Heat treatment method of wheel for rail transit
By adopting double-layer drop-stomp and rotation methods in the heat treatment of rail transit wheels, combined with multi-layer nozzle quenching cooling device, the problems of uneven heating and high energy consumption are solved, and the performance uniformity and toughness of the wheels are significantly improved. .
Patent Information
- Application Number
- CN202410736851.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-11-15
AI Technical Summary
During the heat treatment process of rail transit wheels, there are problems such as uneven heating, high energy consumption and complex process, which affect the performance and service performance of the wheels.
The double-layer drop-stomp heat treatment method is adopted. The blank wheel rotates counterclockwise in the quenching heating furnace and rotates automatically during the quenching and tempering process. Combined with the multi-layer nozzle quenching cooling device, it ensures that the wheel rim is uniformly heated.
It improves heat treatment efficiency, reduces energy consumption, improves the uniformity and hardness of wheel performance, and reduces the impact of furnace temperature unevenness on wheels.
Smart Images

Figure CN118957239A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of wheels for rail transit, and in particular, relates to a heat treatment method for wheels for rail transit. Background Art
[0002] At present, wheels for rail transit are products with long processes and high energy consumption, especially the heat treatment process, which includes a series of heat treatment steps such as quenching heating, quenching, and tempering. The process is complex, energy-intensive, and time-consuming.
[0003] An annular heating furnace is generally used for the production and heating of rail transit wheels. The furnace chamber has a long span and a large width, and there are deviations in the furnace temperature, especially the large temperature difference between the inner and outer rings and the top and bottom of the furnace. This causes uneven heating during the overall heating process of the wheel and large differences in circumferential performance, which affects the wheel's performance and service performance.
[0004] For example, the patent document with publication number CN101818239A discloses a railway wheel heat treatment heating furnace, in which the structure of the induction heating device is that an induction heating coil is arranged on the periphery of the tread of the railway wheel, and an induction heating compensation coil is arranged on the inner side of the rim of the railway wheel and the corresponding position of the transition area from the inner side of the rim to the web. The present invention also discloses a heat treatment process method of the heat treatment heating furnace. The above technical scheme is adopted to achieve the process goals of high strength and high toughness of the rim and low strength and high toughness of the web. The heating speed in the two-phase zone is very fast and the residence time in the austenite temperature zone is very short, which is conducive to uniform grain refinement and improved rim toughness. The technical scheme disclosed in the patent document also has technical problems such as those recorded above. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a heat treatment method for a wheel for rail transit, the purpose of which is to improve the heat treatment efficiency and improve the uniformity of wheel performance.
[0006] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a heat treatment method for a wheel for rail transit, comprising the steps of:
[0007] S1. The blank wheel is put into the quenching heating furnace for heating;
[0008] S2, quenching;
[0009] S3, tempering;
[0010] In step S1, the blank wheel enters the quenching and heating furnace in a double-layer dropping manner; while the quenching and heating furnace rotates, the blank wheel rotates simultaneously.
[0011] In the step S1, the quenching heating furnace and the blank wheel both rotate in a counterclockwise direction.
[0012] In the step S1, the heating temperature is 850-900°C.
[0013] In the step S1, after the heating is completed, the temperature is kept warm, and the temperature keeping time is set to 1.5 to 2.5 hours.
[0014] In step S3, the blank wheel enters the tempering heating furnace in a double-layer dropping manner.
[0015] In the step S3, the tempering temperature is 470-530°C.
[0016] In the step S3, after the tempering treatment is completed, the material is kept warm, and the holding time is set to be ≥5h.
[0017] In the step S1, the blank wheel rotates at a speed of 3-5 minutes per rotation.
[0018] In the step S2, a quenching and cooling device is used, and the quenching and cooling device includes a quenching table and nozzles, which are arranged in multiple layers, and all nozzles in each layer are evenly distributed around the outer side of the blank wheel along the circumferential direction.
[0019] The nozzle is provided with a weak cooling water outlet hole and a strong cooling water outlet hole. In step S2, the water output of the weak cooling water outlet hole is 8-10m 3 / h, the water output of the strong cooling water outlet is 18-24m 3 / h.
