Ternary positive electrode material and preparation method and application thereof

By introducing conductive electron compounds such as nickel boride and cobalt boride, as well as lithium-ion conductive compounds, into the ternary cathode material, the problem of poor cycle life and rate performance of the ternary cathode material under high nickel content is solved, and higher electronic conductivity, ionic conductivity and structural stability are achieved.

CN118969990APending Publication Date: 2024-11-15NINGBO RONBAY LITHIUM BATTERY MATERIAL CO LTD

Patent Information

Application Number
CN202411021638.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The side reactions between ternary cathode materials and electrolytes are aggravated at high nickel content, resulting in reduced cycle life and poor rate performance. Existing carbon coatings are uneven and lack lithium-ion conductivity, making it difficult to effectively improve performance.

Method used

A ternary cathode material is coated with nickel boride and/or cobalt boride, which are conductive electron compounds, and combined with lithium-ion conductive compounds to form a coating layer. The conductive electron compounds exist on the surface of secondary particles and in the grain boundaries of primary particles, constructing electron and lithium-ion transport channels. Uniform coating is achieved by controlling the boron content and sintering process.

Benefits of technology

It improves the electronic and ionic conductivity of ternary cathode materials, enhances structural stability, reduces side reactions with electrolyte, and improves rate performance and cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969990A_ABST
    Figure CN118969990A_ABST
Patent Text Reader

Abstract

The invention relates to a ternary positive electrode material and a preparation method and application thereof.The ternary positive electrode material comprises an inner core and a coating layer coating at least part of the surface of the inner core, the coating layer comprises an electron conducting compound and a lithium ion conducting compound, the electron conducting compound is selected from nickel boride and / or cobalt boride, and the lithium ion conducting compound is selected from a lithium ion conducting compound and a lithium ion conducting compound. The ternary positive electrode material is secondary particles formed by stacking primary particles, the electron conduction compound exists on the surfaces of the secondary particles and in grain boundaries formed among the primary particles, and the mass fraction of boron in the grain boundaries is larger than or equal to 1%. The ternary positive electrode material has excellent rate capability and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a ternary positive electrode material and a preparation method and application thereof. Background Art

[0002] Ternary cathode materials have attracted extensive attention in the field of high energy density lithium-ion batteries due to their higher theoretical specific capacity and higher voltage platform. However, the energy density of ternary cathode materials increases with the increase of nickel content, but higher nickel content will intensify the side reaction between the material and the electrolyte, resulting in a decrease in cycle life and poor rate performance.

[0003] To solve the above problems, the surface of the ternary positive electrode material is usually coated in the prior art, and the commonly used coating layer is mainly carbon coating. However, the carbon material has a certain reducing property and is easy to react with the oxidizing ternary material during sintering, resulting in a decrease in the performance of the ternary material. In addition, the carbon material does not have lithium ion conductivity, and there is still a problem of uneven coating. Therefore, the improvement in the rate performance of the prepared ternary positive electrode material is limited, and the cycle performance is also poor. Summary of the invention

[0004] Based on this, it is necessary to provide a ternary positive electrode material and a preparation method and application thereof to address the above problems. The ternary positive electrode material has excellent rate performance and cycle performance.

[0005] A ternary positive electrode material, comprising a core and a coating layer coated on at least a portion of the surface of the core, the coating layer comprising an electron-conducting compound and a lithium-ion-conducting compound, the electron-conducting compound being selected from nickel boride and / or cobalt boride, the ternary positive electrode material being secondary particles formed by accumulation of primary particles, wherein the electron-conducting compound exists on the surface of the secondary particles and in the grain boundaries formed between the primary particles, and the mass fraction of the boron element in the grain boundaries is greater than or equal to 1%.

[0006] In one embodiment, the coating layer also satisfies at least one of the following conditions:

[0007] (1) The mass fraction of boron in the grain boundary is 1.2%-5%;

[0008] (2) The mass fraction of the coating layer in the ternary positive electrode material is 0.05%-0.5%;

[0009] (3) The mass ratio of the electron-conducting compound to the lithium-ion-conducting compound is 1:10-1:1;

[0010] (4) The lithium ion conductive compound is selected from compounds containing at least one element of Al, B, Ti, La, Zr, P, and Si.

[0011] In one embodiment, the ternary cathode material must also meet at least one of the following conditions:

[0012] (1) The median particle size of the secondary particles is 5 μm-15 μm;

[0013] (2) The average particle size of the primary particles is 150nm-800nm.

[0014] In one embodiment, the molecular formula of the core material is Li n Ni x Co y Mn 1-x-y-z M z O2, wherein 0.9<n<1.2, 0.6≤x<1, 0<y≤0.2, 0≤z≤0.02, and M is selected from at least one of B, Mg, Si, V, Cr, Zn, Sr, Y, Zr, Nb, Mo, Sn, Sb, Ba, W, and Ta.

