Chemical electrode, preparation method, electrochemical sensor and application
By modifying the platinum nanoparticles and tyrosinase-loaded polyaniline surface on the flexible electrode, a chemical electrode for electrochemical sensors was constructed, and the levodopa in the prior art was solved The problem of detecting the problem that expensive instruments are required and the content cannot be measured quickly and accurately, achieving fast and accurate detection results, good stability and anti-interference.
Patent Information
- Application Number
- CN202411149832.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-15
AI Technical Summary
The detection method of levodopa in the prior art requires expensive instruments and cannot quickly and accurately determine its content, and cannot effectively control and prevent the side effects of levodopa.
A flexible electrode was used to modify the PAni-PtNPs/Tyr composite gel material supported by platinum nanoparticles and tyrosinase on the polyaniline surface to form a chemical electrode for levodopa concentration determination by electrochemical sensor.
Fast and accurate levodopa concentration determination is achieved, with excellent stability and anti-interference, providing a new idea for levodopa detection and avoiding the use of expensive instruments.
Smart Images

Figure CN118961849A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrochemical detection, and specifically discloses a chemical electrode, a preparation method, an electrochemical sensor and applications. Background Art
[0002] Levodopa belongs to the catecholamine class of substances, which is a very important neurological substance in the body. It has a wide range of regulatory effects on the human nervous system and organs, especially on maintaining the normal functioning of the kidneys, central nervous system, cardiovascular and cerebrovascular systems, and hormone systems. Since levodopa can pass through the blood-brain barrier into the brain tissue and is converted into dopamine in the brain, it can supplement the dopamine missing in the brain. Clinically, levodopa is often used to treat Parkinson's disease. Because levodopa has very important physiological functions, research on levodopa has become more and more extensive in recent years.
[0003] As the study of levodopa deepens, researchers have found that long-term use of levodopa can cause side effects such as hypotension, nausea, and arrhythmia. Therefore, the detection and control of levodopa concentration is of great significance for treating diseases and preventing side effects.
[0004] In the prior art, the detection methods of levodopa mainly include fluorescence spectroscopy, high performance liquid chromatography, flow injection method and ultraviolet spectrophotometry. These methods can all detect levodopa samples, but these methods require expensive instruments, complicated operations and skilled technicians. Some methods that can quickly detect levodopa have also been reported, which use specific fluorescent materials to combine levodopa to form copolymers to obtain fluorescence quenching or fluorescence enhancement, thereby achieving the purpose of rapid detection of levodopa. However, this detection method can only determine whether levodopa exists, and cannot accurately determine the content of levodopa, and still needs to further analyze and calculate its content with the help of a fluorescence spectrometer. Based on this, developing a detection method that can quickly and accurately determine the content of levodopa is of great significance for the control and application of levodopa. Summary of the invention
[0005] In view of the problem that the detection method of levodopa in the prior art requires the assistance of expensive instruments for determination and cannot quickly determine the content of levodopa, the present invention provides a chemical electrode, a preparation method, an electrochemical sensor and an application. The chemical electrode includes a flexible electrode and a PAni-PtNPs / Tyr composite gel material modified on the surface of the flexible electrode; wherein the PAni is polyaniline; the PtNPs are platinum nanoparticles; and the Tyr is tyrosinase. The electrochemical sensor using the chemical electrode can quickly and accurately determine the concentration of levodopa, and has excellent stability and anti-interference, providing a new design idea for the detection of levodopa.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: The first aspect of the present invention provides a chemical electrode, which includes a flexible electrode and a PAni-PtNPs / Tyr composite gel material modified on the surface of the flexible electrode; wherein the flexible electrode is an AgNWs composite PET electrode; the PAni-PtNPs / Tyr composite gel material is a composite gel material in which platinum nanoparticles and tyrosinase are loaded on the surface of polyaniline.
