Modified manganese-based positive electrode material as well as preparation method and application thereof
By doping iron and oxygen elements in the manganese-based positive electrode material and doping metal and fluorine elements on the surface, the problems of low conductivity and Mn element dissolution of the manganese-based positive electrode material are solved, and the circulation performance and capacity of the battery are significantly improved. .
Patent Information
- Application Number
- CN202410977604.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-15
AI Technical Summary
Manganese-based positive electrode materials such as lithium manganese ferroferric phosphate have low electronic conductivity and Mn elements are easily dissolved during the battery cycle, resulting in low energy conversion efficiency of the battery, poor rate performance and reduced cycle stability, limiting its commercial application.
By doping iron and oxygen elements and doping metal doped elements and fluorine elements on the surface of the manganese-based positive electrode material, the lattice stability and electronic conductivity of the manganese-based positive electrode material are enhanced, the dissolution of Mn elements is suppressed, and discharge is improved. Specific capacity and cycle performance.
It significantly improves the electronic conductivity of manganese-based positive electrode material and the redox stability of lattice oxygen, extends the Mn platform, improves the capacity and circulation performance of the battery, reduces polarization, and improves the energy density and circulation performance of the battery. .
Smart Images

Figure CN118969979A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of battery technology, and specifically relates to a modified manganese-based positive electrode material and a preparation method and application thereof. Background Art
[0002] Among many positive electrode materials, manganese-based positive electrode materials represented by lithium manganese iron phosphate (LMFP) have the advantages of low cost, high safety and good environmental friendliness, but they also have some shortcomings, which restrict the commercial application of manganese-based positive electrode materials. The main shortcomings restricting the application of manganese-based positive electrode materials include:
[0003] (1) The electronic conductivity and lithium ion (Li+) conductivity of manganese-based positive electrode materials such as LMFP are relatively low, which leads to low energy conversion efficiency during the battery charging and discharging process, affecting the battery's rate performance and rapid charging and discharging capabilities; (2) The Mn element is easily dissolved during the battery cycle, resulting in loss of active substances, which in turn causes battery capacity decay and decreased cycle stability. This is one of the main obstacles restricting the large-scale application of LMFP. Summary of the invention
[0004] The purpose of the present application is to overcome the above-mentioned deficiencies of the prior art and to provide a modified manganese-based positive electrode material and a preparation method thereof, so as to solve the technical problems of the existing manganese-based positive electrode materials having poor electronic conductivity and easy dissolution of manganese leading to reduced cyclability and capacity.
[0005] In order to achieve the above application purpose, the first aspect of the present application provides a modified manganese-based positive electrode material. The modified manganese-based positive electrode material of the present application includes a doped manganese-based positive electrode material, wherein the doped manganese-based positive electrode material contains iron and oxygen elements, and also contains a metal doping element and a fluorine element; wherein the metal doping element replaces the iron position, and its ion radius is smaller than the iron ion radius; the fluorine element is doped in the particle surface layer of the manganese-based positive electrode material and replaces the oxygen position.
[0006] The modified manganese-based positive electrode material of the present application is doped with a metal doping element and a F element that are smaller than the radius of an iron ion. The two doping elements play a synergistic role in doping, so that the electron cloud density around the Mn element in the lattice of the doped manganese-based positive electrode material is effectively increased, which significantly inhibits the Mn 3+ The lattice distortion of Mn enhances the stability of the crystal structure of the doped manganese-based cathode material, thereby significantly reducing the 2+The dissolution of the manganese-doped positive electrode material prolongs the Mn platform of the manganese-doped positive electrode material, improves the discharge specific capacity of the Mn segment, and ultimately effectively improves the capacity utilization and cycle performance of the manganese-doped positive electrode material. At the same time, it also improves the electronic conductivity and lattice oxygen redox stability of the manganese-doped positive electrode material. After using the modified manganese-based positive electrode material of the embodiment of the present application as a battery positive electrode material, the polarization of the battery is reduced, which can improve the capacity utilization of the battery, thereby improving the discharge specific capacity and cycle performance of the battery.
[0007] The second aspect of the present application provides a method for preparing the modified manganese-based positive electrode material of the present application. The method for preparing the modified manganese-based positive electrode material of the present application comprises the following steps:
[0008] In a plasma environment, a gaseous fluorine source is used to etch a manganese-based positive electrode material, and a fluorine element is doped into a particle surface layer of the manganese-based positive electrode material to obtain a modified manganese-based positive electrode material;
[0009] The manganese-based positive electrode material contains iron, oxygen and metal doping elements, and the ion radius of the metal doping element is smaller than the ion radius of the iron.
[0010] The preparation method of the modified manganese-based positive electrode material of the present application combines plasma, uses a fluorine source to fluorine etch and dope manganese-based positive electrode material particles doped with metal elements smaller than iron ions, and dopes the surface of manganese-based positive electrode material particles containing metal doping elements, so that the two doping elements can play a synergistic role in doping, so that the electron cloud density around the Mn element in the lattice of the doped manganese-based positive electrode material is effectively increased, and the Mn 3+ Lattice distortion occurs, which enhances the stability of the crystal structure of the doped manganese-based cathode material, thereby significantly reducing the Mn 2+ The dissolution of manganese-doped positive electrode materials prolongs the Mn platform of the manganese-doped positive electrode materials, increases the discharge specific capacity of the Mn segment, and also improves the electronic conductivity and lattice oxygen redox stability of the manganese-doped positive electrode materials.
[0011] In a third aspect of the present application, a positive electrode sheet is provided. The positive electrode sheet of the present application comprises a positive electrode current collector and a positive electrode active layer bonded to the surface of the positive electrode current collector, wherein the positive electrode active layer contains the modified manganese-based positive electrode material of the present application or the modified manganese-based positive electrode material prepared by the modified manganese-based positive electrode material preparation method of the present application.
[0012] The positive electrode sheet of the present application has good cycle performance and high capacity density.
[0013] In a fourth aspect of the present application, a battery is provided. The battery of the present application comprises a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet is the positive electrode sheet of the present application.
[0014] The battery of the present application has high energy density, discharge specific capacity and excellent cycle performance, high capacity retention rate and long life. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0016] Figure 1 This is a schematic diagram of the F element doping structure in the doped manganese-based positive electrode material contained in the modified manganese-based positive electrode material of the embodiment of the present application;
[0017] Figure 2 This is a schematic diagram of the structure of the coating layer contained in the modified manganese-based positive electrode material of the embodiment of the present application;
[0018] Figure 3 A schematic structural diagram of a coating layer included in a modified manganese-based positive electrode material according to an embodiment of the present application, including a metal fluoride coating layer;
[0019] Figure 4 A schematic diagram of the structure of the coating layer contained in the modified manganese-based positive electrode material according to an embodiment of the present application, including a metal fluoride coating layer and other functional coating layers;
[0020] Figure 5 X-ray diffraction patterns of the modified manganese-based positive electrode materials provided in Examples 1 to 3 and the manganese-based positive electrode materials provided in Comparative Examples 1 to 2; wherein, Figure 5 Figure b is an enlarged curve diagram of Figure a;
[0021] Figure 6 Scanning electron microscope (SEM) images of the modified manganese-based positive electrode materials provided in Examples 1 to 3 and the manganese-based positive electrode materials provided in Comparative Examples 1 to 2;
[0022] Figure 7 The cycle curves of the lithium-ion battery containing the modified manganese-based positive electrode materials in Example 2 and Comparative Example 1 at 0.1 and 1C;
[0023] Figure 8 Graphs showing different high temperature cycle curves of lithium ion batteries containing the modified manganese-based positive electrode materials in Example 2 and Comparative Example 1 at 0.1 and 1C.
[0024] The reference numerals in the specific implementation manner are as follows:
[0025] 10-doped manganese-based positive electrode material, 11-surface layer;
[0026] 20-coating layer, 21-metal fluoride coating layer, 22-other functional coating layer. DETAILED DESCRIPTION
[0027] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0028] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0029] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0030] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0031] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0032] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0033] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0034] As the world pays more and more attention to clean energy and sustainable development, lithium-ion batteries, as efficient energy storage devices, have shown great application potential in electric vehicles, portable electronic devices, energy storage systems and other fields. As a key component of lithium-ion batteries, the performance of positive electrode materials directly determines the overall performance and cost of the battery. Among the many positive electrode materials, manganese-based materials, especially lithium manganese iron phosphate (LMFP for short), are regarded as strong candidates for the next generation of lithium-ion battery positive electrode materials due to their low cost, high safety and good environmental friendliness.
