Humidity sensor, intelligent integrated respiration monitoring mask based on humidity sensor, method and application

Through the fluorinated polyimidine-based laser-induced graphene humidity sensor and intelligent breath monitoring mask based on drip-coated GO, the problems of poor shape adaptability of existing humidity sensors and low sensitivity of breath monitoring equipment are solved, and flexible and high sensitivity are achieved. Humidity detection and breath monitoring functions.

CN118961822APending Publication Date: 2024-11-15TIANJIN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410867593.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing humidity sensors mostly use rigid materials, which leads to poor shape adaptability and easily leads to material degradation in high humidity environments; traditional respiratory monitoring equipment has low sensitivity and low integration.

Method used

Using a fluorinated polyimide-based laser-induced graphene (F-LIG/GO) humidity sensor based on drop-coated GO, intelligent development is developed by preparing porous carbon interdigital electrodes and graphene oxide, combined with electronic components such as microcontrollers and WIFI modules. Integrated breath monitoring mask enables flexible, sensitive and highly integrated humidity sensing and breath monitoring.

Benefits of technology

It realizes high sensitivity humidity detection based on ensuring flexibility, has good linearity and stability, can monitor respiratory status in real time and alarm for respiratory arrest, solving the problems of bulky and low sensitivity of traditional equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118961822A_ABST
    Figure CN118961822A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of materials and electronic information, and discloses a preparation method of a humidity sensor based on GO dispensing fluorinated polyimide-based laser-induced graphene (F-LIG / GO), an assembly method of an intelligent integrated respiration monitoring mask based on the F-LIG / GO humidity sensor and APP function development. The F-LIG / GO humidity sensor based on the fluorinated PI has extremely high sensitivity and detection accuracy to water molecules on the basis of ensuring the flexibility, has good linearity of capacitance change in a humidity range, shows excellent humidity sensitivity in the aspects of response / recovery time, repeatability, hysteresis and the like, and gives full play to the advantages of the humidity sensor. After the integrated breathing monitoring equipment is applied to the integrated breathing monitoring mask, the integrated programming enables the breathing monitoring equipment to be light and small, real-time breathing behavior monitoring and breathing arrest alarming can be carried out on a user through an APP, and breathing monitoring is more convenient and economical.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of materials and electronic information technology, and in particular to a humidity sensor based on fluorinated polyimide-based laser-induced graphene F-LIG / GO coated with GO, an intelligent integrated respiratory monitoring mask based on the F-LIG / GO humidity sensor, and a method and application thereof. Background Art

[0002] Many respiratory diseases are transmitted through viruses. Breathing is one of the important physiological activities of the human body. About 63% of the water in the human body can be released through breathing. Therefore, detecting the water content in exhaled gas is a very effective way to achieve respiratory monitoring. Data such as breathing frequency and breathing intensity can reflect a lot of human health information. Respiratory monitoring can help diagnose respiratory diseases such as sleep apnea syndrome, pulmonary asthma, and chronic obstructive pulmonary disease. Traditional respiratory monitoring requires the connection of large medical equipment, which is expensive, limits the patient's range of activities, and is not conducive to daily use at home; and traditional humidity sensors are mostly based on rigid materials such as ceramics, silicon or silicon dioxide. Electronic devices with such rigid substrates cannot be bent, which greatly limits their application in human body detection. Therefore, the development of an intelligent integrated wireless respiratory monitoring device based on a flexible substrate humidity sensor has become a new research hotspot.

[0003] Humidity-sensitive materials are the core components of humidity sensors and largely determine the performance of humidity sensors. As an excellent new carbon-based material, graphene oxide GO has abundant hydrophilic groups that give it excellent dispersibility and humidity-sensitive properties. Its special lattice structure makes it very flexible, and its preparation method is simple and low-cost. It exhibits high proton conductivity under the action of water molecules. In addition, LIG ​​has the advantages of lower cost, no special requirements for the processing environment, and one-step patterned preparation without a mask. At the same time, fluorinated polyimide has a rich carbon content. When the local temperature rises sharply due to laser irradiation, it can break the CO, C=O and NO bonds, so that the C atoms recombine and combine to form a graphene layer; and when the laser is hit, part of the fluorine-containing gas will overflow, which can play a role in pore formation, increasing the area covered by GO, so that it has more water molecule adsorption sites. In addition, fluorinated polyimide has high mechanical strength, good acid and alkali resistance and wear resistance, and is an excellent candidate material for laser-induced graphene precursors. Therefore, the humidity sensor based on fluorinated PI LIG and GO humidity-sensitive materials has extremely high sensitivity and detection accuracy to water molecules while ensuring flexibility, and has good linearity in capacitance changes within the humidity range. It also exhibits excellent humidity-sensitive properties in terms of response / recovery time, repeatability, hysteresis, etc., giving full play to the advantages of humidity sensors.

[0004] At present, the humidity sensor in the prior art has the following defects:

[0005] 1. Most of the existing humidity sensors are based on rigid materials such as ceramics, silicon or silicon dioxide. Such rigid substrates cannot be bent, are not flexible, and have poor shape adaptability when integrated into different devices.

[0006] 2. Currently, long-term exposure to high humidity or long-term use usually causes excessive adsorption of water molecules on the sensor's moisture-sensitive material, leading to device degradation or failure.

[0007] 3. The common respiratory monitoring equipment on the market currently has the disadvantages of poor sensitivity and low integration. Summary of the invention

[0008] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a humidity sensor based on fluorinated polyimide-based laser-induced graphene F-LIG / GO with drop-coated GO, an intelligent integrated respiratory monitoring mask based on the F-LIG / GO humidity sensor, a method and an application.

[0009] The technical solution adopted by the present invention to solve its technical problem is:

[0010] A humidity sensor based on fluorinated polyimide-based laser-induced graphene F-LIG / GO drop-coated GO, the preparation method of which comprises the following steps:

[0011] Step 1, place TPE-Q in a three-necked flask, add DMAC, and mechanically stir until it is completely dissolved, then add 6FDA and BPADA into the three-necked flask in three batches, and mechanically stir to obtain a polyamic acid PAA solution;

[0012] Step 2: The PAA solution is allowed to stand to remove bubbles, then poured onto a pre-cleaned glass plate, scraped into a film of uniform thickness, and the solvent is evaporated, and then a step-by-step thermal imidization is performed, followed by natural cooling, and the glass plate is placed in deionized water, and dried after natural shedding to obtain an F-PI film;

[0013] Step 3, graphite powder, (NH4)2S2O8 and P2O5 are successively placed in H2SO4 solution, followed by heating and stirring;

[0014] Step 4, washing the mixture with deionized water until the pH value of the filtrate becomes neutral, and drying the filtered solid under vacuum to obtain pre-oxidized graphite;

[0015] Step 5, placing the pre-oxidized graphite in a H2SO4 solution in an ice water bath and stirring, slowly adding potassium permanganate, and continuously heating the mixture in a gradient manner;

[0016] Step 6, after cooling to room temperature, adding deionized water and H2O2 solution to terminate the reaction, washing the mixture with HCl solution, and washing with deionized water until neutral to remove residual metal ions;

[0017] Step 7, after the washed mixture is subjected to ultrasonic treatment at low temperature, the obtained graphene oxide dispersion is taken out with a pipette, placed in an oven and dried until completely dry, and then weighed to prepare a GO solution;

[0018] Step 8: Cut the prepared PI sample into rectangles as a substrate, and then fix it on A4 paper with transparent tape. Use a semiconductor laser to perform laser direct writing on the F-PI film in an atmospheric atmosphere to obtain F-LIG interdigital electrodes.

[0019] Step 9: Apply conductive silver paste to the connection between the copper wire and the interdigital electrode, and finally use a pipette to drop the GO solution on the interdigital electrode. Place the device in a fume hood and dry it naturally under indoor conditions to form a uniform GO film, and finally obtain a humidity sensor based on drop-coated GO fluorinated polyimide-based laser-induced graphene (F-LIG / GO).