[0007] The present invention uses PET as a substrate, and coats a layer of AgNWs (silver nanowires) on its surface as a conductive layer to obtain a flexible electrode. Due to the presence of silver nanowires, the flexible electrode has a lower square resistance, is more conducive to charge transfer, and has better bending resistance and mechanical stability, so that the obtained chemical electrode has good working performance. At the same time, the present invention also loads a PAni-PtNPs / Tyr composite gel material on the surface of the flexible electrode, and the PAni-PtNPs / Tyr composite gel material is a composite gel material in which platinum nanoparticles and tyrosinase are loaded on the surface of polyaniline. Among them, polyaniline can form a conductive layered structure on the surface of the flexible electrode, has a large active specific surface area and abundant active sites, can make platinum nanoparticles evenly distributed on its surface, and increase conductivity. In addition, platinum nanoparticles can further amplify the electrocatalytic signal, which is conducive to the efficient detection of levodopa. Furthermore, since platinum nanoparticles have good biocompatibility, they can increase the stability of immobilized enzymes and effectively maintain the biological activity of enzymes. They can also further improve the electronic conductivity between the biological enzymes and the substrate electrode, effectively improving the working performance of the chemical electrode. Tyrosinase has at least two binding sites, one of which has affinity for aromatic compounds and is highly specific for the catalysis of the ortho-hydroxyl group of the substrate. Therefore, tyrosinase can catalyze L-dopa to form quinones, and reduce them on the surface of the chemical electrode to form electrical signals, thereby achieving efficient detection of phenolic substances.
[0008] The second aspect of the present invention provides a method for preparing the chemical electrode, comprising the following steps: Step 1: immersing the PET electrode in deionized water, a low-boiling point organic solvent and an alcohol solvent respectively, and after drying, performing ultraviolet ozone treatment to obtain a pretreated PET electrode; Step 2, dispersing AgNWs in an alcohol solution to obtain an AgNWs dispersion; spin coating the AgNWs dispersion on the pretreated PET electrode surface, and annealing to obtain a flexible electrode; Step 3, mixing the phytic acid solution and the aniline monomer evenly to obtain a first mixed solution; adding a polymerization initiator to the first mixed solution, mixing evenly, and keeping warm at 1° C.-5° C. to obtain a second mixed gel; Step 4: coating the second mixed gel on the surface of the flexible electrode, drying, washing, and obtaining a solid composite electrode; then immersing the solid composite electrode in a chloroplatinic acid solution, washing, and drying to obtain a PAni-PtNPs modified flexible electrode; Step 5: coating a coupling agent on the surface of the PAni-PtNPs modified flexible electrode, and dripping tyrosinase on the surface of the coupling agent, and drying to obtain a chemical electrode.
[0009] Preferably, in step 1, the low boiling point organic solvent is acetone.
[0010] Preferably, in step 1, the alcohol solvent is isopropanol and ethanol in a volume ratio of 0.1:1-0.2:1.
[0011] Preferably, in step 1, the drying is performed by blowing with nitrogen.
[0012] Preferably, in step 2, the mass volume ratio of the AgNWs to the alcohol solution is 5 mg:1 mL-8 mg:1 mL, wherein the alcohol solution is a 20 wt %-30 wt % isopropanol solution.
[0013] Preferably, in step 2, the method for preparing AgNWs comprises the following steps: S1. Dissolve polyvinyl pyrrolidone in ethylene glycol, and heat to 100°C-110°C until the solution becomes clear and transparent to obtain a mixed solvent; S2. Under an inert atmosphere, add sodium chloride solution and silver nitrate solution to the mixed solvent, react at 100°C-110°C for 20min-40min, then heat to 140°C-160°C for a secondary reaction for 1.5h-2h, filter, wash, and dry to obtain AgNWs.
[0014] Further preferably, in S1, the mass volume ratio of polyvinyl pyrrolidone and ethylene glycol is 0.5g:20mL-1g:50mL.
[0015] Further preferably, in S2, the concentration of the sodium chloride solution is 0.2 mol / L-0.4 mol / L.
[0016] Further preferably, in S2, the concentration of the silver nitrate solution is 0.2 mol / L-0.4 mol / L.
[0017] Further preferably, in S2, the added volume of the sodium chloride solution is 6%-7% of the volume of the mixed solvent.