[0015] In the ternary positive electrode material of the present invention, the coating layer includes an electron-conducting compound and a lithium-ion-conducting compound. The electron-conducting property of the electron-conducting compound and the lithium-ion-conducting property of the lithium-ion-conducting compound are utilized to make the coating layer as a whole have the ability to conduct electrons and lithium ions, and can construct an electron transmission channel and a lithium-ion transmission channel, improve the electronic conductivity and ionic conductivity of the ternary positive electrode material, and effectively improve the rate performance of the ternary positive electrode material; at the same time, the electron-conducting compound is limited to exist on the surface of the secondary particles and in the grain boundaries formed between the primary particles, and the content of the boron element in the grain boundaries in the ternary positive electrode material can not only construct a complete electron transmission channel, further improve the rate performance of the positive electrode material, but also can realize the surface and grain boundary position of the ternary positive electrode material. All-round coating improves the structural stability of the ternary positive electrode material; and the electron-conducting compound nickel boride and / or cobalt boride itself has a stable chemical property, can reduce the side reaction with the electrolyte, inhibit HF corrosion, and thus can improve the cycle performance of the ternary positive electrode material. Therefore, the ternary positive electrode material of the present invention has excellent rate performance and cycle performance.

[0016] A method for preparing the ternary cathode material as described above comprises the following steps:

[0017] The core material, polyvinyl pyrrolidone, solvent and transition metal salt solution are mixed, and then a borohydride solution is added at 0°C-10°C for reaction, followed by separation and drying to obtain an intermediate, wherein the transition metal salt solution is selected from a salt solution containing nickel and / or cobalt, the mass fraction of borohydride in the borohydride solution to the mass of the core material is greater than or equal to 0.01%, and the addition rate of the borohydride solution is 10mL / min-40mL / min based on 1kg-5kg of the core material;

[0018] The intermediate and the lithium ion conductive source are mixed and sintered in an oxygen atmosphere to obtain a ternary positive electrode material.

[0019] In one embodiment, the method for preparing the ternary positive electrode material further needs to meet at least one of the following conditions:

[0020] (1) The mass ratio of the core material to the polyvinyl pyrrolidone is 1:0.01-1:0.05;

[0021] (2) The mass ratio of the core material to the solvent is 1:0.5-1:1.2, and the solvent is selected from water and / or alcohol;

[0022] (3) The mass of the transition metal salt in the transition metal salt solution is 0.03% to 1% of the mass of the core material;

[0023] (4) The borohydride solution is selected from at least one of a sodium borohydride solution, a potassium borohydride solution, and a lithium borohydride solution;

[0024] (5) adding the borohydride solution while stirring;

[0025] (6) The mass of the lithium ion source is 0.025%-0.5% of the mass of the intermediate;

[0026] (7) The lithium ion source is selected from a compound containing at least one element of Al, B, Ti, La, Zr, P, and Si;

[0027] (8) The sintering temperature is 250℃-450℃, and the sintering time is 6h-20h.

[0028] In one embodiment, the method for preparing the core material includes: mixing a ternary material precursor and a lithium source and sintering them in an oxygen atmosphere to obtain the core material.

[0029] In one embodiment, the method for preparing the core material further satisfies at least one of the following conditions:

[0030] (1) The molar ratio of the ternary material precursor to the lithium source is 1:1.01-1:1.2;

[0031] (2) The ternary material precursor is selected from at least one of nickel cobalt manganese hydroxide, nickel cobalt manganese oxide, nickel cobalt manganese carbonate, and nickel cobalt manganese acetate, and the lithium source is selected from lithium hydroxide and / or lithium carbonate;

[0032] (3) adding a dopant, wherein the mass of the dopant is 0.01% to 4% of the mass of the ternary material precursor, and the dopant is selected from a compound containing at least one element of B, Mg, Si, V, Cr, Zn, Sr, Y, Zr, Nb, Mo, Sn, Sb, Ba, W, and Ta;

[0033] (4) The sintering temperature is 650℃-850℃, and the sintering time is 8h-15h.

[0034] A positive electrode sheet prepared using the ternary positive electrode material as described above.

[0035] A lithium ion battery prepared using the positive electrode sheet as described above.

[0036] In the preparation method of the ternary positive electrode material of the present invention, borohydride is used as a boron source, a borohydride solution is added at a specific temperature, and the addition speed of the borohydride solution and the amount between the borohydride and the core material are limited, so that the borohydride solution and the transition metal salt solution react in situ and form an electron-conducting compound, and under the strong driving force of the interfacial chemical reaction, the electron-conducting compound is not only wrapped on the surface of the secondary particles, but also penetrates into the grain boundaries of the primary particles, so that the mass fraction of the boron element in the grain boundaries is greater than or equal to 1%, and a complete electron transmission channel can be constructed, and it is uniformly coated under the induction of polyvinyl pyrrolidone, thereby improving the structural stability; and a lithium ion-conducting compound is introduced through sintering and forms a coating layer together with the electron-conducting compound to construct a lithium ion transmission channel, so that the coating layer as a whole has the ability to conduct electrons and lithium ions, thereby improving the electronic conductivity and ionic conductivity of the ternary positive electrode material, thereby effectively improving the rate performance and cycle performance of the ternary positive electrode material.

[0037] A positive electrode sheet prepared using the ternary positive electrode material as described above.

