High-voltage positive electrode material and preparation method thereof, positive plate, lithium ion battery and electric equipment

By adopting a three-layer structure on the lithium cobalt oxide positive electrode material, including the M-doped lithium cobalt oxide core layer, intermediate layer and spinel outer layer, the problem of degradation of lithium cobalt oxide at high voltage is solved, and high Improved rate performance, energy density and cycle stability extend the service life of lithium-ion batteries and improve safety.

CN118969981APending Publication Date: 2024-11-15TIANJIN B&M SCI & TECH LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410985068.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Lithium cobalt oxide (LiCoO2) at high voltages has degraded performance due to side reactions and irreversible phase change, limiting its application. Existing doping and coating methods are difficult to withstand higher voltages when improving cycle stability and may lead to reversibility. Capacity reduction and by-product generation.

Method used

High voltage positive electrode material adopting a three-layer structure, including a M-doped lithium cobalt oxide core layer, a coated intermediate layer and an outermost layer of spinel structure, through doping elements such as Al, Mg, Ti, etc. and lithium source Mix uniformly to form a stable spinel structure, avoid side reactions and irreversible phase change, and improve electron conductivity.

Benefits of technology

The rate performance, energy density and circulation performance of the positive electrode material are significantly improved, the stability at high temperature and high voltage is enhanced, the side reactions and cobalt dissolution phenomenon is reduced, the cycle life of lithium-ion batteries is extended and safety is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969981A_ABST
    Figure CN118969981A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of positive electrode materials, in particular to a high-voltage positive electrode material and a preparation method thereof, a positive plate, a lithium ion battery and electric equipment. The high-voltage positive electrode material comprises an M-doped lithium cobalt oxide core layer, a middle layer and an outermost layer, m comprises at least one of Al, Mg, Ti, Zr, Y, La, Mn, Ni, Sn, Ru, V, Ir, Cr, Fe, Ga, Mo, Sb, W, Na and Nb; the intermediate layer comprises a compound containing A, and A comprises at least one of Al, Co, Mg, Ti, Zr, Y, La, Mn, Ni, Sn, Ru, V, Ir, Cr, Fe, Ga, Mo, Sb, W, Na and Nb; the outermost layer comprises a spinel structure compound, and besides Li, the spinel structure compound comprises at least one of Al, Mg, Ti, Co, La, Ni, Mn, Zr and Y. The material is good in rate capability, high in energy density and good in cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of positive electrode materials, and in particular to a high-voltage positive electrode material and a preparation method thereof, a positive electrode sheet, a lithium-ion battery and an electrical device. Background Art

[0002] In recent years, with the rapid development of digital devices, the requirements for rechargeable secondary energy storage batteries have been increasing. Among the many types of batteries, lithium-ion batteries have attracted much attention due to their high energy density, high power density, high coulomb efficiency, and environmental friendliness. Among the many lithium-ion battery positive electrode materials, lithium cobalt oxide (LiCoO2, referred to as LCO) has been widely used in the field of consumer electronics due to its high compaction density and good cycle stability.

[0003] In order to meet consumers' requirements for higher and higher energy density of lithium-ion batteries and continuous working time of equipment, the compaction density of particles can be increased, the mass ratio of active materials can be adjusted, the charging cut-off voltage of materials can be increased, and the use of inactive materials such as binders and conductive agents in electrodes can be reduced. However, as the voltage rises to 4.5V, LCO particles will have serious side reactions with the electrolyte under high voltage; the irreversible phase structure change from hexagonal O3 phase to H1-3 phase increases the stress of LCO particles, resulting in cracks in the crystal particles; the loss of lattice oxygen causes the layered structure to collapse and deform, resulting in rapid capacity decay or reduced battery cycle stability. These factors cause LCO performance to decline severely under high voltage, which greatly limits its practical application. Lithium cobalt oxide can only be modified to meet the use under high voltage. There are currently two forms: doping modification and coating modification.

[0004] At present, the crystal structure of LiCoO2 is mainly stabilized by doping with a single element (Mg, Al, Ti, Ni, Zr, La, Na, Y, Sr, Nb, etc.) to inhibit its irreversible phase change at high voltage. Doping with a single element Al will react with LiPF6 in the electrolyte during the cycle, making the positive electrode material and the electrolyte react and unstable or causing the loss of the Al element in the bulk phase. At a voltage of 4.6V, multi-element doping can achieve cycle stability, such as a multilayer structure surface modification strategy including a zinc-rich surface coating, a rock salt phase buffer layer, and a surface gradient aluminum doping layer to achieve stable cycling of LCO, but there is a lack of further modification of the lattice oxygen and the LCO band structure, and it cannot withstand higher voltage cycles. In addition, if excessive element doping is used, the reversible capacity of LCO may be reduced. On the other hand, the surface coating can protect the electrode surface from direct contact with the electrolyte. Metal phosphates, metal fluorides, and metal oxides have been widely used as surface coatings to prevent surface side reactions. In addition, during the sintering process, the diffusion of the coating elements will lead to surface doping, which can alleviate the irreversible structural transformation at the surface. However, the less reactive sites on the LCO surface usually result in a lack of sufficient driving force to direct the precursor ions onto the LCO. As a result, byproducts and island aggregation of coating materials are often generated during the crystal growth process, which negatively affects the performance of LCO.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The first purpose of the present invention is to provide a high-voltage positive electrode material, which has an outer layer with a spinel structure that can improve the surface ion conductivity and electronic conductivity of lithium cobalt oxide, inhibit the side reaction between lithium cobalt oxide and the electrolyte, and improve the rate performance, energy density and cycle performance of the positive electrode material; the middle layer can prevent the coating material from falling off from the surface of the positive electrode material during battery charging and discharging, and is beneficial to electron conduction; the lithium cobalt oxide core layer can prevent the irreversible phase transition to lithium delayed spinel.

[0007] The second object of the present invention is to provide a method for preparing a high voltage positive electrode material, which is simple, easy to operate, energy-saving and environmentally friendly, low in cost, and easy to industrialize.

[0008] The third object of the present invention is to provide a positive electrode sheet, which has the advantages of high capacity, high initial efficiency, good rate performance, excellent cycle performance, etc., and can meet the use under high voltage.

[0009] A fourth object of the present invention is to provide a lithium ion battery having good rate performance, high energy density, good cycle stability under high temperature and high voltage, and high safety.

[0010] A fifth object of the present invention is to provide an electrical device.

[0011] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0012] The present invention first provides a high-voltage positive electrode material, comprising a lithium cobalt oxide core layer doped with M, an intermediate layer coated on the surface of the lithium cobalt oxide core layer, and an outermost layer coated on the surface of the intermediate layer;

[0013] Wherein, the M includes at least one of Al, Mg, Ti, Zr, Y, La, Mn, Ni, Sn, Ru, V, Ir, Cr, Fe, Ga, Mo, Sb, W, Na and Nb elements;

[0014] The intermediate layer includes a compound containing A, wherein A includes at least one of Al, Co, Mg, Ti, Zr, Y, La, Mn, Ni, Sn, Ru, V, Ir, Cr, Fe, Ga, Mo, Sb, W, Na, Nb and F;

[0015] The outermost layer includes a spinel structure compound, the spinel structure compound includes Li element and element J, and the element J includes at least one of Al, Mg, Ti, Co, La, Ni, Mn, Zr, Y and F;

[0016] The intermediate layer also includes a spinel structure compound formed by element penetration when forming the outermost layer.