[0020] Furthermore, the ratio of the mass of DMAC added in step 1 to the total mass of the remaining monomers is 17:3, the ratio of the total molar amount of 6FDA and BPADA to the molar amount of TPE-Q is 1:1, and they are added in three batches at an interval of 10 minutes each, and mechanically stirred for 4 hours to obtain a PAA solution with a solid content of 15%;

[0021] Furthermore, in step 2, the standing time is 12 h, the scraper distance is set to 200 μm, and the volatilization is performed at 80°C for 2 h; the step-by-step heating steps are as follows: 100°C for 1 h, 200°C for 1 h, and 250°C for 1 h. By controlling the amount of 6FDA, F with different fluorination degrees can be obtained. x -PI (x is the mole fraction of 6FDA in the anhydride, 0, 25, 50, 75, 100%) films.

[0022] Furthermore, in step 3, 2 g of 325 mesh graphite powder was used, the mass concentration of the H2SO4 solution was 98%, and the mixture was heated to 80°C and stirred for 4 h; the ratio of graphite powder: (NH4)2S2O8: P2O5: H2SO4 solution g:g:g:mL was 2:2:2:10;

[0023] Alternatively, in step 4, dry under vacuum for 2 h.

[0024] Furthermore, in step 5, the mass concentration of the H2SO4 solution is 98%; the continuous gradient heating step is as follows: heating at 35°C for 2 hours, then heating to 95°C for 30 minutes; the ratio of pre-oxidized graphite: H2SO4 solution: potassium permanganate is 0.6:24:3 in g:mL:g;

[0025] Alternatively, in step 6, the mass concentration of the H2O2 solution is 30%, the HCl solution is an HCl solution with a volume ratio of HCl: water of 1:10, and the number of washing times of the HCl solution washing mixture is 4 times; the ratio of pre-oxidized graphite: deionized water: H2O2 solution g: mL: mL is 0.6:200:6.

[0026] Furthermore, in step 7, the low temperature is 0°C, the ultrasonic frequency is 10 kHz for 2 h, 5 mL of the graphene oxide dispersion is taken out with a pipette, and the temperature of the oven is controlled at 50°C during drying; the concentration of the dispersion is calculated by weighing, and GO solutions of 1, 2, and 4 mg / mL are prepared.

[0027] Furthermore, the wavelength of the semiconductor laser used in step 8 is 450 nm, the maximum power is 7 W, the laser power is set to 1.4 W, and the scanning speed is set to a fixed value of 100 mm / s. x -The pattern size of LIG interdigitated electrodes is 8 mm*12 mm, where x is the mole fraction of 6FDA in the anhydride, i.e., 0, 25, 50, 75, and 100%;

[0028] Alternatively, in step 9, the amount of GO solution applied by a pipette is 100 μL, and the natural drying time is 1 day.

[0029] The use of humidity sensors in integrated respiratory monitoring masks as described above,

[0030] The intelligent integrated respiratory monitoring mask made by using the humidity sensor as described above, the assembly method of the intelligent integrated respiratory monitoring mask comprises the following steps:

[0031] The F-LIG / GO humidity sensor is placed inside the breathing mask and then connected to the AD converter, microcontroller, WIFI module, voltage regulator module and lithium battery through wires. After programming, all the above electronic components are integrated and placed outside the breathing mask.

[0032] The functional APP of the intelligent integrated respiratory monitoring mask as described above can remotely monitor the user's respiratory status in real time, that is, three types of respiratory status monitoring are set: slow breathing, normal breathing, and fast breathing; a normal adult breathes about 12-20 times per minute, and the APP is set with a respiratory arrest alarm, that is, no breathing within 1 minute, to remotely remind the user's family in real time.

[0033] The advantages and positive effects achieved by the present invention are:

[0034] 1. The pre-oxidized graphite GO obtained in the present invention is an excellent new carbon-based material. The rich hydrophilic groups give it excellent dispersibility and humidity-sensitive properties. The special lattice structure makes it have very good flexibility. The preparation method is simple and the cost is low. It exhibits high proton conductivity under the action of water molecules. After absorbing moisture, the protons spontaneously generated by oxygen-containing groups and water molecules have rapid diffusion behavior.

[0035] 2. The LIG preparation method used in the present invention has the advantages of lower cost, no special requirements for the processing environment, and one-step patterned preparation without the need for a mask.

[0036] 3. The fluorinated polyimide film obtained in the present invention has a rich carbon content. When the local temperature rises sharply due to laser irradiation, C atoms can be recombined to form a graphene layer. When the laser is hit, part of the fluorine-containing gas will overflow, which can play a role in pore formation, increasing the area covered by GO, so that it has more water molecule adsorption sites. In addition, the fluorinated polyimide has high mechanical strength, good acid and alkali resistance and wear resistance, and is an excellent material for laser-induced graphene precursor.

[0037] 4. The humidity sensor of LIG and GO humidity-sensitive materials based on fluorinated PI obtained in the present invention has extremely high sensitivity and detection accuracy to water molecules while ensuring flexibility, and has good linearity in capacitance change within the humidity range, and exhibits excellent humidity-sensitive properties in terms of response / recovery time, repeatability, hysteresis, etc., giving full play to the advantages of humidity sensors.

[0038] 5. The intelligent integrated respiratory monitoring mask based on the F-LIG / GO humidity sensor of the present invention is light and compact through integrated programming, and can monitor the user's respiratory behavior in real time and accurately through the APP and issue a respiratory arrest alarm, making respiratory monitoring more convenient and economical. The present invention assembles an intelligent integrated respiratory monitoring mask based on the F-LIG / GO humidity sensor, which solves the problem that traditional respiratory monitoring equipment is bulky and expensive.

[0039] 6. The present invention has developed an APP for an intelligent integrated respiratory monitoring mask based on the F-LIG / GO humidity sensor to solve the problem of inconvenience in wearing traditional respiratory monitoring equipment.

[0040] 7. From the perspective of electrodes, the present invention proposes a method for preparing porous carbon interdigital electrodes based on laser-induced graphene of fluorine-doped polyimide, synthesizes graphene oxide according to the improved hummer method, and drop-casts the graphene oxide solution on LIG. The pore structure is adjusted by different degrees of fluorination. The change of the pore structure can affect the degree of water infiltration. The porous LIG has a large specific surface area, which increases the area of ​​GO covered on it, so that it has more water molecule adsorption sites. After GO absorbs moisture, the protons spontaneously generated by oxygen-containing groups and water molecules have rapid diffusion behavior. Supported by this principle, the substrate electrode integrated flexible capacitive humidity sensor prepared by the present invention can be used to monitor different relative humidity of 11% to 97%. The results show that the sensor has good linearity in capacitance change within the humidity range, and exhibits excellent humidity-sensitive properties in terms of sensitivity, response / recovery time, repeatability, hysteresis, etc., and can be used stably within thirty days. In addition, the present invention also combines it with electronic components such as single-chip microcomputers and WIFI modules, assembles it into an integrated respiratory monitoring mask after programming, and monitors the respiratory state in real time through the developed APP and performs respiratory arrest alarm.

[0041] 8. The F-LIG / GO humidity sensor in the present invention is applied to the integrated respiratory monitoring mask, and it also needs to be matched with electronic components such as a single-chip microcomputer and a WIFI module. As a single-chip microcomputer based on the ARM Cortex-M core, the STM32 single-chip microcomputer has the following advantages: fast running speed and strong performance; low power consumption design, suitable for battery-powered applications; support for multiple bus interfaces, such as CAN, SPI, I2C, etc.; rich peripherals, such as ADC, DAC, PWM, USART, USB, etc.; integrated with multiple functional modules, such as clock module, interrupt controller, power management, etc.; perfect development tool chain, support for multiple development environments, such as Keil, IAR, GCC, etc. In addition, as a low-cost WiFi microcontroller, ESP8266 integrates the TCP / IP protocol stack, supports the 802.11b / g / n standard, has the characteristics of low power consumption, high cost performance and easy to use, and its combination with the respiratory monitoring APP developed based on the Alibaba Cloud server has very accurate remote real-time data transmission capabilities. Therefore, the programmed and assembled intelligent integrated respiratory monitoring mask based on F-LIG / GO humidity sensor can monitor the user's respiratory behavior in real time and accurately through APP and issue a respiratory arrest alarm, making respiratory monitoring more convenient and economical.

[0042] 9. The humidity sensor of the present invention has high flexibility and stability. The output capacitance signal value of the sensor manufactured in the present invention remains stable within the deformation angle of 0 to 90 degrees.