[0038] A lithium ion battery prepared using the positive electrode sheet as described above. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0040] Figure 1 This is an electron microscope image of the ternary positive electrode material prepared in Example 1 of the present invention;

[0041] Figure 2 This is a cross-sectional SEM image of the ternary positive electrode material prepared in Example 1 of the present invention, wherein in the image, A1 represents grain boundary 1, B1 represents grain boundary 2, C1 represents primary particles, and D1 represents the surface of secondary particles;

[0042] Figure 3 This is a cross-sectional SEM image of the ternary positive electrode material prepared in Example 2 of the present invention, wherein in the figure, A2 represents grain boundary 1, B2 represents grain boundary 2, C2 represents primary particles, and D2 represents the surface of secondary particles;

[0043] Figure 4 This is a cross-sectional SEM image of the ternary positive electrode material prepared in Example 3 of the present invention, wherein in the figure, A3 represents grain boundary 1, B3 represents grain boundary 2, C3 represents primary particles, and D3 represents the surface of secondary particles;

[0044] Figure 5 This is a cross-sectional SEM image of the ternary positive electrode material prepared in Comparative Example 2 of the present invention, wherein in the image, A4 represents grain boundary 1, B4 represents grain boundary 2, C4 represents primary particles, and D4 represents the surface of secondary particles. DETAILED DESCRIPTION

[0045] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.

[0047] The present invention provides a ternary positive electrode material, which includes a core and a coating layer coated on at least a portion of the surface of the core, wherein the coating layer includes an electron-conducting compound and a lithium-ion-conducting compound, wherein the electron-conducting compound is selected from nickel boride and / or cobalt boride, and the ternary positive electrode material is a secondary particle formed by the accumulation of primary particles, wherein the electron-conducting compound exists on the surface of the secondary particles and in the grain boundaries formed between the primary particles, and the mass fraction of the boron element in the grain boundaries is greater than or equal to 1%.

[0048] In the ternary positive electrode material of the present invention, the coating layer includes an electron-conducting compound and a lithium-ion-conducting compound. The electron-conducting property of the electron-conducting compound and the lithium-ion-conducting property of the lithium-ion-conducting compound are utilized to make the coating layer as a whole have the ability to conduct electrons and lithium ions, and can construct an electron transmission channel and a lithium-ion transmission channel, improve the electronic conductivity and ionic conductivity of the ternary positive electrode material, and effectively improve the rate performance of the ternary positive electrode material; at the same time, the electron-conducting compound is limited to exist on the surface of the secondary particles and in the grain boundaries formed between the primary particles, and the content of the boron element in the grain boundaries in the ternary positive electrode material can not only construct a complete electron transmission channel, further improve the rate performance of the positive electrode material, but also can realize the surface and grain boundary position of the ternary positive electrode material. All-round coating improves the structural stability of the ternary positive electrode material; and the electron-conducting compound nickel boride and / or cobalt boride itself has a stable chemical property, can reduce the side reaction with the electrolyte, inhibit HF corrosion, and thus can improve the cycle performance of the ternary positive electrode material. Therefore, the ternary positive electrode material of the present invention has excellent rate performance and cycle performance.

[0049] Optionally, the mass fraction of the boron element in the grain boundary is 1.2%-5%. Such an arrangement can effectively improve the rate performance of the ternary positive electrode material while improving the energy density of the ternary positive electrode material.

[0050] Optionally, the mass fraction of the coating layer in the ternary cathode material is 0.05%-0.5%. Such an arrangement can further improve the ionic conductivity and electronic conductivity of the ternary cathode material while forming a more favorable barrier to inhibit side reactions, further improving its structural stability and the electrochemical performance and cycle stability of the battery.

[0051] It can be understood that the mass fraction of the boron element in the grain boundary in the present invention refers to the mass fraction of the boron element in the specific region of the grain boundary.

[0052] Optionally, the mass ratio of the electron-conducting compound to the lithium-ion-conducting compound is 1:10-1:1; such an arrangement is conducive to constructing a more complete lithium-ion transmission channel and electron transmission channel, and further improving the rate performance of the ternary positive electrode material.

[0053] Optionally, the lithium ion conducting compound is selected from compounds containing at least one element of Al, B, Ti, La, Zr, P, and Si.

[0054] Optionally, the median particle size of the secondary particles is 5 μm-15 μm, and the average particle size of the primary particles is 150 nm-800 nm. This arrangement can help improve the structural stability of the ternary positive electrode material, thereby improving the cycle performance of the ternary positive electrode material.

[0055] In one embodiment, the core material is selected from at least one of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, doped modified lithium nickel cobalt manganese oxide, and doped modified lithium nickel cobalt aluminum oxide.

[0056] Optionally, the molecular formula of the core material is Li n Ni x Co y Mn 1-x-y-z M z O2, wherein 0.9<n<1.2, 0.6≤x<1, 0<y≤0.2, 0≤z≤0.02, and M is selected from at least one of B, Mg, Si, V, Cr, Zn, Sr, Y, Zr, Nb, Mo, Sn, Sb, Ba, W, and Ta.

[0057] In the present invention, the molar amount of each element in the molecular formula of the core material can be adjusted according to demand. At the same time, by doping a small amount of M doping element, it is beneficial to further enhance the layered structure stability of the ternary positive electrode material, thereby improving the thermal stability and cycle stability of the ternary positive electrode material.