[0017] Furthermore, the lithium cobalt oxide core layer includes a large-particle lithium cobalt oxide material with a median particle size of 7 to 17 μm and a small-particle lithium cobalt oxide material with a median particle size of 2 to 7 μm.

[0018] Furthermore, the mass ratio of the large-particle-size lithium cobalt oxide material to the small-particle-size lithium cobalt oxide material is 1 to 5:1.

[0019] The present invention further provides a method for preparing the high voltage positive electrode material, comprising the following steps:

[0020] (a), mixing a lithium source, a cobalt source not doped with M and an M-containing dopant, or mixing a lithium source and an M-containing cobalt source, or mixing a lithium source, an M-containing cobalt source and an M-containing dopant, and then performing a first calcination to obtain a lithium cobalt oxide material; wherein M comprises at least one of Al, Mg, Ti, Zr, Y, La, Mn, Ni, Sn, Ru, V, Ir, Cr, Fe, Ga, Mo, Sb, W, Na and Nb elements;

[0021] (b), mixing the lithium cobalt oxide material with a coating agent containing A and performing a second calcination to obtain an intermediate material; wherein A comprises at least one of Al, Mg, Co, Ti, Zr, Y, La, Mn, Ni, Sn, Ru, V, Ir, Cr, Fe, Ga, Mo, Sb, W, Na, Nb and F;

[0022] (c) mixing the intermediate material with a lithium source and a J-containing coating agent and performing a third calcination to obtain the high-voltage positive electrode material; wherein J includes at least one of Al, Mg, Ti, Co, La, Ni, Mn, Zr, Y and F.

[0023] Furthermore, in step (a), in the process of mixing the lithium source, the cobalt source not doped with M and the M-containing dopant, or mixing the lithium source and the M-containing cobalt source, or mixing the lithium source, the M-containing cobalt source and the M-containing dopant, the molar ratio of the Li element to the Co element is 1 to 1.1:1.

[0024] Furthermore, in step (a), the mass of the M-containing dopant accounts for 1000 to 30000 ppm of the mass of the undoped M cobalt source or the M-containing cobalt source.

[0025] Furthermore, in step (a), the mass of the M-containing compound in the M-containing cobalt source accounts for 1000 to 15000 ppm of the mass of the M-containing cobalt source.

[0026] Furthermore, in step (b), the mass of the A-containing coating agent accounts for 1000 to 50000 ppm of the mass of the lithium cobalt oxide material.

[0027] Furthermore, in step (c), the mass of the J-containing coating agent accounts for 1000 to 30000 ppm of the mass of the intermediate material.

[0028] Furthermore, in step (c), the mass of the lithium source accounts for 1000 to 20000 ppm of the mass of the intermediate material.

[0029] Furthermore, the first calcination comprises: firstly keeping the temperature at 400-900° C. for 3-8 hours, and then keeping the temperature at 950-1200° C. for 5-12 hours.

[0030] Furthermore, the temperature of the second calcination is 700-1000° C., and the holding time is 5-12 hours.

[0031] Furthermore, the temperature of the third calcination is 400-500° C., and the insulation time is 10-14 hours.

[0032] Furthermore, the undoped M cobalt source comprises a large-particle Co-containing compound with a median particle size of 7 to 17 μm and a small-particle Co-containing compound with a median particle size of 2 to 7 μm.

[0033] Furthermore, the M-containing cobalt source includes a large-particle M-containing cobalt source with a median particle size of 7 to 17 μm and a small-particle M-containing cobalt source with a median particle size of 2 to 7 μm.

[0034] Furthermore, the material after the first calcination is crushed and sieved to obtain a lithium cobalt oxide material with a median particle size of 14 to 17 μm.

[0035] Furthermore, the material after the second calcination is crushed and sieved to obtain an intermediate material with a median particle size of 14 to 17 μm.

[0036] Furthermore, the material after the third calcination is crushed and sieved to obtain a high-voltage positive electrode material with a median particle size of 14 to 17 μm.

[0037] The present invention further provides a positive electrode sheet, comprising the high-voltage positive electrode material.

[0038] The present invention further provides a lithium-ion battery, comprising the positive electrode sheet.

[0039] The present invention also provides an electrical device, comprising the lithium-ion battery.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] (1) The high-voltage positive electrode material provided by the present invention has an outermost layer that can improve the surface ionic conductivity and electronic conductivity of lithium cobalt oxide, inhibit the side reaction between lithium cobalt oxide and the electrolyte, and improve the rate performance, energy density and cycle performance of the positive electrode material; the middle layer can bridge the migration gap between the bulk phase and the surface to prevent lattice mismatch, and the formed embedded point-like coating structure can effectively prevent the coating material from falling off from the surface of the positive electrode material during the charging and discharging process of the lithium ion battery, and the point-like embedded structure retains a part of the electron channel, which is beneficial to electron conduction, thereby further improving the electrochemical performance of the positive electrode material; the bulk phase structure of the innermost lithium cobalt oxide core layer is doped with strongly stable lattice O, which can prevent the irreversible phase transition to lithium delayed spinel.

[0042] (2) The high voltage positive electrode material provided by the present invention can improve the cycle stability of lithium ion batteries under high temperature and high voltage.

[0043] (3) The high-voltage positive electrode material provided by the present invention can reduce direct contact with the electrolyte and reduce the occurrence of side reactions by coating lithium cobalt oxide. At the same time, it can improve the structural stability of the positive electrode material under high voltage, reduce the occurrence of cobalt dissolution and gas production, overcome the shortcomings of a single coating material, and improve the rate performance, cycle life and safety of lithium-ion batteries.

[0044] (4) The method for preparing the high voltage positive electrode material provided by the present invention mixes and grades large and small particle cobalt sources, which can increase the compaction density of lithium cobalt oxide.

[0045] (5) In the preparation method of the high voltage positive electrode material provided by the present invention, low temperature sintering is selected for the third calcination, which can not only improve the processing performance of the material, reduce cracks in the particles, increase the particle strength, ensure the consistency and stability in the battery preparation process, but also ensure that the outermost coating is a spinel structure.

[0046] (6) The method for preparing the high voltage positive electrode material provided by the present invention uses a cobalt source doped with M as a precursor, and the uniformity of M is good, which can improve the cycle performance of the prepared positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0048] Figure 1 This is a schematic structural diagram of the high voltage positive electrode material provided by the present invention. DETAILED DESCRIPTION

[0049] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0050] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0051] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0052] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.

[0053] In a first aspect, the present invention provides a three-layer high voltage positive electrode material coated with spinel, see Figure 1 As shown, it includes a lithium cobalt oxide core layer doped with M, an intermediate layer coated on the surface of the lithium cobalt oxide core layer, and an outermost layer coated on the surface of the intermediate layer.

[0054] That is, the high voltage positive electrode material has a three-layer structure, which includes, from the inside to the outside: a lithium cobalt oxide core layer doped with M, a middle layer and an outermost layer.

[0055] Wherein, the M includes at least one of Al, Mg, Ti, Zr, Y, La, Mn, Ni, Sn, Ru, V, Ir, Cr, Fe, Ga, Mo, Sb, W, Na and Nb elements, for example, one, two, three, four, five or more thereof are selected. The M-doped lithium cobalt oxide core layer is a lithium cobalt oxide core with a layered structure.