[0043] The design of the humidity sensor based on the porous graphene electrode and the graphene oxide film of the present invention greatly increases the contact area between the electrode material and the humidity-sensitive material, thereby increasing the rate of water molecule desorption and effectively preventing water molecules from being retained and aggregated for a long time. The humidity sensor of the present invention has stable humidity detection performance within thirty days.

[0044] The humidity sensor of the present invention has the advantages of high integration, ultra-fast response and portability. So far, the fastest response recovery time of the sensor manufactured by the present invention to respond to humidity and recover from it is 5 seconds.

[0045] In summary, the humidity sensor of the present invention can solve the technical problems existing in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 A schematic diagram of a preparation route of the F-LIG / GO humidity sensor of the present invention;

[0047] Figure 2 The fluorinated polyimide-based laser-induced graphene (F 75 -LIG / GO 4mg / mL ) obtained in the method for preparing a humidity sensor 75 - SEM image of LIG;

[0048] Figure 3 The fluorinated polyimide-based laser-induced graphene (F 75 -LIG / GO 4mg / mL ) obtained in the method for preparing a humidity sensor 75 -LIG / GO 4mg / mL SEM images of

[0049] Figure 4 The GO and F obtained in the preparation method provided in Example 1 of the present invention 75 - Raman spectrum of LIG;

[0050] Figure 5 F obtained in the preparation method provided in Example 1 of the present invention 75 -PI, F 75 -XPS spectrum of LIG;

[0051] Figure 6 F obtained in the preparation method provided in Example 1 of the present invention 75 -C1s spectrum of LIG;

[0052] Figure 7 F obtained in the preparation method provided in Example 1 of the present invention 75- F1s spectrum of LIG;

[0053] Figure 8 Capacitance response curves of humidity sensors at different GO concentrations prepared by a method for preparing a humidity sensor based on fluorinated polyimide-based laser induced graphene (F-LIG / GO) drop-coated with GO provided in Example 1, Example 2, Example 3 and Comparative Example 1 of the present invention;

[0054] Fig. 9 Capacitance response curves of humidity sensors at different fluorine contents prepared by a method for preparing a humidity sensor based on fluorinated polyimide-based laser induced graphene (F-LIG / GO) drop-coated GO provided in Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5 of the present invention;

[0055] Fig.10 F obtained in the preparation method provided in Example 1 of the present invention 75 -LIG / GO 4mg / mL Various sensing performance diagrams of humidity sensors;

[0056] Fig.11 A schematic diagram of an assembly structure of an intelligent integrated respiratory monitoring mask based on the F-LIG / GO humidity sensor in the present invention;

[0057] Fig.12 This is a real-time monitoring waveform diagram of the APP of the intelligent integrated respiratory monitoring mask based on the F-LIG / GO humidity sensor in the present invention. DETAILED DESCRIPTION

[0058] The present invention will be further described below in conjunction with the embodiments. The following embodiments are descriptive rather than restrictive, and the protection scope of the present invention cannot be limited by the following embodiments.

[0059] The various experimental operations involved in the specific embodiments are all routine techniques in the art. For parts not specially annotated in this document, ordinary technicians in the art can implement them by referring to various commonly used reference books, scientific and technological literature or related instructions, manuals, etc. before the filing date of this invention.

[0060] A humidity sensor based on fluorinated polyimide-based laser-induced graphene F-LIG / GO drop-coated GO, the preparation method of which comprises the following steps:

[0061] Step 1, place TPE-Q in a three-necked flask, add DMAC, and mechanically stir until it is completely dissolved, then add 6FDA and BPADA into the three-necked flask in three batches, and mechanically stir to obtain a polyamic acid PAA solution;

[0062] Step 2: The PAA solution is allowed to stand to remove bubbles, then poured onto a pre-cleaned glass plate, scraped into a film of uniform thickness, and the solvent is evaporated, and then a step-by-step thermal imidization is performed, followed by natural cooling, and the glass plate is placed in deionized water, and dried after natural shedding to obtain an F-PI film;

[0063] Step 3, graphite powder, (NH4)2S2O8 and P2O5 are successively placed in H2SO4 solution, followed by heating and stirring;

[0064] Step 4, washing the mixture with deionized water until the pH value of the filtrate becomes neutral, and drying the filtered solid under vacuum to obtain pre-oxidized graphite;

[0065] Step 5, placing the pre-oxidized graphite in a H2SO4 solution in an ice water bath and stirring, slowly adding potassium permanganate, and continuously heating the mixture in a gradient manner;

[0066] Step 6, after cooling to room temperature, adding deionized water and H2O2 solution to terminate the reaction, washing the mixture with HCl solution, and washing with deionized water until neutral to remove residual metal ions;

[0067] Step 7, after the washed mixture is subjected to ultrasonic treatment at low temperature, the obtained graphene oxide dispersion is taken out with a pipette, placed in an oven and dried until completely dry, and then weighed to prepare a GO solution;

[0068] Step 8: Cut the prepared PI sample into rectangles as a substrate, and then fix it on A4 paper with transparent tape. Use a semiconductor laser to perform laser direct writing on the F-PI film in an atmospheric atmosphere to obtain F-LIG interdigital electrodes.

[0069] Step 9: Apply conductive silver paste to the connection between the copper wire and the interdigital electrode, and finally use a pipette to drop the GO solution on the interdigital electrode. Place the device in a fume hood and dry it naturally under indoor conditions to form a uniform GO film, and finally obtain a humidity sensor based on drop-coated GO fluorinated polyimide-based laser-induced graphene (F-LIG / GO).

[0070] Preferably, the ratio of the mass of DMAC added in step 1 to the total mass of the remaining monomers is 17:3, the ratio of the total molar amount of 6FDA and BPADA to the molar amount of TPE-Q is 1:1, and they are added in three batches at an interval of 10 minutes each, and mechanically stirred for 4 hours to obtain a PAA solution with a solid content of 15%;

[0071] Preferably, the standing time in step 2 is 12 hours, the scraper distance is set to 200 μm, and the volatilization is performed at 80°C for 2 hours; the step-by-step heating steps are as follows: 100°C for 1 hour, 200°C for 1 hour, and 250°C for 1 hour. By controlling the amount of 6FDA, F with different fluorination degrees can be obtained. x -PI (x is the mole fraction of 6FDA in the anhydride, 0, 25, 50, 75, 100%) films.

[0072] Preferably, 2 g of 325 mesh graphite powder is used in step 3, the mass concentration of H2SO4 solution is 98%, and the mixture is heated to 80°C and stirred for 4 hours; the ratio of graphite powder: (NH4)2S2O8: P2O5: H2SO4 solution g:g:g:mL is 2:2:2:10;

[0073] Alternatively, in step 4, dry under vacuum for 2 h.

[0074] Preferably, the mass concentration of the H2SO4 solution in step 5 is 98%; the continuous gradient heating step is as follows: heating at 35°C for 2 hours, then heating to 95°C for 30 minutes; the ratio of pre-oxidized graphite: H2SO4 solution: potassium permanganate is 0.6:24:3 in g:mL:g;

[0075] Alternatively, in step 6, the mass concentration of the H2O2 solution is 30%, the HCl solution is an HCl solution with a volume ratio of HCl: water of 1:10, and the number of washing times of the HCl solution washing mixture is 4 times; the ratio of pre-oxidized graphite: deionized water: H2O2 solution g: mL: mL is 0.6:200:6.

[0076] Preferably, in step 7, the low temperature is 0°C, the ultrasonic frequency is 10kHz for 2h, 5mL of the graphene oxide dispersion is taken out with a pipette, and the temperature of the oven is controlled at 50°C during drying; the concentration of the dispersion is calculated by weighing, and 1, 2, and 4mg / mL GO solutions are prepared.

[0077] Preferably, the wavelength of the semiconductor laser used in step 8 is 450nm, the maximum power is 7W, the laser power is set to 1.4W, the scanning speed is set to a fixed value of 100mm / s, and the obtained F x -The pattern size of LIG interdigitated electrodes is 8 mm*12 mm, where x is the mole fraction of 6FDA in the anhydride, i.e., 0, 25, 50, 75, and 100%;

[0078] Alternatively, in step 9, the amount of GO solution applied by a pipette is 100 μL, and the natural drying time is 1 day.

