Production method of low-cost Ti alloyed X42M pipeline steel plate for export

Through the process of combining Ti microalloy refined grains and multi-process, the problem of high cost of Nb and Mo alloyed X42M pipeline steel in the prior art is solved, and the production of low-cost X42M pipeline steel plates is realized, which improves product profitability. and competitiveness.

CN118957407AActive Publication Date: 2024-11-15BAOTOU IRON & STEEL (GROUP) CO LTD

Patent Information

Application Number
CN202410974921.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-15
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

In the prior art, the production method of Nb and Mo alloyed X42M pipeline steel is relatively expensive, and it is difficult to reduce production costs while ensuring product performance.

Method used

Ti microalloy is used to refine the grains, and control process parameters such as temperature through converter, LF refining, continuous casting, heating, rolling mill, straightening and flaw detection processes combined with the use of aluminum, ferrosilicon, ferromanganese and ferrotitanium alloys. and time to ensure that the chemical composition and performance of the steel plate complies with API Spec 5L 46th standard.

Benefits of technology

While ensuring product performance, it greatly reduces production costs, reduces the cost per ton of steel by more than 400 yuan, and improves the profitability of the product and the competitiveness of the foreign market.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957407A_ABST
    Figure CN118957407A_ABST
Patent Text Reader

Abstract

The invention discloses a production method of a low-cost exported Ti alloyed X42M pipeline steel plate. The production method comprises the following steps: (1) a converter process; (2) an LF refining procedure; (3) a continuous casting process; (4) heating; (5) rolling mill working procedure; (6) straightening; (7) flaw detection; the X42M pipeline steel plate comprises the following chemical components in percentage by weight: 0.05 to 0.08 percent of C, 0.10 to 0.30 percent of S i, 1.30 to 1.50 percent of Mn, less than or equal to 0.015 percent of P, less than or equal to 0.005 percent of S, 0.015 to 0.030 percent of T i, 0.020 to 0.050 percent of A l and the balance of Fe and inevitable impurities. According to the invention, grains are refined through Ti microalloying, so that the production cost is greatly reduced while the product performance is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron and steel metallurgy, and in particular relates to a method for producing a low-cost Ti alloyed X42M pipeline steel plate for export. Background Art

[0003] Patent CN 110735084 A discloses a pipeline steel X42M hot-rolled steel strip and its preparation method, and patent CN112111689 A discloses a hot-rolled steel strip for export with Nb+Mo composition X42M pipeline steel and its preparation process. Both inventions use Nb and Mo alloying, which greatly improves the production cost. Summary of the invention

[0004] The purpose of the present invention is to provide a low-cost production method of Ti alloyed X42M pipeline steel plate for export. By refining the grains through Ti microalloying, the product meets the requirements of API Spec 5L 46th standard, and the production cost is greatly reduced while ensuring the product performance.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] The present invention discloses a method for producing a low-cost Ti alloyed X42M pipeline steel plate for export, comprising:

[0007] (1) Converter process: oxygen blowing decarburization, slag making and dephosphorization in converter, converter tapping temperature ≥ 1620°C, and ferroaluminum, ferrosilicon and ferromanganese are added during converter tapping for deoxidation and alloying;

[0008] (2) LF refining process: LF refining slag desulfurization, and adding aluminum iron, silicon iron, manganese iron, titanium iron alloy. After the LF treatment, calcium treatment is carried out, and the soft blowing time is guaranteed to be more than 8 minutes after calcium treatment;

[0009] (3) Continuous casting process: The casting machine adopts constant casting speed control, and the casting speed is controlled at 1.0-1.5 m / min;

[0010] (4) Heating process: heating temperature ≥ 1180°C, furnace time ≥ 180 minutes;

[0011] (5) Rolling mill process: The rolling process adopts two processes: rough rolling and finishing rolling. The starting rolling temperature of rough rolling is ≥1150℃, the final rolling temperature of rough rolling is ≥1100℃, the starting rolling temperature of finishing rolling is ≤1000℃, and the final rolling temperature of finishing rolling is 830-860℃. After rolling, ACC cooling is adopted, and the cooling temperature is 500-560℃.

[0012] (6) Straightening process: straightening temperature ≥ 500°C, steel plate straightness ≤ 12 mm / m;

[0013] The chemical composition of the X42M pipeline steel plate is C: 0.05-0.08%, Si: 0.10-0.30%, Mn: 1.30-1.50%, P: ≤0.015%, S: ≤0.005%, Ti: 0.015-0.030%, Al: 0.020-0.050%, and the balance is Fe and unavoidable impurities.

[0014] Furthermore, it also includes: (7) NDT process: the NDT is carried out by scanning and judging in accordance with the provisions of EN10160 standard, the delamination inspection coverage accounts for 100% of the steel plate surface, and there is no delamination defect within 50mm of the longitudinal plate edge of the steel plate.

[0015] Furthermore, the chemical composition of the X42M pipeline steel plate is C: 0.060%, Si: 0.20%, Mn: 1.35%, P: 0.013%, S: 0.005%, Ti: 0.020%, Al: 0.035%, and the balance is Fe and unavoidable impurities.

[0016] Furthermore, the chemical composition of the X42M pipeline steel plate is C: 0.065%, Si: 0.115%, Mn: 1.40%, P: 0.013%, S: 0.004%, Ti: 0.020%, Al: 0.040% by weight, and the balance is Fe and unavoidable impurities.

[0017] Furthermore, the elongation of the produced X42M pipeline steel plate is ≥25%.