[0018] Further preferably, in S2, the added volume of the silver nitrate solution is 20%-25% of the volume of the mixed solvent.
[0019] Further preferably, in S2, the diameter of the AgNWs is 20 nm-60 nm, and the length is 30 μm-50 μm.
[0020] Preferably, in step 2, the spin coating speed is 2000rpm-3000rpm, and the spin coating time is 50s-60s.
[0021] The spin coating speed can make the AgNWs dispersed more sparsely during the spin coating process, which is more conducive to charge transfer.
[0022] Preferably, in step 2, the annealing temperature is 90° C.-110° C., and the annealing time is 8 min-12 min.
[0023] Preferably, in step three, the volume ratio of the phytic acid solution to the aniline monomer is 5:1-7:1, wherein the mass percentage of phytic acid in the phytic acid solution is 40%-50%.
[0024] Preferably, in step three, the polymerization initiator is 1 mol / L-1.5 mol / L ammonium persulfate solution.
[0025] Preferably, in step three, the added volume of the polymerization initiator is 25%-35% of the volume of the first mixed solution.
[0026] Preferably, in step three, the insulation time is 10h-30h.
[0027] Preferably, in step 4, the coating thickness of the second mixed gel is 0.5 mm-1 mm.
[0028] Preferably, in step 4, the concentration of chloroplatinic acid in the chloroplatinic acid mixed solution is 1 mol / L-1.2 mol / L.
[0029] Preferably, in step 4, the immersion time is 1 min-4 min.
[0030] Preferably, in step five, the coupling agent is a PBS solution of glutaraldehyde, wherein the mass percentage of glutaraldehyde is 2%-3%; the concentration of the PBS solution is 0.2 mol / L-0.3 mol / L, and the pH is 5.8-6.2.
[0031] Further preferably, in step five, the mass ratio of the tyrosinase to the glutaraldehyde is 1:1-1:1.2.
[0032] A third aspect of the present invention provides an electrochemical sensor comprising the chemical electrode.
[0033] The fourth aspect of the present invention provides the use of the electrochemical sensor in detecting levodopa.
[0034] In summary, the present invention provides a chemical electrode, which includes a flexible electrode formed by AgNWs composite PET electrode and a PAni-PtNPs / Tyr composite gel material modified on the surface of the flexible electrode. The electrochemical sensor obtained by using the chemical electrode can achieve the purpose of rapid and efficient detection of levodopa without the need for expensive instruments. The technical solution of the present invention effectively solves the problem that the detection method of levodopa in the prior art requires the assistance of expensive instruments for determination and cannot quickly determine the content of levodopa, and provides a new idea for the detection of levodopa. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The DPV curve of the electrochemical sensor obtained in Experimental Example 1-4 for detecting levodopa; Figure 2 This is a standard curve diagram of the electrochemical sensor obtained in Experimental Example 1 for detecting levodopa. DETAILED DESCRIPTION
[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] The preparation method of AgNWs described in the following examples and comparative examples comprises the following steps: S1. Disperse 0.5 g of polyvinyl pyrrolidone in 23 mL of ethylene glycol, heat to 105° C., and stir at 500 rpm for 1 h until the solution becomes clear and transparent to obtain a mixed solvent; S2. Under an inert atmosphere, add 1.5 mL of 0.3 mol / L sodium chloride solution and 5 mL of 0.3 mol / L silver nitrate solution to the mixed solvent, react at 105° C. for 30 min, then heat to 150° C. for a secondary reaction for 1.5 h, filter, wash, and dry to obtain AgNWs.
[0038] Example 1 This embodiment provides a chemical electrode, which specifically includes the following contents: The chemical electrode comprises an AgNWs composite PET electrode and a PAni-PtNPs / Tyr composite gel material modified on the surface of the AgNWs composite PET electrode; wherein the PAni is polyaniline; the PtNPs are platinum nanoparticles; and the Tyr is tyrosinase.
