Method for producing green steel from vanadium-containing molten iron and green steel

By using thin scrap steel for temperature control and electrode heating during the production of green steel from vanadium-containing molten iron, and combining the coordinated operation of two LF furnaces, the problems of heat source shortage and heat loss were solved, achieving efficient production of high-quality green steel and reducing scrap steel consumption and environmental impact.

CN118957195APending Publication Date: 2024-11-15PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411170430.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the process of producing green steel, vanadium-containing molten iron suffers from a heat source shortage and a large amount of heat loss after vanadium extraction, resulting in low scrap steel consumption and high production difficulty, which cannot be effectively solved by existing technologies.

Method used

Lightweight scrap steel is used as a coolant for temperature control. Combined with electrode heating and multiple heating processes, two LF furnaces are operated in tandem. High-carbon scrap steel and lightweight scrap steel are added to supplement heat, and clean energy is used for smelting.

Benefits of technology

It has improved production efficiency, reduced scrap steel consumption, optimized steel quality, reduced environmental pollution, and achieved efficient resource utilization and environmental protection and emission reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957195A_ABST
    Figure CN118957195A_ABST
Patent Text Reader

Abstract

The invention discloses a method for producing green steel from vanadium-containing molten iron and the green steel. The method comprises the following steps that S1, converter vanadium extraction and blowing desulfurization are conducted, specifically, converter vanadium extraction adopts light and thin waste steel as a cooling agent for temperature control, and the adding amount of the light and thin waste steel accounts for 20-35% of the total adding amount of metal materials; s2, LF temperature rising is conducted, specifically, the desulfurized molten iron is hoisted to an LF working procedure, semisteel temperature rising is conducted in a first LF furnace in an electrode heating mode, and ferrosilicon is added before the semisteel is discharged from a station; s3, converter smelting is conducted, specifically, the heated semisteel is added into a steelmaking converter, high-carbon waste steel is added before iron is added, and the final temperature of the converter is controlled to be 1630-1650 DEG C; s4, LF secondary heating is conducted, specifically, after tapping, molten steel enters a second LF furnace to be heated, and after light and thin waste steel is added, heating is conducted; and S5, RH refining and continuous casting. According to the method, equipment of existing enterprises is better utilized, the characteristics of vanadium-containing molten iron production are combined, and the problems of low waste steel consumption and high green steel production difficulty caused by shortage of a vanadium-containing molten iron heat source and loss of a large amount of heat after vanadium extraction are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel smelting, and in particular to a method for producing green steel from vanadium-containing molten iron and the green steel. Background Art

[0002] Green and low-carbon is one of the important development themes of the world's steel industry. Comprehensive decarbonization will be a huge challenge facing the world's steel industry. In order to achieve this goal, the world's major economies have launched their own low-carbon roadmaps for the steel industry, and advanced technologies such as "hydrogen-based reduction-electric furnace steelmaking" and "CO2 capture, recovery and storage" have also emerged. However, these technologies are still in the research and development stage, and there is great uncertainty in technology research and development. Before these technologies mature, transitional technologies are needed to support the steady advancement of low-carbon and green development in the steel industry. Solving problems such as excessive resource consumption, large carbon emissions, and continuous accumulation of metallurgical slag in the steel industry is the only way for the current green, low-carbon and sustainable development of the steel industry. With the implementation of my country's dual-carbon strategy, the operation of the EU Carbon Border Adjustment Mechanism (CBMA), and the promotion of carbon footprint assessment (LCA) of the entire life cycle of steel products, the development of low-carbon emission and green production technologies in the current steel industry is imminent, and domestic and foreign steel companies, universities, and research and development institutions have also carried out a lot of work. At present, in the case of insufficient resources such as hydrogen-based direct reduced iron, the production of low-carbon green steel products characterized by social scrap steel + green electricity has become the focus of research and development.

