to be inserted into the melt to a depth of 25mm, smelting for 2h, and obtaining green iron (including the following percentage components: iron 96%, Si 0.65%, P <0.7%, S <0.6%) after slagging;
[0100] This smelting furnace adopts electromagnetic induction furnace. Figure 4 As shown, it includes an upper hydrogen blowing port 1, an electrode 2, an oblique hydrogen blowing port 3, a side hydrogen blowing port 4, molten iron 5, a furnace shell 6, a bottom hydrogen blowing port 7 and an electromagnetic coil 8. The electromagnetic coil 8 is arranged outside the furnace shell 6 of the electromagnetic induction furnace, and the upper hydrogen blowing port 1, the electrode 2, the oblique hydrogen blowing port 3 and the side hydrogen blowing port are inserted from the furnace shell 6. The present invention heats and melts the reduced iron by adding the electromagnetic coil 8 and the electrode 2 in the electromagnetic induction furnace, and finally obtains green iron;
[0101] (3) collecting tail gas from the reduction furnace in step (1) and the smelting furnace in step (2); a portion of the tail gas from the smelting furnace is introduced into the reduction furnace to participate in the heating and reduction of the iron ore; a portion of the tail gas is collected and enters the flue gas circulation system for cooling to obtain cooling water and industrial hydrogen with high chemical heat; a portion of the tail gas is used to preheat green hydrogen, and the industrial hydrogen is returned to the smelting furnace or the reduction furnace; Figure 3As shown, the flue gas circulation system realizes heat exchange to heat the newly produced green hydrogen. After the industrial exhaust gas is cooled, cooling water and industrial hydrogen with high chemical heat are generated for recycling and reuse, including dust removal and cooling to obtain cooling water and industrial hydrogen. The industrial hydrogen is returned to the reduction furnace after secondary dust removal.
[0102] In this embodiment, the reduced iron with a reduction degree of 88% is obtained by the reduction furnace treatment in step (1). After the treatment in the smelting furnace in step (2) of the present invention, compared with the conventional blast furnace adding 0.3 tons of calcium-magnesium flux per ton of green iron, the present invention can save half of the calcium-magnesium flux. At the same time, the top and bottom blowing pipes are inserted into the molten liquid to a depth of 8 mm, which solves the problem that the hydrogen molecules are small and the air flow in the vortex zone of the tuyere will change when spraying hydrogen, so that the injection amount of green hydrogen is significantly reduced, thereby reducing the production cost.
[0103] The specific implementation modes of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A long-process iron and steel metallurgical production method for producing iron and steel products by consuming iron-containing materials through an electric hydrogen cycle, characterized in that: Including reduction furnace, smelting furnace, flue gas circulation system and steelmaking furnace, (1) The reduction furnace is electrically heated by green electricity, and a mixture of green hydrogen, smelting furnace tail gas and industrial hydrogen is continuously introduced into the reduction furnace to reduce the iron ore in the reduction furnace into reduced iron; (2) adding the reduced iron in step (1) into a smelting furnace, electrically heating the smelting furnace using green electricity, continuously introducing green hydrogen into the smelting furnace, melting and slagging the reduced iron, and smelting into green iron; (3) The tail gas in the reduction furnace of step (1) and the smelting furnace of step (2) is collected. A portion of the tail gas in the smelting furnace is introduced into the reduction furnace to participate in the heating and reduction of the iron ore. A portion of the tail gas is collected and enters the flue gas circulation system for cooling to obtain cooling water and industrial hydrogen with high chemical heat. A portion of the tail gas is used to preheat the green hydrogen. The industrial hydrogen is returned to the smelting furnace or the reduction furnace to achieve hydrogen recycling.
2. The long-process iron and steel metallurgical production method for producing iron and steel products by consuming iron-containing materials through electric hydrogen circulation according to claim 1, characterized in that: The reduction furnace in step (1) is an improved rotary kiln, vertical furnace, mixed iron furnace, rotary hearth furnace or fluidized bed; the rotary kiln, vertical furnace, mixed iron furnace, rotary hearth furnace or fluidized bed is improved by adding electromagnetic induction, electric arc, resistor or electrode, providing green electricity to the electromagnetic induction, electric arc, resistor or electrode for heating, thereby increasing the physical heat in the furnace, and the hydrogen reducing gas entering the reduction furnace provides chemical energy for the reduction of the iron ore.
