Al-Cr-Fe-Ti-Si lightweight high-entropy alloy and preparation method thereof

By introducing Si element and employing vacuum induction melting technology, the problems of performance and cost of lightweight materials were solved through the preparation of Al-Cr-Fe-Ti-Si lightweight high-entropy alloy, thus realizing the preparation of high-performance, low-cost lightweight high-entropy alloy.

CN118957385APending Publication Date: 2024-11-15KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411086605.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing lightweight materials have limited performance and high manufacturing costs. Traditional preparation methods result in significant losses of low-melting-point materials, which restricts the development of lightweight high-entropy alloys.

Method used

A lightweight high-entropy alloy of Al-Cr-Fe-Ti-Si is used, and Si element is introduced for solid solution strengthening, grain refinement strengthening and second phase strengthening. The alloy is prepared by vacuum induction melting technology to avoid the use of low melting point elements and expensive metals, and to control the melting process to reduce impurities and oxidation.

Benefits of technology

A high-strength, high-hardness alloy with a density of less than 5 g/cm3 was prepared. It has excellent comprehensive performance and low cost, and is suitable for wear-resistant and high-temperature applications. The vacuum induction melting technology improves the purity and stability of the alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004985354200000061
    Figure BDA0004985354200000061
Patent Text Reader

Abstract

The embodiment of the invention discloses an Al-Cr-Fe-Ti-Si light high-entropy alloy and a preparation method of the Al-Cr-Fe-Ti-Si light high-entropy alloy. The Al-Cr-Fe-Ti-Si light high-entropy alloy has the following molecular formula: AlaCrFeTiSib, a is more than or equal to 0.5 and less than or equal to 2, and b is more than 0 and less than or equal to 2. The Al-Cr-Fe-Ti-Si alloy provided by the embodiment of the invention has the density of 3.93-4.56 g / cm < 3 >, meets the light high-entropy alloy standard, has high-strength and high-hardness comprehensive mechanical properties and excellent chemical properties, and has outstanding advantages compared with traditional metal materials and other system high-entropy alloys.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present invention relate to the technical field of high entropy alloy materials, and specifically to an Al-Cr-Fe-Ti-Si lightweight high entropy alloy and a preparation method thereof. Background Art

[0002] Weight reduction remains the most cost-effective means of reducing fuel consumption and greenhouse gas emissions in the transport sector. It has been calculated that for every 10% reduction in the total weight of a vehicle, fuel consumption will decrease by 7%, which means that for every 1kg of weight reduction in a vehicle, approximately 20kg of CO2 will be saved. 2 The limited performance and high manufacturing costs of existing lightweight materials restrict their further development. Therefore, it is necessary to develop new lightweight alloys with low cost and able to meet performance requirements.

[0003] Compared with traditional alloys, high entropy alloys are composed of multiple main elements, and the elements work synergistically, which gives them characteristic effects such as high mixing entropy, lattice distortion, slow atomic diffusion and "cocktail", and generally have simple phase structures and excellent properties, such as high strength, high hardness, wear resistance, corrosion resistance and high temperature oxidation resistance. The lightweighting of high entropy alloys is a new development direction of lightweight alloy materials, which has important academic research value and huge engineering application potential. Lightweight high entropy alloys are defined as having a density of less than 6g cm -3 High entropy alloys are equiatomic or nearly equiatomic alloys composed of at least five elements. Low-density elements, such as Al, Mg, Li, Ti, and Si, are key ingredients in the design of these alloys, resulting in reduced overall density and improved performance.

[0004] Existing studies, such as Al 20 Be 20 Fe 10 Ti 35 Si 15 The density of the lightweight high entropy alloy is 3.91 g cm -3 , with a hardness of 911HV, higher than quartz, and its hardness and hardness-to-density ratio are the highest among all light alloys reported previously. In addition, it has excellent oxidation resistance at 700℃ and 900℃, far exceeding the traditional Ti-6Al-4V alloy. Al 2 CrFeTiMn lightweight high-entropy alloys, prepared by mechanical alloying followed by subsequent casting, have excellent mechanical properties, which, together with their reduced weight and cost, have high potential for wear-resistant and high-temperature applications.