[0079] The use of humidity sensors in integrated respiratory monitoring masks as described above,

[0080] The intelligent integrated respiratory monitoring mask made by using the humidity sensor as described above, the assembly method of the intelligent integrated respiratory monitoring mask comprises the following steps:

[0081] The F-LIG / GO humidity sensor is placed inside the breathing mask and then connected to the AD converter, microcontroller, WIFI module, voltage regulator module and lithium battery through wires. After programming, all the above electronic components are integrated and placed outside the breathing mask.

[0082] The functional APP of the intelligent integrated respiratory monitoring mask as described above can remotely monitor the user's respiratory status in real time, that is, three types of respiratory status monitoring are set: slow breathing, normal breathing, and fast breathing; a normal adult breathes about 12-20 times per minute, and the APP is set with a respiratory arrest alarm, that is, no breathing within 1 minute, to remotely remind the user's family in real time.

[0083] Specifically, the relevant preparation and detection are as follows:

[0084] Example 1

[0085] A fluorinated polyimide-based laser-induced graphene (F-PIG) based on drop-coated GO 75 -LIG / GO 4mg / mL ) is a method for preparing a humidity sensor, the method comprising the following steps:

[0086] Step 1: Place TPE-Q in a three-necked flask, add DMAC, the total mass ratio of DMAC to the remaining monomers is 17:3, stir mechanically until it is completely dissolved, and then add 6FDA and BPADA to the three-necked flask in three batches, each time with an interval of 10 minutes. Among them, the total molar ratio of 6FDA and BPADA to the molar amount of TPE-Q is 1:1, and the molar fraction of 6FDA in the acid anhydride is controlled to be 75%. After mechanical stirring for 4 hours, a polyamic acid (PAA) solution with a solid content of 15% is obtained.

[0087] Step 2: The PAA solution was allowed to stand for 12 hours to remove bubbles, and then the PAA solution was poured onto a pre-cleaned glass plate. The scraper was set to 200 μm and scraped into a film of uniform thickness. The film was evaporated at 80°C for 2 hours to remove the solvent, and then the film was subjected to step-by-step thermal imidization. The step-by-step heating steps were as follows: 100°C for 1 hour, 200°C for 1 hour, and 250°C for 1 hour. After that, the film was cooled naturally, and the glass plate was placed in deionized water, and dried after natural shedding to obtain F. 75 -PI film.

[0088] Step 3: Graphite powder (2 g, 325 mesh), (NH4)2S2O8 (2 g) and P2O5 (2 g) were successively placed in H2SO4 solution (98%, 10 mL), and then stirred at 80°C for 4 h.

[0089] Step 4: Wash the mixture with deionized water until the pH value of the filtrate becomes neutral. Dry the filtered solid in a vacuum atmosphere for 2 hours to obtain pre-oxidized graphite.

[0090] Step 5: 0.6 g of pre-oxidized graphite was placed in an H2SO4 solution (98%, 24 mL) in an ice-water bath and stirred, and 3 g of potassium permanganate was slowly added. Then, the mixture was heated to 35° C. and maintained for 2 h. Subsequently, the temperature was raised to 95° C. and maintained for 30 min.

[0091] Step 6: After cooling to room temperature, the reaction was terminated by adding deionized water (200 mL) and H2O2 solution (30%, 6 mL). The mixture was washed 4 times with HCl solution (HCl: water volume ratio of 1:10), and washed with deionized water until neutral to remove residual metal ions.

[0092] Step 7: After treating at a low temperature of 0°C with an ultrasonic frequency of 10 kHz for 2 hours, a graphene oxide dispersion is obtained. 5 mL of the graphene oxide dispersion is taken out with a pipette, placed in an oven at 50°C until completely dry, and the dispersion concentration is calculated by weighing, and a GO solution of 4 mg / mL is prepared.

[0093] Step 8: Cut the prepared PI sample into a rectangular shape as a substrate, and then fix it on an A4 paper with transparent tape. Next, use a semiconductor laser with a wavelength of 450nm and a maximum power of 7W to irradiate the F 75 -PI film was laser-written. The laser power was set to 1.4W and the scanning speed was set to a fixed value of 100mm / s. 75 -The size of the LIG interdigital electrode patterns is 8*12mm.

[0094] Step 9: Apply conductive silver paste to the junction between the copper wire and the interdigital electrode to enhance the electrical contact. Finally, 100 μL of GO solution was dropped onto the interdigital electrode using a pipette, and the device was placed in a fume hood and dried naturally for 1 day under indoor conditions to form a uniform GO film.

[0095] Finally, fluorinated polyimide-based laser-induced graphene (F 75 -LIG / GO 4mg / mL ) humidity sensor.

[0096] Example 2

[0097] A fluorinated polyimide-based laser-induced graphene (F-PIG) based on drop-coated GO 75 -LIG / GO 2mg / mL ) is a method for preparing a humidity sensor, the method comprising the following steps:

[0098] Step 1: Place TPE-Q in a three-necked flask, add DMAC, the total mass ratio of DMAC to the remaining monomers is 17:3, stir mechanically until it is completely dissolved, and then add 6FDA and BPADA to the three-necked flask in three batches, each time with an interval of 10 minutes. Among them, the total molar ratio of 6FDA and BPADA to the molar amount of TPE-Q is 1:1, and the molar fraction of 6FDA in the acid anhydride is controlled to be 75%. After mechanical stirring for 4 hours, a polyamic acid (PAA) solution with a solid content of 15% is obtained.

[0099] Step 2: The PAA solution was allowed to stand for 12 hours to remove bubbles, and then the PAA solution was poured onto a pre-cleaned glass plate. The scraper was set to 200 μm and scraped into a film of uniform thickness. The film was evaporated at 80°C for 2 hours to remove the solvent, and then the film was subjected to step-by-step thermal imidization. The step-by-step heating steps were as follows: 100°C for 1 hour, 200°C for 1 hour, and 250°C for 1 hour. After that, the film was cooled naturally, and the glass plate was placed in deionized water, and dried after natural shedding to obtain F. 75 -PI film.

[0100] Step 3: Graphite powder (2 g, 325 mesh), (NH4)2S2O8 (2 g) and P2O5 (2 g) were successively placed in H2SO4 solution (98%, 10 mL), and then stirred at 80°C for 4 h.

[0101] Step 4: Wash the mixture with deionized water until the pH value of the filtrate becomes neutral. Dry the filtered solid in a vacuum atmosphere for 2 hours to obtain pre-oxidized graphite.

[0102] Step 5: 0.6 g of pre-oxidized graphite was placed in an H2SO4 solution (98%, 24 mL) in an ice-water bath and stirred, and 3 g of potassium permanganate was slowly added. Then, the mixture was heated to 35° C. and maintained for 2 h. Subsequently, the temperature was raised to 95° C. and maintained for 30 min.

[0103] Step 6: After cooling to room temperature, the reaction was terminated by adding deionized water (200 mL) and H2O2 solution (30%, 6 mL). The mixture was washed 4 times with HCl solution (HCl: water volume ratio of 1:10), and washed with deionized water until neutral to remove residual metal ions.

[0104] Step 7: After treating at a low temperature of 0°C with an ultrasonic frequency of 10 kHz for 2 hours, a graphene oxide dispersion is obtained. 5 mL of the graphene oxide dispersion is taken out with a pipette, placed in an oven at 50°C until completely dry, and the dispersion concentration is calculated by weighing, and a 2 mg / mL GO solution is prepared.

[0105] Step 8: Cut the prepared PI sample into a rectangular shape as a substrate, and then fix it on an A4 paper with transparent tape. Next, use a semiconductor laser with a wavelength of 450nm and a maximum power of 7W to irradiate the F 75 -PI film was laser-written. The laser power was set to 1.4W and the scanning speed was set to a fixed value of 100mm / s. 75 -The size of the LIG interdigital electrode patterns is 8*12mm.

[0106] Step 9: Apply conductive silver paste to the junction between the copper wire and the interdigital electrode to enhance the electrical contact. Finally, 100 μL of GO solution was dropped onto the interdigital electrode using a pipette, and the device was placed in a fume hood and dried naturally for 1 day under indoor conditions to form a uniform GO film.

[0107] Finally, fluorinated polyimide-based laser-induced graphene (F 75 -LIG / GO 2mg / mL ) humidity sensor.