3. The long-process iron and steel metallurgical production method for producing iron and steel products by consuming iron-containing materials through electric hydrogen circulation according to claim 1, characterized in that: In the step (2), the smelting furnace is an electromagnetic induction furnace or an electric arc furnace, and the electromagnetic induction furnace or the electric arc furnace uses green electricity for heating.
4. The long-process iron and steel metallurgical production method for producing iron and steel products by consuming iron-containing materials through electric hydrogen circulation according to claim 1, characterized in that: In the step (1) and the step (2), the green hydrogen is introduced through a hydrogen blowing port, more than one hydrogen blowing port is provided, and the orientation of the hydrogen blowing port is arranged to enter the furnace in a top blowing, bottom blowing, oblique blowing, or side blowing manner.
5. The long-process iron and steel metallurgical production method for producing iron and steel products by consuming iron-containing materials through electric hydrogen circulation according to claim 1, characterized in that: The green hydrogen reduction in the reduction furnace in step (1) includes preheating, drying, pre-reduction and deep reduction processes.
6. The long-process iron and steel metallurgical production method for producing iron and steel products by consuming iron-containing materials through electric hydrogen circulation according to claim 5, characterized in that: The step (1) of preheating, drying and pre-reduction is as follows: placing the iron ore in a reduction furnace, preheating to a temperature of 25-1245° C., introducing a mixture of green hydrogen at a temperature of 435-1600° C., reduction furnace tail gas and industrial hydrogen, and preheating for 15-120 minutes to fill the reduction furnace with a green hydrogen atmosphere.
7. The long-process iron and steel metallurgical production method for producing iron and steel products by consuming iron-containing materials through electric hydrogen circulation according to claim 5, characterized in that: The deep reduction in step (1) is as follows: the ore is further heated to a temperature of 780-1750°C, green hydrogen at a temperature of 20-1700°C is introduced, and reduction smelting is performed for 0.2-4h, molten iron and slag are discharged from the iron mouth, and high-temperature hydrogen is discharged from the furnace top for reuse.
8. The long-process iron and steel metallurgical production method for producing iron and steel products by consuming iron-containing materials through electric hydrogen circulation according to claim 1, characterized in that: The specific process of full green hydrogen smelting in the smelting furnace in step (2) is as follows: 2.
1. Add reduced iron and calcium-magnesium flux into the smelting furnace, and continuously spray green hydrogen at a temperature of 20-1700°C into the smelting furnace to fill the smelting furnace with a green hydrogen atmosphere; 2.
2. The reduced iron is heated to a temperature of 1435-1650°C. After melting, green hydrogen at a temperature of 20-1700°C is sprayed into the melt by top blowing and bottom blowing. The top blowing pipe is inserted into the melt to a depth of 8-30mm. The smelting is performed for 0.2-4h, and green iron is obtained after slag removal.
9. The long-process iron and steel metallurgical production method for producing iron and steel products by consuming iron-containing materials through electric hydrogen circulation according to claim 1, characterized in that: In the step (3), the flue gas circulation system realizes heat exchange heating of the newly produced green hydrogen. After the industrial tail gas is cooled, cooling water and industrial hydrogen with high chemical heat are generated for recycling and reuse, including dust removal and cooling to obtain cooling water and industrial hydrogen. The industrial hydrogen is returned to the reduction furnace after secondary dust removal.
10. The long-process iron and steel metallurgical production method for producing iron and steel products by consuming iron-containing materials through electric hydrogen circulation according to claim 1, characterized in that: The green iron is pretreated by molten iron to remove silicon, phosphorus and sulfur, and then enters the steelmaking furnace to obtain molten steel. The heat for steelmaking comes from hydrogen-oxygen reaction, silicon-oxygen reaction and electric heating. The electric heating includes electromagnetic induction, electrode discharge or resistance heating. The hydrogen and silicon elements in the molten iron entering the furnace react with the blown oxygen to release heat, achieving four removals and two removals and two reductions. The molten steel is formed by a casting process, and the required steel is produced by hot rolling and cold rolling.
Citation Information
Patent Citations
Direct steelmaking system and process for electric energy all-hydrogen flash reduction
CN110423854A
Electric heating hydrogen smelting reduction ironmaking method
CN115287387A
Zero-carbon-emission steel smelting process based on green electricity and green hydrogen
CN118007011A
Method for production of molten steel
JP2016141873A
Straight grate-based pre-reduced pellet preparation device and method
WO2022262812A1
Cited By
Analysis method of electrothermal pure hydrogen metallurgy integrated system
CN120700223A