[0035] However, despite the many advantages of manganese-based materials, their commercialization process is still limited by a series of technical bottlenecks. First, the electronic conductivity of manganese-based materials such as LMFP is relatively low, which leads to low energy conversion efficiency during the battery charging and discharging process, affecting the battery's rate performance and rapid charging and discharging capabilities; secondly, the Mn element is easily dissolved during the battery cycle, resulting in loss of active substances, which in turn causes battery capacity decay and decreased cycle stability, which is one of the main obstacles to the large-scale application of manganese-based materials.
[0036] Research has found that the problem of Mn dissolution in manganese-based materials is mainly due to the structural instability of manganese-based materials during charge and discharge cycles. Especially under high voltage or high temperature conditions, Mn ions are easily released from the lattice and dissolved into the electrolyte, which not only reduces the energy density and cycle life of the battery, but also may pose a threat to the safety of the battery. Therefore, how to effectively inhibit Mn dissolution and improve the structural stability and cycle performance of manganese-based materials has become a hot topic and difficulty in current research.
[0037] At present, there are reports of coating manganese-based cathode materials with metal oxides (Al2O3, ZrO2, etc.), phosphates (Li3PO4, etc.) or polymers (PEDOT, PPy, etc.), or doping manganese-based cathode materials in an attempt to change their crystal structure and inhibit the dissolution of manganese. However, studies have found that these current methods are still not ideal in improving the electronic conductivity and crystal structure stability of manganese-based materials and inhibiting the dissolution of manganese elements. At the same time, they will also lead to a decrease in other electrochemical properties of manganese-based cathode materials and an increase in cost.
[0038] In order to effectively improve the electronic conductivity of manganese-based positive electrode materials and enhance the stability of their crystal structure, reducing the Mn 2+ The present invention provides a modified manganese-based positive electrode material, a preparation method thereof, and an application thereof in a battery.
[0039] In the first aspect, the embodiment of the present application provides a modified manganese-based positive electrode material. The modified manganese-based positive electrode material of the embodiment of the present application includes a doped manganese-based positive electrode material. The doped manganese-based positive electrode material contains iron (Fe) and oxygen (O), and also contains a metal doping element and a fluorine (F) element; wherein the metal doping element replaces the iron position, and its ion radius is smaller than that of Fe. 2+ ion radius; the F element is doped in the particle surface of the manganese-based positive electrode material and replaces the oxygen site.
[0040] In the doped manganese-based positive electrode material, the manganese-based positive electrode material containing Fe and O elements constitutes the positive electrode material matrix. The F element and the metal doping element dope the manganese-based positive electrode material. Therefore, the manganese-based positive electrode material doped with the F element and the metal doping element contains the F element, the metal doping element, the manganese element (Mn), the Fe element and the O element at the same time, and of course, it can also contain other elements contained in the manganese-based positive electrode material. Among them, the F element is doped in the surface layer of the manganese-based positive electrode material, and the surface layer refers to the doping area at a certain distance from the surface of the manganese-based positive electrode material to the inside of the particle, and the doping depth of the doping area is less than the particle radius of the modified manganese-based positive electrode material.
[0041] The modified manganese-based positive electrode material of the present application embodiment has an ion radius smaller than that of the iron ion (generally Fe) in the iron position of the doped manganese-based positive electrode material. 2+ ) radius of the metal doping element, so after the metal doping element replaces the iron position, the unit cell parameters and unit cell volume of the doped manganese-based positive electrode material are significantly reduced compared with the manganese-based positive electrode material, which shortens the Mn-O bond length in the unit cell of the doped manganese-based positive electrode material, thereby inhibiting the Mn 3+ The lattice distortion of the manganese-doped cathode material enhances the stability of the crystal structure of the manganese-doped cathode material. At the same time, the doping of the iron site with metal doping elements introduces impurity energy levels into the manganese-based cathode material, which makes the manganese-doped cathode material have a narrower bandgap than the manganese-based cathode material, and significantly improves the electronic conductivity of the manganese-doped cathode material.
[0042] The F element doped in the surface layer of the doped manganese-based cathode material has a stronger electronegativity than the O element. The F element replaces the oxygen position in the surface layer, which can significantly increase the redox potential of the anions in the doped manganese-based cathode material, thereby improving the stability of the lattice oxygen in the doped manganese-based cathode material, and thus effectively inhibiting the Mn 2+ At the same time, since the F ion is -1 and the O ion is -2, the F - Replace O 2- After that, F- The electron cloud density of the surrounding metal elements has been increased, which indirectly increases the electron cloud density around the Mn element and suppresses the Mn 3+ The formation of Mn 3+ lattice distortion.
[0043] Therefore, the modified manganese-based cathode material is doped with metal doping elements and F elements. The two doping elements play a synergistic role in doping, which effectively increases the electron cloud density around the Mn element in the lattice of the doped manganese-based cathode material, and significantly inhibits the Mn 3+ Lattice distortion occurs, which enhances the stability of the crystal structure of the doped manganese-based cathode material, thereby significantly reducing the Mn 2+ The dissolution of the manganese-doped positive electrode material prolongs the Mn platform of the manganese-doped positive electrode material, improves the discharge specific capacity of the Mn segment, effectively improves the capacity utilization and cycle performance of the manganese-doped positive electrode material, and also improves the electronic conductivity and lattice oxygen redox stability of the manganese-doped positive electrode material. Therefore, when the modified manganese-based positive electrode material of the embodiment of the present application is used as a positive electrode material for a battery, the polarization resistance of the battery will be significantly reduced, the capacity utilization of the battery will be significantly improved, and finally the discharge specific capacity and cycle performance of the battery will be improved.
[0044] F doping elements in doped manganese-based cathode materials:
[0045] In some embodiments, the structure of the manganese-based positive electrode material doped with F element in the surface layer is as follows: Figure 1 As shown, the surface layer 11 of the doped manganese-based positive electrode material particle 10 is doped with F element. The surface layer 11 refers to the surface region doped with F element.
[0046] In some embodiments, from the surface to the interior of the doped manganese-based positive electrode material particle, the ratio of the depth of the F element doping to the radius of the manganese-based positive electrode material particle 10 is (0.01-0.2):1, optionally (0.03-0.16):1, and in the exemplary embodiment, it can be 0.01:1, 0.02:1, 0.026:1, 0.03:1, 0.041:1, 0.074:1, 0.1:1, 0.13:1, 0.16:1, 0.18:1, 0.2:1 and other typical but non-limiting ratios or the range between any two ratios. Among them, the depth of the F element doping can be as follows: Figure 1 As shown in a in the figure, the radius of the manganese-based positive electrode material particle is Figure 1 As shown in r, therefore, the ratio of the depth of F element doping to the radius of the manganese-based positive electrode material particles can be as follows: Figure 1 The ratio of a:r.
[0047] In some embodiments, the molar ratio of the fluorine element doped in the surface layer of the doped manganese-based positive electrode material to the iron element in the doped manganese-based positive electrode material is (5-70):100, optionally (10-50):100. In the exemplary embodiments, it can be a typical but non-limiting molar ratio of 5:100, 10:100, 20:100, 30:100, 40:100, 50:100, 60:100, 70:100, or a range between any two molar ratios.
[0048] By controlling the doping depth and content of the F element in the surface layer of the doped manganese-based positive electrode material within the above range, the redox potential of the anions in the doped manganese-based positive electrode material can be further improved and the F - The electron cloud density of the surrounding metal elements, together with the metal doping elements, further suppresses the Mn 3+ to inhibit the formation of Mn 3+ The lattice distortion is further improved to further enhance the stability of lattice oxygen in the doped manganese-based positive electrode material and inhibit the dissolution of Mn, further extend the Mn platform of the doped manganese-based positive electrode material, and improve the discharge specific capacity and cycle performance of the Mn segment of the doped manganese-based positive electrode material.
[0049] In some embodiments, the doping amount of fluorine element gradually decreases from the surface to the inside of the doped manganese-based positive electrode material particles. By controlling the non-uniform doping distribution of F element on the surface of the doped manganese-based positive electrode material particles, the redox potential of the anions on the surface of the doped manganese-based positive electrode material particles and the F element can be adjusted. - The electron cloud density of the surrounding metal elements is greater than the redox potential of the anions near the interior and the F - The electron cloud density of the surrounding metal elements makes the lattice on the surface of the doped manganese-based positive electrode material particles more stable than the internal lattice, thereby further reducing the Mn 2+ The dissolution of manganese-doped positive electrode materials further improves the cycle stability performance.