[0020] The heat treatment method for rail transit wheels of the present invention adopts a double-layer drop-stomp heat treatment method, which can greatly improve the heat treatment efficiency and reduce the heat treatment energy consumption. At the same time, the wheel is rotated during the quenching and heating process, so that the wheel rim can be heated evenly, reducing the influence of uneven furnace temperature on the wheel rim temperature, improving the uniformity of wheel quenching temperature, and improving the uniformity of wheel performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] This specification includes the following drawings, which show the following contents:
[0022] Figure 1 This is a cross-sectional view of a quenching heating furnace.
[0023] Figure 2 This is a top view of the quenching heating furnace.
[0024] Figure 3 It is a cross-sectional view of the quenching table;
[0025] Figure 4The wheel rim microstructure diagrams of Example 1 and Comparative Example 1 are shown. The microstructure of Example 1 is finer and more uniform, and the actual grain size is 8.5; some microstructures in Comparative Example 1 are coarser, and the actual grain size is 7.5;
[0026] The markings in the figure are:
[0027] 1. Burner; 2. Furnace bottom; 3. Furnace wall; 4. Furnace center ring line; 5. Plum blossom pile; 6. Flue; 7. Furnace discharge door; 8. Furnace charging door; 9. Nozzle; 10. Lifting platform; 11. Rotating roller; 12. Rotating motor; 13. Quenching wheels. DETAILED DESCRIPTION
[0028] The specific implementation methods of the present invention are further explained in detail below by describing the embodiments with reference to the accompanying drawings, with the aim of helping those skilled in the art to have a more complete, accurate and in-depth understanding of the inventive concept and technical solution of the present invention and facilitating their implementation.
[0029] The present invention provides a heat treatment method for a rail transit wheel, comprising the following steps:
[0030] S1. The blank wheel is put into the quenching heating furnace for heating;
[0031] S2, quenching;
[0032] S3. Tempering.
[0033] Specifically, the production process of rail transit wheels is electric furnace → LF furnace refining → RH furnace vacuum degassing → continuous casting → ingot cutting → upsetting → preforming → forming → slow cooling to room temperature → quenching and heating → quenching → high temperature tempering → machining → inspection. During the production process, the wheels are rolled and formed, slowly cooled to room temperature, and then quenched and heated.
[0034] like Figure 1 As shown, in the above step S1, the blank wheel enters the quenching heating furnace in a double-layer dropping manner. During the rotation of the quenching heating furnace, the blank wheel rotates at the same time. The quenching heating furnace is a ring-shaped heating furnace. The blank wheel after dropping is placed on the plum blossom pile. The plum blossom pile moves along the bottom of the furnace along the quenching heating furnace ( Figure 2 ) rotates counterclockwise at a certain speed, and at the same time the plum blossom pile rotates counterclockwise, thereby driving the blank wheel to rotate around its axis.
[0035] like Figure 1 As shown, the bottom of the quenching heating furnace is provided with a plurality of plum blossom piles, on each of which two blank wheels are placed, and the two blank wheels are placed on the plum blossom piles in a stacked manner, and the two blank wheels on the plum blossom piles are in a coaxial state with the plum blossom piles. The plum blossom piles are connected to a driving mechanism, and the driving mechanism drives the plum blossom piles and the blank wheels placed in a double-layered manner on them to rotate.
[0036] In the above step S1, the quenching heating furnace and the blank wheel both rotate in the counterclockwise direction. The quenching heating furnace rotates evenly, and the blank wheel also keeps rotating in the quenching heating furnace during the rotation of the quenching heating furnace. The quenching heating furnace and the blank wheel both rotate in the counterclockwise direction to ensure that the blank wheel is heated evenly. The blank wheel is heated in the quenching heating furnace at a heating temperature of 850 to 900°C. After the heating is completed, the blank wheel is kept warm for 1.5 to 2.5 hours, and finally taken out of the furnace for quenching.