[0018] Furthermore, the produced X42M pipeline steel plate has excellent strength and low-temperature toughness.

[0019] Compared with the prior art, the beneficial technical effects of the present invention are:

[0020] The X42M pipeline steel plate of the present invention refines the grains through Ti microalloying, which greatly reduces the production cost while ensuring product performance. Compared with the design of Nb and Mo components, the cost per ton of steel is reduced by more than 400 yuan. In the context that steel products no longer enjoy export tax rebate dividends, the profitability of the product and the competitiveness in foreign markets are greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The present invention will be further described below in conjunction with the accompanying drawings.

[0022] Figure 1 This is the organization of Example 1 of the present invention. DETAILED DESCRIPTION

[0023] The present invention will be further described in detail below in conjunction with specific examples. These examples are merely descriptions of the best mode of carrying out the present invention and do not limit the scope of the present invention in any way.

[0024] Examples 1-2 are the chemical compositions and process parameters used in the X42M pipeline steel plate of the present invention. The chemical compositions of the embodiments and comparative examples are shown in Table 1; the process parameters are shown in Table 2; and the mechanical properties are shown in Table 3.

[0025] Table 1 Chemical composition of each embodiment and comparative example (%)

[0026]

[0027]

[0028] Table 2 Process parameters

[0029]

[0030] Table 3 Mechanical properties

[0031]

[0032]

[0033] It can be seen from the above table that the performance of the embodiment and the comparative example is basically the same, but compared with the comparative example, the alloy cost of the embodiment is greatly reduced, which greatly improves the profitability of the product and the competitiveness in the foreign market.

[0034] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for producing low-cost Ti alloyed X42M pipeline steel plate for export, characterized in that: include: (1) Converter process: oxygen blowing decarburization, slag making and dephosphorization in converter, converter tapping temperature ≥ 1620°C, and ferroaluminum, ferrosilicon and ferromanganese are added during converter tapping for deoxidation and alloying; (2) LF refining process: LF refining slag desulfurization, and adding aluminum iron, silicon iron, manganese iron, titanium iron alloy. After the LF treatment, calcium treatment is carried out, and the soft blowing time is guaranteed to be more than 8 minutes after calcium treatment; (3) Continuous casting process: The casting machine adopts constant casting speed control, and the casting speed is controlled at 1.0-1.5 m / min; (4) Heating process: heating temperature ≥ 1180°C, furnace time ≥ 180 minutes; (5) Rolling mill process: The rolling process adopts two processes: rough rolling and finishing rolling. The starting rolling temperature of rough rolling is ≥1150℃, the final rolling temperature of rough rolling is ≥1100℃, the starting rolling temperature of finishing rolling is ≤1000℃, and the final rolling temperature of finishing rolling is 830-860℃. After rolling, ACC cooling is adopted, and the cooling temperature is 500-560℃. (6) Straightening process: straightening temperature ≥ 500°C, steel plate straightness ≤ 12 mm / m; The chemical composition of the X42M pipeline steel plate is C: 0.05-0.08%, Si: 0.10-0.30%, Mn: 1.30-1.50%, P: ≤0.015%, S: ≤0.005%, Ti: 0.015-0.030%, Al: 0.020-0.050%, and the balance is Fe and unavoidable impurities.

2. The method for producing low-cost Ti alloyed X42M pipeline steel plate for export according to claim 1, characterized in that: Also includes: (7) NDT process: The NDT shall be carried out in accordance with the provisions of EN10160 standard. The delamination inspection coverage shall account for 100% of the steel plate surface, and there shall be no delamination defects within 50 mm of the longitudinal edge of the steel plate.

3. The method for producing low-cost Ti alloyed X42M pipeline steel plate for export according to claim 1, characterized in that: The chemical composition of the X42M pipeline steel plate is C: 0.060%, Si: 0.20%, Mn: 1.35%, P: 0.013%, S: 0.005%, Ti: 0.020%, Al: 0.035% by weight, and the balance is Fe and unavoidable impurities.

4. The method for producing low-cost Ti alloyed X42M pipeline steel plate for export according to claim 1, characterized in that: The chemical composition of the X42M pipeline steel plate is C: 0.065%, Si: 0.115%, Mn: 1.40%, P: 0.013%, S: 0.004%, Ti: 0.020%, Al: 0.040% by weight, and the balance is Fe and unavoidable impurities.

5. The method for producing low-cost Ti alloyed X42M pipeline steel plate for export according to claim 1, characterized in that: The elongation of the produced X42M pipeline steel plate is ≥25%.

6. The method for producing low-cost Ti alloyed X42M pipeline steel plate for export according to claim 1, characterized in that: The produced X42M pipeline steel plate has excellent strength and low-temperature toughness.

Citation Information

Patent Citations

  • Pipeline steel X42M hot-rolled steel strip and preparation method thereof

    CN110735084A

  • Hot rolled steel strip for Nb+Mo component system X42M pipeline steel for export and preparation process of hot rolled steel strip

    CN112111689A

  • Micro-alloying steel for oil gas transport seamless pipeline and its preparation method

    CN101186994A

  • Large-wall-thickness X52MS acid-resistant pipeline steel plate produced by LF-RH refining process and manufacturing method thereof

    CN110295320A

  • Production method of extremely-low-cost manganese-containing thin-specification exported pipeline steel

    CN111793765A

Cited By

  • Method for producing a peritectic carbon tube line steel x42m

    CN122855986A