[0005] At present, most lightweight high-entropy alloys are prepared by arc melting. Since arc heating can reach very high temperatures in an instant, it causes a large loss of low-melting-point materials. Therefore, it is urgent to develop a lightweight high-entropy alloy and its preparation method that is superior in strength, hardness, cost and other aspects. Summary of the invention

[0006] To this end, an embodiment of the present invention provides an Al-Cr-Fe-Ti-Si lightweight high entropy alloy and a preparation method thereof. The present invention selects to retain the Al-Cr-Fe-Ti alloy system and introduces a low-cost metal-like Si element to obtain a high-performance new lightweight high-entropy alloy.

[0007] In order to achieve the above purpose, the embodiment of the present invention provides the following technical solutions:

[0008] According to a first aspect of an embodiment of the present invention, the present invention provides an Al-Cr-Fe-Ti-Si lightweight high entropy alloy having the following molecular formula: Al a CrFeTiSi b , where 0.5≤a≤2, 0<b≤2.

[0009] The present invention finds that by introducing metal-like Si elements to induce strengthening mechanisms such as solid solution strengthening, grain refinement strengthening, and second phase strengthening in the Al-Cr-Fe-Ti-Si lightweight high entropy alloy, the comprehensive properties of the high entropy alloy are improved.

[0010] According to a second aspect of an embodiment of the present invention, the present invention provides a method for preparing the Al-Cr-Fe-Ti-Si light high entropy alloy as described above, wherein Al, Cr, Fe, Ti, and Si single metals are prepared according to the molecular formula Al a CrFeTiSi b The atomic ratios of the elements are prepared, mixed, and subjected to vacuum induction melting.

[0011] Furthermore, the purity of the Al, Cr, Fe, Ti, and Si single metals is greater than 99.99%.

[0012] Furthermore, the vacuum induction melting conditions are: vacuum degree 1×10 -4 Order of magnitude, melting temperature 1800℃, melting time 30min.

[0013] Furthermore, the method comprises the following steps:

[0014] (1) Ingredients: Use an electronic balance to accurately weigh high-purity single metals of Al, Cr, Fe, Ti, and Si with a purity higher than 99.99%. a CrFeTiSi b preparing a raw material;

[0015] (2) Melting: The raw materials prepared in step (1) are placed in a graphite crucible in the order of melting point from low to high, and then placed in a vacuum induction furnace. The induction furnace is evacuated to 1×10 -4 Magnitude, vacuum induction melting;

[0016] (3) Casting: The high entropy alloy melt obtained by smelting in step (2) is cast into a specified water-cooled copper mold, cooled in a vacuum environment, and finally a high entropy alloy ingot of a specific size is obtained.

[0017] The embodiments of the present invention have the following advantages:

[0018] 1. The present invention provides a method for preparing a novel AlCrFeTiSi series lightweight high entropy alloy with Si element added, which does not use low melting point elements, Li, Mg and Zn and overly expensive Sc, but uses oxidation-resistant Al and Si and cheap Fe together with Ti to adjust the properties of the high entropy alloy. The density of the alloy is less than 5g / cm 3 , meeting the standards of lightweight high entropy alloys.

[0019] 2. The present invention introduces metallic Si elements to induce strengthening mechanisms such as solid solution strengthening, fine grain strengthening, and second phase strengthening in the Al-Cr-Fe-Ti-Si lightweight high entropy alloy, thereby improving the comprehensive performance of the high entropy alloy. The prepared lightweight high entropy alloy has a density lower than that of titanium alloy, comprehensive mechanical properties of high strength and hardness, and excellent chemical properties, which has outstanding advantages over traditional metal materials and other system high entropy alloys.

[0020] 3. The main elements of the high entropy alloy selected in the present invention, Al, Cr, Ti, Fe, and Si, are all common and widely used metals with low raw material costs.