[0056] That is to say, the main component of the lithium cobalt oxide core layer is lithium cobalt oxide doped with M.

[0057] The intermediate layer includes a compound containing A, wherein A includes at least one of the elements Al, Co, Mg, Ti, Zr, Y, La, Mn, Ni, Sn, Ru, V, Ir, Cr, Fe, Ga, Mo, Sb, W, Na, Nb and F, for example, one, two, three, four, five or more thereof are selected.

[0058] The outermost layer includes a spinel structure compound, the spinel structure compound includes Li element and element J, and the element J includes at least one of Al, Mg, Ti, Co, La, Ni, Mn, Zr, Y and F, for example, one, two, three, four, five or more thereof are selected. That is, the main component of the outermost layer is a spinel structure compound containing Li and J.

[0059] The intermediate layer also includes a spinel structure compound formed by the penetration of elements when forming the outermost layer. That is, the intermediate layer has a spinel-like structure. In other words, the main components of the intermediate layer are the compound containing A and the spinel structure compound containing Li and J.

[0060] The high-voltage positive electrode material provided by the present invention is coated with a spinel structure compound on the surface of the lithium cobalt oxide core layer, which can inhibit the side reaction between lithium cobalt oxide and the electrolyte, improve the structural stability of lithium cobalt oxide, and improve the electrochemical performance of the positive electrode material. Compared with the layered structure, the spinel structure has a more stable structure and can be used as an oxygen stabilization layer to inhibit the escape of oxygen on the surface, thereby inhibiting the occurrence of interface side reactions. This unique spinel-coated three-layer structure positive electrode material has excellent cycle performance under high voltage, and because the spinel structure has better kinetic characteristics, the rate performance of the positive electrode material is improved.

[0061] At the same time, the spinel-like transition phase layer in the middle layer (a composite layer mainly composed of A-containing compounds and spinel structure compounds formed by element penetration when forming the outermost layer, and this layer of material has a spinel-like structure) can bridge the migration gap between the bulk phase and the surface to prevent lattice mismatch. The formed embedded point-like coating structure can effectively prevent the coating material from falling off from the surface of the positive electrode material during the charging and discharging process of the lithium-ion battery; and the point-like embedded structure retains a part of the electron channel, which is beneficial to electron conduction, thereby further improving the electrochemical properties of the positive electrode material.

[0062] In addition, the bulk structure of the M-doped lithium cobalt oxide core layer is doped with strongly stabilized lattice O, which can prevent the irreversible phase transition to lithium delayed spinel.

[0063] In some specific embodiments, the lithium cobalt oxide core layer includes a large-particle lithium cobalt oxide material having a median particle size (Dv50) of 7 to 17 μm (including but not limited to any point value of 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm or a range value between any two) and a small-particle lithium cobalt oxide material having a median particle size of 2 to 7 μm (including but not limited to any point value of 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm or a range value between any two). That is, the lithium cobalt oxide core layer is mainly composed of lithium cobalt oxide doped with M of different particle sizes. The lithium cobalt oxide material containing different median particle sizes can widen the half-peak width of the primary material, thereby increasing the compaction density of the material.

[0064] In some specific embodiments, in order to further improve the electrochemical properties of the prepared positive electrode material, the mass ratio of the large-particle lithium cobalt oxide material to the small-particle lithium cobalt oxide material is 1 to 5:1, including but not limited to any point value of 1:1, 2:1, 3:1, 4:1, 5:1 or a range value between any two of them.

[0065] In a second aspect, the present invention provides a method for preparing the high voltage positive electrode material, comprising the following steps:

[0066] (a) mixing a lithium source, a cobalt source not doped with M and a dopant containing M, or mixing a lithium source and a cobalt source containing M, or mixing a lithium source, a cobalt source containing M (i.e. a cobalt source doped with M) and a dopant containing M, and then performing a first calcination, and cooling to obtain a lithium cobalt oxide material; wherein M includes at least one of Al, Mg, Ti, Zr, Y, La, Mn, Ni, Sn, Ru, V, Ir, Cr, Fe, Ga, Mo, Sb, W, Na and Nb elements.

[0067] It is preferred to use a cobalt source doped with M, so that the uniformity of the doping element M is good.

[0068] (b), mixing the lithium cobalt oxide material with a coating agent containing A and performing a second calcination, and cooling to obtain an intermediate material; wherein A includes at least one of the elements Al, Mg, Co, Ti, Zr, Y, La, Mn, Ni, Sn, Ru, V, Ir, Cr, Fe, Ga, Mo, Sb, W, Na, Nb and F. The intermediate material is a composite material of a lithium cobalt oxide material coated with a coating agent containing A.

[0069] (c) mixing the intermediate material with a lithium source and a J-containing coating agent and performing a third calcination, and cooling to obtain the high voltage positive electrode material; wherein J comprises at least one of Al, Mg, Ti, Co, La, Ni, Mn, Zr, Y and F. During the third calcination, the lithium source and the J-containing coating agent react to form a spinel structure compound and coat the surface of the intermediate material. At the same time, a small amount of the lithium source and the J-containing coating agent penetrate into the intermediate material and form a transition layer of a spinel-like structure.

[0070] The positive electrode material prepared by the preparation method of the high-voltage positive electrode material provided by the present invention has higher conductivity under high voltage, thereby improving the cycle performance and rate performance, has good application prospects in lithium batteries, and the preparation process of the present invention is simple and easy.

[0071] The high-voltage positive electrode material provided by the present invention can improve the cycle stability of lithium-ion batteries under high temperature and high voltage, and has a simple preparation process, convenient operation, energy saving and environmental protection, low cost, easy industrial production, and can improve the utilization rate of the production line, reduce costs and increase efficiency.

[0072] In addition, the present invention uses a cobalt source doped with M as a precursor, and the uniformity of the doping element M is good, which can improve the cycle performance of the prepared positive electrode material.

[0073] In some specific embodiments, in step (a), during the mixing of the lithium source, the cobalt source not doped with M and the M-containing dopant, or the mixing of the lithium source and the M-containing cobalt source, or the mixing of the lithium source, the M-containing cobalt source and the M-containing dopant, the molar ratio of the Li element to the Co element is 1 to 1.1:1, including but not limited to any one of 1:1, 1.01:1, 1.03:1, 1.05:1, 1.08:1, 1.1:1 or the range between any two of them.

[0074] In some specific embodiments, in step (a), the mass of the M-containing dopant accounts for 1000 to 30000 ppm of the mass of the undoped M cobalt source or the M-containing cobalt source; including but not limited to any point value of 1000 ppm, 3000 ppm, 5000 ppm, 8000 ppm, 10000 ppm, 15000 ppm, 20000 ppm, 25000 ppm, 30000 ppm or a range value between any two of them.

[0075] Among them, 10000ppm=1wt.%.

[0076] In some specific embodiments, in step (a), the mass of the M-containing compound in the M-containing cobalt source accounts for 1000 to 15000 ppm of the mass of the M-containing cobalt source; including but not limited to any point value of 1000 ppm, 3000 ppm, 5000 ppm, 8000 ppm, 10000 ppm, 15000 ppm or a range value between any two of them.