[0039] Step 1: ultrasonically immerse the PET electrode in deionized water, acetone and alcohol solvent for 30 minutes respectively, blow dry with nitrogen, and treat with ultraviolet ozone for 30 minutes to obtain a pretreated PET electrode; wherein the alcohol solvent is a mixed solvent of isopropanol and ethanol in a volume ratio of 0.1:1; Step 2: Disperse 6 mg of AgNWs in 1 mL of 25 wt% isopropanol solution to obtain an AgNWs dispersion; spin-coat the AgNWs dispersion on the pretreated PET electrode surface at a speed of 2500 rpm for 50 s. After spin coating, let stand for 5 min, transfer the electrode to a drying oven, and anneal at 100 ° C for 10 min to obtain a flexible electrode; Step 3: Evenly mix 5 mL of 45 wt% phytic acid solution and 1 mL of aniline monomer to obtain a first mixed solution; add 1.5 mL of 1 mol / L sodium persulfate solution to the first mixed solution, mix evenly, and keep warm at 4° C. for 24 h to obtain a second mixed gel; Step 4: coating the second mixed gel on the surface of the flexible electrode with a coating thickness of 0.8 mm, and then immersing the electrode in deionized water for cleaning after natural drying for 10 minutes to obtain a solid composite electrode; then immersing the solid composite electrode in a 1 mol / L chloroplatinic acid solution for 3 minutes, washing with deionized water twice after solid-liquid separation, and drying at 80°C for 30 minutes to obtain a PAni-PtNPs modified flexible electrode; Step 5: Add a coupling agent to the surface of the PAni-PtNPs modified flexible electrode, and add tyrosinase to the surface of the coupling agent, dry naturally, and store at 4° C. to obtain a chemical electrode.
[0040] The coupling agent is a PBS solution containing 3 wt % glutaraldehyde, wherein the concentration of the PBS solution is 0.3 mol / L and the pH is 6.
[0041] Example 2 This embodiment provides a chemical electrode, which specifically includes the following contents: The chemical electrode comprises an AgNWs composite PET electrode and a PAni-PtNPs / Tyr composite gel material modified on the surface of the AgNWs composite PET electrode; wherein the PAni is polyaniline; the PtNPs are platinum nanoparticles; and the Tyr is tyrosinase.
[0042] Step 1: ultrasonically immerse the PET electrode in deionized water, acetone and alcohol solvent for 25 minutes respectively, blow dry with nitrogen, and treat with ultraviolet ozone for 25 minutes to obtain a pretreated PET electrode; wherein the alcohol solvent is a mixed solvent of isopropanol and ethanol in a volume ratio of 0.2:1; Step 2: Disperse 5 mg of AgNWs in 1 mL of 20 wt% isopropanol solution to obtain an AgNWs dispersion; spin-coat the AgNWs dispersion on the pretreated PET electrode surface at a speed of 3000 rpm for 50 s. After spin coating, let stand for 5 min, transfer the electrode to a drying oven, and anneal at 100 ° C for 9 min to obtain a flexible electrode; Step 3: Mix 6 mL of 45 wt% phytic acid solution and 1 mL of aniline monomer to obtain a first mixed solution; add 2 mL of 1 mol / L sodium persulfate solution to the first mixed solution, mix well, and keep warm at 4° C. for 24 hours to obtain a second mixed gel; Step 4: coating the second mixed gel on the surface of the flexible electrode with a coating thickness of 0.8 mm, and then immersing the electrode in deionized water for cleaning after natural drying for 10 minutes to obtain a solid composite electrode; then immersing the solid composite electrode in a 1.2 mol / L chloroplatinic acid solution for 3 minutes, washing with deionized water twice after solid-liquid separation, and drying at 80°C for 30 minutes to obtain a PAni-PtNPs modified flexible electrode; Step 5: Add a coupling agent to the surface of the PAni-PtNPs modified flexible electrode, and add tyrosinase to the surface of the coupling agent, dry naturally, and store at 4° C. to obtain a chemical electrode.
[0043] The coupling agent is a PBS solution containing 2.5 wt % glutaraldehyde, wherein the concentration of the PBS solution is 0.2 mol / L and the pH is 6.