[0050] Metal doping elements in doped manganese-based cathode materials:
[0051] In some embodiments, the molar ratio of the total molar amount of the metal doping element contained in the doped manganese-based positive electrode material in the above embodiments to the iron element is (0.5-8):100, optionally (1.25-5):100. In the exemplary embodiment, it can be 0.5:100, 1:100, 1.25:100, 2:100, 2.5:100, 3:100, 4:100, 5:100, etc. Typical but non-limiting molar ratios or the range between any two molar ratios. By controlling the doping amount of the metal doping element within this range, the amount of the metal doping element replacing the iron position can be further adjusted, and on the basis of increasing the capacity of the doped manganese-based positive electrode material, the unit cell parameters and unit cell volume of the doped manganese-based positive electrode material can be further reduced, and at the same time, the impurity energy level can be further adjusted, so that the metal doping element and the above F element can further enhance the inhibition of Mn 3+ The lattice distortion effect and further reduction of the band gap width can further improve the stability of the crystal structure of the doped manganese-based positive electrode material, extend the Mn platform of the doped manganese-based positive electrode material, and improve the discharge specific capacity, cycle performance and electronic conductivity of the Mn segment of the doped manganese-based positive electrode material.
[0052] In the embodiment, the metal doping element in each of the above embodiments includes at least one element of aluminum (Al), vanadium (V), chromium (Cr), and nickel (Ni). The radius of these metal ions is smaller than that of iron ions. After the iron position of the doped manganese-based positive electrode material is doped, the Mn-O bond length is effectively shortened, which can significantly reduce the unit cell parameters and unit cell volume of the doped manganese-based positive electrode material, further inhibiting the Mn 3+ The lattice distortion of the metal reduces the dissolution of manganese and improves the cycle performance of the doped manganese-based cathode material. 2+ ) is high, such as Al element can form Al 3+ , V elements can form V 3+ , Cr element can form Cr 3+ , Ni element can form Ni 3+ After these doped metals replace the iron position, they can play a charge compensation effect, and finally suppress the Mn by increasing the electron cloud density around the Mn element in the doped manganese-based positive electrode material. 2+ Therefore, the metal ion radius and valence characteristics of these metal doping elements can inhibit the dissolution of Mn 3+ The synergistic effect of lattice distortion reduces the Mn 2+ At the same time, these metal doping elements can effectively introduce impurity energy levels into the doped manganese-based positive electrode material, and further improve the electronic conductivity of the doped manganese-based positive electrode material by shortening the band gap width of the doped manganese-based positive electrode material.
[0053] In an exemplary embodiment, the metal doping element may include aluminum. In this case, Al 3+ Valence ratio of iron ion (Fe 2+ ) is high, and after replacing the iron position, it can play a charge supplement effect, thereby increasing the electron cloud density around the Mn element in the doped manganese-based positive electrode material. 3+ The ionic radius is smaller than that of iron ions (Fe 2+ ) ion radius, which can effectively shorten the bond length of Mn-O bond in doped manganese-based cathode materials, reduce the unit cell parameters and unit cell volume of doped manganese-based cathode materials, and inhibit the 3+ The lattice distortion of the doped manganese-based cathode material is improved, and the structural stability of the doped manganese-based cathode material is improved. At the same time, the introduction of impurity energy levels can effectively shorten the band gap width of the doped manganese-based cathode material, thereby improving the electronic conductivity of the doped manganese-based cathode material.
[0054] Manganese-based positive electrode materials in doped manganese-based positive electrode materials:
[0055] In some embodiments, the manganese-based positive electrode material in the above-mentioned embodiments can be lithium iron manganese phosphate. These manganese-based positive electrode materials have relatively high capacity, high safety, good environmental friendliness and other properties, and after being doped with metal doping elements and surface doping with F elements, the electronic conductivity of the doped manganese-based positive electrode material can be effectively improved and the Mn 3+ lattice distortion, thereby improving the cycle performance of doped manganese-based positive electrode materials.
[0056] The coating layer of the modified manganese-based positive electrode material includes:
[0057] In a further embodiment, the modified manganese-based positive electrode material of the embodiment of the present application includes a coating layer in addition to the doped manganese-based positive electrode material, and the coating layer covers the surface of the particles of the above doped manganese-based positive electrode material. In this case, the modified manganese-based positive electrode material of the embodiment of the present application is a core-shell structure material. For example, in some embodiments, the structure of the modified manganese-based positive electrode material containing the coating layer can be as follows: Figure 2 As shown, the surface of the particle 10 of the doped manganese-based positive electrode material is also coated with a coating layer 20. The coating layer coats the doped manganese-based positive electrode material, and can play a protective role, an interface modification role or other corresponding roles on the doped manganese-based positive electrode material, which can be determined according to the performance of the material of the coating layer.
[0058] In some embodiments, Figure 3As shown, the coating layer 20 includes a metal fluoride coating layer 21, and the metal fluoride coating layer 21 is combined with the surface of the particles 10 of the doped manganese-based positive electrode material. By coating the metal fluoride coating layer 21 on the surface of the particles 10 of the doped manganese-based positive electrode material, the metal fluoride coating layer 21 constitutes a chemically inert coating layer, which effectively reduces the corrosion of the doped manganese-based positive electrode material by adverse factors in the electrolyte, such as HF, thereby effectively improving the stability of the contact interface with the electrolyte and the crystal structure stability of the doped manganese-based positive electrode material.
[0059] In an embodiment, the thickness of the metal fluoride coating layer may be 1 nm to 20 nm, optionally 2 nm to 16 nm, and in an exemplary embodiment, may be 1 nm, 2 nm, 2.1 nm, 2.3 nm, 3 nm, 4 nm, 5.1 nm, 5.3 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15.4 nm, 16 nm, 17 nm, 18 nm, 20 nm, or a range between any two thickness values. The metal fluoride coating layer in this thickness range can further improve the stability of the contact interface with the electrolyte, reduce the adverse effects of external adverse factors such as HF generated in the battery cell on the doped manganese-based positive electrode material, and thus improve the crystal stability of the doped manganese-based positive electrode material.
[0060] In an embodiment, the metal element contained in the metal fluoride coating layer is the same as the metal doping element contained in the doped manganese-based positive electrode material. In an embodiment, based on the type of metal doping element contained in the doped manganese-based positive electrode material described above, the metal fluoride coating layer may include at least one of metal fluorides such as AlF3, VF3, CrF3, NiF3, etc. As in the exemplary embodiment, the metal doping element contained in the doped manganese-based positive electrode material includes Al, and in this case, the metal fluoride coating layer includes AlF3. In this way, on the basis of giving full play to the above-mentioned role of the metal fluoride coating layer, the mechanical strength of the metal fluoride coating layer combined with the surface of the doped manganese-based positive electrode material can be improved, and the structural stability of the modified manganese-based positive electrode material can be improved.
[0061] In some embodiments, Figure 4 As shown, the coating layer may further include other functional coating layers 22, which are coated on the surface of the particles 10 of the metal fluoride coating layer 21 away from the doped manganese-based positive electrode material. The presence of the other functional coating layer 22 can effectively coat the metal fluoride coating layer and modify the properties of the metal fluoride coating layer, such as electronic conductivity, ionic conductivity or other properties, thereby improving the corresponding electrochemical properties of the modified manganese-based positive electrode material.
[0062] Therefore, in the embodiment, Figure 4The other functional coating layer 22 in the embodiment can be a layered structure such as an ion conductor encapsulation layer or an electronic conductor encapsulation layer or a composite layer structure of an ion conductor encapsulation layer or an electronic conductor encapsulation layer. Among them, the ion conductor encapsulation layer can improve the insertion and extraction effect of the modified manganese-based positive electrode material on lithium ions and the ionic conductivity of lithium ions.
[0063] When the other functional coating layer 22 includes an ion conductor encapsulation layer, the material of the ion conductor encapsulation layer may be a material that is conducive to improving ion conductivity, such as but not limited to at least one of perovskite type, NASICON type, and garnet type. The perovskite type may include Li 3x La 2 / 3-x TiO3(LLTO), specifically Li 0.5 La 0.5 TiO3、Li 0.33 La 0.57 TiO3、Li 0.29 La 0.57 TiO3、Li 0.33 Ba 0.25 La 0.39 TiO3, (Li 0.33 La 0.56 ) 1.005 Ti 0.99 Al 0.01 O3、Li 0.5 La 0.5 Ti 0.95 Zr 0.05 O3, etc., NASICON type such as but not limited to Li1.4Al0.4Ti1.6(PO4)3(LATP), garnet type may include Li7La3Zr2O 12 (LLZO), Li 6.4 LqCy 1.4 Ta 0.6 O 12 , Li 6.5 LqCy 1.5 Ta 0.5 O 12 By selecting the material of the ion conductor encapsulation layer, the ion conductivity of the ion conductor encapsulation layer can be further improved. The thickness of the ion conductor encapsulation layer can also be adjusted as needed.