[0077] In some specific embodiments, in step (b), the mass of the A-containing coating agent accounts for 1000 to 50000 ppm of the mass of the lithium cobalt oxide material; including but not limited to any point value of 1000 ppm, 3000 ppm, 5000 ppm, 8000 ppm, 10000 ppm, 15000 ppm, 20000 ppm, 25000 ppm, 30000 ppm, 40000 ppm, 50000 ppm or any range value between two of them.

[0078] In some specific embodiments, in step (c), the mass of the J-containing coating agent accounts for 1000 to 30000 ppm of the mass of the intermediate material; including but not limited to any point value of 1000 ppm, 5000 ppm, 10000 ppm, 15000 ppm, 20000 ppm, 25000 ppm, 30000 ppm or a range value between any two of them.

[0079] In some specific embodiments, in step (c), the mass of the lithium source accounts for 1000-20000 ppm of the mass of the intermediate material, including but not limited to any one of 1000 ppm, 3000 ppm, 5000 ppm, 8000 ppm, 10000 ppm, 15000 ppm, 20000 ppm or any range between two of them.

[0080] The positive electrode material prepared by adopting the above ratio has better capacity, cycle performance and rate performance.

[0081] In some specific embodiments, the first calcination includes: first keeping warm at 400-900°C (including but not limited to any point value of 400°C, 500°C, 600°C, 700°C, 800°C, 900°C or any range value between two thereof) for 3-8h (including but not limited to any point value of 3h, 4h, 5h, 6h, 7h, 8h or any range value between two thereof), and then keeping warm at 950-1200°C (including but not limited to any point value of 950°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C) for 5-12h (including but not limited to any point value of 5h, 6h, 7h, 8h, 9h, 10h, 12h or any range value between two thereof).

[0082] In the above sintering process, using low temperature first and then high temperature calcination can make the particle structure more stable.

[0083] In some specific embodiments, the heating rate of the first calcination is 2-10° C. / min.

[0084] In some specific implementations, the temperature is first increased to 400-900° C. at a heating rate of 2-10° C. / min and kept for 3-8 hours, and then increased to 950-1200° C. at a heating rate of 2-6° C. / min and kept for 5-12 hours.

[0085] In some specific embodiments, the temperature of the second calcination is 700-1000°C, including but not limited to any one of 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, and 1000°C, or a range between any two of them; the holding time of the second calcination is 5-12h, including but not limited to any one of 5h, 6h, 7h, 8h, 9h, 10h, and 12h, or a range between any two of them.

[0086] In some specific embodiments, the heating rate of the second calcination is 2-5° C. / min.

[0087] In some specific embodiments, the temperature of the third calcination is 400-500°C, including but not limited to any one of 400°C, 420°C, 430°C, 450°C, 460°C, 480°C, and 500°C, or a range between any two of them; the holding time of the third calcination is 10-14h, including but not limited to any one of 10h, 12h, 13h, and 14h, or a range between any two of them.

[0088] During the third calcination, low-temperature sintering is used to form a layer of spinel phase structure on the surface. Too high a temperature will cause the spinel phase to transform into a layered lithium cobalt oxide structure, so low-temperature sintering is performed here.

[0089] In some specific implementations, the heating rate of the third calcination is 2-10° C. / min.

[0090] In some specific embodiments, the equipment used for the first calcination, the second calcination, and the third calcination may be a muffle furnace, a tunnel furnace, a roller kiln, a tubular furnace, or other types of calcination equipment, which is not limited in the present invention.

[0091] In some specific embodiments, the undoped M cobalt source includes a large-particle Co-containing compound with a median particle size of 7 to 17 μm (including but not limited to any point value of 7 μm, 8 μm, 10 μm, 12 μm, 14 μm, 15 μm, 16 μm, 17 μm or a range value between any two thereof) and a small-particle Co-containing compound with a median particle size of 2 to 7 μm (including but not limited to any point value of 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm or a range value between any two thereof).

[0092] In some specific embodiments, the mass ratio of the large-particle Co-containing compound to the small-particle Co-containing compound is 1 to 5:2, including but not limited to any point value of 1:2, 2:2, 3:2, 4:2, 5:2 or a range value between any two of them.

[0093] In some specific embodiments, the M-containing cobalt source includes a large-particle M-containing cobalt source with a median particle size of 7 to 17 μm (including but not limited to any point value of 7 μm, 8 μm, 10 μm, 12 μm, 14 μm, 15 μm, 16 μm, 17 μm or a range value between any two of them) and a small-particle M-containing cobalt source with a median particle size of 2 to 7 μm (including but not limited to any point value of 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm or a range value between any two of them).

[0094] In some specific embodiments, the mass ratio of the large-particle M-containing cobalt source to the small-particle M-containing cobalt source is 1 to 5:2, including but not limited to any point value of 1:2, 2:2, 3:2, 4:2, 5:2 or a range value between any two of them.

[0095] The present invention mixes and grades large and small particle precursors, mixes them with a lithium source and calcines them, and then coats and sinters them to obtain a spinel-coated lithium cobalt oxide positive electrode material. The doped lithium cobalt oxide only uses a single calcination process to obtain lithium cobalt oxide containing both large and small particles, which greatly shortens the preparation cycle of the lithium cobalt oxide positive electrode material and reduces the production cost. At the same time, the prepared doped lithium cobalt oxide has a higher compaction density.

[0096] By adjusting the particle size ratio of the precursor and testing it with Malvern particle size software, the normal material can be optimized to form a hump line with a low front and high back and a clear concave point in the middle through the grading of lithium cobalt oxide with different doping particle sizes. The precursor grading adjustment can make the concave point almost disappear to form a continuous curve and thus widen the half-peak width of the primary material. Among them, the positive electrode material particles are selected from materials with widened half-peak width.

[0097] In addition, the present invention uses large and small particle size lithium cobalt oxide prepared in one step as a matrix for coating. Compared with separately preparing large-particle lithium cobalt oxide and small-particle lithium cobalt oxide and then mixing and coating them, it can reduce the number of sintering times and reduce the fusion problem between the grading of large and small particle lithium cobalt oxide after mixing. It can improve the ionic conductivity and electronic conductivity respectively, and exert higher specific capacity, high voltage, and excellent rate performance and cycle retention rate.

[0098] In some specific embodiments, the material after the first calcination is crushed and sieved to obtain a lithium cobalt oxide material with a median particle size of 14 to 17 μm (including but not limited to any point value of 14 μm, 15 μm, 16 μm, 17 μm or a range value between any two of them).

[0099] In some specific embodiments, the material after the second calcination is crushed and sieved to obtain an intermediate material with a median particle size of 14 to 17 μm (including but not limited to any point value of 14 μm, 15 μm, 16 μm, 17 μm or a range value between any two of them).

[0100] In some specific embodiments, the material after the third calcination is crushed and sieved to obtain a high-voltage positive electrode material with a median particle size of 14 to 17 μm (including but not limited to any point value of 14 μm, 15 μm, 16 μm, 17 μm or a range value between any two of them).

[0101] In some specific embodiments, the lithium source includes a lithium-containing compound, such as one or more of lithium carbonate, lithium nitrate, lithium acetate, lithium hydroxide, lithium oxide, lithium chloride, lithium bromide, lithium fluoride, lithium difluorophosphate, lithium tetrafluoroborate, bis(fluorosulfonyl)imide lithium salt, and the like.