[0044] Example 3 This embodiment provides a chemical electrode, which specifically includes the following contents: The chemical electrode comprises an AgNWs composite PET electrode and a PAni-PtNPs / Tyr composite gel material modified on the surface of the AgNWs composite PET electrode; wherein the PAni is polyaniline; the PtNPs are platinum nanoparticles; and the Tyr is tyrosinase.
[0045] Step 1: ultrasonically immerse the PET electrode in deionized water, acetone and alcohol solvent for 30 minutes respectively, blow dry with nitrogen, and treat with ultraviolet ozone for 35 minutes to obtain a pretreated PET electrode; wherein the alcohol solvent is a mixed solvent of isopropanol and ethanol in a volume ratio of 0.2:1; Step 2: Disperse 6 mg of AgNWs in 1 mL of 20 wt% isopropanol solution to obtain an AgNWs dispersion; spin-coat the AgNWs dispersion on the pretreated PET electrode surface at a speed of 2800 rpm for 50 s. After spin coating, let stand for 5 min, transfer the electrode to a drying oven, and anneal at 90 ° C for 12 min to obtain a flexible electrode; Step 3: Mix 5 mL of 45 wt% phytic acid solution and 1 mL of aniline monomer to obtain a first mixed solution; add 1.5 mL of 1.2 mol / L sodium persulfate solution to the first mixed solution, mix well, and keep warm at 4° C. for 24 hours to obtain a second mixed gel; Step 4: coating the second mixed gel on the surface of the flexible electrode with a coating thickness of 1 mm, and then immersing the electrode in deionized water for cleaning after natural drying for 10 minutes to obtain a solid composite electrode; then immersing the solid composite electrode in a 1 mol / L chloroplatinic acid solution for 3 minutes, washing with deionized water twice after solid-liquid separation, and drying at 80°C for 30 minutes to obtain a PAni-PtNPs modified flexible electrode; Step 5: Add a coupling agent to the surface of the PAni-PtNPs modified flexible electrode, and add tyrosinase to the surface of the coupling agent, dry naturally, and store at 4° C. to obtain a chemical electrode.
[0046] The coupling agent is a PBS solution containing 3 wt % glutaraldehyde, wherein the concentration of the PBS solution is 0.3 mol / L and the pH is 6.
[0047] Comparative Example 1 This embodiment provides a chemical electrode, which is different from the embodiment 1 in that the electrode is a PET electrode, and specifically includes the following contents: The chemical electrode comprises a PET electrode and a PAni-PtNPs / Tyr composite gel material modified on the surface of the AgNWs composite PET electrode; wherein the PAni is polyaniline; the PtNPs are platinum nanoparticles; and the Tyr is tyrosinase.
[0048] Step 1: ultrasonically immerse the PET electrode in deionized water, acetone and alcohol solvent for 30 minutes respectively, blow dry with nitrogen, and treat with ultraviolet ozone for 30 minutes to obtain a pretreated PET electrode; wherein the alcohol solvent is a mixed solvent of isopropanol and ethanol in a volume ratio of 0.1:1; Step 2: Evenly mix 5 mL of 45 wt% phytic acid solution and 1 mL of aniline monomer to obtain a first mixed solution; add 1.5 mL of 1 mol / L sodium persulfate solution to the first mixed solution, mix evenly, and keep warm at 4° C. for 24 hours to obtain a second mixed gel; Step 4: coating the second mixed gel on the surface of the pretreated PET electrode with a coating thickness of 0.8 mm, and then immersing the electrode in deionized water for cleaning after natural drying for 10 minutes to obtain a solid composite electrode; then immersing the solid composite electrode in a 1 mol / L chloroplatinic acid solution for 3 minutes, washing with deionized water twice after solid-liquid separation, and drying at 80°C for 30 minutes to obtain a PAni-PtNPs modified PET electrode; Step 5: Add a coupling agent to the surface of the PAni-PtNPs-modified PET electrode, and add tyrosinase to the surface of the coupling agent, dry naturally, and store at 4° C. to obtain a chemical electrode.
[0049] The coupling agent is a PBS solution containing 3 wt % glutaraldehyde, wherein the concentration of the PBS solution is 0.3 mol / L and the pH is 6.