[0064] When the other functional coating layer 22 includes an electronic conductor encapsulation layer, the material of the electronic conductor encapsulation layer may be a material that is conducive to improving electronic conductivity, such as but not limited to at least one of carbon materials, conductive oxides, and conductive organic matter. Wherein, when the material of the electronic conductor encapsulation layer is a carbon material, the carbon material may include at least one of amorphous carbon, graphite, carbon black, graphene, etc. When the material of the electronic conductor encapsulation layer is a conductive oxide, the conductive oxide may include at least one of In2O3, ZnO, and SnO2. The conductive organic matter may be a conductive polymer, etc. By selecting the material of the electronic conductor encapsulation layer, the electronic conductivity of the electronic conductor encapsulation layer can be further improved. The thickness of the electronic conductor encapsulation layer can also be adjusted as needed. In addition, the other functional coating layer 22 may also include other functional coating layers as needed, and the types of other functional coating layers may be flexibly selected as needed.
[0065] According to the test, the particle size of the modified manganese-based positive electrode material in the above embodiments, such as Dv50, can be 0.11 μm to 0.27 μm, and can be 0.115 μm to 0.263 μm, and the BET specific surface area can be 15 m 2 / g~19m 2 / g, its compacted density can be 2.3m 2 / g~2.4m 2 / g. Therefore, its particle size is controllable and the compacted density is high.
[0066] After further testing, it was found that the discharge specific capacities of the modified manganese-based positive electrode materials in the above embodiments at 0.1C and 1C were as high as 152.57 mAh·g -1 、148.87mAh·g -1 , it has high capacity and good cycle performance.
[0067] In a second aspect, the present invention also provides a method for preparing the modified manganese-based positive electrode material. The method for preparing the modified manganese-based positive electrode material in the present invention comprises the following steps:
[0068] S10: In a plasma environment, a gaseous fluorine source is used to etch the manganese-based positive electrode material, and fluorine element is doped into the particle surface layer of the manganese-based positive electrode material to obtain a modified manganese-based positive electrode material.
[0069] Step S10:
[0070] The manganese-based positive electrode material in step S10 refers to the manganese-based positive electrode material contained in the modified manganese-based positive electrode material above (excluding metal doping elements and F elements). Therefore, the manganese-based positive electrode material also contains elements such as iron elements and oxygen elements. At the same time, the manganese-based positive electrode material also contains metal doping elements, that is, the manganese-based positive electrode material is a manganese-based positive electrode material doped with metal doping elements.
[0071] The preparation method of the modified manganese-based positive electrode material in the embodiment of the present application combines plasma, uses a fluorine source to fluorine etch and dope the manganese-based positive electrode material particles doped with metal elements smaller than iron ions, and dopes the surface of the manganese-based positive electrode material particles containing the metal doping elements, so that the two doping elements can play a synergistic role in doping, so that the electron cloud density around the Mn element in the lattice of the doped manganese-based positive electrode material is effectively increased, and the Mn 3+ Lattice distortion occurs, which enhances the stability of the crystal structure of the doped manganese-based cathode material, thereby significantly reducing the Mn 2+ The dissolution of manganese-doped positive electrode materials prolongs the Mn platform of the Mn-doped positive electrode materials, increases the discharge specific capacity of the Mn segment, and improves the electronic conductivity and lattice oxygen redox stability of the manganese-doped positive electrode materials.
[0072] In some embodiments, the manganese-based positive electrode material doped with a metal doping element can be prepared according to the following method:
[0073] S11: preparing a precursor slurry by mixing a raw material containing a metal doping element and a precursor of a manganese-based positive electrode material in a solvent;
[0074] S12: spray drying the precursor slurry to form precursor particles;
[0075] S13: In a protective atmosphere, the precursor particles are calcined to obtain a manganese-based positive electrode material doped with a metal doping element.
[0076] Among them, the precursor of the manganese-based positive electrode material in step S11 can be determined according to the type of manganese-based positive electrode material. For example, in the exemplary embodiment, when it is lithium manganese iron phosphate, it includes a lithium source, a manganese source, an iron source, a phosphorus source, etc., and the lithium source, manganese source, iron source, and phosphorus source can be mixed according to the molar ratio of Li, Mn, Fe, and P elements of (0.8-1.2): (0.48:0.72): (0.32-0.48): (0.8-1.2). Among them, the iron source may include at least one of ferric nitrate, ferrous chloride, ferric phosphate, ferric pyrophosphate, ferric citrate, ferric oxalate, ferric sulfate, and ferrous sulfate; the lithium source may include at least one of lithium dihydrogen phosphate, lithium hydroxide, lithium carbonate, lithium acetate, lithium phosphate, and lithium nitrate; the phosphorus source may include at least one of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, dipotassium hydrogen phosphate, sodium dihydrogen phosphate, phosphoric acid, ferric phosphate, and lithium dihydrogen phosphate; the manganese source may include at least one of manganese acetate tetrahydrate, manganese oxalate, manganese tetraoxide, manganese dioxide, manganese carbonate, manganese sulfate, manganese chloride, and ammonium manganate.
[0077] In the embodiment, the raw material containing the metal doping element in step S11 can be mixed with the precursor in a ratio of (0.5-5) to 100 in a molar ratio of the metal doping element to the iron element. In the exemplary embodiment, the raw material containing the metal doping element can include at least one of the halides, nitrates, organic compounds, and composite salts of the metal doping element. For example, when the metal doping element includes at least one element of aluminum, vanadium, chromium, nickel, etc., the raw material containing the metal doping element can include at least one of the halides, nitrates, organic compounds, oxides, and composite salts of at least one element of aluminum, vanadium, chromium, nickel, etc. Among them, the organic compound can be a trimethyl organic substance or a triethyl organic substance of the metal doping elements, and the composite salt can be a potassium sulfate dodecahydrate composite salt of the metal doping elements.
[0078] The solvent of the slurry may be, but is not limited to, water.
[0079] In the embodiment, the slurry preparation process can be controlled so that the particle size Dv50 in the slurry is controlled within 0.20 μm to 0.25 μm. This particle size range can effectively improve the uniformity of the precursor dispersion in the slurry and improve the stability of the slurry.
[0080] In order to improve the dispersion uniformity of the precursor contained in the precursor slurry, in the embodiment, the mixture slurry can be ground during the preparation of the precursor slurry. For example, the mixture slurry can be ground and stirred at a grinding rate of 200 r / min to 600 r / min for 0.5 h to 2 h until the particle size Dv50 is controlled to be 0.20 μm to 0.25 μm.
[0081] In the embodiment, the air inlet temperature of the spray drying process in step S12 is 140° C. to 250° C., so that the precursor slurry forms precursor particles.
[0082] After the calcination treatment in step S13, the precursor particles in step S12 are sintered to form manganese-based positive electrode material particles doped with metal doping elements, and the metal doping elements are uniformly doped in the manganese-based positive electrode material.
[0083] In an embodiment, the protective atmosphere in step S13 may be an oxygen-free atmosphere, such as at least one of nitrogen and argon, or a vacuum environment.
[0084] In the embodiment, the calcination treatment in step S13 may include a secondary calcination treatment, wherein the temperature of the primary calcination treatment may be 300°C to 580°C, the heating rate may be but not limited to 5°C / min, and the calcination time may be 2h to 10h; the temperature of the secondary calcination treatment may be 700°C to 950°C, the heating rate may be but not limited to 5°C / min, and the calcination time may be 4h to 10h. The secondary calcination treatment can fully sinter the precursor particles to generate manganese-based positive electrode material particles doped with metal doping elements, and the metal doping elements are mainly used to dope or replace the iron position in the manganese-based positive electrode material.
[0085] The plasma environment in step S10 means that the etching process in step S10 is performed in a plasma environment, that is, in an environment containing charged particles. Therefore, the etching process in step S10 can also be understood as a plasma etching process involving a fluorine source.
[0086] In the embodiment, during the etching process, the gaseous fluorine source is continuously introduced into the plasma environment, and the gaseous fluorine source has an introduction gas flow rate of 5sccm to 20sccm. By continuously introducing the gaseous fluorine source at this rate, the manganese-based positive electrode material, specifically the manganese-based positive electrode material containing metal doping elements, is subjected to fluorine plasma etching, so that fluorine can relatively evenly etch the surface of the manganese-based positive electrode material particles, and dope the F element in the particle surface. Or further form a fluoride of the metal doping element on the surface of the manganese-based positive electrode material particles. In the embodiment, the metal fluoride can form Figure 3 and Figure 4 The metal fluoride coating layer 21 shown has good inertness, thereby improving the interface stability of the generated modified manganese-based positive electrode material.