[0003] Green steel refers to steel products with low carbon emissions per ton of steel produced by using scrap steel or green non-carbon reducing agents and green electricity as energy. At present, the company has realized the process of producing green automobile plates with 100% scrap steel as raw materials by using electric furnace + green electricity; it has also achieved continuous production of green steel with a large scrap steel ratio of 50% in the converter, with the number of continuous casting furnaces reaching 7 furnaces; it has also carried out relevant research on the production of green steel based on direct reduced iron + blast furnace hot metal; and it is also developing a complete set of technologies for producing green steel based on direct reduced iron production technology + smelting furnace / electric furnace. However, these technologies cannot be applied to enterprises that use vanadium-containing molten iron for steelmaking. The main reason is that vanadium-titanium magnetite has not been used to directly reduce molten iron, and the carbon content of vanadium-containing molten iron produced by blast furnace is only 4.0%~4.3%, much lower than the 4.5% of ordinary blast furnace molten iron; the content of [Si]+[Mn] in the molten iron is only 0.3%~0.5%, much lower than the content of more than 1.0% in ordinary blast furnace molten iron; the molten iron temperature is only 1450℃, which is also lower than the iron-out temperature of more than 1500℃ of ordinary molten iron; and the vanadium-containing molten iron needs to be blown with oxygen to extract vanadium, and the thermal mass elements are lost, resulting in scrap steel consumption far less than ordinary molten iron. Therefore, it is extremely difficult to produce green steel with vanadium-containing molten iron.

[0004] In view of this, the existing technology should be improved. Summary of the invention

[0005] The main purpose of the present invention is to provide a method for producing green steel from vanadium-containing molten iron and green steel. Through precise process control, the problems of shortage of heat source of vanadium-containing molten iron, low scrap steel consumption caused by large amount of heat loss after vanadium extraction and great difficulty in producing green steel are solved.

[0006] According to one aspect of the present invention, a method for producing green steel from vanadium-containing molten iron is provided, which comprises the following steps: S1. Converter vanadium extraction and injection desulfurization: Converter vanadium extraction uses light scrap steel as a coolant for temperature control. The amount of light scrap steel added accounts for 20-35% of the total amount of metal materials added, and the terminal temperature is controlled at 1360-1400℃; S2, LF heating: After desulfurization, the molten iron is hoisted to the LF process, and the first LF furnace is heated by electrode heating to heat the semi-steel. Before leaving the station, 3~5kg / (t steel) of ferrosilicon is added; S3, converter smelting: after heating, the semi-steel is added into the steelmaking converter, and high carbon scrap steel is added before adding iron, and the final temperature of the converter is controlled at 1630~1650℃; S4, LF secondary heating: After tapping, the molten steel enters the second LF furnace for heating, and light and thin scrap steel is added before heating; S5, RH refining and continuous casting: RH refining treatment, continuous casting process according to the preset steel type.

[0007] According to one embodiment of the present invention, high carbon scrap steel is scrap steel with a carbon content greater than 0.75%.

[0008] According to one embodiment of the present invention, the light and thin scrap steel is small-sized scrap steel that has been pre-processed, and the maximum length, width and height of the light and thin scrap steel are <150mm and the weight of a single piece is <5kg.

[0009] According to one embodiment of the present invention, the heating time of the electrode heating is 30 to 40 minutes.

[0010] According to one embodiment of the present invention, in step S4, the amount of thin scrap steel added is 5% to 10% of the steel inclusion volume.

[0011] According to one embodiment of the present invention, in step S3, the amount of high carbon scrap steel added is 30-50% of the nominal capacity of the converter.

[0012] According to an embodiment of the present invention, in step S4, the temperature range of the heating after adding the light and thin scrap steel is ≥1600°C.

[0013] According to one embodiment of the present invention, in step S1, the metal material includes solid iron and scrap steel.

[0014] According to one embodiment of the present invention, the electric energy used in the method is clean energy, and the clean energy includes wind power generation and / or photovoltaic power generation.

[0015] According to another aspect of the present invention, a green steel is provided, which is prepared by using any one of the methods in the above technical solutions.