[0058] At the same time, the present invention also provides a method for preparing the ternary positive electrode material as described above, comprising the following steps:

[0059] S1, mixing a core material, polyvinyl pyrrolidone, a solvent and a transition metal salt solution, then adding a borohydride solution at 0°C-10°C for reaction, and then separating and drying to obtain an intermediate, wherein the transition metal salt solution is selected from a salt solution containing nickel and / or cobalt, the mass fraction of borohydride in the borohydride solution to the mass of the core material is greater than or equal to 0.01%, and the addition rate of the borohydride solution is 10mL / min-40mL / min based on 1kg-5kg of the core material;

[0060] S2, mixing the intermediate and the lithium ion conductive source and sintering them in an oxygen atmosphere to obtain a ternary positive electrode material.

[0061] Specifically, in step S1, borohydride is used as a boron source, a borohydride solution is added at a specific temperature for reaction, and the addition rate of the borohydride solution is controlled so that the borohydride solution and the transition metal salt solution react in situ and form an electron-conducting compound, and under the strong driving force of the interfacial chemical reaction, the electron-conducting compound is not only wrapped on the surface of the secondary particles, but also penetrates into the grain boundaries of the primary particles, that is, the double coating of the surface and the grain boundaries is achieved simultaneously, which not only can construct a complete electron transmission channel, but also improves the stability of the structure of the ternary positive electrode material, thereby improving the rate performance and cycle performance of the ternary positive electrode material.

[0062] At the same time, by controlling the content of borohydride and core material, the mass fraction of boron in the grain boundary can be made greater than or equal to 1%, thereby constructing a more complete electron transmission channel and improving the rate performance of the ternary positive electrode.

[0063] Also, in the process of adding borohydride solution to the reaction, the use of polyvinyl pyrrolidone can reduce the surface energy, inhibit the particle sedimentation problem during the liquid phase stirring process, and improve the uniformity of the coating, that is, under the induction of polyvinyl pyrrolidone, the uniform coating of the metal boron compound is achieved, thereby improving the structural stability of the ternary positive electrode material, thereby improving its rate performance and cycle life.

[0064] In step S2, by mixing the intermediate and the lithium ion conductive source and sintering them in an oxygen atmosphere, during the sintering process, the lithium ion conductive compound can be introduced and together with the electron conductive compound form a coating layer to construct a lithium ion transmission channel, so that the coating layer as a whole has the ability to conduct electrons and lithium ions, thereby improving the electronic conductivity and ionic conductivity of the ternary positive electrode material, and effectively improving the rate performance and cycle performance of the ternary positive electrode material.

[0065] It can be understood that in step S1 of the present invention, the addition rate of the borohydride solution is regulated based on the mass of the core material as a reference standard. If the mass of the core material is not within the range of 1kg-5kg, the addition rate of the borohydride solution needs to be changed in proportion to the change in the mass of the core material.

[0066] It should be noted that in the present invention, a borohydride solution is used as a boron source, and the addition conditions and order of the borohydride solution are controlled. Compared with directly adding a borohydride solution or directly adding electron-conducting compound particles, the coating layer of the present invention is more uniform. If the borohydride solution or electron-conducting compound particles are directly mixed with a ternary material precursor, polyvinyl pyrrolidone and a transition metal salt solution, it is difficult to achieve coating at the grain boundaries of the ternary positive electrode material, and only the surface of the secondary particles can be coated separately, and the desired more stable coating effect cannot be achieved.

[0067] In addition, while polyvinyl pyrrolidone is used in the present invention to improve the uniformity of the coating layer, the polyvinyl pyrrolidone itself can be removed in the subsequent sintering process, thereby not affecting the performance of the ternary positive electrode material.

[0068] In step S1, the mass of the borohydride in the borohydride solution is 0.015%-0.2% of the mass of the core material. This arrangement can better wrap the electron-conducting compound on the surface of the secondary particles and penetrate into the grain boundaries of the primary particles, and better control the mass fraction of the boron element in the grain boundaries to be 1.2%-5%, thereby building a more complete electron transmission channel and improving the rate performance of the ternary positive electrode.

[0069] Optionally, the mass of the transition metal salt in the transition metal salt solution is 0.03%-1% of the mass of the core material. This arrangement is conducive to controlling the mass fraction of the electron-conducting compound in the coating layer, while further improving the rate performance of the ternary positive electrode material and ensuring the energy density of the material.

[0070] Optionally, the mass ratio of the core material to the polyvinyl pyrrolidone is 1:0.01-1:0.05. Such a configuration can further improve the uniformity of the coating layer.

[0071] Optionally, the mass ratio of the core material to the solvent is 1:0.5-1:1.2, and the solvent is selected from water and / or alcohol. This arrangement is conducive to improving the uniform mixing of the components.

[0072] Optionally, the borohydride solution is selected from at least one of a sodium borohydride solution, a potassium borohydride solution, and a lithium borohydride solution. This arrangement is conducive to further realizing the formation of the electron-conducting compound, and injecting it into the grain boundary position during the reaction to complete the coating, thereby achieving the effect of improving the stability and safety of the ternary positive electrode material.