[0087] In an embodiment, the pressure of the plasma environment can be 600Pa to 1200Pa, and the power can be 100W to 400W. In an embodiment, under the above-mentioned etching conditions, the etching time of the etching process can be 300s to 1200s. By further controlling the etching conditions and time within this range, the doping depth and doping amount of the F element on the surface layer of the manganese-based positive electrode material particles containing metal doping elements can be adjusted. On this basis, the amount of metal fluoride generated can be further regulated by adjusting the reaction between the F element and the metal doping element, and the coverage rate of the metal fluoride on the manganese-based positive electrode material particles doped with the metal doping element and the F element can be increased.
[0088] In an embodiment, the gaseous fluorine source may include at least one of fluorine gas, carbon tetrafluoride, nitrogen trifluoride, sulfur hexafluoride, hydrofluoroolefins, and freon. These fluorine-containing sources are rich in fluorine elements, and can etch and dope the surface of manganese-based positive electrode material particles in a plasma environment, thereby forming a doped region rich in F elements in the surface region of the manganese-based positive electrode material particles. Or it can further react with the metal doping elements on the surface of the manganese-based positive electrode material particles to form fluorides containing metal doping elements on the surface of the manganese-based positive electrode material particles, thereby improving the inertness and stability of the surface of the prepared modified manganese-based positive electrode material.
[0089] In some embodiments, the etching process in step S10 of the method for preparing the modified manganese-based positive electrode material in the embodiment of the present application further includes the following step S20:
[0090] S20: a step of forming other functional coating layers on the etched material surface.
[0091] In step S02, the method for forming other functional coating layers can be flexibly selected according to the structure and material type of other functional coating layers. For example, in-situ coating followed by sintering can be selected according to the material characteristics of the layer structure. Other functional layers can also be formed by other methods.
[0092] In the embodiment, when the other functional coating layer is an electronic conductive layer, and the electronic conductive layer is a carbon coating layer, the carbon coating layer can be prepared by the following method:
[0093] In a protective atmosphere, the manganese-based positive electrode material particles after fluorine etching are mixed with a carbon source and then sintered to form a carbon coating layer on the manganese-based positive electrode material particles after fluorine etching to obtain a modified manganese-based positive electrode material with a core-shell structure.
[0094] In the embodiment, the carbon source can be added in a ratio of 5% to 20% of the mass of the manganese-based positive electrode material particles after fluorine etching and mixed with the manganese-based positive electrode material particles after fluorine etching. By controlling the amount of carbon source added, the content and thickness of the carbon coating layer can be adjusted to enhance the improvement effect on the electronic conductivity of the prepared modified manganese-based positive electrode material.
[0095] In the embodiment, the sintering process includes a first stage sintering process and a second stage sintering process. In the embodiment, the temperature of the first stage sintering process can be 400°C to 550°C, and the time can be 2h to 5h. In the embodiment, the temperature can be increased to 400°C to 550°C at a heating rate of 5°C / min but is not limited thereto.
[0096] In the embodiment, the temperature of the second stage sintering treatment can be 650°C to 750°C, and the time can be 4h to 7h. In the embodiment, the temperature can be increased to 650°C to 750°C at a heating rate of 5°C / min but is not limited thereto.
[0097] By sintering, the carbon source can be effectively carbonized to form a carbon coating layer covering the fluorine-etched manganese-based positive electrode material particles. At the same time, the sintering treatment can further improve the surface performance of the prepared modified manganese-based positive electrode material particles, further improve the structural stability of the particles and improve their interface properties, and improve the stability of their electrochemical performance.
[0098] In the embodiment, the protective atmosphere may be an inert gas atmosphere or a vacuum environment, wherein the inert gas may include at least one of nitrogen and argon.
[0099] In an embodiment, the carbon source may include at least one of glucose, fructose, sucrose, starch, lactic acid, citric acid, dextrin, chitosan, and polyethylene glycol. These carbon sources can form carbon materials with high electronic conductivity during the sintering process.
[0100] In the third aspect, the embodiment of the present application also provides a positive electrode sheet. The positive electrode sheet of the embodiment of the present application includes a positive electrode current collector and a positive electrode active material layer bonded to the surface of the positive electrode current collector, and the positive electrode active material layer contains the modified manganese-based positive electrode material in the embodiment of the present application above. Since the positive electrode sheet of the embodiment of the present application contains the modified manganese-based positive electrode material in the embodiment of the present application above, the positive electrode sheet of the embodiment of the present application has good cycle performance and high capacity density.
[0101] In an embodiment, the mass content of the modified manganese-based positive electrode material of the above-mentioned embodiment of the application contained in the positive electrode active layer can be 80wt% to 95wt%. The positive electrode active layer includes a binder and a conductive agent in addition to the modified manganese-based positive electrode material. Among them, the content of the binder can be 0.5 to 20wt%, and the binder can be a commonly used electrode binder, such as one or more of polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylonitrile copolymer, sodium alginate, chitosan and chitosan derivatives. The content of the conductive agent can be 0.2wt% to 20wt%, and the conductive agent can also be a commonly used conductive agent, such as one or more of graphite, carbon black, acetylene black, graphene, carbon fiber, C60 and carbon nanotubes.
[0102] In the embodiment, the positive electrode sheet preparation process can be: the positive electrode lithium supplement additive, the conductive agent and the binder are mixed or further mixed with the positive electrode active material to obtain an electrode slurry, the positive electrode slurry is coated on the positive electrode collector, and the positive electrode sheet is prepared through drying, rolling, die cutting and other steps.
[0103] In a fourth aspect, the present application also provides a battery. The battery of the present application includes necessary components such as a positive electrode sheet and a negative electrode sheet, and of course other necessary or auxiliary components. Among them, the positive electrode sheet is the positive electrode sheet of the present application embodiment, that is, the positive electrode active layer contained in the positive electrode sheet contains the modified manganese-based positive electrode material of the present application embodiment.
[0104] Since the battery of the embodiment of the present application contains the modified manganese-based positive electrode material of the above-mentioned embodiment of the text application, based on the good cycle performance and high energy density of the modified manganese-based positive electrode material of the above-mentioned embodiment of the text application, the battery of the embodiment of the present application has high energy density, discharge specific capacity and excellent cycle performance, high capacity retention rate and long life.
[0105] The following uses a number of specific embodiments to illustrate the modified manganese-based positive electrode material, its preparation method, and application, etc., according to the embodiments of the present application.
[0106] 1. Modified manganese-based positive electrode material and preparation method thereof Example:
[0107] Embodiment 1:
[0108] The present embodiment provides a modified manganese-based positive electrode material and a preparation method thereof. The modified manganese-based positive electrode material includes aluminum-doped lithium manganese iron phosphate particles (aluminum-doped LMFP particles) and a coating layer coating the doped manganese-based positive electrode material particles. Among them, the surface layer of the aluminum-doped lithium manganese iron phosphate particles is doped with F elements, and replaces the oxygen position of LMFP, so the aluminum and F-doped lithium manganese iron phosphate particles can be recorded as Al-F co-doped LMFP; the coating layer includes an aluminum fluoride layer and a carbon layer, the aluminum fluoride layer coats the Al-Fco-doped LMFP particles, and the carbon layer is coated on the surface of the aluminum fluoride layer away from the Al-F co-doped LMFP particles. The relevant parameters and performances of the modified manganese-based positive electrode material of this embodiment are specifically shown in Table 1 below.
[0109] The preparation method of the modified manganese-based positive electrode material in this embodiment includes the following steps:
[0110] S1: 1.0 mol of ammonium dihydrogen phosphate, 0.52 mol of lithium carbonate, 0.6 mol of manganese acetate tetrahydrate, 0.4 mol of ferric nitrate nonahydrate, and 0.005 mol of aluminum nitrate were added into water and stirred continuously at a speed of 300 r / min for 1 h to obtain a uniform mixed slurry;
[0111] S2: spray drying the mixed slurry in step S1 at 200° C. to obtain Al-containing lithium manganese iron phosphate precursor particles;
[0112] S3: calcining the lithium iron manganese phosphate precursor particles in step S2 under argon protection, first calcining at 550° C. for 4 hours to remove moisture in the mixture and preliminarily form lithium iron manganese phosphate crystals from the lithium iron manganese phosphate precursor, and then raising the temperature to 720° C. and maintaining it for 8 hours. The heating rate of the calcination process is 5° C. / min, and after cooling, Al-doped lithium iron manganese phosphate positive electrode material particles (referred to as Al-doped LMFP particles) can be obtained;
[0113] S4: 5 g of the Al-doped LMFP particles in step S3 are placed in a plasma instrument, the pressure of the instrument is adjusted to 800 Pa, the temperature is room temperature (25° C.), the power is 200 W, and F2 is introduced to etch the Al-doped LMFP, the fluorine gas flow rate is 15 sccm, and the etching time is 900 s, to obtain a surface F-doped Al-F co-doped LMFP material. After testing, an aluminum fluoride layer is also formed on the surface of the Al-Fco-doped LMFP particles;
[0114] S5: The Al-F co-doped LMFP material etched in step S4 is mixed with glucose and sintered under argon gas protection, wherein the mass ratio of glucose to Al-F co-doped LMFP material is 8%. The above sample is first calcined at 500°C for 3h, and then calcined at 700°C for 5h. The heating rate of the two sintering processes is 5°C / min. After cooling, a modified manganese-based positive electrode material of carbon-coated Al-F co-doped LMFP is obtained, which is recorded as Al-F co-doped LMFP@C.