[0037] In the above step S1, the speed at which the plum blossom pile rotates along the annular heating furnace is determined by the wheel heating time, and the plum blossom pile drives the blank wheel to rotate at a speed of 3-5 minutes per rotation. Rotating along the circumference of the annular heating furnace during the heating process can effectively ensure the continuity of wheel heating, ensure that all wheels go through various stages such as low temperature → medium temperature → high temperature, and ensure that the temperature stability of batch products is consistent, which is conducive to the stability consistency of the product. Wheel rotation can ensure that the circumferential heating environment of each wheel is consistent, and each part of the wheel can reach the target temperature, promoting more uniform circumferential hardness and structure of the wheel.
[0038] like Figure 3 As shown, in the above step S2, a quenching and cooling device is used, and the quenching and cooling device includes a quenching table and nozzles. All nozzles are arranged in multiple layers up and down, and all nozzles in each layer are evenly distributed along the circumferential direction around the outer side of a blank wheel.
[0039] Preferably, the nozzle is provided with a plurality of weak cooling water outlet holes and a plurality of strong cooling water outlet holes, and the water output of the strong cooling water outlet holes is greater than the water output of the weak cooling water outlet holes. In the above step S2, during the quenching process, the water pressure is 0.1±0.01MPa, and the water output of the weak cooling water outlet holes is 8-10m 3 / h, the water output of the strong cooling water outlet is 18-24m 3 / h. The method of first weak and then strong can ensure that the near-surface cooling rate is consistent with the deep-layer cooling rate, thereby ensuring that the near-surface hardness structure of the wheel tread is consistent with the deep-layer hardness structure, thereby ensuring that the service performance of the wheel is consistent throughout its service life.
[0040] like Figure 3 As shown, in the above step S2, 6 nozzles are evenly distributed along the circumferential direction on the outer side of each blank wheel, and 24 weak cooling water outlet holes and 48 strong cooling water outlet holes are arranged on the nozzles.
[0041] In the above step S2, the quenching and cooling device can work in two working conditions. The first working condition is weak cooling + strong cooling working condition. When the quenching and cooling device works in the first working condition, the blank wheel is subjected to weak cold spray quenching and strong cold spray quenching in sequence. The weak cold spray quenching time is 60-120s, and the strong cold spray quenching time is set to 180-480s. The second working condition is the strong cooling working condition. When the quenching and cooling device works in the second working condition, only the blank wheel is subjected to strong cold spray quenching, and the strong cold spray quenching time is 200-480s. The specific spray quenching time depends on the thickness of the rim. The thicker the rim, the longer the spray quenching time; the thinner the rim, the shorter the spray quenching time.
[0042] When weak cold spray quenching is performed on the blank wheel, water is sprayed on the blank wheel through the weak cold water outlet hole of the nozzle; when strong cold spray quenching is performed on the blank wheel, water is sprayed on the blank wheel through the strong cold water outlet hole of the nozzle.
[0043] In the above step S3, after quenching, the blank wheel enters the tempering heating furnace in a double-layer drop-down manner. The blank wheel is directly placed at the bottom of the tempering heating furnace and rotates counterclockwise along the annular heating furnace at a certain speed. The tempering temperature is 470-530°C. After the tempering treatment is completed, the heat preservation is carried out, and the heat preservation time is set to ≥5h. Finally, the blank wheel is taken out of the furnace and air-cooled.
[0044] The above-mentioned heat treatment method for rail transit wheels has the following advantages:
[0045] On the one hand, the wheel production process is long and energy consumption is high, especially the heat treatment process, which includes a series of heat treatment procedures such as quenching heating, quenching, and tempering. The use of double-layer drop-stomp heat treatment can greatly improve the heat treatment efficiency and reduce the heat treatment energy consumption; on the other hand, since the quenching heating furnace is an annular heating furnace, the furnace chamber has a long span and a large width, and there is a deviation in the furnace temperature, especially the large temperature difference between the inner and outer rings and the top and bottom of the furnace, increasing the wheel (plum blossom pile) self-rotation function can make the wheel rim evenly heated and reduce the impact of uneven furnace temperature on the wheel rim temperature; furthermore, the present invention adopts a rapid heating method for heat treatment, combined with the double-layer drop-stomp self-rotation function of the wheel, during the heating process of the wheel, the rim is fully in contact with the furnace gas, can reach a higher temperature, and can obtain a higher level of hardness after quenching. However, the residual furnace gas contact at the hub spoke plate is insufficient, the temperature is low, the austenitization is insufficient, and the austenite grains are fine. The fine austenite grains can improve the performance of the hub spoke plate, which is extremely beneficial to the wheel.