[0050] Comparative Example 2 This embodiment provides a chemical electrode, which is different from the embodiment 1 in that the gel material is a PtNPs / Tyr composite gel material, specifically including the following contents: The chemical electrode comprises an AgNWs composite PET electrode and a PtNPs / Tyr composite gel material modified on the surface of the AgNWs composite PET electrode; wherein the PtNPs are platinum nanoparticles and the Tyr is tyrosinase.
[0051] Step 1: ultrasonically immerse the PET electrode in deionized water, acetone and alcohol solvent for 30 minutes respectively, blow dry with nitrogen, and treat with ultraviolet ozone for 30 minutes to obtain a pretreated PET electrode; wherein the alcohol solvent is a mixed solvent of isopropanol and ethanol in a volume ratio of 0.1:1; Step 2: Disperse 6 mg of AgNWs in 1 mL of 25 wt% isopropanol solution to obtain an AgNWs dispersion; spin-coat the AgNWs dispersion on the pretreated PET electrode surface at a speed of 2500 rpm for 50 s. After spin coating, let stand for 5 min, transfer the electrode to a drying oven, and anneal at 100 ° C for 10 min to obtain a flexible electrode; Step 4, immersing the flexible electrode in a 1 mol / L chloroplatinic acid solution for 3 min, washing with deionized water twice after solid-liquid separation, and drying at 80° C. for 30 min to obtain a PtNPs-modified flexible electrode; Step 5: Add a coupling agent to the surface of the PtNPs-modified flexible electrode, and add tyrosinase to the surface of the coupling agent, dry naturally, and store at 4° C. to obtain a chemical electrode.
[0052] The coupling agent is a PBS solution containing 3 wt % glutaraldehyde, wherein the concentration of the PBS solution is 0.3 mol / L and the pH is 6.
[0053] Comparative Example 3 This embodiment provides a chemical electrode, which is different from the embodiment 1 in that the gel material is a PAni / Tyr composite gel material, specifically including the following contents: The chemical electrode comprises an AgNWs composite PET electrode and a PAni / Tyr composite gel material modified on the surface of the AgNWs composite PET electrode; wherein the PAni is polyaniline; and the Tyr is tyrosinase.
[0054] Step 1: ultrasonically immerse the PET electrode in deionized water, acetone and alcohol solvent for 30 minutes respectively, blow dry with nitrogen, and treat with ultraviolet ozone for 30 minutes to obtain a pretreated PET electrode; wherein the alcohol solvent is a mixed solvent of isopropanol and ethanol in a volume ratio of 0.1:1; Step 2: Disperse 6 mg of AgNWs in 1 mL of 25 wt% isopropanol solution to obtain an AgNWs dispersion; spin-coat the AgNWs dispersion on the pretreated PET electrode surface at a speed of 2500 rpm for 50 s. After spin coating, let stand for 5 min, transfer the electrode to a drying oven, and anneal at 100 ° C for 10 min to obtain a flexible electrode; Step 3: Evenly mix 5 mL of 45 wt% phytic acid solution and 1 mL of aniline monomer to obtain a first mixed solution; add 1.5 mL of 1 mol / L sodium persulfate solution to the first mixed solution, mix evenly, and keep warm at 4° C. for 24 h to obtain a second mixed gel; Step 4: coating the second mixed gel on the surface of the flexible electrode with a coating thickness of 0.8 mm, drying naturally for 10 min, and then immersing the electrode in deionized water for cleaning to obtain a PANi-modified flexible electrode; Step 5: Add a coupling agent to the surface of the PANi-modified flexible electrode, and add tyrosinase to the surface of the coupling agent, dry naturally, and store at 4° C. to obtain a chemical electrode.
[0055] The coupling agent is a PBS solution containing 3 wt % glutaraldehyde, wherein the concentration of the PBS solution is 0.3 mol / L and the pH is 6.
[0056] Test Example 1 The chemical electrode obtained in Example 1 was used as the working electrode, the platinum electrode was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode to assemble a three-electrode test system, and connected to an electrochemical workstation to obtain an electrochemical sensor for levodopa detection.