[0115] Embodiment 2:
[0116] This embodiment provides a modified manganese-based positive electrode material and a preparation method thereof. The modified manganese-based positive electrode material is different from the modified manganese-based positive electrode material in Example 1 in that the amount of aluminum doping is different, as shown in Table 1 below, and the rest is the same as the modified manganese-based positive electrode material in Example 1.
[0117] The preparation method of the modified manganese-based positive electrode material in this embodiment refers to the preparation method in Example 1, except that 0.01 mol of aluminum nitrate is added in step S1, and the other steps are the same.
[0118] Embodiment 3:
[0119] This embodiment provides a modified manganese-based positive electrode material and a preparation method thereof. The modified manganese-based positive electrode material is different from the modified manganese-based positive electrode material in Example 1 in that the amount of aluminum doping is different, as shown in Table 1 below, and the rest is the same as the modified manganese-based positive electrode material in Example 1.
[0120] The preparation method of the modified manganese-based positive electrode material in this embodiment refers to the preparation method in Example 1, except that 0.02 mol of aluminum nitrate is added in step S1, and the other steps are the same.
[0121] Embodiment 4:
[0122] This embodiment provides a modified manganese-based positive electrode material and a preparation method thereof. The modified manganese-based positive electrode material is different from the modified manganese-based positive electrode material in Example 2 in that the F doping amount is different, as shown in Table 1 below, and the rest is the same as the modified manganese-based positive electrode material in Example 2.
[0123] The preparation method of the modified manganese-based positive electrode material in this embodiment refers to the preparation method in Example 2, except that F / Fe is controlled to be 0.1 in step S4, and the other steps are the same.
[0124] Embodiment 5:
[0125] This embodiment provides a modified manganese-based positive electrode material and a preparation method thereof. The modified manganese-based positive electrode material is different from the modified manganese-based positive electrode material in Example 2 in that the F doping amount is different, as shown in Table 1 below, and the rest is the same as the modified manganese-based positive electrode material in Example 2.
[0126] The preparation method of the modified manganese-based positive electrode material in this embodiment refers to the preparation method in Example 2, except that F / Fe is controlled to be 0.5 in step S4, and the other steps are the same.
[0127] Embodiment 6:
[0128] This embodiment provides a modified manganese-based positive electrode material and a preparation method thereof. The modified manganese-based positive electrode material is different from the modified manganese-based positive electrode material in Example 2 in that the type of metal doping is different, as shown in Table 1 below, and the rest is the same as the modified manganese-based positive electrode material in Example 2.
[0129] The preparation method of the modified manganese-based positive electrode material in this embodiment refers to the preparation method in Example 2, except that 0.01 mol V2O5 is added in step S1, and the other steps are the same.
[0130] Embodiment 7:
[0131] This embodiment provides a modified manganese-based positive electrode material and a preparation method thereof. The modified manganese-based positive electrode material is different from the modified manganese-based positive electrode material in Example 2 in that the type of metal doping is different, as shown in Table 1 below, and the rest is the same as the modified manganese-based positive electrode material in Example 2.
[0132] The preparation method of the modified manganese-based positive electrode material in this embodiment refers to the preparation method in Example 2, except that 0.01 mol Cr2O5 is added in step S1, and the other steps are the same.
[0133] Embodiment 8:
[0134] This embodiment provides a modified manganese-based positive electrode material and a preparation method thereof. The modified manganese-based positive electrode material is different from the modified manganese-based positive electrode material in Example 2 in that the type of metal doping is different, as shown in Table 1 below, and the rest is the same as the modified manganese-based positive electrode material in Example 2.
[0135] The preparation method of the modified manganese-based positive electrode material in this embodiment refers to the preparation method in Example 2, except that 0.01 mol Ni2O5 is added in step S1, and the other steps are the same.
[0136] Comparative Example 1:
[0137] This comparative example provides a manganese-based positive electrode material and a preparation method thereof. Compared with the modified manganese-based positive electrode material in Example 1, the manganese-based positive electrode material does not contain aluminum and F doping elements, that is, it only contains lithium manganese iron phosphate that is not doped with aluminum and F in Example 1, and the rest is the same as the modified manganese-based positive electrode material in Example 1. Therefore, the manganese-based positive electrode material in this comparative example can be recorded as LMFP@C.
[0138] Comparative Example 2:
[0139] This comparative example provides a modified manganese-based positive electrode material and a preparation method thereof. Compared with the modified manganese-based positive electrode material in Example 1, the modified manganese-based positive electrode material does not contain aluminum doping elements, that is, only the F element is doped in the surface layer of the LMFP particles, and the rest is the same as the modified manganese-based positive electrode material in Example 1. Therefore, the modified manganese-based positive electrode material in this comparative example can be recorded as F doped LMFP@C.
[0140] The preparation method of the modified manganese-based positive electrode material in this comparative example refers to the preparation method in Example 1, except that 0.02 mol of aluminum nitrate is not added in step S1, and the other steps are the same.
[0141] Comparative Example 3:
[0142] This comparative example provides a modified manganese-based positive electrode material and a preparation method thereof. Compared with the modified manganese-based positive electrode material in Example 1, the modified manganese-based positive electrode material is uniformly doped with aluminum doping elements and F elements to LMFP particles (that is, F is not only doped on the surface of LMFP particles, but also doped inside LMFP particles), and the rest is the same as the modified manganese-based positive electrode material in Example 1.
[0143] The preparation method of the modified manganese-based positive electrode material in this comparative example has the following specific steps:
[0144] S1: First, 1.0 mol of ammonium dihydrogen phosphate, 0.52 mol of lithium carbonate, 0.6 mol of manganese acetate tetrahydrate, 0.4 mol of ferric nitrate nonahydrate, 0.01 mol of aluminum nitrate, and 0.02 mol of potassium fluoride were added to water and stirred at a speed of 300 r / min for 1 h to obtain a uniform mixed slurry;
[0145] S2: spray drying the mixed slurry at 200° C. to obtain lithium manganese iron phosphate precursor particles containing Al and F;
[0146] S3: The lithium iron manganese phosphate precursor particles in S2 are calcined under argon protection. The above mixture is first calcined at 550°C for 4 hours to remove moisture in the mixture and preliminarily form lithium iron manganese phosphate crystals from the lithium iron manganese phosphate precursor. The temperature is then raised to 720°C and maintained for 8 hours. The heating rate during the calcination process is 5°C / min. After cooling, Al and F co-doped lithium iron manganese phosphate positive electrode material can be obtained.
[0147] S4: The Al and F co-doped lithium manganese iron phosphate positive electrode material in step S3 is mixed with glucose and sintered under argon gas protection, wherein the mass ratio of glucose to Al-F co-doped LMFP material is 8%. The above sample is first calcined at 500°C for 3h, and then calcined at 700°C for 5h. The heating rate of the two sintering processes is 5°C / min. After cooling, a modified manganese-based positive electrode material of carbon-coated Al-F co-doped LMFP is obtained, which is recorded as Al-F co-doped LMFP@C.
[0148] Table 1
[0149]
[0150] 2. Lithium-ion battery example:
[0151] The modified manganese-based positive electrode materials provided in the above-mentioned Examples 1 to 8 and the manganese-based positive electrode materials provided in the comparative example are respectively assembled into positive electrodes and lithium-ion batteries according to the following methods:
[0152] Positive electrode: under the same conditions, the positive electrode material, polyvinylidene fluoride and SP-Li were mixed and ball-milled in a mass ratio of 95:3:2 to obtain a positive electrode slurry, and the positive electrode slurry was coated on the surface of aluminum foil, rolled, and vacuum dried overnight at 110°C to obtain a positive electrode sheet; wherein the positive electrode materials were the modified manganese-based positive electrode materials provided in the above-mentioned Examples 1 to 8 and the manganese-based positive electrode materials provided in Comparative Examples 1 to 3, respectively;
[0153] Negative electrode: lithium metal sheet;
[0154] Electrolyte: Ethylene carbonate and ethyl methyl carbonate were mixed in a volume ratio of 3:7, and LiPF6 was added to form an electrolyte, the concentration of LiPF6 was 1 mol / L;
[0155] Diaphragm: Polypropylene microporous separator;
[0156] Lithium-ion battery assembly: The structure of lithium metal sheet-diaphragm-electrolyte-positive electrode sheet is assembled into a lithium-ion battery in an inert atmosphere glove box.