[0102] In some specific embodiments, the cobalt source not doped with M includes a cobalt-containing compound, such as one or more of cobalt tetroxide, cobalt hydroxide, cobaltous oxide, cobalt oxyhydroxide, cobalt nitrate, cobalt chloride, cobalt sulfate and cobalt oxalate.

[0103] In some specific embodiments, the M-containing cobalt source includes a cobalt-containing compound doped with M, such as cobalt tetroxide, cobalt hydroxide, cobaltous oxide, cobalt oxyhydroxide, cobalt nitrate, cobalt chloride, cobalt sulfate and cobalt oxalate doped with M, wherein M includes at least one of Al, Mg, Ti, Zr, Y, La, Mn, Ni, Sn, Ru, V, Ir, Cr, Fe, Ga, Mo, Sb, W, Na and Nb elements.

[0104] In some specific embodiments, the M-containing dopant includes a compound containing M, such as one or more of an oxide, a hydroxide, a fluoride, and a carbonate containing M.

[0105] In some specific embodiments, the A-containing dopant includes an A-containing compound, such as one or more of an oxide, hydroxide, fluoride, and carbonate containing M.

[0106] In some specific embodiments, the J-containing dopant includes a J-containing compound, such as one or more of an oxide, hydroxide, fluoride, and carbonate containing M.

[0107] In a third aspect, the present invention provides a positive electrode sheet comprising the high voltage positive electrode material.

[0108] The positive electrode sheet provided by the present invention has the advantages of high capacity, high initial efficiency, good rate performance, excellent cycle performance, etc., and can meet the requirements of use under high voltage.

[0109] Optionally, the positive electrode sheet further includes a binder and / or a conductive agent, which is not limited in the present invention.

[0110] In a fourth aspect, the present invention provides a lithium-ion battery, comprising the positive electrode sheet.

[0111] The lithium ion battery provided by the present invention has good rate performance, high energy density, good cycle stability under high temperature and high voltage, and high safety.

[0112] Optionally, the lithium-ion battery further includes a negative electrode sheet, a separator and an electrolyte, which is not limited in the present invention.

[0113] In a fifth aspect, the present invention provides an electrical device comprising the lithium-ion battery.

[0114] Among them, the electrical equipment includes any equipment or device using the above-mentioned lithium-ion battery, such as electric vehicles, electric motorcycles, electric bicycles, electric tools, starting power supplies, energy storage equipment, electronic products, and office equipment, etc., and the present invention is not limited to this.

[0115] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0116] Example 1

[0117] The method for preparing the high voltage positive electrode material provided in this embodiment comprises the following steps:

[0118] (1) Large Co3O4 particles doped with 10000 ppm Al, small Co3O4 particles doped with 10000 ppm Al, Li2CO3 and MgF2 were mixed in a high-speed mixer at 1200 r / min for 25 min, wherein the median particle size of the large Co3O4 particles was 16 μm, the median particle size of the small Co3O4 particles was 4 μm, the mass ratio of the large Co3O4 particles to the small Co3O4 particles was 3:1; the molar ratio of the Li element to the Co element was 1.06:1, and the amount of MgF2 added was 2500 ppm of the sum of the mass of the large Co3O4 particles and the small Co3O4 particles. In an air atmosphere, the mixture was heated to 650°C at a heating rate of 5°C / min, kept warm for 5 h, and then heated to 1050°C at a heating rate of 3°C / min, kept warm for 8 h, and then crushed and sieved after cooling to obtain a lithium cobalt oxide material with a median particle size of 15 μm.

[0119] (2) The lithium cobalt oxide material obtained in step (1) is mixed with Al2O3, MgCO3, La2O3 and ZrO2 in a high-speed mixer at 1200 r / min for 25 min, wherein the addition amounts of Al2O3, MgCO3, La2O3 and ZrO2 are 500 ppm, 1000 ppm, 400 ppm and 600 ppm of the lithium cobalt oxide material, respectively. The mixture is heated to 900°C at a heating rate of 3°C / min in an air atmosphere, kept warm for 10 h, and crushed and sieved after cooling to obtain an intermediate material with a median particle size of 15.3 μm.

[0120] (3) The intermediate material obtained in step (2) is uniformly mixed with 0.45 wt% of LiOH, 2 wt% of Co(OH)2 and 800 ppm of Al2O3, respectively, and sintered in an air atmosphere at a heating rate of 6°C / min from room temperature to 450°C, and kept warm for 12 h; then cooled to room temperature and crushed to obtain a high-voltage positive electrode material of spinel-coated lithium cobalt oxide with a median particle size of 15.5 μm.

[0121] Example 2

[0122] The method for preparing the high voltage positive electrode material provided in this embodiment comprises the following steps:

[0123] (1) Co3O4 doped with 10000ppm Al and Co3O4 doped with 10000ppm Al Small particles of Al Co3O4, Li2CO3, LiF and Mg(OH)2 are mixed in a high-speed mixer at 1200r / min for 25min, wherein the median particle size of large particles of Co3O4 is 16μm, the median particle size of small particles of Co3O4 is 4μm, and the mass ratio of large particles of Co3O4 to small particles of Co3O4 is 2:1; the molar ratio of Li element to Co element is 1.05:1, the amount of LiF added is 2000ppm of the sum of the mass of large particles of Co3O4 and small particles of Co3O4, and the amount of Mg(OH)2 added is 1500ppm of the sum of the mass of large particles of Co3O4 and small particles of Co3O4, and then heated to 700℃ at a heating rate of 5℃ / min, kept warm for 4h, and then heated to 1050℃ at a heating rate of 3℃ / min, kept warm for 8h, and crushed and sieved after cooling to obtain a lithium cobalt oxide material with a median particle size of 14.5μm.

[0124] (2) The lithium cobalt oxide material obtained in step (1) is mixed with Al2O3, La2O3, ZrO2, Y2O3 and MgO in a high-speed mixer at 1200 r / min for 25 min, wherein the addition amounts of Al2O3, La2O3, ZrO2, Y2O3 and MgO are 500 ppm, 400 ppm, 600 ppm, 800 ppm and 1000 ppm of the lithium cobalt oxide material, respectively; then, the mixture is heated to 900°C at a heating rate of 3°C / min, kept warm for 10 h, and crushed and sieved after cooling to obtain an intermediate material with a median particle size of 14.8 μm.

[0125] (3) The intermediate material obtained in step (2) is uniformly mixed with 0.45 wt% of LiOH, 2 wt% of Co(OH)2 and 800 ppm of Al(OH)3, respectively, and sintered in an air atmosphere at a heating rate of 6°C / min from room temperature to 480°C, and kept warm for 11 hours; then cooled to room temperature and crushed to obtain a high-voltage positive electrode material of spinel-coated lithium cobalt oxide with a median particle size of 15 μm.