[0016] In a method for producing green steel from vanadium-containing molten iron according to an embodiment of the present invention, precise process control is used to solve the problems of shortage of heat source for vanadium-containing molten iron, low consumption of scrap steel due to large amount of heat loss after vanadium extraction, and difficulty in producing green steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings required for use in the embodiment will be briefly introduced below. Obviously, the drawings described below are only some implementation cases of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 A process flow chart of a method for producing green steel from vanadium-containing molten iron according to an exemplary embodiment of the present invention is shown. DETAILED DESCRIPTION

[0019] The detailed description of the following embodiments is used to exemplify the principles of the present invention, but cannot be used to limit the scope of the present invention. The present invention can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

[0020] The present invention provides these embodiments to make this disclosure thorough and complete, and fully express the scope of the present invention to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of materials, numerical expressions and numerical values ​​set forth in these embodiments should be interpreted as being merely exemplary, rather than as limiting.

[0021] It should be noted that, in the description of the present invention, unless otherwise specified, the meaning of "multiple" is greater than or equal to two; the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating the orientation or positional relationship, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.

[0022] It should also be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances. When a specific device is described as being located between a first device and a second device, there may or may not be an intermediate device between the specific device and the first device or the second device.

[0023] All terms used in the present invention have the same meanings as those understood by those of ordinary skill in the art to which the present disclosure belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, for example, should be interpreted as having meanings consistent with their meanings in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined herein.

[0024] Technologies, methods, and apparatus known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, these technologies, methods, and apparatus should be considered part of the specification.

[0025] like Figure 1 As shown, the present invention provides a method for producing green steel from vanadium-containing molten iron, which comprises the following steps: S1, converter vanadium extraction, spray desulfurization: converter vanadium extraction uses light and thin scrap steel as a coolant for temperature control, the amount of light and thin scrap steel added accounts for 20-35% of the total amount of metal material added, and the terminal temperature is controlled at 1360-1400°C; S2, LF heating: after desulfurization, the molten iron is hoisted to the LF process, and the semi-steel is heated by electrode heating in the first LF furnace, and 3-5kg / (t steel) of ferrosilicon is added before leaving the station; S3, converter smelting: after heating, the semi-steel is added into the steelmaking converter, and high-carbon scrap steel is added before adding iron, and the terminal temperature of the converter is controlled at 1630-1650°C; S4, LF secondary heating: after steel tapping, the molten steel enters the second LF furnace for heating, and is heated after adding light and thin scrap steel; S5, RH refining, continuous casting: RH refining treatment, continuous casting process according to the preset steel type. Steel grades can be classified according to criteria including chemical composition (such as carbon content) or quality or use or forming method. The type of steel grade must be taken into account during the continuous casting process and the continuous casting process must be carried out according to the preset steel grade type.

[0026] In the method for producing green steel from vanadium-containing molten iron according to an embodiment of the present invention, the equipment of existing enterprises can be better utilized. Combined with the characteristics of vanadium-containing molten iron production, precise process control is used to solve the problems of shortage of heat sources for vanadium-containing molten iron, low scrap steel consumption caused by large-scale heat loss after vanadium extraction, and difficulty in producing green steel.

[0027] After the molten steel has been initially smelted and refined, and the steel-tapping operation is completed, the molten steel will be transferred to the second LF furnace for secondary heating and desulfurization treatment. This link not only helps to further improve the purity and quality of the molten steel, but also consumes more scrap steel in the process, thereby achieving efficient utilization of resources. The simultaneous operation of the two LF furnaces means that the molten steel from the two furnaces can be refined and heated at the same time in the same period of time. This mode of operation can greatly improve production efficiency and meet the market's demand for high-yield and high-efficiency steel. At the same time, the collaborative work of the two LF furnaces can also make the entire process smoother and reduce production delays caused by equipment waiting or shutdown.

[0028] Using thin scrap steel as a coolant achieves resource recycling, reduces the mining of new resources, and thus reduces damage to the environment. Thin scrap steel can quickly absorb heat during the smelting process, effectively reducing the furnace temperature, thereby maintaining the stability of the smelting process. It has a wide range of sources and low cost, which can reduce smelting costs.