[0157] 3. Related performance tests
[0158] 3.1 Related tests of modified manganese-based positive electrode materials:
[0159] a. X-ray diffraction analysis of modified manganese-based cathode materials:
[0160] The modified manganese-based positive electrode materials provided in Examples 1 to 8 and the manganese-based positive electrode materials provided in Comparative Examples were subjected to X-ray diffraction analysis, wherein the X-ray diffraction patterns of the modified manganese-based positive electrode materials provided in Examples 1 to 3 and the manganese-based positive electrode materials provided in Comparative Examples 1 to 2 are as follows: Figure 5 shown.
[0161] Depend on Figure 5 It can be seen that the diffraction peak positions of the modified manganese-based positive electrode materials provided in Examples 1 to 3 and the manganese-based positive electrode materials provided in Comparative Examples 1 to 2 are consistent with the diffraction peaks of the lithium manganese phosphate standard card (PDF#77-0178), which confirms that the lattice structure of the materials provided in the comparative examples and the embodiments is consistent with that of lithium manganese phosphate, and the diffraction angles of the sample diffraction peaks relative to the diffraction peaks of the standard card are large, which confirms that the Fe element successfully replaces the position of Mn in lithium manganese phosphate. In summary, it can be seen that the materials in the comparative examples and the embodiments are lithium iron manganese phosphate.
[0162] b. Scanning electron microscopy (SEM) analysis of modified manganese-based cathode materials:
[0163] The modified manganese-based positive electrode materials provided in Examples 1 to 8 and the manganese-based positive electrode materials provided in the comparative examples were subjected to SEM analysis, respectively. The SEM images of the modified manganese-based positive electrode materials provided in Examples 1 to 3 and the manganese-based positive electrode materials provided in Comparative Examples 1 to 2 are as follows: Figure 6 shown.
[0164] Depend on Figure 6It can be seen that the particles of the manganese-based positive electrode materials prepared in Comparative Examples 1 and 2 are seriously agglomerated, and the primary particle size of the F-doped LMFP@C (D50=192.8nm) in Comparative Example 2 is smaller than that of the undoped LMFP@C (D50=263.2nm) in Comparative Example 1. In comparison, the Al-F co-doped LMFP@C particles provided in Examples 1 to 3 are more dispersed, and the particle size is smaller than that of the LMFP in Comparative Examples 1 and 2. This may be because the co-doping of Al and F reduces the unit cell parameters and unit cell volume of the doped manganese-based positive electrode material, thereby reducing the particle size. The reduction and dispersion of the particles make the modified manganese-based positive electrode material easier to be wetted by the electrolyte and effectively shorten the Li + The transmission path is improved to enhance the rate performance of the modified manganese-based positive electrode material.
[0165] Further comparison of the modified manganese-based positive electrode materials in Examples 1 to 3 shows that, as the amount of Al doping increases, the particle size of the prepared modified manganese-based positive electrode material begins to decrease.
[0166] 3.2 Lithium-ion battery performance testing:
[0167] The lithium-ion batteries assembled in the above lithium-ion battery embodiments were tested for discharge specific capacity, first effect, discharge median voltage and high temperature cycling performance at 45° C. The test conditions for the discharge specific capacity, first effect and discharge median voltage were as follows:
[0168] Discharge specific capacity: First, let the battery stand at 25℃ for 4h, then charge it at a constant current of 0.1C until the cut-off voltage is 4.3V and charge it at a constant voltage. After the constant voltage charging is completed, let the battery stand for 5min, and then discharge it at a constant current (0.1C) until the voltage is 2.0V, thus completing one charge and discharge cycle; then let the battery stand for 5min, and charge it at a constant current of 1C until the cut-off voltage is 4.3V and charge it at a constant voltage. After the constant voltage charging is completed, let the battery stand for 5min, and then discharge it at a constant current (1C) until the voltage is 2.0V, thus completing the second charge and discharge cycle.
[0169] First effect: The test method is the same as the discharge specific capacity.
[0170] Discharge median voltage: Same as the test method for discharge specific capacity.
[0171] High temperature cycling at 45°C:
[0172] S1: First, the battery is left at rest for 4 hours at 45°C, then charged at a constant current of 0.1C until the cut-off voltage is 4.3V and then charged at a constant voltage. After the constant voltage charging is completed, the battery is left at rest for 5 minutes, and then discharged at a constant current (0.1C) until the voltage is 2.0V, thus completing a charge and discharge cycle.
[0173] S2: Then the battery is left to stand for 5 minutes, and constant current charging is performed at 1C current until the cut-off voltage is 4.3V and constant voltage charging is performed. After the constant voltage charging is completed, the battery is left to stand for 5 minutes, and then constant current discharge (1C) is performed until the voltage is 2.0V, thus completing the second charge and discharge cycle;
[0174] S2: Repeat step S2 99 times to complete the high temperature cycle test procedure of testing the battery at 0.1C for one cycle and at 1C for 100 cycles.
[0175] The test results of the discharge specific capacity, first efficiency and discharge median voltage of the lithium ion batteries of each embodiment are shown in Table 2 below. The cycle curves of the lithium ion batteries containing the modified manganese-based positive electrode materials in Example 2 and Comparative Example 1 are shown in Table 2 below. Figure 7 As shown:
[0176] Table 2
[0177]
[0178] Combination Figure 7 As shown in Table 2, compared with Comparative Example 1, the discharge capacity of Comparative Example 2 at 0.1C and 1C is increased by 2.14 mAh·g -1 and 7.04 mAh g -1 This is mainly due to the fact that F doping leads to a significant decrease in the primary particle size of the doped LMFP, shortening the Li + The transmission distance of Li + In addition, compared with the comparative example, the discharge specific capacity of the modified manganese-based positive electrode material in the embodiment is higher. Among them, the discharge specific capacity of the modified manganese-based positive electrode material in Example 2 at 0.1C and 1C is 152.57 mAh·g -1 and 148.87 mAh g -1 This proves that metal doping elements such as Al and surface F elements play a synergistic role in doping, which can effectively improve the electrochemical performance of modified manganese-based cathode materials. After analysis, on the one hand, metal doping elements such as Al and surface F elements can reduce the primary particle size of doped LMFP by reducing the unit cell volume of doped LMFP, thereby shortening the Li + Transmission distance, improve Li +The transmission rate of the doped LMFP is increased, its polarization degree is reduced, and its discharge capacity and rate performance are improved; on the other hand, after doping LMFP with metal doping elements such as Al, impurity energy levels can be introduced, thereby shortening the band gap of the doped LMFP, improving the electronic conductivity of the doped LMFP, and thus improving the electrochemical performance of the doped LMFP. Comparing Examples 1 to 3, it can be seen that with the increase of the Al doping amount, the discharge capacity of the doped LMFP shows a trend of first increasing and then decreasing. This may be because the appropriate amount of Al doping can improve the electronic and ionic conductivity of the doped LMFP, while a relatively large amount of Al doping will make the particle size of the doped LMFP too small, causing a certain degree of agglomeration of the particles, reducing the infiltration of the electrolyte, and prolonging the Li + transmission path, reducing the Li + The transfer rate of LMFP is reduced, thus reducing the electrochemical performance of LMFP.
[0179] The high temperature cycling results of the lithium ion battery containing the modified manganese-based positive electrode material in Comparative Example 1 and the manganese-based positive electrode material in Example 2 at 45°C are shown in Table 3 (Comparative Example 1) and Table 4 (Example 2) respectively. The high temperature cycling curves of the lithium ion battery containing the modified manganese-based positive electrode material in Example 2 and Comparative Example 1 are shown in Table 3 (Comparative Example 1) and Table 4 (Example 2). Figure 8 As shown:
[0180] Table 3
[0181]
[0182] Table 4
[0183]
[0184] Combination Figure 8 As shown in Table 3, after the lithium-ion battery containing the manganese-based positive electrode material in Comparative Example 1 was cycled for 100 cycles at 1C rate at 45°C, the Mn platform ratio lost 5.75% and the discharge specific capacity lost 26.17%. Among them, from the 80th to the 100th cycle, the Mn platform ratio and the discharge specific capacity lost 2.26% and 23.65% respectively, which may be due to the serious Mn dissolution at this stage, resulting in a rapid decrease in the Mn platform and capacity. Figure 8 As shown in Table 4, in comparison, the lithium-ion battery containing the modified manganese-based cathode material in Example 2 loses only 3.09% of the Mn platform proportion and 0.95% of the discharge specific capacity after 100 cycles at 45°C and 1C rate, which confirms that the Al-F co-doped LMFP@C particles have better cycle stability than the undoped LMFP@C particles.