[0126] Example 3

[0127] The method for preparing the high voltage positive electrode material provided in this embodiment comprises the following steps:

[0128] (1) Large Co3O4 particles doped with 10000 ppm Al, small Co3O4 particles doped with 10000 ppm Al, Li2CO3, (MgCO3)4·Mg(OH)2·5H2O, La2O3 and Y2O3 were mixed in a high-speed mixer at 1200 r / min for 25 min, wherein the median particle size of the large Co3O4 particles was 14 μm, the median particle size of the small Co3O4 particles was 6 μm, the mass ratio of the large Co3O4 particles to the small Co3O4 particles was 1:1; the molar ratio of Li element to Co element was 1.06:1, (MgCO3)4·Mg(OH)2·5H2O, La2O3 and Y2O3 were mixed in a high-speed mixer at 1200 r / min for 25 min. The addition amounts of Co2O3, La2O3 and Y2O3 are 1000ppm, 400ppm and 2000ppm of the sum of the masses of large-particle Co3O4 and small-particle Co3O4, respectively. The mixture is then heated to 760°C at a heating rate of 5°C / min and kept warm for 3h. The mixture is then heated to 1000°C at a heating rate of 3°C / min and kept warm for 8h. After cooling, the mixture is crushed and sieved to obtain a lithium cobalt oxide material with a median particle size of 15μm.

[0129] (2) The lithium cobalt oxide material obtained in step (1) is mixed with Al2O3, Co(OH)2, La2O3, ZrO2 and TiO2 in a high-speed mixer at 1200 r / min for 25 min, wherein the added amounts of Al2O3, Co(OH)2, La2O3, ZrO2 and TiO2 are 500 ppm, 4 wt%, 400 ppm, 600 ppm and 700 ppm of the lithium cobalt oxide material, respectively; then, the mixture is heated to 900°C at a heating rate of 3°C / min, kept warm for 10 h, and crushed and sieved after cooling to obtain an intermediate material with a median particle size of 15.3 μm.

[0130] (3) The intermediate material obtained in step (2) is uniformly mixed with 0.45 wt% of LiOH, 2 wt% of Co(OH)2, 800 ppm of Al(OH)3 and 1000 ppm of MgCO3, respectively, and sintered in an air atmosphere at a heating rate of 6°C / min from room temperature to 430°C, and kept warm for 13 h; then cooled to room temperature and crushed to obtain a high-voltage positive electrode material of spinel-coated lithium cobalt oxide with a median particle size of 15.5 μm.

[0131] Example 4

[0132] The preparation method of the high voltage positive electrode material provided in this embodiment is basically the same as that in Embodiment 1, except that in step (3), Co(OH)2 and 800ppm Al2O3, which respectively account for 2wt% of the mass of the intermediate material, are replaced by TiO2, which accounts for 2wt% of the mass of the intermediate material.

[0133] Example 5

[0134] The preparation method of the high voltage positive electrode material provided in this embodiment is basically the same as that in Embodiment 1, except that in step (3), Co(OH)2 and 800ppm of Al2O3, which respectively account for 2wt% of the mass of the intermediate material, are replaced by: Al(OH)3, 1000ppm of La2O3 and 1000ppm of Y2O3, which respectively account for 2wt% of the mass of the intermediate material.

[0135] Example 6

[0136] The preparation method of the high voltage positive electrode material provided in this embodiment is basically the same as that in Example 1, except that in step (2), Al2O3, MgCO3, La2O3 and ZrO2 are replaced by: SnO2, V2O5, NiO and WO3, wherein the added amounts of SnO2, V2O5, NiO and WO3 are 800ppm, 800ppm, 700ppm and 900ppm of the lithium cobalt oxide material, respectively.

[0137] Example 7

[0138] The preparation method of the high voltage positive electrode material provided in this embodiment is basically the same as that in Example 1, except that in step (2), Al2O3, MgCO3, La2O3 and ZrO2 are replaced by: MnO2, Sb2O3 and MoO3, wherein the added amounts of MnO2, Sb2O3 and MoO3 are 5000ppm, 8000ppm and 10000ppm of the lithium cobalt oxide material respectively.

[0139] Example 8

[0140] The preparation method of the high voltage positive electrode material provided in this embodiment is basically the same as that in Example 1, except that in step (1), MgF2 is replaced by: Sb2O3 and SnO2, wherein the added amount of Sb2O3 is 1000ppm of the sum of the masses of large particles Co3O4 and small particles Co3O4, and the added amount of SnO2 is 1000ppm of the sum of the masses of large particles Co3O4 and small particles Co3O4.

[0141] Comparative Example 1

[0142] The method for preparing the positive electrode material provided in this comparative example comprises the following steps:

[0143] (1) Large-particle Co3O4 (median particle size of 16 μm) doped with 10000 ppm Al, Li2CO3 and MgF2 were mixed in a high-speed mixer at 1200 r / min for 25 min, wherein the molar ratio of Li element to Co element was 1.06:1, and the amount of MgF2 added was 2500 ppm of the mass of the large-particle Co3O4. The mixture was then heated to 650°C at a heating rate of 5°C / min and kept warm for 5 h. The mixture was then heated to 1050°C at a heating rate of 3°C / min and kept warm for 8 h. After cooling, the mixture was crushed and sieved to obtain a lithium cobalt oxide material with a median particle size of 15 μm.

[0144] (2) The lithium cobalt oxide material obtained in step (1) is mixed with Al2O3, MgCO3, La2O3 and ZrO2 in a high-speed mixer at 1200 r / min for 25 min, wherein the addition amounts of Al2O3, MgCO3, La2O3 and ZrO2 are 500 ppm, 1000 ppm, 400 ppm and 600 ppm of the lithium cobalt oxide material, respectively; then, the mixture is heated to 900°C at a heating rate of 3°C / min, kept warm for 10 h, and crushed and sieved after cooling to obtain an intermediate material with a median particle size of 15.3 μm.

[0145] (3) The intermediate material obtained in step (2) is uniformly mixed with 0.45 wt% of LiOH, 2 wt% of Co(OH)2 and 800 ppm of Al2O3, respectively, and sintered in an air atmosphere at a heating rate of 6°C / min from room temperature to 500°C, and kept warm for 12 h; then cooled to room temperature and crushed to obtain a positive electrode material with a median particle size of 15.5 μm.

[0146] Comparative Example 2

[0147] The method for preparing the positive electrode material provided in this comparative example comprises the following steps:

[0148] (1) Small particles of Co3O4 doped with 10000ppm Al (median particle size of 4μm), Li2CO3, LiF and Mg(OH)2 were mixed in a high-speed mixer at 1200r / min for 25min, wherein the molar ratio of Li element to Co element was 1.05:1, the amount of LiF added was 2000ppm of the mass of the small particles of Co3O4, and the amount of Mg(OH)2 added was 1500ppm of the mass of the small particles of Co3O4. The mixture was then heated to 700°C at a heating rate of 5°C / min and kept warm for 4h. The mixture was then heated to 1050°C at a heating rate of 3°C / min and kept warm for 8h. After cooling, the mixture was crushed and sieved to obtain a lithium cobalt oxide material with a median particle size of 4.5μm.

[0149] (2) The lithium cobalt oxide material obtained in step (1) is mixed with Al2O3, La2O3, ZrO2, Y2O3 and MgO in a high-speed mixer at 1200 r / min for 25 min, wherein the addition amounts of Al2O3, La2O3, ZrO2, Y2O3 and MgO are 500 ppm, 400 ppm, 600 ppm, 800 ppm and 1000 ppm of the lithium cobalt oxide material, respectively; then, the mixture is heated to 900°C at a heating rate of 3°C / min, kept warm for 10 h, and crushed and sieved after cooling to obtain an intermediate material with a median particle size of 4.8 μm.