[0057] Test Example 2 The chemical electrode obtained in Comparative Example 1 was used as the working electrode, the platinum electrode was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode to assemble a three-electrode test system, which was then connected to an electrochemical workstation to obtain an electrochemical sensor for levodopa detection.
[0058] Test Example 3 The chemical electrode obtained in Comparative Example 2 was used as the working electrode, the platinum electrode was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode to assemble a three-electrode test system, and connected to an electrochemical workstation to obtain an electrochemical sensor for levodopa detection.
[0059] Test Example 4 The chemical electrode obtained in Comparative Example 3 was used as the working electrode, the platinum electrode was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode to assemble a three-electrode test system, and connected to an electrochemical workstation to obtain an electrochemical sensor for levodopa detection.
[0060] In order to further demonstrate the technical effect of the present invention, the present invention conducted the following tests on the electrochemical sensors obtained in Experimental Examples 1-4: 1.1 Differential Pulse Voltammetry (DPV) Test conditions: potential range -0.4~1.0V, potential increment 0.01V, amplitude 0.05V, pulse width 0.2s; Test solution: accurately weigh the levodopa sustained-release tablets and grind them into powder, add 0.1 mol / L dilute hydrochloric acid solution to make it solvent, transfer to a 100 mL volumetric flask, add ultrapure water to make up to volume to obtain the sample solution; take 1 mL of the sample solution and dilute it 5 times with PBS solution to obtain the test solution; the results are as follows Figure 1 shown.
[0061] according to Figure 1 It can be seen that the electrochemical sensors made from the four chemical electrodes of Example 1 and Comparative Examples 1-3 all have independent oxidation current responses at 0.64V, but the response of the electrochemical sensor made using the chemical electrode provided in Example 1 is the most sensitive, which indicates that the chemical electrode provided by the present invention can effectively detect levodopa.
[0062] 1.2 Standard curve The present invention uses the electrochemical sensor obtained in Experimental Example 1 to detect a series of DPV response curves of levodopa sample solutions with different concentrations (2-100 μmol / L), and plots the oxidation peak current of levodopa sample solutions of various concentrations at 0.64 V. The results are shown in FIG. Figure 2 shown.
[0063] according to Figure 2It can be seen that the oxidation peak current of L-DOPA shows a good linear relationship with the L-DOPA sample concentration in the range of 2-100 μmol / L. The linear equation is y=0.0283X+0.6741, and the correlation coefficient is R 2 =0.9913, and the minimum detection limit was 0.76μmol / L.
[0064] 1.3 Stability test According to the steps of Example 1, 6 chemical electrodes were prepared, and the 6 chemical electrodes were used as working electrodes, the platinum electrode was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode to assemble a three-electrode test system, and connected to an electrochemical workstation to obtain an electrochemical sensor for levodopa detection. The levodopa sample solution of the same concentration was measured by differential pulse voltammetry, and the measurement parameters were: potential range -0.4~1.0V, potential increment of 0.01V, amplitude of 0.05V, pulse width of 0.2s; the relative standard deviation of the measurement was 2.01%; One of the chemical electrodes was stored in a refrigerator at 4°C, and the above test was performed on it at 6 different time periods. The relative standard deviation was 1.98%, which indicates that the chemical electrode provided by the present invention has good stability.
[0065] 1.4 Anti-interference test In order to further investigate the detection specificity of the chemical electrode for levodopa samples, the present invention adds common coexisting substances such as ascorbic acid, uric acid, dopamine and carbodopa to the levodopa sample, and detects the levodopa content in the composite sample. The chemical electrode provided in Example 1 is used as the working electrode, the platinum electrode is used as the counter electrode, and the Ag / AgCl electrode is used as the reference electrode to assemble a three-electrode test system, and the electrochemical workstation is connected to obtain an electrochemical sensor for detection. The results show that the electrochemical sensor can only specifically identify levodopa; after 5 parallel measurements, the result error is only 0.01%. This shows that the electrochemical sensor provided by the present invention has good anti-interference performance.