[0073] In one embodiment, the transition metal salt solution is selected from at least one of nickel chloride solution, cobalt chloride solution, nickel bromide, cobalt bromide, nickel sulfate or cobalt sulfate.

[0074] Optionally, the borohydride solution is added with stirring, wherein the stirring rate is 100 rpm-200 rpm and the stirring time is 1 min-5 min. Such an arrangement is conducive to improving the coating uniformity of the electronic conductive compound.

[0075] Optionally, the method for preparing the core material comprises: mixing a ternary material precursor and a lithium source and sintering the mixture under an oxygen atmosphere to obtain the core material.

[0076] Furthermore, the molar ratio of the ternary material precursor to the lithium source is 1:1.01-1:1.2. Such an arrangement is conducive to forming the molecular formula of the core material in the present invention and forming a ternary positive electrode material with structural stability.

[0077] Optionally, the ternary material precursor is selected from at least one of nickel cobalt manganese hydroxide, nickel cobalt manganese oxide, nickel cobalt manganese carbonate and nickel cobalt manganese acetate, and the lithium source is selected from lithium hydroxide and / or lithium carbonate.

[0078] Optionally, in the preparation method of the core material, a dopant is further added, the mass of the dopant is 0.01%-4% of the mass of the ternary material precursor, and the dopant is selected from a compound containing at least one element of B, Mg, Si, V, Cr, Zn, Sr, Y, Zr, Nb, Mo, Sn, Sb, Ba, W, and Ta, which is conducive to forming the core material with a molecular formula of Li n Ni x Co y Mn 1-x-y-z M z O2, where 0.9<n<1.2, 0.6≤x<1, 0<y≤0.2, 0≤z≤0.02.

[0079] Optionally, in the preparation method of the core material, the sintering temperature is 650°C-850°C, the sintering time is 8h-15h, wherein the heating rate is 1°C / min-5°C / min, preferably 1°C / min-3°C / min. Such a setting is conducive to the formation of secondary particles composed of primary particles, and at the same time, it can make the doped metal elements easily enter the bulk phase during the high-temperature sintering process, which helps to improve the structural stability of the core material, thereby improving the thermal stability and cycle stability of the ternary positive electrode material.

[0080] In one embodiment, in step S1, after the reaction is completed, filtration and vacuum drying are performed in sequence to obtain an intermediate.

[0081] In step S2, the mass of the lithium ion source is 0.03%-1% of the mass of the intermediate, preferably 0.05%-0.2%, which is conducive to the formation of a better coating layer to construct an ion transmission channel, thereby improving the ionic conductivity of the ternary positive electrode material, and cooperating with the electron-conducting compound to improve the rate performance of the ternary positive electrode material.

[0082] Optionally, the lithium ion source is selected from a compound containing at least one element of Al, B, Ti, La, Zr, P, and Si, preferably an oxide, hydroxide, phosphate, or lithium ion solid electrolyte containing at least one element of Al, B, Ti, La, Zr, P, and Si, and more preferably at least one of aluminum oxide, boric acid, boron trioxide, aluminum hydroxide, and lithium aluminum titanium phosphate (LATP). Such a configuration is conducive to further improving the ionic conductivity of the ternary positive electrode material.

[0083] Optionally, the sintering temperature is 250°C-450°C, preferably 300°C-400°C, and the sintering time is 6h-20h, preferably 10h-15h. In this way, low-temperature sintering is beneficial to control the particle size of the ternary positive electrode material, thereby better improving the structural stability of the ternary positive electrode material.

[0084] In addition, the present invention also provides a positive electrode sheet prepared using the ternary positive electrode material as described above.

[0085] And, a lithium ion battery prepared by using the positive electrode sheet as described above. The lithium ion battery has excellent rate performance and cycle performance, and high energy density.

[0086] The following specific examples will further illustrate the ternary cathode material, its preparation method and application. However, those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.

[0087] Example 1

[0088] Ni 0.92 Co 0.04 Mn 0.04 The (OH)2 precursor, lithium hydroxide and zirconium dioxide are mixed evenly, wherein lithium hydroxide and Ni 0.92 Co 0.04 Mn 0.04 The molar ratio of (OH)2 precursor is 1.05:1, and the mass of zirconium dioxide is Ni 0.92 Co 0.04 Mn 0.04 The precursor was 0.26% by weight of (OH)2, and then sintered in a box furnace in an oxygen atmosphere, where the temperature was raised to 720°C at 2°C / min and sintered for 12 hours to obtain a Li 1.05 Ni 0.92 Co 0.04 Mn 0.04 Zr 0.002 O2 core material;

[0089] The core material obtained above is uniformly mixed with 0.5 mol / L nickel chloride solution, polyvinyl pyrrolidone and deionized water to obtain a mixed solution, and then 2 mol / L sodium borohydride solution is added to the mixed solution at a rate of 20 mL / min while stirring at about 0° C. for reaction, wherein the stirring rate is 120 rpm and the stirring time is 2 min. After the reaction is completed, filtering and vacuum drying are performed in sequence to obtain an intermediate; wherein the mass ratio of the core material to polyvinyl pyrrolidone is 1:0.01, the mass ratio of the core material to deionized water is 1:1, the mass of sodium borohydride is 0.03% of the mass of the core material, the mass of nickel chloride is 0.2% of the mass of the core material, and the molar ratio of nickel element to boron element is 2:1;

[0090] The intermediate obtained above is mixed with aluminum oxide, wherein the mass of aluminum oxide is 0.15% of the mass of the intermediate, and then sintered in a furnace in an oxygen atmosphere, wherein the temperature is increased to 350°C at 2°C / min and sintered for 8 hours to obtain a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.3%, and the mass ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:2.