[0150] (3) The intermediate material obtained in step (2) is uniformly mixed with 0.45 wt% of LiOH, 2 wt% of Co(OH)2 and 800 ppm of Al(OH)3, respectively, and sintered in an air atmosphere at a heating rate of 6°C / min from room temperature to 480°C, and kept warm for 11 h; then cooled to room temperature and crushed to obtain a positive electrode material with a median particle size of 5.0 μm.

[0151] Comparative Example 3

[0152] The preparation method of the high voltage positive electrode material provided in this comparative example comprises the following steps:

[0153] (1) Large Co3O4 particles, small Co3O4 particles, Li2CO3, Al2O3, (MgCO3)4·Mg(OH)2·5H2O, La2O3 and Y2O3 were mixed in a high-speed mixer at 1200 r / min for 25 min, wherein the median particle size of the large Co3O4 particles was 14 μm, the median particle size of the small Co3O4 particles was 6 μm, the mass ratio of the large Co3O4 particles to the small Co3O4 particles was 1:1; the molar ratio of the Li element to the Co element was 1.06:1, ( The addition amounts of MgCO3)4·Mg(OH)2·5H2O, Al2O3, La2O3 and Y2O3 are 1000ppm, 10000ppm, 400ppm and 2000ppm of the sum of the masses of large-particle Co3O4 and small-particle Co3O4, and then heated to 760℃ at a heating rate of 5℃ / min, kept warm for 3h, and then heated to 1000℃ at a heating rate of 3℃ / min, kept warm for 8h, and then crushed and sieved after cooling to obtain lithium cobalt oxide material with a median particle size of 15μm.

[0154] (2) The lithium cobalt oxide material obtained in step (1) is mixed with Al2O3, Co(OH)2, La2O3, ZrO2 and TiO2 in a high-speed mixer at 1200 r / min for 25 min, wherein the added amounts of Al2O3, Co(OH)2, La2O3, ZrO2 and TiO2 are 500 ppm, 4 wt%, 400 ppm, 600 ppm and 700 ppm of the lithium cobalt oxide material, respectively; then, the mixture is heated to 900°C at a heating rate of 3°C / min, kept warm for 10 h, and crushed and sieved after cooling to obtain an intermediate material with a median particle size of 15.3 μm.

[0155] (3) The intermediate material obtained in step (2) is mixed evenly with 0.45 wt% of LiOH, 2 wt% of Co(OH)2, 800 ppm of Al(OH)3 and 10000 ppm of MgCO3, respectively, and sintered in an air atmosphere at a heating rate of 6°C / min from room temperature to 400°C, and sintered for 12 h; then cooled to room temperature and crushed to obtain a positive electrode material with a median particle size of 15.5 μm.

[0156] Comparative Example 4

[0157] The preparation method of the positive electrode material provided in this comparative example is basically the same as that of comparative example 3, except that (MgCO3)4·Mg(OH)2·5H2O, La2O3 and Y2O3 are not added in step (1), that is, the lithium cobalt oxide core layer of the positive electrode material prepared in this comparative example is not doped with M.

[0158] Comparative Example 5

[0159] The positive electrode material provided in this comparative example is the intermediate material obtained in step (2) of Example 1.

[0160] Comparative Example 6

[0161] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 1, except that in step (3), LiOH is not added, that is, the outermost layer of the positive electrode material prepared in this comparative example does not contain a spinel structure compound.

[0162] Comparative Example 7

[0163] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 1, except that step (2) is not included, and the lithium cobalt oxide material obtained in step (1) is directly used as the intermediate material to perform step (3). That is, the positive electrode material prepared in this comparative example has a two-layer structure and does not contain an intermediate layer.

[0164] Experimental example

[0165] The electrical conductivity, tap density, compacted density and specific surface area of ​​the positive electrode materials prepared in each embodiment and each comparative example were tested respectively. The results are shown in Table 1.

[0166] The positive electrode materials prepared in each embodiment and each comparative example were used as positive electrode active materials, and batteries were made according to the following method. The electrochemical performance of each battery was tested, and the results are shown in Table 1.

[0167] Among them, the preparation method of the battery is: the positive electrode active material is mixed with the conductive agent carbon black (Super P) and the binder polyvinylidene fluoride (PVDF) in a mass ratio of 80:10:10, and N-methylpyrrolidone is added thereto to make a positive electrode slurry, and the obtained slurry is evenly applied to the A1 foil with a scraper, and then vacuum dried at 100°C for 10 hours to obtain the required positive electrode sheet. The button lithium-ion battery is assembled from the above-mentioned positive electrode sheet, lithium sheet negative electrode, separator between the positive and negative electrodes, and electrolyte. In a glove box with Ar atmosphere, the positive electrode and the metal negative electrode are assembled into a button battery for electrochemical performance testing. The test results are shown in Tables 1 and 2.

[0168] The testing method for button batteries is as follows: capacity test: voltage 4.6V for the first cycle, 0.1C charging, 0.1C discharging; cycle performance test method: at 45°C, charge the button battery at 0.2C, and discharge at 0.2C for 100 cycles, with a voltage range of 3V to 4.62V; rate performance test: at a voltage platform of 4.6V, charge the button battery at 0.1C, and discharge at different rates (0.1C, 0.2C, 0.5C, 1C, 2C).

[0169] Table 1 Performance of positive electrode materials and battery capacity and cycle performance test results

[0170]

[0171]

[0172] Table 2 Battery rate performance test results (discharge capacity mAh / g)

[0173] Group 0.1C 0.2C 0.5C 1C 2C Example 1 205.6 201.9 196.0 191.2 185.6 Example 2 205.2 201.3 195.8 191.0 185.5 Example 3 205.1 201.4 195.7 190.9 185.3 Example 4 204.8 200.9 195.3 190.4 184.6 Example 5 204.5 200.7 195.1 190.0 184.1 Example 6 203.9 199.9 194.8 189.6 183.8 Example 7 203.8 199.4 194.4 189.2 183.5 Example 8 202.9 199.0 193.2 187.9 181.7 Comparative Example 1 200.5 196.7 190.6 185.6 179.5 Comparative Example 2 200.4 196.5 190.4 185.2 179.3 Comparative Example 3 200.2 196.2 190.1 185.0 178.7 Comparative Example 4 200.3 196.4 190.3 185.1 178.8 Comparative Example 5 199.7 196.0 190.1 185.0 178.9 Comparative Example 6 199.6 195.7 189.8 184.6 178.5 Comparative Example 7 199.2 195.3 188.9 183.8 177.9

[0174] It can be seen from Table 1 and Table 2 that the positive electrode materials prepared in each embodiment have higher conductivity and compaction density, more suitable tap density and specific surface area, and each embodiment has higher capacity and first efficiency, better rate performance, and better cycle stability. Among them, the greater the tap density, the better the fluidity of the material, which is conducive to subsequent battery homogenization and other processes; when the specific surface area is large, the rate characteristics of the battery are better.

[0175] Specifically, by comparing Example 1 and Comparative Example 1, it can be seen that Comparative Example 1 only uses a large particle cobalt source without adding a small particle cobalt source, resulting in a decrease in conductivity and specific surface area, and a decrease in capacity and cycle performance.

[0176] By comparing Example 2 and Comparative Example 2, it can be seen that Comparative Example 2 only uses a small particle cobalt source without adding a large particle cobalt source, resulting in a decrease in conductivity, an excessively large specific surface area, and reduced capacity and cycle performance.