[0108] Example 3

[0109] A fluorinated polyimide-based laser-induced graphene (F-PIG) based on drop-coated GO 75 -LIG / GO 1mg / mL ) is a method for preparing a humidity sensor, the method comprising the following steps:

[0110] Step 1: Place TPE-Q in a three-necked flask, add DMAC, the total mass ratio of DMAC to the remaining monomers is 17:3, stir mechanically until it is completely dissolved, and then add 6FDA and BPADA to the three-necked flask in three batches, each time with an interval of 10 minutes. Among them, the total molar ratio of 6FDA and BPADA to the molar amount of TPE-Q is 1:1, and the molar fraction of 6FDA in the acid anhydride is controlled to be 75%. After mechanical stirring for 4 hours, a polyamic acid (PAA) solution with a solid content of 15% is obtained.

[0111] Step 2: The PAA solution was allowed to stand for 12 hours to remove bubbles, and then the PAA solution was poured onto a pre-cleaned glass plate. The scraper was set to 200 μm and scraped into a film of uniform thickness. The film was evaporated at 80°C for 2 hours to remove the solvent, and then the film was subjected to step-by-step thermal imidization. The step-by-step heating steps were as follows: 100°C for 1 hour, 200°C for 1 hour, and 250°C for 1 hour. After that, the film was cooled naturally, and the glass plate was placed in deionized water, and dried after natural shedding to obtain F. 75 -PI film.

[0112] Step 3: Graphite powder (2 g, 325 mesh), (NH4)2S2O8 (2 g) and P2O5 (2 g) were successively placed in H2SO4 solution (98%, 10 mL), and then stirred at 80°C for 4 h.

[0113] Step 4: Wash the mixture with deionized water until the pH value of the filtrate becomes neutral. Dry the filtered solid in a vacuum atmosphere for 2 hours to obtain pre-oxidized graphite.

[0114] Step 5: 0.6 g of pre-oxidized graphite was placed in an H2SO4 solution (98%, 24 mL) in an ice-water bath and stirred, and 3 g of potassium permanganate was slowly added. Then, the mixture was heated to 35° C. and maintained for 2 h. Subsequently, the temperature was raised to 95° C. and maintained for 30 min.

[0115] Step 6: After cooling to room temperature, the reaction was terminated by adding deionized water (200 mL) and H2O2 solution (30%, 6 mL). The mixture was washed 4 times with HCl solution (HCl: water volume ratio of 1:10), and washed with deionized water until neutral to remove residual metal ions.

[0116] Step 7: After treating at a low temperature of 0°C with an ultrasonic frequency of 10 kHz for 2 hours, a graphene oxide dispersion is obtained. 5 mL of the graphene oxide dispersion is taken out with a pipette, placed in an oven at 50°C until completely dry, and the dispersion concentration is calculated by weighing, and a 1 mg / mL GO solution is prepared.

[0117] Step 8: Cut the prepared PI sample into a rectangular shape as a substrate, and then fix it on an A4 paper with transparent tape. Next, use a semiconductor laser with a wavelength of 450nm and a maximum power of 7W to irradiate the F 75 -PI film was laser-written. The laser power was set to 1.4W and the scanning speed was set to a fixed value of 100mm / s. 75 -The size of the LIG interdigital electrode patterns is 8*12mm.

[0118] Step 9: Apply conductive silver paste to the junction between the copper wire and the interdigital electrode to enhance the electrical contact. Finally, 100 μL of GO solution was dropped onto the interdigital electrode using a pipette, and the device was placed in a fume hood and dried naturally for 1 day under indoor conditions to form a uniform GO film.

[0119] Finally, fluorinated polyimide-based laser-induced graphene (F 75 -LIG / GO 1mg / mL ) humidity sensor.

[0120] Comparative Example 1

[0121] This comparative example is a fluorinated polyimide-based laser-induced graphene (F 75 -LIG) humidity sensor preparation method, the method comprising the following steps:

[0122] Step 1: Place TPE-Q in a three-necked flask, add DMAC, the total mass ratio of DMAC to the remaining monomers is 17:3, stir mechanically until it is completely dissolved, and then add 6FDA and BPADA to the three-necked flask in three batches, each time with an interval of 10 minutes. Among them, the total molar ratio of 6FDA and BPADA to the molar amount of TPE-Q is 1:1, and the molar fraction of 6FDA in the acid anhydride is controlled to be 75%. After mechanical stirring for 4 hours, a polyamic acid (PAA) solution with a solid content of 15% is obtained.

[0123] Step 2: The PAA solution was allowed to stand for 12 hours to remove bubbles, and then the PAA solution was poured onto a pre-cleaned glass plate. The scraper was set to 200 μm and scraped into a film of uniform thickness. The film was evaporated at 80°C for 2 hours to remove the solvent, and then the film was subjected to step-by-step thermal imidization. The step-by-step heating steps were as follows: 100°C for 1 hour, 200°C for 1 hour, and 250°C for 1 hour. After that, the film was cooled naturally, and the glass plate was placed in deionized water, and dried after natural shedding to obtain F. 75 -PI film.

[0124] Step 8: Cut the prepared PI sample into a rectangular shape as a substrate, and then fix it on an A4 paper with transparent tape. Next, use a semiconductor laser with a wavelength of 450nm and a maximum power of 7W to irradiate the F 75 -PI film was laser-written. The laser power was set to 1.4W and the scanning speed was set to a fixed value of 100mm / s. 75 -The size of the LIG interdigital electrode patterns is 8*12mm.

[0125] Step 9: Apply conductive silver paste to the connection between the copper wire and the interdigital electrode to enhance the electrical contact.

[0126] Finally, fluorinated polyimide-based laser-induced graphene (F 75 -LIG) humidity sensor.

[0127] Comparative Example 2

[0128] This comparative example is based on drop-coated GO fluorinated polyimide-based laser-induced graphene (F0-LIG / GO 2mg / mL ) is a method for preparing a humidity sensor, the method comprising the following steps:

[0129] Step 1: Place TPE-Q in a three-necked flask, add DMAC, the total mass ratio of DMAC to the remaining monomers is 17:3, stir mechanically until it is completely dissolved, and then add 6FDA and BPADA to the three-necked flask in three batches, each time with an interval of 10 minutes. Among them, the total molar ratio of 6FDA and BPADA to the molar amount of TPE-Q is 1:1, and the molar fraction of 6FDA in the acid anhydride is controlled to be 0%. After mechanical stirring for 4 hours, a polyamic acid (PAA) solution with a solid content of 15% is obtained.

[0130] Step 2: The PAA solution was allowed to stand for 12 hours to remove bubbles, and then the PAA solution was poured onto a pre-cleaned glass plate. The scraper was set to 200 μm, and a film of uniform thickness was scraped. The film was evaporated at 80°C for 2 hours to remove the solvent, and then the film was subjected to step-by-step thermal imidization. The step-by-step heating steps were as follows: 100°C for 1 hour, 200°C for 1 hour, and 250°C for 1 hour. After that, the film was cooled naturally, and the glass plate was placed in deionized water. After natural shedding, the film was dried to obtain the F0-PI film.

[0131] Step 3: Graphite powder (2 g, 325 mesh), (NH4)2S2O8 (2 g) and P2O5 (2 g) were successively placed in H2SO4 solution (98%, 10 mL), and then stirred at 80°C for 4 h.

[0132] Step 4: Wash the mixture with deionized water until the pH value of the filtrate becomes neutral. Dry the filtered solid in a vacuum atmosphere for 2 hours to obtain pre-oxidized graphite.

[0133] Step 5: 0.6 g of pre-oxidized graphite was placed in an H2SO4 solution (98%, 24 mL) in an ice-water bath and stirred, and 3 g of potassium permanganate was slowly added. Then, the mixture was heated to 35° C. and maintained for 2 h. Subsequently, the temperature was raised to 95° C. and maintained for 30 min.

[0134] Step 6: After cooling to room temperature, the reaction was terminated by adding deionized water (200 mL) and H2O2 solution (30%, 6 mL). The mixture was washed 4 times with HCl solution (HCl: water volume ratio of 1:10), and washed with deionized water until neutral to remove residual metal ions.

[0135] Step 7: After treating at a low temperature of 0°C with an ultrasonic frequency of 10 kHz for 2 hours, a graphene oxide dispersion is obtained. 5 mL of the graphene oxide dispersion is taken out with a pipette, placed in an oven at 50°C until completely dry, and the dispersion concentration is calculated by weighing, and a 2 mg / mL GO solution is prepared.