[0021] 4. Compared with vacuum arc melting preparation technology, the present invention selects vacuum induction melting, which has the advantage of helping to remove gases and impurities in the molten metal, which is especially beneficial for metals and alloys that are sensitive to pollution, such as titanium, zirconium and high-temperature alloys. In addition, vacuum induction melting helps to reduce the oxidation of the molten metal, which is very important for easily oxidized metals such as aluminum, copper and magnesium. The use of a high vacuum environment and an induction coil can better control the melting process, which can achieve precise temperature control, reduce stirring and pollution, and thus produce a more stable high-entropy alloy product. DETAILED DESCRIPTION

[0022] The following is a description of the implementation of the present invention by specific embodiments. People familiar with the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Example 1

[0024] This embodiment provides an Al-Cr-Fe-Ti-Si lightweight high entropy alloy, and the preparation method thereof comprises the following steps:

[0025] (1) Use a high-precision electronic balance (with an accuracy of ±0.001g) to accurately weigh Al, Cr, Fe, Ti, and Si elemental metals with a purity higher than 99.99%, and calculate the molar ratio of Al 1.5 CrFeTiSi x (x=0.5) to prepare the raw materials; before smelting, the metal raw materials need to be immersed in anhydrous ethanol and cleaned by ultrasonic oscillation to remove the oil and oxide scale on the surface, and finally the prepared raw materials are dried for use;

[0026] (2) placing the alloy raw materials prepared in step (1) in a graphite crucible or a corundum crucible, with the element with the lowest melting point at the bottom and the element with the highest melting point at the top; before melting, evacuate the vacuum induction melting furnace to 1×10 -4 The furnace chamber is purged twice with high-purity argon gas, and filled with high-purity argon gas for the third time to provide a protective gas atmosphere;

[0027] (3) Turn on the current of the vacuum induction melting furnace, set the melting temperature to 1800°C, and the melting time to 30 minutes; perform program temperature control and start vacuum induction heating; after melting to the highest temperature, keep the temperature for 1 to 2 hours to fully melt the main element of the alloy; under the stirring action of the eddy current formed by electromagnetic induction, the alloy composition is more uniform;

[0028] (4) casting the high entropy alloy melt obtained by smelting in step (3) into a water-cooled copper mold or graphite mold of a specified size placed in advance; turning off the power supply and cooling to room temperature under vacuum; finally obtaining a high entropy alloy ingot of a specific size;

[0029] (5) The high entropy alloy ingot obtained in step (4) is processed into a suitable size by a cutting machine. The cut samples are successively cut with 240-2000 # SiC water sandpaper is polished step by step until each surface is bright, then immersed in anhydrous ethanol for ultrasonic oscillation cleaning, and placed in a sample bag for later use after drying.

[0030] Example 2

[0031] This embodiment provides an Al-Cr-Fe-Ti-Si lightweight high entropy alloy, and the preparation method thereof comprises the following steps:

[0032] (1) Use a high-precision electronic balance (with an accuracy of ±0.001g) to accurately weigh Al, Cr, Fe, Ti, and Si elemental metals with a purity higher than 99.99%, and calculate the molar ratio of Al 1.5 CrFeTiSi x (x=1) to prepare the raw materials; before smelting, the metal raw materials need to be immersed in anhydrous ethanol and cleaned by ultrasonic oscillation to remove the oil and oxide scale on the surface, and finally the prepared raw materials are dried for use;

[0033] (2)~(5) are the same as Example 1.

[0034] Example 3

[0035] This embodiment provides an Al-Cr-Fe-Ti-Si light high entropy alloy, and the preparation method thereof comprises the following steps:

[0036] (1) Use a high-precision electronic balance (accuracy up to ±0.001g) to accurately weigh Al, Cr, Fe, Ti, and Si elemental metals with a purity higher than 99.99%, and calculate the molar ratio of Al 1.5 CrFeTiSi x (x=1.5) to prepare the raw materials; before smelting, the metal raw materials need to be immersed in anhydrous ethanol and cleaned by ultrasonic oscillation to remove the oil and oxide scale on the surface, and finally the prepared raw materials are dried for use;

[0037] (2)~(5) are the same as Example 1.

[0038] Example 4

[0039] This embodiment provides an Al-Cr-Fe-Ti-Si light high entropy alloy, and the preparation method thereof comprises the following steps:

[0040] (1) Use a high-precision electronic balance (accuracy up to ±0.001g) to accurately weigh Al, Cr, Fe, Ti, and Si elemental metals with a purity higher than 99.99%, and calculate the molar ratio of Al 1.5 CrFeTiSi x (x=2) to prepare the raw materials; before smelting, the metal raw materials need to be immersed in anhydrous ethanol and cleaned by ultrasonic oscillation to remove the oil and oxide scale on the surface, and finally the prepared raw materials are dried for use;

[0041] (2)~(5) are the same as Example 1.