[0177] By comparing Example 3 and Comparative Example 3, it can be seen that compared with Example 3 which uses a doped cobalt source, since the cobalt source in Comparative Example 3 is not doped with metal elements, the bulk structure is easily destroyed, resulting in reduced capacity and cycle performance.

[0178] By comparing Example 1 and Comparative Example 4, it can be seen that the lithium cobalt oxide core layer of Comparative Example 4 is not doped with M, resulting in a decrease in conductivity, a decrease in compaction density and specific surface area, and a decrease in capacity, cycle performance and rate performance.

[0179] By comparing Example 1 and Comparative Example 5, it can be seen that the positive electrode material of Comparative Example 5 does not have an outermost layer composed of a spinel structure compound, resulting in a significant decrease in conductivity, a decrease in compaction density and specific surface area, and a decrease in capacity, cycle performance and rate performance.

[0180] By comparing Example 1 and Comparative Example 6, it can be seen that although Comparative Example 6 contains an outermost layer, its outermost layer does not contain a spinel structure compound, resulting in a significant decrease in conductivity, a decrease in compaction density and specific surface area, and a decrease in capacity, cycle performance and rate performance.

[0181] By comparing Example 1 and Comparative Example 7, it can be seen that Comparative Example 7 does not contain an intermediate layer, resulting in the loss of barrier between the oxygen atoms in the Li layer and repulsion after delithiation, leading to unstable surface structure, and then gas overflow causes the surface Co atoms to become less stable and dissolve, etc., which deteriorates the capacity and cycle performance of the material.

[0182] In summary, the high-voltage positive electrode material with a specific three-layer structure provided by the present invention can improve the physical and chemical properties of the positive electrode material and the electrochemical properties of the battery prepared therefrom.

[0183] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A high voltage positive electrode material, characterized in that: It comprises a lithium cobalt oxide core layer doped with M, an intermediate layer coated on the surface of the lithium cobalt oxide core layer, and an outermost layer coated on the surface of the intermediate layer; Wherein, the M includes at least one of Al, Mg, Ti, Zr, Y, La, Mn, Ni, Sn, Ru, V, Ir, Cr, Fe, Ga, Mo, Sb, W, Na and Nb elements; The intermediate layer includes a compound containing A, wherein A includes at least one of Al, Co, Mg, Ti, Zr, Y, La, Mn, Ni, Sn, Ru, V, Ir, Cr, Fe, Ga, Mo, Sb, W, Na, Nb and F; The outermost layer includes a spinel structure compound, the spinel structure compound includes Li element and element J, and the element J includes at least one of Al, Mg, Ti, Co, La, Ni, Mn, Zr, Y and F; The intermediate layer also includes a spinel structure compound formed by element penetration when forming the outermost layer.

2. The high voltage positive electrode material according to claim 1, characterized in that: The lithium cobalt oxide core layer includes a large-particle lithium cobalt oxide material with a median particle size of 7 to 17 μm and a small-particle lithium cobalt oxide material with a median particle size of 2 to 7 μm; Preferably, the mass ratio of the large-particle-size lithium cobalt oxide material to the small-particle-size lithium cobalt oxide material is 1 to 5:

1.

3. The method for preparing a high voltage positive electrode material according to claim 1 or 2, characterized in that: The steps include: (a), mixing a lithium source, a cobalt source not doped with M and an M-containing dopant, or mixing a lithium source and an M-containing cobalt source, or mixing a lithium source, an M-containing cobalt source and an M-containing dopant, and then performing a first calcination to obtain a lithium cobalt oxide material; wherein M comprises at least one of Al, Mg, Ti, Zr, Y, La, Mn, Ni, Sn, Ru, V, Ir, Cr, Fe, Ga, Mo, Sb, W, Na and Nb elements; (b), mixing the lithium cobalt oxide material with a coating agent containing A and performing a second calcination to obtain an intermediate material; wherein A comprises at least one of Al, Mg, Co, Ti, Zr, Y, La, Mn, Ni, Sn, Ru, V, Ir, Cr, Fe, Ga, Mo, Sb, W, Na, Nb and F; (c) mixing the intermediate material with a lithium source and a J-containing coating agent and performing a third calcination to obtain the high-voltage positive electrode material; wherein J includes at least one of Al, Mg, Ti, Co, La, Ni, Mn, Zr, Y and F.

4. The method for preparing a high voltage positive electrode material according to claim 3, characterized in that: At least one of the following conditions is met: (1) In step (a), the molar ratio of Li element to Co element is 1 to 1.1:1 in the process of mixing the lithium source, the cobalt source not doped with M and the M-containing dopant, or mixing the lithium source and the M-containing cobalt source, or mixing the lithium source, the M-containing cobalt source and the M-containing dopant; (2) In step (a), the mass of the M-containing dopant accounts for 1000 to 30000 ppm of the mass of the undoped M cobalt source or the M-containing cobalt source; (3) In step (a), the mass of the M-containing compound in the M-containing cobalt source accounts for 1000 to 15000 ppm of the mass of the M-containing cobalt source; (4) In step (b), the mass of the coating agent containing A accounts for 1000 to 50000 ppm of the mass of the lithium cobalt oxide material; (5) In step (c), the mass of the J-containing coating agent accounts for 1000 to 30000 ppm of the mass of the intermediate material; (6) In step (c), the mass of the lithium source accounts for 1000 to 20000 ppm of the mass of the intermediate material.

5. The method for preparing a high voltage positive electrode material according to claim 3, characterized in that: At least one of the following conditions is met: (1) The first calcination comprises: firstly keeping the temperature at 400-900°C for 3-8 hours, and then keeping the temperature at 950-1200°C for 5-12 hours; (2) The temperature of the second calcination is 700-1000° C. and the holding time is 5-12 hours; (3) The temperature of the third calcination is 400-500° C., and the insulation time is 10-14 hours.

6. The method for preparing a high voltage positive electrode material according to claim 3, characterized in that: The undoped M cobalt source comprises a large-particle Co-containing compound with a median particle size of 7 to 17 μm and a small-particle Co-containing compound with a median particle size of 2 to 7 μm; And / or, the M-containing cobalt source includes a large-particle M-containing cobalt source with a median particle size of 7 to 17 μm and a small-particle M-containing cobalt source with a median particle size of 2 to 7 μm.

7. The method for preparing a high voltage positive electrode material according to claim 3, characterized in that: At least one of the following conditions is met: (1) crushing and sieving the material after the first calcination to obtain a lithium cobalt oxide material with a median particle size of 14 to 17 μm; (2) crushing and sieving the material after the second calcination to obtain an intermediate material with a median particle size of 14 to 17 μm; (3) Crushing and sieving the material after the third calcination to obtain a high-voltage positive electrode material with a median particle size of 14 to 17 μm.

8. A positive electrode sheet, characterized in that: Comprising the high voltage positive electrode material as claimed in claim 1 or 2.

9. A lithium ion battery, characterized in that: Comprising the positive electrode sheet as claimed in claim 8.

10. An electrical device, characterized in that: Comprising the lithium ion battery as claimed in claim 9.

Citation Information

Cited By

  • Positive electrode active materials, and positive electrodes and rechargeable lithium batteries including the same

    EP4813923A1