[0029] In some specific embodiments, high carbon scrap steel is scrap steel with a carbon content of >0.75%. In order to save resources and reduce the waste of scrap steel, high carbon scrap steel comes from scrap steel recycled by the society. After recycling, in order to ensure the carbon content after the converter, the scrap steel will be preliminarily screened, and the scrap steel with a carbon content of >0.75% will be defined as high carbon scrap steel, and high carbon scrap steel will be added before adding iron. High carbon scrap steel has a high carbon content, and after adding, it can provide an additional carbon source for the smelting process, which helps to accelerate chemical reactions and improve smelting efficiency. The addition of high carbon scrap steel can introduce chemical elements such as low carbon and low phosphorus, thereby improving the characteristics of slag and facilitating the treatment of slag.

[0030] In some specific embodiments, the thin scrap steel is a small-sized scrap steel after pretreatment, and the maximum size of the length, width and height of the thin scrap steel is less than 150mm and the weight of a single piece is less than 5kg. In order to save resources and reduce the waste of scrap steel, the thin scrap steel also comes from the scrap steel recycled by the society. When the thin scrap steel is processed into a small size, the ratio of its surface area to volume increases, so that the surface area in contact with the vanadium-containing molten iron is larger, thereby improving the efficiency of heat exchange and helping to react more quickly. The small-sized thin scrap steel can be used as a coolant to more effectively absorb the excess heat in the converter during the melting process, which not only reduces energy consumption, but also helps to reduce the emission of greenhouse gases such as carbon dioxide. Due to the improvement of cooling efficiency, the smelting cycle of the converter is shortened, thereby also improving production efficiency. In addition, the small-sized thin scrap steel is more easily penetrated by the slag in the converter, reducing the possibility of secondary oxidation and further improving the smelting efficiency.

[0031] On the basis of the above embodiment, in step S2, the heating time of the electrode heating is 30 to 40 minutes. By means of electrode heating, the temperature of the semi-steel can be quickly and evenly increased, thereby shortening the heating time and improving production efficiency. In addition, precise temperature control also helps to reduce energy waste and reduce production costs. When the electrode is heated, the heat energy transferred to the discharge point will diffuse to other parts of the electrode, avoiding or reducing the concentrated heating of the electrode, reducing the loss of the electrode, which has a positive effect on reducing production costs and improving economic benefits. In order to ensure complete heating, the heating time of the electrode heating is 30 to 40 minutes.

[0032] On the basis of the above embodiments, in step S4, the amount of thin scrap steel added is 5% to 10% of the steel inclusion amount. Thin scrap steel contains certain alloy elements, such as carbon, iron, manganese, chromium, etc. When added to the smelting process in an amount of 5% to 10% of the steel inclusion amount, the composition of molten steel can be effectively adjusted and controlled to optimize the performance and quality of steel. The appropriate amount of scrap steel added can improve the organizational structure of steel and optimize the mechanical properties of steel, such as strength, ductility and impact toughness. Adding 5% to 10% of thin scrap steel can achieve this effect and improve the overall quality of steel.

[0033] Based on the above embodiment, in step S3, the amount of high carbon scrap steel added is 30-50% of the nominal capacity of the converter. The nominal capacity refers to the standard capacity claimed by the product for market promotion and consumer selection. In this application, the amount of high carbon scrap steel added is 30-50% of the nominal capacity of the converter. Preferably, the amount added is 40% of the nominal capacity.

[0034] Based on the above embodiment, in step S4, the temperature range of the heating after adding thin scrap steel is ≥1600°C. The rapid preheating and heating of thin scrap steel can help improve the temperature distribution in the furnace, make the temperature in the furnace more uniform, and be beneficial to the stability and consistency of the smelting process. It can reduce energy consumption, and correspondingly reduce the emission of waste gas and waste slag generated during the combustion process, thereby reducing the impact on the environment. In this application, after adding thin scrap steel, the temperature is raised to 1600°C and then RH refining is performed. On the basis of the above embodiments, in step S1, the metal material includes solid iron and scrap steel. As raw materials, solid iron and scrap steel can directly participate in the steelmaking process, reducing the secondary processing and conversion of raw materials, thereby improving the production efficiency of steelmaking. In addition, the recycling of scrap steel can also reduce the mining of new resources and reduce production costs. In the converter vanadium extraction, solid iron and scrap steel can be used as reducing agents to participate in the reduction reaction of vanadium, thereby improving the recovery rate and extraction efficiency of vanadium. In addition, the vanadium element that may be contained in the scrap steel can also be recycled in the vanadium extraction process, further improving the resource utilization rate.