[0042] Comparative Example 1

[0043] This comparative example provides an Al-Cr-Fe-Ti lightweight high entropy alloy, and the preparation method thereof comprises the following steps:

[0044] (1) Use a high-precision electronic balance (with an accuracy of ±0.001g) to accurately weigh Al, Cr, Fe, and Ti metals with a purity higher than 99.99%, and calculate the molar ratio of Al 1.5 CrFeTi is prepared to obtain raw materials; before smelting, the metal raw materials need to be immersed in anhydrous ethanol and cleaned by ultrasonic oscillation to remove oil and oxide scale on the surface, and finally the prepared raw materials are dried for use;

[0045] (2)~(5) are the same as Example 1.

[0046] Test Case

[0047] Performance Testing

[0048] Density: The density of high entropy alloy ingots was measured by Archimedes drainage method.

[0049] Vickers hardness: The hardness is tested using a Vickers hardness tester at a load of 1 kgf and a loading time of 10 s.

[0050] Strength: According to the requirements of GB228.1-2021, tensile specimens were obtained by mechanical processing, and tensile properties were tested by electronic universal testing machine. The axial loading rate was set to 1×10 -3 , Each group of high entropy alloys was measured at least three times to ensure the accuracy of the experiment.

[0051] Specific hardness: the ratio of Vickers hardness to density.

[0052] Specific strength: the ratio of strength to density.

[0053] Oxidation resistance: The oxidation resistance of the samples in air was determined by measuring the weight gain of the samples after annealing in an air furnace at 900°C for 10, 50, 100 and 150 h.

[0054] The test results of the alloys of Examples 1-4 and Comparative Example 1 are shown in Table 1 below.

[0055] Table 1

[0056]

[0057] The results show that the density of the Al-Cr-Fe-Ti-Si alloy provided in the embodiment of the present invention is 3.93-4.56 g / cm 3It meets the standards of lightweight high-entropy alloys, and at the same time has comprehensive mechanical properties of high strength and hardness, and excellent chemical properties. It has outstanding advantages over traditional metal materials and other system high-entropy alloys.

[0058] Although the present invention has been described in detail above by general description and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements can be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all belong to the scope of protection claimed by the present invention.

Claims

1. An Al-Cr-Fe-Ti-Si lightweight high entropy alloy, characterized in that: Has the following molecular formula: Al a CrFeTiSi b , where 0.5≤a≤2, 0<b≤2.

2. The method for preparing the Al-Cr-Fe-Ti-Si lightweight high entropy alloy according to claim 1, characterized in that: Al, Cr, Fe, Ti, Si single metals are divided into a CrFeTiSi b The atomic ratios of the elements are prepared, mixed, and subjected to vacuum induction melting.

3. The method for preparing the Al-Cr-Fe-Ti-Si light high entropy alloy according to claim 2, characterized in that: The purity of the Al, Cr, Fe, Ti and Si single metals is greater than 99.99%.

4. The method for preparing the Al-Cr-Fe-Ti-Si light high entropy alloy according to claim 2, characterized in that: The vacuum induction melting conditions are: vacuum degree 1×10 -4 Order of magnitude, melting temperature 1800℃, melting time 30min.

5. The method for preparing the Al-Cr-Fe-Ti-Si light high entropy alloy according to claim 2, characterized in that: The method comprises the following steps: (1) Ingredients: Use an electronic balance to accurately weigh high-purity single metals of Al, Cr, Fe, Ti, and Si with a purity higher than 99.99%. a CrFeTiSi b preparing a raw material; (2) Melting: The raw materials prepared in step (1) are placed in a graphite crucible in the order of melting point from low to high, and then placed in a vacuum induction furnace. The induction furnace is evacuated to 1×10 -4 Magnitude, vacuum induction melting; (3) Casting: The high entropy alloy melt obtained by smelting in step (2) is cast into a specified water-cooled copper mold, cooled in a vacuum environment, and finally a high entropy alloy ingot of a specific size is obtained.

Citation Information

Cited By

  • Lightweight high-entropy alloy, preparation method, component and terminal product

    CN122609931A