[0136] Step 8: Cut the prepared PI sample into rectangles as a substrate and fix it on A4 paper with transparent tape. Next, use a semiconductor laser with a wavelength of 450nm and a maximum power of 7W to perform laser direct writing on the F0-PI film in an atmospheric atmosphere. The laser power is set to 1.4w, and the scanning speed is set to a fixed value of 100mm / s. The size of the obtained F0-LIG interdigital electrode pattern is 8*12mm.

[0137] Step 9: Apply conductive silver paste to the junction between the copper wire and the interdigital electrode to enhance the electrical contact. Finally, 100 μL of GO solution was dropped onto the interdigital electrode using a pipette, and the device was placed in a fume hood and dried naturally for 1 day under indoor conditions to form a uniform GO film.

[0138] Finally, fluorinated polyimide-based laser-induced graphene (F0-LIG / GO) based on drop-coated GO was obtained. 2mg / mL ) humidity sensor.

[0139] Comparative Example 3

[0140] This comparative example is based on drop-coated GO fluorinated polyimide-based laser-induced graphene (F 25 -LIG / GO 2mg / mL ) is a method for preparing a humidity sensor, the method comprising the following steps:

[0141] Step 1: Place TPE-Q in a three-necked flask, add DMAC, the total mass ratio of DMAC to the remaining monomers is 17:3, stir mechanically until it is completely dissolved, and then add 6FDA and BPADA to the three-necked flask in three batches, each time with an interval of 10 minutes. Among them, the total molar ratio of 6FDA and BPADA to the molar amount of TPE-Q is 1:1, and the molar fraction of 6FDA in the acid anhydride is controlled to be 25%. After mechanical stirring for 4 hours, a polyamic acid (PAA) solution with a solid content of 15% is obtained.

[0142] Step 2: The PAA solution was allowed to stand for 12 hours to remove bubbles, and then the PAA solution was poured onto a pre-cleaned glass plate. The scraper was set to 200 μm and scraped into a film of uniform thickness. The film was evaporated at 80°C for 2 hours to remove the solvent, and then the film was subjected to step-by-step thermal imidization. The step-by-step heating steps were as follows: 100°C for 1 hour, 200°C for 1 hour, and 250°C for 1 hour. After that, the film was cooled naturally, and the glass plate was placed in deionized water, and dried after natural shedding to obtain F. 25 -PI film.

[0143] Step 3: Graphite powder (2 g, 325 mesh), (NH4)2S2O8 (2 g) and P2O5 (2 g) were successively placed in H2SO4 solution (98%, 10 mL), and then stirred at 80°C for 4 h.

[0144] Step 4: Wash the mixture with deionized water until the pH value of the filtrate becomes neutral. Dry the filtered solid in a vacuum atmosphere for 2 hours to obtain pre-oxidized graphite.

[0145] Step 5: 0.6 g of pre-oxidized graphite was placed in an H2SO4 solution (98%, 24 mL) in an ice-water bath and stirred, and 3 g of potassium permanganate was slowly added. Then, the mixture was heated to 35° C. and maintained for 2 h. Subsequently, the temperature was raised to 95° C. and maintained for 30 min.

[0146] Step 6: After cooling to room temperature, the reaction was terminated by adding deionized water (200 mL) and H2O2 solution (30%, 6 mL). The mixture was washed 4 times with HCl solution (HCl: water volume ratio of 1:10), and washed with deionized water until neutral to remove residual metal ions.

[0147] Step 7: After treating at a low temperature of 0°C with an ultrasonic frequency of 10 kHz for 2 hours, a graphene oxide dispersion is obtained. 5 mL of the graphene oxide dispersion is taken out with a pipette, placed in an oven at 50°C until completely dry, and the dispersion concentration is calculated by weighing, and a 2 mg / mL GO solution is prepared.

[0148] Step 8: Cut the prepared PI sample into a rectangular shape as a substrate, and then fix it on an A4 paper with transparent tape. Next, use a semiconductor laser with a wavelength of 450nm and a maximum power of 7W to irradiate the F 25 -PI film was laser-written. The laser power was set to 1.4W and the scanning speed was set to a fixed value of 100mm / s. 25 -The size of the LIG interdigital electrode patterns is 8*12mm.

[0149] Step 9: Apply conductive silver paste to the junction between the copper wire and the interdigital electrode to enhance the electrical contact. Finally, 100 μL of GO solution was dropped onto the interdigital electrode using a pipette, and the device was placed in a fume hood and dried naturally for 1 day under indoor conditions to form a uniform GO film.

[0150] Finally, fluorinated polyimide-based laser-induced graphene (F 25 -LIG / GO 2mg / mL ) humidity sensor.

[0151] Comparative Example 4

[0152] This comparative example is based on drop-coated GO fluorinated polyimide-based laser-induced graphene (F 50 -LIG / GO 2mg / mL ) is a method for preparing a humidity sensor, the method comprising the following steps:

[0153] Step 1: Place TPE-Q in a three-necked flask, add DMAC, the total mass ratio of DMAC to the remaining monomers is 17:3, stir mechanically until it is completely dissolved, and then add 6FDA and BPADA to the three-necked flask in three batches, each time with an interval of 10 minutes. Among them, the total molar ratio of 6FDA and BPADA to the molar amount of TPE-Q is 1:1, and the molar fraction of 6FDA in the anhydride is controlled to be 50%. After mechanical stirring for 4 hours, a polyamic acid (PAA) solution with a solid content of 15% is obtained.

[0154] Step 2: The PAA solution was allowed to stand for 12 hours to remove bubbles, and then the PAA solution was poured onto a pre-cleaned glass plate. The scraper was set to 200 μm and scraped into a film of uniform thickness. The film was evaporated at 80°C for 2 hours to remove the solvent, and then the film was subjected to step-by-step thermal imidization. The step-by-step heating steps were as follows: 100°C for 1 hour, 200°C for 1 hour, and 250°C for 1 hour. After that, the film was cooled naturally, and the glass plate was placed in deionized water, and dried after natural shedding to obtain F. 50 -PI film.

[0155] Step 3: Graphite powder (2 g, 325 mesh), (NH4)2S2O8 (2 g) and P2O5 (2 g) were successively placed in H2SO4 solution (98%, 10 mL), and then stirred at 80°C for 4 h.

[0156] Step 4: Wash the mixture with deionized water until the pH value of the filtrate becomes neutral. Dry the filtered solid in a vacuum atmosphere for 2 hours to obtain pre-oxidized graphite.

[0157] Step 5: 0.6 g of pre-oxidized graphite was placed in an H2SO4 solution (98%, 24 mL) in an ice-water bath and stirred, and 3 g of potassium permanganate was slowly added. Then, the mixture was heated to 35° C. and maintained for 2 h. Subsequently, the temperature was raised to 95° C. and maintained for 30 min.

[0158] Step 6: After cooling to room temperature, the reaction was terminated by adding deionized water (200 mL) and H2O2 solution (30%, 6 mL). The mixture was washed 4 times with HCl solution (HCl: water volume ratio of 1:10), and washed with deionized water until neutral to remove residual metal ions.

[0159] Step 7: After treating at a low temperature of 0°C with an ultrasonic frequency of 10 kHz for 2 hours, a graphene oxide dispersion is obtained. 5 mL of the graphene oxide dispersion is taken out with a pipette, placed in an oven at 50°C until completely dry, and the dispersion concentration is calculated by weighing, and a 2 mg / mL GO solution is prepared.

[0160] Step 8: Cut the prepared PI sample into a rectangular shape as a substrate, and then fix it on an A4 paper with transparent tape. Next, use a semiconductor laser with a wavelength of 450nm and a maximum power of 7W to irradiate the F 50 -PI film was laser-written. The laser power was set to 1.4W and the scanning speed was set to a fixed value of 100mm / s. 50 -The size of the LIG interdigital electrode patterns is 8*12mm.

[0161] Step 9: Apply conductive silver paste to the junction between the copper wire and the interdigital electrode to enhance the electrical contact. Finally, 100 μL of GO solution was dropped onto the interdigital electrode using a pipette, and the device was placed in a fume hood and dried naturally for 1 day under indoor conditions to form a uniform GO film.

[0162] Finally, fluorinated polyimide-based laser-induced graphene (F 50 -LIG / GO 2mg / mL ) humidity sensor.