[0035] On the basis of the above embodiments, the electric energy used in the method is clean energy, and the clean energy includes wind power generation and / or photovoltaic power generation. Wind power generation and photovoltaic power generation are clean renewable energy sources that do not produce greenhouse gas and harmful substance emissions. The use of these two energy sources for smelting can significantly reduce the emission of pollutants such as sulfur dioxide and nitrogen oxides, which helps to protect the atmospheric environment and has a significant effect on improving the environment, reducing pollution and reducing greenhouse gas emissions. In addition, the use of wind and solar energy can reduce dependence on fossil fuels, thereby saving limited natural resources. The use of renewable energy for smelting is of great strategic significance.

[0036] The present invention also provides a green steel, which is prepared by any method of the above technical solutions.

[0037] The solution of the present application is described below through specific embodiments.

[0038] Example 1 The production process is "converter vanadium extraction → injection desulfurization → LF heating → converter smelting → LF secondary heating → RH refining → continuous casting". The vanadium extraction converter is loaded with 80t of vanadium-containing molten iron, and light high-carbon scrap steel is used as a coolant for temperature control. The amount of high-carbon scrap steel added is 40t. No other coolant is used for temperature control, and the terminal temperature is controlled at 1400℃; injection desulfurization is still carried out according to the original process; after desulfurization, the molten iron is hoisted to the LF process, and the semi-steel is heated by electrode heating. The heating time is controlled at 30min, and 5kg / (t steel) of ferrosilicon is added before leaving the station, and the exit temperature is 1400℃; after heating, the semi-steel Add to the steelmaking converter, and add 50t of high-carbon scrap steel before adding iron, and then add 80t of semi-steel. The converter blowing process remains unchanged, and the terminal temperature is controlled at 1630℃; after 110t of steel is tapped, the ladle enters the second LF furnace for heating, and 10t of light and thin scrap steel is added. After heating to 1600℃, RH refining treatment is carried out; the continuous casting process is carried out according to the requirements of specific steel grades; the electricity involved comes from clean energy such as wind power and photovoltaic power generation, and the scrap steel comes from social recycled scrap steel. The scrap steel ratio of the whole process reaches 62%.

[0039] Example 2 The production process is "converter vanadium extraction → injection desulfurization → LF heating → converter smelting → LF secondary heating → RH refining → continuous casting". The vanadium extraction converter is loaded with 170t of vanadium-containing molten iron, and light high-carbon scrap steel is used as a coolant for temperature control. The amount of high-carbon scrap steel added is 60t. No other coolant is used for temperature control, and the terminal temperature is controlled at 1360℃; injection desulfurization is still carried out according to the original process; after desulfurization, the molten iron is hoisted to the LF process, and the semi-steel is heated by electrode heating. The heating time is controlled at 30min, and 3kg / (t steel) of ferrosilicon is added before leaving the station, and the exit temperature is 1400℃; after heating, the semi-steel Add to the steelmaking converter, and add 80t of high-carbon scrap steel before adding iron, and then add 160t of semi-steel. The converter blowing process remains unchanged, and the terminal temperature is controlled at 1650℃; after 200t of steel is tapped, the ladle enters the second LF furnace for heating, and 20t of light and thin scrap steel is added. After heating to 1600℃, RH refining treatment is carried out; the continuous casting process is carried out according to the requirements of specific steel grades; the electricity involved comes from clean energy such as wind power and photovoltaic power generation, and the scrap steel comes from social recycled scrap steel. The scrap steel ratio of the whole process reaches 55%.

[0040] After the implementation of the present invention, at least the following beneficial effects are achieved: (1) Making full use of the LF heating function can not only effectively increase the temperature of the molten steel, ensuring that it reaches the smelting temperature required by the process, but also ensure the quality and performance of the steel. This measure not only optimizes the production process, but also improves production efficiency, providing a strong guarantee for the production of high-quality steel.