[0091] Example 2

[0092] Ni 0.93 Co 0.04 Mn 0.03 The (OH)2 precursor, lithium hydroxide and zirconium dioxide are mixed evenly, wherein lithium hydroxide and Ni 0.93 Co 0.04 Mn 0.03 The molar ratio of (OH)2 precursor is 1.1:1, and the mass of zirconium dioxide is Ni 0.93 Co 0.04 Mn 0.03 The precursor was 0.39% by weight of (OH)2, and then sintered in a box furnace in an oxygen atmosphere, where the temperature was raised to 650°C at 2°C / min and sintered for 15 hours to obtain a Li 1.1 Ni 0.93 Co 0.04 Mn 0.03 Zr 0.003 O2 core material;

[0093] The core material obtained above is uniformly mixed with 0.5 mol / L nickel chloride solution, polyvinyl pyrrolidone and ethanol to obtain a mixed solution, and then 2 mol / L sodium borohydride solution is added to the mixed solution at a rate of 10 mL / min while stirring at about 8° C. to react, wherein the stirring rate is 150 rpm and the stirring time is 5 min. After the reaction is completed, filtering and vacuum drying are performed in sequence to obtain an intermediate; wherein the mass ratio of the core material to polyvinyl pyrrolidone is 1:0.02, the mass of sodium borohydride is 0.03% of the mass of the core material, the mass ratio of the core material to ethanol is 1:1, the mass of nickel chloride is 0.2% of the mass of the core material, and the molar ratio of nickel element to boron element is 2:1;

[0094] The intermediate obtained above is mixed with aluminum oxide, wherein the mass of aluminum oxide is 0.075% of the mass of the intermediate, and then sintered in a furnace in an oxygen atmosphere, wherein the temperature is increased to 400°C at 2°C / min and sintered for 7 hours to obtain a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.1%, and the mass ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:1.

[0095] Example 3

[0096] Ni 0.94 Co 0.03 Mn 0.03 (OH)2 precursor, lithium hydroxide, zirconium dioxide and strontium hydroxide are mixed evenly, wherein lithium hydroxide and Ni 0.94 Co 0.03 Mn 0.03 The molar ratio of (OH)2 precursor is 1.05:1, and the mass of zirconium dioxide and strontium hydroxide are Ni 0.94 Co 0.03 Mn 0.03 The precursor was 0.26% and 0.13% by weight of (OH)2, and then sintered in a box furnace in an oxygen atmosphere, where the temperature was raised to 720°C at 2°C / min and sintered for 12 hours to obtain a Li 1.05 Ni 0.94 Co 0.03 Mn 0.03 Zr 0.002 Sr 0.001 O2 core material;

[0097] The core material obtained above is uniformly mixed with 0.5 mol / L cobalt chloride solution, polyvinyl pyrrolidone and deionized water to obtain a mixed solution, and then 2 mol / L lithium borohydride solution is added to the mixed solution at a rate of 35 mL / min while stirring at about 2° C. for reaction, wherein the stirring rate is 110 rpm and the stirring time is 2 min. After the reaction is completed, filtering and vacuum drying are performed in sequence to obtain an intermediate; wherein the mass ratio of the core material to polyvinyl pyrrolidone is 1:0.02, the mass ratio of the core material to deionized water is 1:1, the mass of lithium borohydride is 0.03% of the mass of the core material, the mass of cobalt chloride is 0.2% of the mass of the core material, and the molar ratio of cobalt element to boron element is 1:1;

[0098] The intermediate obtained above is mixed with aluminum hydroxide, wherein the mass of aluminum hydroxide is 0.24% of the mass of the intermediate, and then sintered in a furnace in an oxygen atmosphere, wherein the temperature is increased to 350°C at 2°C / min and sintered for 8 hours to obtain a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.3%, and the mass ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:2.

[0099] Example 4

[0100] Ni 0.94 Co 0.02 Mn 0.04 (OH)2 precursor, lithium hydroxide, zirconium dioxide and yttrium trioxide are mixed evenly, wherein lithium hydroxide and Ni 0.94 Co 0.02 Mn 0.04 The molar ratio of (OH)2 precursor is 1.05:1, and the mass of zirconium dioxide and yttrium trioxide are Ni 0.94 Co 0.02 Mn 0.04 The precursor was 0.26% and 0.12% by weight of (OH)2, and then sintered in a box furnace in an oxygen atmosphere, where the temperature was raised to 720°C at 2°C / min and sintered for 12 hours to obtain a Li 1.05 Ni 0.94 Co 0.02 Mn 0.04 Zr 0.002 Y 0.001 O2 core material;

[0101] The core material obtained above was used to prepare an intermediate by the method of Example 1;

[0102] The intermediate obtained above is mixed with boron trioxide, wherein the mass of boron trioxide is 0.28% of the mass of the intermediate, and then sintered in a furnace in an oxygen atmosphere, wherein the temperature is increased to 350°C at 2°C / min and sintered for 8 hours to obtain a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.5%, and the mass ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:4.