[0163] Comparative Example 5

[0164] This comparative example is based on drop-coated GO fluorinated polyimide-based laser-induced graphene (F 100 -LIG / GO 2mg / mL ) is a method for preparing a humidity sensor, the method comprising the following steps:

[0165] Step 1: Place TPE-Q in a three-necked flask, add DMAC, the total mass ratio of DMAC to the remaining monomers is 17:3, stir mechanically until it is completely dissolved, and then add 6FDA and BPADA to the three-necked flask in three batches, each time with an interval of 10 minutes. Among them, the total molar ratio of 6FDA and BPADA to the molar amount of TPE-Q is 1:1, and the molar fraction of 6FDA in the acid anhydride is controlled to be 100%. After mechanical stirring for 4 hours, a polyamic acid (PAA) solution with a solid content of 15% is obtained.

[0166] Step 2: The PAA solution was allowed to stand for 12 hours to remove bubbles, and then the PAA solution was poured onto a pre-cleaned glass plate. The scraper was set to 200 μm and scraped into a film of uniform thickness. The film was evaporated at 80°C for 2 hours to remove the solvent, and then the film was subjected to step-by-step thermal imidization. The step-by-step heating steps were as follows: 100°C for 1 hour, 200°C for 1 hour, and 250°C for 1 hour. After that, the film was cooled naturally, and the glass plate was placed in deionized water, and dried after natural shedding to obtain F. 100 -PI film.

[0167] Step 3: Graphite powder (2 g, 325 mesh), (NH4)2S2O8 (2 g) and P2O5 (2 g) were successively placed in H2SO4 solution (98%, 10 mL), and then stirred at 80°C for 4 h.

[0168] Step 4: Wash the mixture with deionized water until the pH value of the filtrate becomes neutral. Dry the filtered solid in a vacuum atmosphere for 2 hours to obtain pre-oxidized graphite.

[0169] Step 5: 0.6 g of pre-oxidized graphite was placed in an H2SO4 solution (98%, 24 mL) in an ice-water bath and stirred, and 3 g of potassium permanganate was slowly added. Then, the mixture was heated to 35° C. and maintained for 2 h. Subsequently, the temperature was raised to 95° C. and maintained for 30 min.

[0170] Step 6: After cooling to room temperature, the reaction was terminated by adding deionized water (200 mL) and H2O2 solution (30%, 6 mL). The mixture was washed 4 times with HCl solution (HCl: water volume ratio of 1:10), and washed with deionized water until neutral to remove residual metal ions.

[0171] Step 7: After treating at a low temperature of 0°C with an ultrasonic frequency of 10 kHz for 2 hours, a graphene oxide dispersion is obtained. 5 mL of the graphene oxide dispersion is taken out with a pipette, placed in an oven at 50°C until completely dry, and the dispersion concentration is calculated by weighing, and a 2 mg / mL GO solution is prepared.

[0172] Step 8: Cut the prepared PI sample into a rectangular shape as a substrate, and then fix it on an A4 paper with transparent tape. Next, use a semiconductor laser with a wavelength of 450nm and a maximum power of 7W to irradiate the F 100 -PI film was laser-written. The laser power was set to 1.4W and the scanning speed was set to a fixed value of 100mm / s. 100 -The size of the LIG interdigital electrode patterns is 8*12mm.

[0173] Step 9: Apply conductive silver paste to the junction between the copper wire and the interdigital electrode to enhance the electrical contact. Finally, 100 μL of GO solution was dropped onto the interdigital electrode using a pipette, and the device was placed in a fume hood and dried naturally for 1 day under indoor conditions to form a uniform GO film.

[0174] Finally, fluorinated polyimide-based laser-induced graphene (F 100 -LIG / GO 2mg / mL ) humidity sensor.

[0175] The ratios of PI monomers with different fluorination degrees in the above embodiments and comparative examples can be shown in Table 1.

[0176] Table 1 Preparation of PI monomer ratios with different degrees of fluorination

[0177]

[0178]

[0179] Figure 1 This is a schematic diagram of the production process of F-LIG / GO humidity sensor. First, PI films with different degrees of fluorination are prepared by ternary copolymerization of 6FDA, BPADA and TPE-Q. F-PI films with different fluorine contents are obtained by introducing trifluoromethyl groups by adjusting the content of 6FDA in the anhydride. Then, a preset interdigitated electrode pattern is etched on the F-PI by laser. Then, the electrodes and copper wires are fixed with conductive silver paste and copper tape, and GO solution is dripped on. After GO is dried and formed into a film, the F-LIG humidity sensor is obtained. PI serves as both a precursor of LIG and a substrate of the humidity sensor to provide good flexible support.

[0180] Figure 2 is F in Example 1 75 -SEM image of LIG. It can be seen that it has a uniform and stable pore structure with a pore size of about 10 μm.

[0181] Figure 3 is F in Example 1 75 -LIG / GO 4mg / mLSEM image. It can be seen that the LIG pore structure is completely covered by GO, and its surface presents a worm-like structure, indicating that LIG and GO are tightly bound.

[0182] Figure 4 The GO and F obtained in Example 1 75 - Raman spectrum of LIG. In the Raman spectrum, we can clearly see the -1 The D peak caused by defects and 1580cm -1 The G peak is caused by the in-plane stretching vibration of sp2 hybridization of C atoms, where the D peak represents the amorphous carbon structure and the G peak represents the carbon-carbon bond stretching, proving that the prepared GO and LIG have typical graphene structures, and the intensity ratios of the D peak and the G peak are both less than 1, indicating a high degree of graphitization.

[0183] Figure 5 is the F obtained in Example 1 75 -PI, F 75 -LIG XPS spectrum. It can be found that the carbon content of laser-induced graphene is higher than that before laser treatment, while the F, N, and O contents are lower. This is because fluorinated carbon or aromatic polymers will defluorinate during pyrolysis at 1000°C to form a porous structure, especially the trifluoromethyl part (-CF 3 ) Additional gas products (such as CHF2, CH2F, and COF2) can be generated during laser photothermal treatment. In addition, part of the nitrogen element is also converted into nitrogen-containing gas, and the resulting heterogeneous and porous LIG structure has a high specific surface area.

[0184] Figure 6 is the F obtained in Example 1 75 -LIG C1s spectrum. From this we can see that there are still four C1s characteristic peaks, but the position of the CF bond peak has shifted from 293eV to 291eV, indicating that the trifluoromethyl group in PI has not completely turned into gas during the laser direct writing process, and some of the fluorine element still exists in the laser-induced graphene in the form of CF bonds.

[0185] Figure 7 is the F obtained in Example 1 75 - F1s spectrum of LIG. From this we can see that the F1s spectrum of LIG shows that there are two types of FC bonds, covalent bonds FC and semi-ionic bonds FC bonds (685.4 eV), proving that under the high-temperature laser etching, some FC bonds of the trifluoromethyl group of PI are broken, and the fluorine atoms combine with the carbon atoms at the defects of LIG to form semi-ionic CF bonds with strong polarity and conductivity, which corresponds to the shift of the CF bonds in the above C1s spectrum.

[0186] Figure 8The capacitance response curves of the humidity sensors prepared in Example 1, Example 2, Example 3 and Comparative Example 1 at different GO concentrations are shown. It can be seen that compared with the humidity sensor without GO, the addition of GO can increase the sensitivity of the humidity sensor by 3 orders of magnitude, and the higher the GO concentration, the greater the sensitivity. However, different GO concentrations have little effect on its capacitance change, and too high a concentration will affect the uniformity of the GO humidity-sensitive film, resulting in cracking and loose adhesion to LIG, and the humidity sensor is susceptible to damage. Therefore, for the operability of the experiment, a GO concentration of 4 mg / ml is the most appropriate.

[0187] Fig. 9 2 is the capacitance response curve of the humidity sensors with different fluorine contents prepared in Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5. It can be clearly observed that the humidity sensor with 75% fluorine content has the highest sensitivity and the highest linearity. This is due to the fact that F 75 -LIG has a uniform three-dimensional carbon structure, and its interconnected pores can serve as an excellent carrier for GO, increasing the contact area between GO and LIG, thereby providing more active sites for water molecules. In addition, the water contact angle of F0-LIG is 148.43°, which is a hydrophobic surface. With the increase of fluorine content, F 75 -LIG water contact angle decreased to 89.05°, which indicates that due to the doping of F, the change of pore structure improves the hydrophilicity of the electrode, strengthens the electrode's adsorption capacity for water, and thus improves the sensitivity of the sensor. 75 -LIG was dripped with GO on top to prepare a humidity sensor for research.