[0046] Example 1
[0047] The present invention adopts a double-layer drop heat treatment method and a wheel rotation heating method, which can greatly improve the heat treatment efficiency, reduce the heat treatment energy consumption, and make the wheel rim evenly heated, reducing the influence of uneven furnace temperature on the wheel rim temperature. At the same time, during the heating process of the wheel, the rim part is fully in contact with the furnace gas, which can reach a higher temperature, and can obtain a higher level of strength and hardness after quenching; while the hub spoke plate is not fully in contact with the furnace gas, the temperature is low, the austenitization is not sufficient, and the austenite grains are fine. The fine austenite grains can improve the performance of the hub spoke plate.
[0048] The wheel production process of this embodiment is electric furnace → LF furnace refining → RH furnace vacuum degassing → continuous casting → ingot cutting → upsetting → preforming → forming → slow cooling to room temperature → quenching and heating → quenching → high temperature tempering → machining → inspection. The outer diameter of the finished wheel is 920mm, the rim thickness is 68mm, and the chemical composition of the wheel is as shown in Table 1 for wheel 1. Before quenching and heating, the double-layer drop-stomp method is used to enter the quenching and heating furnace, such as Figure 1 As shown, the wheel after falling is placed on the plum blossom pile, and the plum blossom pile moves along the annular heating furnace ( Figure 2 ) rotates counterclockwise, and at the same time the plum blossom pile rotates counterclockwise at a speed of 3 minutes per rotation.
[0049] The wheel quenching heating temperature is 860±10℃, and the wheel is quenched after being kept warm for 2.0h. Figure 3 The quenching process adopts the strong cold heat treatment process, the quenching time is 300s, the water pressure is 0.1±0.01MPa, and the water output of the strong cold water outlet is 21m 3 / h. After quenching, the wheels are still put into the tempering heating furnace in a double-layer dropping way. The wheels are directly placed on the bottom of the furnace and rotate counterclockwise along the annular heating furnace at a certain speed. The tempering temperature is 480±10℃. After keeping warm for ≥5h, they are taken out of the furnace and air-cooled.
[0050] Comparative Example 1
[0051] The wheel production process of this comparative example is electric furnace → LF furnace refining → RH furnace vacuum degassing → continuous casting → ingot cutting → upsetting → preforming → forming → slow cooling to room temperature → quenching and heating → quenching → high temperature tempering → machining → inspection. The outer diameter of the finished wheel is 920mm, the rim thickness is 68mm, and the chemical composition of the wheel is as shown in Table 1 for wheel 1. The quenching and heating adopts a single-layer method to enter the quenching and heating furnace. The wheel is directly placed on the bottom of the furnace. As the furnace bottom rotates counterclockwise along the annular heating furnace, the wheel quenching and heating temperature is 860±10℃. After keeping warm for 3.0h, it is taken out of the furnace for quenching. The quenching is carried out by a single-piece single-layer heat treatment method. The quenching adopts a strong cold heat treatment process. The quenching time is 300s, the water pressure is 0.1±0.01MPa, and the water output of the water outlet is 21m 3 / h. After quenching, the wheels are put into the tempering heating furnace in a single-piece and single-layer manner. The wheels are placed directly on the bottom of the furnace and rotated counterclockwise along the annular heating furnace at a certain speed. The tempering temperature is 480±10℃. After keeping warm for ≥5h, they are taken out of the furnace and air-cooled.