[0103] Example 5

[0104] The core material is prepared according to the method of Example 1; the core material obtained above is uniformly mixed with 2 mol / L cobalt sulfate solution, polyvinyl pyrrolidone and deionized water to obtain a mixed solution, and then 2 mol / L sodium borohydride solution is added to the mixed solution at a rate of 40 mL / min while stirring at about 2° C. to react, wherein the stirring rate is 120 rpm, the stirring time is 2 min, and after the reaction is completed, filtering and vacuum drying are performed in sequence to obtain an intermediate; wherein the mass ratio of the core material to polyvinyl pyrrolidone is 1:0.01, the mass ratio of the core material to deionized water is 1:1, the mass of sodium borohydride is 0.1% of the mass of the core material, the mass of cobalt sulfate is 0.444% of the mass of the core material, and the molar ratio of cobalt element to boron element is 1:1;

[0105] The intermediate obtained above, boric acid and solid electrolyte Li7La3Zr2O 12 (LLZO) is mixed, wherein the mass of boric acid is 0.125% of the mass of the intermediate, and the mass of LLZO is 0.1% of the mass of the intermediate, and then sintered in a furnace in an oxygen atmosphere, wherein the temperature is increased to 280°C at 2°C / min and the sintering is maintained for 8 hours to obtain a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.4%, and the ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:1.

[0106] Example 6

[0107] A core material is prepared according to the method of Example 1; the core material obtained above is uniformly mixed with a 2 mol / L nickel chloride solution, polyvinyl pyrrolidone and deionized water to obtain a mixed solution; and then a 2 mol / L lithium borohydride solution is added to the mixed solution at a rate of 15 mL / min while stirring at about 2° C. for reaction, wherein the stirring rate is 120 rpm and the stirring time is 2 min. After the reaction is completed, filtering and vacuum drying are performed in sequence to obtain an intermediate; wherein the mass ratio of the core material to polyvinyl pyrrolidone is 1:0.01, the mass ratio of the core material to deionized water is 1:1, the mass of lithium borohydride is 0.01% of the mass of the core material, the mass of nickel chloride is 0.12% of the mass of the core material, and the molar ratio of nickel element to boron element is 2:1;

[0108] The intermediate obtained above, boric acid and solid electrolyte lithium aluminum titanium phosphate (LATP) are mixed, wherein the mass of boric acid is 0.4% of the mass of the intermediate, and the mass of LATP is 0.1% of the mass of the intermediate, and then sintered in a furnace in an oxygen atmosphere, wherein the temperature is increased to 280°C at 2°C / min and sintered for 8 hours to obtain a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.42%, and the ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:6.

[0109] Example 7

[0110] Compared with Example 1, Example 7 differs only in that, in the step of preparing the core material, zirconium dioxide is not added, and other conditions are the same, thereby obtaining a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.3%, and the mass ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:2.

[0111] Example 8

[0112] The core material was prepared according to the method of Example 1; the core material obtained above was uniformly mixed with 2 mol / L cobalt bromide solution, polyvinyl pyrrolidone and deionized water to obtain a mixed solution, and then 2 mol / L potassium borohydride solution was added to the mixed solution at a rate of 40 mL / min while stirring at about 2°C for reaction, wherein the stirring rate was 120 rpm and the stirring time was 3 min. After the reaction was completed, filtering and vacuum drying were performed in sequence to obtain an intermediate; wherein the mass ratio of the core material to polyvinyl pyrrolidone was 1:0.02, the mass ratio of the core material to deionized water was 1:1, the mass of potassium borohydride was 0.2% of the mass of the core material, the mass of cobalt bromide was 0.46% of the mass of the core material, and the molar ratio of cobalt element to boron element was 1:1;

[0113] The intermediate obtained above is mixed with aluminum oxide, wherein the mass of aluminum oxide is 0.2% of the mass of the intermediate, and then sintered in a furnace in an oxygen atmosphere, wherein the temperature is increased to 350°C at 2°C / min and sintered for 8 hours to obtain a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.5%, and the mass ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:1.

[0114] Example 9

[0115] Compared with Example 1, Example 9 differs only in that the mass ratio of the core material and the polyvinyl pyrrolidone is 1:0.2, and the other conditions are the same, thereby obtaining a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.3%, and the mass ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:2.

[0116] Example 10

[0117] Compared with Example 1, Example 10 differs only in that the mass of the aluminum oxide is 1% of the mass of the intermediate, and the other conditions are the same, thereby obtaining a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 1.4%, and the mass ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:13.

[0118] Comparative Example 1

[0119] The only difference between Comparative Example 1 and Example 1 is that, in the step of preparing the intermediate, nickel chloride solution, polyvinyl pyrrolidone and sodium borohydride solution are not added, and the other conditions are the same, thereby obtaining a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.2%.