[0188] Fig.10 is the F obtained in Example 1 75 -LIG / GO4 mg / mL The sensing performance of humidity sensor. (a) is the dynamic response curve of capacitance in the relative humidity range of 11% to 97%; (b) is the dynamic response curve of capacitance repeated 6 times in the RH range of 11% to 75%; (c) is the response and recovery time in the RH range of 11% to 75%; (d) is the hysteresis curve of the sensor; (e) is the capacitance when the sensor is bent at different angles; (f) is the long-term stability of the sensor at 11%, 33%, 43%, 57%, 75%, and 97% relative humidity. The above sensing performances show that the humidity sensor has excellent long-term stability and can meet the research and development and application needs of wearable devices.

[0189] Fig.11 This is the assembly structure diagram of the intelligent integrated respiratory monitoring mask. From it we can see that the mask is highly integrated, light in weight and easy to wear.

[0190] Fig.12This is the real-time monitoring waveform of the smart integrated respiratory monitoring mask. From it, we can see that the functions developed by the APP include: remote real-time monitoring of the user's respiratory status (three types of respiratory status monitoring are set: slow breathing, normal breathing, and fast breathing; a normal adult breathes about 12-20 times per minute), and the APP sets a respiratory arrest (no breathing within 1 minute) alarm to remotely remind the user's family in real time. The waveform monitored by the APP in real time is accurate, stable, and very intelligent.

[0191] At present, some capacitive humidity sensors have been made, such as sputtering metal ions on polymer substrates, using vacuum filtration technology to deposit humidity-sensitive materials on paper, screen printing electrodes and humidity-sensitive films, etc. to achieve humidity sensing, but the electrode preparation process of these methods is usually complicated and time-consuming, which hinders their practical application in large-scale production. In the present invention, the humidity sensor is simple and reliable to make, does not require complicated process steps, and is easy to achieve mass production.

[0192] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.

Claims

1. A humidity sensor based on fluorinated polyimide-based laser-induced graphene F-LIG / GO drop-coated GO, characterized in that: The preparation method thereof comprises the following steps: Step 1, place TPE-Q in a three-necked flask, add DMAC, and mechanically stir until it is completely dissolved, then add 6FDA and BPADA into the three-necked flask in three batches, and mechanically stir to obtain a polyamic acid PAA solution; Step 2: The PAA solution is allowed to stand to remove bubbles, then poured onto a pre-cleaned glass plate, scraped into a film of uniform thickness, and the solvent is evaporated, and then a step-by-step thermal imidization is performed, followed by natural cooling, and the glass plate is placed in deionized water, and dried after natural shedding to obtain an F-PI film; Step 3, graphite powder, (NH4)2S2O8 and P2O5 are successively placed in H2SO4 solution, followed by heating and stirring; Step 4, washing the mixture with deionized water until the pH value of the filtrate becomes neutral, and drying the filtered solid under vacuum to obtain pre-oxidized graphite; Step 5, placing the pre-oxidized graphite in a H2SO4 solution in an ice water bath and stirring, slowly adding potassium permanganate, and continuously heating the mixture in a gradient manner; Step 6, after cooling to room temperature, adding deionized water and H2O2 solution to terminate the reaction, washing the mixture with HCl solution, and washing with deionized water until neutral to remove residual metal ions; Step 7, after the washed mixture is subjected to ultrasonic treatment at low temperature, the obtained graphene oxide dispersion is taken out with a pipette, placed in an oven and dried until completely dry, and then weighed to prepare a GO solution; Step 8: Cut the prepared PI sample into rectangles as a substrate, and then fix it on A4 paper with transparent tape. Use a semiconductor laser to perform laser direct writing on the F-PI film in an atmospheric atmosphere to obtain F-LIG interdigital electrodes. Step 9: Apply conductive silver paste to the connection between the copper wire and the interdigital electrode, and finally use a pipette to drop the GO solution on the interdigital electrode. Place the device in a fume hood and dry it naturally under indoor conditions to form a uniform GO film, and finally obtain a humidity sensor based on drop-coated GO fluorinated polyimide-based laser-induced graphene (F-LIG / GO).

2. The humidity sensor according to claim 1, characterized in that: The ratio of the mass of DMAC added in step 1 to the total mass of the remaining monomers is 17:3, the ratio of the total molar amount of 6FDA and BPADA to the molar amount of TPE-Q is 1:1, and they are added in three batches with an interval of 10 minutes each, and mechanically stirred for 4 hours to obtain a PAA solution with a solid content of 15%.

3. The humidity sensor according to claim 1, characterized in that: In step 2, the standing time is 12 h, the scraper distance is set to 200 μm, and the volatilization is performed at 80 ° C for 2 h; the step-by-step heating steps are as follows: 100 ° C for 1 h, 200 ° C for 1 h, and 250 ° C for 1 h. By controlling the amount of 6FDA, F with different fluorination degrees can be obtained. x -PI (x is the mole fraction of 6FDA in the anhydride, 0, 25, 50, 75, 100%) films.

4. The humidity sensor according to claim 1, characterized in that: In step 3, 2 g of 325 mesh graphite powder is used, the mass concentration of H2SO4 solution is 98%, and the mixture is heated to 80°C and stirred for 4 h; the ratio of graphite powder: (NH4)2S2O8: P2O5: H2SO4 solution is 2:2:2:10 in g:g:g:mL; Alternatively, in step 4, dry under vacuum for 2 h.

5. The humidity sensor according to claim 1, characterized in that: The mass concentration of the H2SO4 solution in step 5 is 98%; the continuous gradient heating steps are as follows: heating at 35°C for 2 hours, then heating to 95°C for 30 minutes; the ratio of pre-oxidized graphite: H2SO4 solution: potassium permanganate is 0.6:24:3 in g:mL:g; Alternatively, in step 6, the mass concentration of the H2O2 solution is 30%, the HCl solution is an HCl solution with a volume ratio of HCl: water of 1:10, and the number of washing times of the HCl solution washing mixture is 4 times; the ratio of pre-oxidized graphite: deionized water: H2O2 solution g: mL: mL is 0.6:200:

6.

6. The humidity sensor according to claim 1, characterized in that: In step 7, the low temperature is 0°C, the ultrasonic frequency is 10kHz, and the treatment is performed for 2h. 5 mL of the graphene oxide dispersion is taken out with a pipette, and the temperature of the oven is controlled at 50°C during drying; the concentration of the dispersion is calculated by weighing, and GO solutions of 1, 2, and 4 mg / mL are prepared.

7. The humidity sensor according to any one of claims 1 to 6, characterized in that: The wavelength of the semiconductor laser used in step 8 is 450nm, the maximum power is 7W, the laser power is set to 1.4W, and the scanning speed is set to a fixed value of 100mm / s. The obtained F x -The pattern size of LIG interdigitated electrodes is 8 mm*12 mm, where x is the mole fraction of 6FDA in the anhydride, i.e., 0, 25, 50, 75, and 100%; Alternatively, in step 9, the amount of GO solution applied by a pipette is 100 μL, and the natural drying time is 1 day.

8. Use of the humidity sensor according to any one of claims 1 to 7 in an integrated respiratory monitoring mask.

9. An intelligent integrated respiratory monitoring mask made using the humidity sensor according to any one of claims 1 to 7, characterized in that: The assembly method of the intelligent integrated respiratory monitoring mask comprises the following steps: The F-LIG / GO humidity sensor is placed inside the breathing mask and then connected to the AD converter, microcontroller, WIFI module, voltage regulator module and lithium battery through wires. After programming, all the above electronic components are integrated and placed outside the breathing mask.

10. The functional APP of the intelligent integrated respiratory monitoring mask as claimed in claim 9, characterized in that: The functional APP can remotely monitor the user's breathing status in real time, that is, it has three types of breathing status monitoring: slow breathing, normal breathing, and fast breathing; a normal adult breathes about 12-20 times per minute, and the APP has a respiratory arrest alarm, that is, no breathing within 1 minute, to remotely remind the user's family in real time.