[0052] According to BS EN 13262 "Railway Applications - Wheelsets and Bogies - Wheels - Product Requirements", tensile, impact and hardness analysis were performed on Example 1 and Comparative Example 1. Tensile tests were performed according to GB / T 228.1 "Metallic Materials Tensile Test Part 1: Room Temperature Test Method", pendulum impact tests were performed at room temperature and -20°C according to GB / T 229 "Metallic Materials Charpy Pendulum Impact Test Method", and hardness measurements were performed according to GB / T231.1 "Metallic Brinell Hardness Test Part 1: Test Method". The performance of the wheels of Example 1 and Comparative Example 1 are shown in Tables 2, 3 and 4. Figure 4 It can be seen that the use of the scheme of the present invention can appropriately improve the performance of the wheel rim, significantly improve the uniformity of the circumferential hardness of the rim, and make the rim structure more uniform and fine, which is very beneficial to improving the performance of the wheel. Table 5 shows the time required for heat treatment of the wheels of the embodiment and the comparative example. It is obvious that the heat treatment capacity of the embodiment 1 of the scheme of the present invention has been greatly improved.
[0053] Table 1 Main chemical compositions of wheels of embodiment and comparative example
[0054]
[0055] Table 2 Mechanical properties of wheel rims of the embodiment and the comparative example
[0056]
[0057] Table 3 Mechanical properties of wheel rims of the embodiments and comparative examples
[0058]
[0059] Table 4 Uniformity of circumferential hardness of wheel rims of the embodiment and the comparative example
[0060]
[0061]
[0062] Table 5 Yield comparison
[0063] Number of wheels heat treated per day / pieces Average time for a single wheel / min Example 1 1850 0.78 Comparative Example 1 900 1.6 Example 2 850 1.7 Comparative Example 2 400 3.6
[0064] Example 2
[0065] The wheel production process of this embodiment is electric furnace → LF furnace refining → RH furnace vacuum degassing → continuous casting → ingot cutting → upsetting → preforming → forming → slow cooling to room temperature → quenching and heating → quenching → high temperature tempering → machining → inspection. The outer diameter of the finished wheel is 1250mm, the rim thickness is 85mm, and the chemical composition of the wheel is as shown in Table 1 for wheel 1. Before quenching and heating, the double-layer drop-stomp method is used to enter the quenching and heating furnace, such as Figure 1 As shown, the wheel after falling is placed on the plum blossom pile, and the plum blossom pile moves along the annular heating furnace ( Figure 2 ) rotates counterclockwise, and the plum blossom pile rotates counterclockwise at a speed of 3 minutes per revolution. The wheel quenching heating temperature is 880±10℃, and after keeping warm for 2.5 hours, it is taken out of the furnace for quenching. Figure 3 The quenching is carried out as shown. The quenching adopts weak cooling + strong cooling heat treatment process, the weak cooling spray quenching time is 80s, the strong cooling spray quenching time is 480s, the water pressure is 0.1±0.01MPa, and the water output of the weak cooling water outlet is 10m 3 / h, the water output of the strong cooling water outlet is 22m 3 / h. After quenching, the wheels are put into the tempering furnace in a double-layer dropping way. The wheels are placed directly on the bottom of the furnace and rotate counterclockwise along the annular heating furnace at a certain speed. The tempering temperature is 500±10℃. After keeping warm for ≥5h, they are taken out of the furnace and air-cooled.
[0066] Comparative Example 2
[0067] The wheel production process of this comparative example is electric furnace → LF furnace refining → RH furnace vacuum degassing → continuous casting → ingot cutting → upsetting → preforming → forming → slow cooling to room temperature → quenching and heating → quenching → high temperature tempering → machining → inspection. The outer diameter of the finished wheel is 1250mm, the rim thickness is 85mm, and the chemical composition of the wheel is as shown in Wheel 1 in Table 1. The quenching and heating adopts a single-layer method to enter the quenching and heating furnace. The wheel is directly placed on the bottom of the furnace. As the furnace bottom rotates counterclockwise along the annular heating furnace, the wheel quenching and heating temperature is 880±10℃. After keeping warm for 3.5h, it is taken out of the furnace for quenching. The quenching is carried out by a single-piece single-layer heat treatment method. The quenching adopts a weak cooling + strong cooling heat treatment process. The weak cooling time is 80s, the strong cooling time is 480s, the water pressure is 0.1±0.01MPa, and the water output of the weak cooling outlet is 10m 3 / h, the water output of the strong cooling water outlet is 22m 3 / h. After quenching, the wheels are put into the tempering heating furnace in a single-piece and single-layer manner. The wheels are placed directly on the bottom of the furnace and rotated counterclockwise along the annular heating furnace at a certain speed. The tempering temperature is 480±10℃. After keeping warm for ≥5h, they are taken out of the furnace and air-cooled.