[0185] In order to further verify the stability of the modified manganese-based positive electrode material, the Fe and Mn dissolution amounts of the manganese-based positive electrode materials in Comparative Examples 1 to 3 and the modified manganese-based positive electrode materials in Examples 1 to 8 were further detected.
[0186] The detection method of the Fe and Mn dissolution amount is:
[0187] S1: Sample pretreatment: First, treat the sample to be tested by acid digestion. The acid used can be nitric acid. During the digestion process, the acid concentration is controlled at 3mol / L to 16mol / L, the temperature is between 100℃ and 300℃, and the digestion time is about 15 to 20 minutes. After digestion, transfer the solution and make it constant, then let it stand. After the solution is separated, take the clear part in the middle as the test solution.
[0188] S2: Draw a standard curve: According to the types of main elements to be tested, prepare a series of standard solutions containing lithium (Li), iron (Fe), manganese (Mn) and phosphorus (P). Use inductively coupled plasma optical emission spectrometer (ICP-OES) to test these standard solutions, and draw a standard curve with element concentration as the horizontal axis and emission intensity as the vertical axis.
[0189] S3: Determination of main element content: ICP-OES is used to determine the main element content in the solution to be tested. By comparing with the standard curve, the dissolution amount of Fe and Mn in the sample can be quantitatively analyzed.
[0190] The Fe and Mn dissolution test results are shown in Table 5:
[0191] Table 5
[0192] Test items Fe dissolution (mg / L) Mn dissolution (mg / L) Example 1 3.42 2.14 Example 2 2.15 1.23 Example 3 2.24 1.45 Example 4 3.14 1.73 Example 5 1.97 1.14 Example 6 2.37 1.36 Example 7 2.42 1.43 Example 8 2.57 1.65 Comparative Example 1 5.04 6.02 Comparative Example 2 4.57 5.45 Comparative Example 3 4.36 3.87
[0193] It can be seen from Table 5 that compared with Comparative Examples 1 to 3, the Fe and Mn dissolution amounts of the modified manganese-based positive electrode materials in Examples 1 to 8 are significantly lower. Among them, the Mn dissolution amount of the modified manganese-based positive electrode material in Example 2 is the lowest, which is only 1.23 mg·L -1 , which is much lower than the Mn dissolution amount of the manganese-based positive electrode material in Comparative Example 1 (6.02 mg·L -1 ), which confirms that the doping of metal doping elements including Al can significantly enhance the lattice stability of doped LMFP and inhibit the Mn 2+ The main reason is that Al doping at the Fe site can reduce the lattice constant and unit cell volume of doped LMFP, shorten the bond length of Mn-O bond, and inhibit the dissolution of Mn 3+ lattice distortion, thereby reducing the Mn 2+ In addition, Al doping can also inhibit the dissolution of Mn by reducing the charge density of Mn element. 3+The F element replaces the oxygen site in the layer, which can significantly increase the redox potential of the anions in the doped LMFP, thereby improving the stability of the lattice oxygen in the doped manganese-based positive electrode material, thereby significantly inhibiting the Mn 2+ At the same time, since the F ion is -1 and the O ion is -2, the F - Replace O 2- After that, F - The electron cloud density of the surrounding metal elements has been increased, and the electron cloud density around the Mn element has been increased, which has suppressed the Mn 3+ The formation of Mn 3+ Therefore, the synergistic doping of metal doping elements including Al and F elements on manganese-based cathode materials such as LMFP can effectively reduce the lattice constant and unit cell volume of doped manganese-based cathode materials, shorten the bond length of Mn-O bonds, and inhibit the growth of Mn 3+ lattice distortion, thereby reducing the Mn 2+ dissolution.
[0194] In addition, compared with Comparative Examples 1 and 2, Examples 1 to 8 have lower Fe and Mn dissolution amounts. Analysis shows that this is because the co-doping of Al and F leads to the formation of metal fluorides on the surface of manganese-based positive electrode materials such as LMFP. These metal fluorides have strong corrosion resistance and can resist HF corrosion to a certain extent, thereby improving the stability of the surface of the modified manganese-based positive electrode material.
[0195] The above embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.
Claims
1. A modified manganese-based positive electrode material, characterized in that: It includes a doped manganese-based positive electrode material, which contains iron and oxygen elements, and also contains metal doping elements and fluorine elements; wherein the metal doping element replaces the iron position, and its ion radius is smaller than the iron ion radius; the fluorine element is doped in the particle surface layer of the manganese-based positive electrode material and replaces the oxygen position.
2. The modified manganese-based positive electrode material according to claim 1, characterized in that: The fluorine element includes one or more of the following (1) to (3): (1) From the surface of the particles of the doped manganese-based positive electrode material to the inside, the ratio of the depth of the fluorine element doping to the radius of the particles of the manganese-based positive electrode material is (0.01-0.20):1; (2) The molar ratio of the fluorine element to the iron element doped in the surface layer of the doped manganese-based positive electrode material is (10-50):100; (3) From the particle surface to the inner part of the doped manganese-based positive electrode material, the doping amount of the fluorine element gradually decreases; and / or The molar ratio of the total molar amount of the metal doping element to the iron element is (0.5-8):100; and / or The metal doping element includes at least one element selected from the group consisting of aluminum, vanadium, chromium and nickel.
3. The modified manganese-based positive electrode material according to claim 1 or 2, characterized in that: The manganese-based positive electrode material in the doped manganese-based positive electrode material comprises lithium iron manganese phosphate; and / or The modified manganese-based positive electrode material further includes a coating layer, and the coating layer coats the doped manganese-based positive electrode material.
4. The modified manganese-based positive electrode material according to claim 3, characterized in that: The coating layer comprises a metal fluoride coating layer, and the metal fluoride coating layer is combined with the particle surface of the doped manganese-based positive electrode material.
5. The modified manganese-based positive electrode material according to claim 4, characterized in that: The metal fluoride coating layer is one or more of the following (1) to (3): (1) The thickness of the metal fluoride coating layer is 1 nm to 20 nm; (2) the metal element contained in the metal fluoride coating layer is the same as the metal doping element; and / or (3) The metal fluoride coating layer includes AlF3; and / or The coating layer further comprises other functional coating layers, and the other functional coating layers are coated on the surface of the metal fluoride coating layer away from the doped manganese-based positive electrode material.
6. The modified manganese-based positive electrode material according to any one of claims 1 to 2, 4 and 5, characterized in that: The modified manganese-based positive electrode material includes one or more of the following (1) to (4): (1) The particle size of the modified manganese-based positive electrode material is 0.11 μm to 0.27 μm; (2) The BET specific surface area of the modified manganese-based positive electrode material is 15 m 2 / g~19m 2 / g; (3) The compaction density of the modified manganese-based positive electrode material is 2.3 g / cm 3 ~2.4g / cm 3 .
7. A method for preparing a modified manganese-based positive electrode material, characterized in that: The steps include: In a plasma environment, a gaseous fluorine source is used to etch a manganese-based positive electrode material, and a fluorine element is doped into a particle surface layer of the manganese-based positive electrode material to obtain a modified manganese-based positive electrode material; The manganese-based positive electrode material contains iron, oxygen and metal doping elements, and the ion radius of the metal doping element is smaller than the ion radius of the iron.
8. The preparation method according to claim 7, characterized in that: The etching process conditions include one or more of the following (1) to (3): (1) During the etching process, the gaseous fluorine source is continuously introduced into the plasma environment, and the gas flow rate of the gaseous fluorine source is 5 sccm to 20 sccm; (2) The pressure of the plasma environment is 600Pa to 1200Pa, and the power is 100W to 400W; (3) The etching time of the etching process is 300s to 1200s; and / or The gaseous fluorine source includes at least one of fluorine gas, carbon tetrafluoride, nitrogen trifluoride, sulfur hexafluoride, hydrofluoroolefins, and freon; and / or In the manganese-based positive electrode material, the molar ratio of the metal doping element to the iron element is (0.5-5):100; and / or After the etching process, the method further includes forming other functional coating layers on the surface of the material subjected to the etching process.
9. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode active material layer bonded to the surface of the positive electrode current collector, characterized in that: The positive electrode active material layer contains the modified manganese-based positive electrode material according to any one of claims 1 to 6 or the modified manganese-based positive electrode material prepared by the preparation method according to any one of claims 7 to 8.
10. A battery, comprising a positive electrode sheet, characterized in that: The positive electrode sheet is the positive electrode sheet according to claim 9.
Citation Information
Cited By
Lattice distortion analysis-based lithium manganese iron phosphate positive electrode cycle life evaluation method
CN120908224A