[0041] (2) During the smelting process, light and thin scrap steel is used to control the temperature of the converter for vanadium extraction. This method aims to effectively adjust and control the temperature in the converter by adding light and thin scrap steel to ensure the stability of the smelting process. At the same time, the addition of scrap steel also increases the proportion of scrap steel used, reduces production costs, and achieves effective resource utilization and environmental emission reduction. This not only reflects the importance attached to environmental protection and resource conservation, but also demonstrates the innovation ability and technical level in the field of steel production.

[0042] (3) The transfer of molten steel during the secondary heating of the LF and the simultaneous operation of two LF furnaces can not only achieve efficient utilization of scrap steel and optimization of steel performance, but also improve production efficiency and make the process flow smoother. Such process design is of great significance to the sustainable development of steel enterprises.

[0043] (4) In the entire production process, all the electricity used comes from green energy. This means that the production activities not only meet the production needs, but also actively respond to the national call for energy conservation and emission reduction, and make positive contributions to protecting the environment and promoting sustainable development. By adopting clean energy and environmental protection technology, the negative impact on the environment is reduced, achieving a win-win situation of economic and environmental benefits.

[0044] The above are exemplary embodiments disclosed in the present invention. The order disclosed in the above embodiments of the present invention is for description only and does not represent the advantages and disadvantages of the embodiments. However, it should be noted that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope disclosed in the embodiments of the present invention (including the claims) is limited to these examples. Various changes and modifications may be made without departing from the scope defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.

[0045] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.

Claims

1. A method for producing green steel from vanadium-containing molten iron, characterized in that: The following steps are involved: S1. Converter vanadium extraction and injection desulfurization: The converter vanadium extraction uses light and thin scrap steel as a coolant for temperature control. The amount of light and thin scrap steel added accounts for 20-35% of the total amount of metal material added, and the terminal temperature is controlled at 1360-1400°C; S2, LF heating: After desulfurization, the molten iron is hoisted to the LF process, and the first LF furnace is heated by electrode heating to heat the semi-steel. Before leaving the station, 3~5kg / (t steel) of ferrosilicon is added; S3, converter smelting: after heating, the semi-steel is added into the steelmaking converter, and high carbon scrap steel is added before adding iron, and the final temperature of the converter is controlled at 1630~1650℃; S4, LF secondary heating: After tapping, the molten steel enters the second LF furnace for heating, and light and thin scrap steel is added before heating; S5, RH refining and continuous casting: RH refining treatment, continuous casting process according to the preset steel type.

2. The method for producing green steel from vanadium-containing molten iron according to claim 1, characterized in that: The high carbon scrap steel is scrap steel with a carbon content greater than 0.75%.

3. The method for producing green steel from vanadium-containing molten iron according to claim 1, characterized in that: The light and thin scrap steel is small-sized scrap steel that has been pre-processed, and the maximum length, width and height of the light and thin scrap steel are <150mm and the weight of a single piece is <5kg.

4. The method for producing green steel from vanadium-containing molten iron according to claim 1, characterized in that: In step S2, the heating time of the electrode heating is 30 to 40 minutes.

5. The method for producing green steel from vanadium-containing molten iron according to claim 1, characterized in that: In step S4, the amount of thin scrap steel added is 5% to 10% of the steel inclusion volume.

6. The method for producing green steel from vanadium-containing molten iron according to claim 1, characterized in that: In step S3, the amount of high carbon scrap steel added is 30-50% of the nominal capacity of the converter.

7. The method for producing green steel from vanadium-containing molten iron according to claim 1, characterized in that: In step S4, the temperature range of the heating after adding the light and thin scrap steel is ≥1600°C.

8. The method for producing green steel from vanadium-containing molten iron according to claim 1, characterized in that: In step S1, the metal material includes solid iron and scrap steel.

9. The method for producing green steel from vanadium-containing molten iron according to claim 1, characterized in that: The electric energy used in the method is clean energy, which includes wind power generation and / or photovoltaic power generation.

10. A green steel, characterized in that: The method is prepared by any one of claims 1 to 9.