[0066] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A chemical electrode, characterized in that: The chemical electrode comprises a flexible electrode and a PAni-PtNPs / Tyr composite gel material modified on the surface of the flexible electrode; wherein the flexible electrode is an AgNWs composite PET electrode; and the PAni-PtNPs / Tyr composite gel material is a composite gel material in which platinum nanoparticles and tyrosinase are loaded on the surface of polyaniline.
2. The method for preparing a chemical electrode according to claim 1, characterized in that: The steps include: Step 1: immersing the PET electrode in deionized water, a low-boiling point organic solvent and an alcohol solvent respectively, and after drying, performing ultraviolet ozone treatment to obtain a pretreated PET electrode; Step 2, dispersing AgNWs in an alcohol solution to obtain an AgNWs dispersion; spin coating the AgNWs dispersion on the pretreated PET electrode surface, and annealing to obtain a flexible electrode; Step 3, mixing the phytic acid solution and the aniline monomer evenly to obtain a first mixed solution; adding a polymerization initiator to the first mixed solution, mixing evenly, and keeping warm at 1° C.-5° C. to obtain a second mixed gel; Step 4, coating the second mixed gel on the surface of the flexible electrode, drying, and washing to obtain a solid composite electrode; Then, the solid composite electrode is immersed in a chloroplatinic acid solution, washed, and dried to obtain a PAni-PtNPs modified flexible electrode; Step 5: coating a coupling agent on the surface of the PAni-PtNPs modified flexible electrode, and dripping tyrosinase on the surface of the coupling agent, and drying to obtain a chemical electrode.
3. The method for preparing a chemical electrode according to claim 2, characterized in that: In step 1, the low boiling point organic solvent is acetone; and / or In step 1, the alcohol solvent is isopropanol and ethanol in a volume ratio of 0.1:1-0.2:1; and / or In step 1, the drying is performed by blowing with nitrogen.
4. The method for preparing a chemical electrode according to claim 2, characterized in that: In step 2, the mass volume ratio of the AgNWs to the alcohol solution is 5 mg:1 mL-8 mg:1 mL, wherein the alcohol solution is a 20 wt %-30 wt % isopropanol solution; and / or In step 2, the spin coating speed is 2000rpm-3000rpm, and the spin coating time is 50s-60s; and / or In step 2, the annealing temperature is 90° C.-110° C., and the annealing time is 8 min-12 min.
5. The method for preparing a chemical electrode according to claim 2, characterized in that: In step 3, the volume ratio of the phytic acid solution to the aniline monomer is 5:1-7:1; wherein the mass percentage of phytic acid in the phytic acid solution is 40%-50%; and / or In step 3, the polymerization initiator is 1 mol / L-1.5 mol / L ammonium persulfate solution; and / or In step 3, the volume of the polymerization initiator added is 25%-35% of the volume of the first mixed solution; and / or In step 3, the insulation time is 10h-30h.
6. The method for preparing a chemical electrode according to claim 2, characterized in that: In step 4, the coating thickness of the second mixed gel is 0.5 mm-1 mm; and / or In step 4, the concentration of the chloroplatinic acid solution is 1 mol / L-1.2 mol / L; and / or In step 4, the immersion time is 1 min-4 min.
7. The method for preparing a chemical electrode according to claim 2, characterized in that: In step five, the coupling agent is a PBS solution of glutaraldehyde, wherein the mass percentage of glutaraldehyde is 2%-3%; the concentration of the PBS solution is 0.2mol / L-0.3mol / L, and the pH is 5.8-6.
2.
8. The method for preparing a chemical electrode according to claim 7, characterized in that: In step 5, the mass ratio of the tyrosinase to the glutaraldehyde is 1:1-1:1.
2.
9. An electrochemical sensor, characterized in that: Comprising the chemical electrode as claimed in claim 1.
10. Use of the electrochemical sensor according to claim 9 in detecting levodopa.
Citation Information
Cited By
Levodopa specific sensing electrode based on local acidification of hollow confinement structure as well as preparation method and application of levodopa specific sensing electrode
CN119413870A