[0068] According to BS EN 13262 "Railway Applications - Wheelsets and Bogies - Wheels - Product Requirements", the tensile, impact, hardness analysis and rim residual application measurement were carried out on Example 2 and Comparative Example 2, the tensile test was carried out according to GB / T 228.1 "Metallic Materials Tensile Test Part 1: Room Temperature Test Method", the pendulum impact test was carried out at room temperature and -20°C according to GB / T 229 "Metallic Materials Charpy Pendulum Impact Test Method", and the hardness measurement was carried out according to GB / T231.1 "Metallic Brinell Hardness Test Part 1: Test Method". The performance of the wheel rims of Example 2 and Comparative Example 2 is shown in Tables 2, 3 and 4. It can be seen that the use of the scheme of the present invention can appropriately improve the performance of the wheel rim part, significantly improve the circumferential hardness uniformity of the rim, and is very beneficial to improving the performance of the wheel. Table 5 shows the time required for heat treatment of the wheels of the embodiment and comparative example. Obviously, the heat treatment capacity of Example 2 using the scheme of the present invention has been greatly improved.
[0069] The present invention is described above by way of example in conjunction with the accompanying drawings. Obviously, the specific implementation of the present invention is not limited to the above-mentioned methods. As long as various non-substantial improvements are made using the method concept and technical solution of the present invention; or the above concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A heat treatment method for a rail transit wheel, comprising the steps of: S1. The blank wheel is put into the quenching heating furnace for heating; S2, quenching; S3, tempering; It is characterized in that In step S1, the blank wheel enters the quenching and heating furnace in a double-layer dropping manner; during the rotation of the quenching and heating furnace, the blank wheel rotates simultaneously.
2. The heat treatment method for rail transit wheels according to claim 1, characterized in that: In the step S1, the quenching heating furnace and the blank wheel both rotate in a counterclockwise direction.
3. The heat treatment method for rail transit wheels according to claim 1, characterized in that: In the step S1, the heating temperature is 850-900°C.
4. The heat treatment method for rail transit wheels according to any one of claims 1 to 3, characterized in that: In the step S1, after the heating is completed, the temperature is kept warm, and the temperature keeping time is set to 1.5-2.5 hours.
5. The heat treatment method for rail transit wheels according to any one of claims 1 to 3, characterized in that: In step S3, the blank wheel enters the tempering heating furnace in a double-layer dropping manner.
6. The heat treatment method for rail transit wheels according to claim 5, characterized in that: In the step S3, the tempering temperature is 470-530°C.
7. The heat treatment method for rail transit wheels according to claim 5, characterized in that: In the step S3, after the tempering treatment is completed, the material is kept warm, and the holding time is set to be ≥5h.
8. The heat treatment method for rail transit wheels according to any one of claims 1 to 7, characterized in that: In the step S1, the blank wheel rotates at a speed of 3-5 minutes per rotation.
9. The heat treatment method for rail transit wheels according to any one of claims 1 to 7, characterized in that: In the step S2, a quenching and cooling device is used, and the quenching and cooling device includes a quenching table and nozzles, which are arranged in multiple layers, and all nozzles in each layer are evenly distributed around the outer side of the blank wheel along the circumferential direction.
10. The heat treatment method for rail transit wheels according to claim 9, characterized in that: The nozzle is provided with a weak cooling water outlet hole and a strong cooling water outlet hole. In step S2, the water output of the weak cooling water outlet hole is 8-10m 3 / h, the water output of the strong cooling water outlet is 18-24m 3 / h.
Citation Information
Patent Citations
Blank wheel capable of improving performance of wheel rim and production method of blank wheel
CN115805414A
Corrosion-resistant and wear-resistant wheel and production method thereof
CN115896632A
Heat treatment method and device for wheel-mounted brake disc
CN117385151A
Method for manufacturing a railway wheel and railway wheel so obtained
EP0884396A1