[0120] Comparative Example 2

[0121] The only difference between Comparative Example 2 and Example 1 is that, in the step of preparing the intermediate, nickel chloride solution, polyvinyl pyrrolidone and sodium borohydride solution are not added to prepare the intermediate, and then the obtained intermediate, nickel boride and aluminum oxide are mixed, wherein the mass of nickel boride is 0.1% of the mass of the intermediate, and the mass of aluminum oxide is 0.2% of the mass of the intermediate, and then sintered in a furnace in an oxygen atmosphere, wherein the temperature is increased to 350°C at 2°C / min and sintered for 8 hours, while the other conditions are the same, to obtain a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.3%, and the mass ratio of the nickel boride and the ion conductor in the coating layer is 1:2.

[0122] Comparative Example 3

[0123] Compared with Example 1, Comparative Example 3 differs only in that, in the step of preparing the intermediate, the core material obtained above is evenly mixed with 0.5 mol / L nickel chloride solution, polyvinyl pyrrolidone, deionized water and 2 mol / L sodium borohydride solution, and stirred at about 0°C, wherein the stirring rate is 120 rpm and the stirring time is 15 min. After the reaction is completed, the reaction is filtered and vacuum dried in turn to obtain an intermediate. The other conditions are the same, and a ternary positive electrode material with a coating layer is obtained, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.3%, and the mass ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:2.

[0124] Comparative Example 4

[0125] Compared with Example 6, Comparative Example 4 differs only in that, in the step of preparing the intermediate, the addition rate of the sodium borohydride solution is 6 mL / min, and the other conditions are the same, thereby obtaining a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.3%, and the mass ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:2.

[0126] Comparative Example 5

[0127] Compared with Example 1, Comparative Example 5 differs only in that, in the step of preparing the intermediate, the addition rate of the sodium borohydride solution is 100 mL / min, and the other conditions are the same, thereby obtaining a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.3%, and the mass ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:2.

[0128] Comparative Example 6

[0129] Compared with Example 1, Comparative Example 6 differs only in that, in the step of preparing the intermediate, polyvinyl pyrrolidone is not added, and the other conditions are the same, thereby obtaining a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.3%, and the mass ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:2.

[0130] Comparative Example 7

[0131] Compared with Example 1, Comparative Example 7 differs only in that aluminum oxide is not added, and other conditions are the same, thereby obtaining a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.1%.

[0132] Comparative Example 8

[0133] Compared with Example 1, Comparative Example 8 differs only in that, in the step of preparing the intermediate, the mass of sodium borohydride is 0.002% of the mass of the core material, the mass of nickel chloride is 0.02% of the mass of the core material, and the other conditions are the same, thereby obtaining a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.21%, and the mass ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:20.

[0134] Comparative Example 9

[0135] Compared with Example 1, Comparative Example 9 differs only in that, in the step of preparing the intermediate, sodium lauryl sulfate is used instead of polyvinyl pyrrolidone, and the other conditions are the same, thereby obtaining a ternary positive electrode material with a coating layer, wherein the mass fraction of the coating layer in the ternary positive electrode material is 0.3%, and the mass ratio of the electron-conducting compound to the lithium-ion-conducting compound in the coating layer is 1:2.

[0136] The boron content in the grain boundaries formed between the primary particles, the primary particles and the surfaces of the secondary particles in the ternary positive electrode materials prepared in Examples 1-10 and Comparative Examples 1-9 was measured respectively, and the specific method was as follows:

[0137] The sample to be tested was cut by an ion beam cutter, and then the cross-section of the processed sample was observed by a scanning electron microscope (SEM). Two of the grain boundaries formed between the primary particles were selected as grain boundary 1 and grain boundary 2, respectively, and the boron content was measured by energy dispersive spectrometer (EDS) point scanning. At the same time, one of the primary particles and the surface of the secondary particles were selected, and the boron content was measured by energy dispersive spectrometer (EDS) point scanning. The test results are shown in Table 1.

[0138] At the same time, the morphology and structure of the ternary positive electrode materials of the above-mentioned embodiments and comparative examples were tested by scanning electron microscopy, and in the electron microscope image, the sizes of 100 primary particles were measured respectively, and the average value was obtained, that is, the particle size of the primary particles was obtained, and the measurement results are shown in Table 1; the median particle size of the secondary particles of the ternary positive electrode materials of the above-mentioned embodiments and comparative examples was measured by laser particle size analyzer, and the measurement results are shown in Table 1.

[0139] Table 1

[0140]

[0141]

[0142] from Figure 1-5 It can be seen that the ternary positive electrode materials prepared in Examples 1-3 and Comparative Example 2 are secondary particles formed by the accumulation of primary particles, and grain boundaries are formed between the primary particles, such as Figure 2-4Grain boundaries 1 and 2 are randomly marked in Figure 1 Combined with the data in Table 1, it can be seen that the surface of the ternary positive electrode material prepared in Example 1 is coated with an electron-conducting compound (nickel boride) and a lithium-ion-conducting compound, and the electron-conducting compound (nickel boride) enters the grain boundary position of the primary particles.

[0143] It can be seen from the data in Table 1 that in the ternary positive electrode materials prepared in Examples 1-10 of the present invention, the electron-conducting compound exists on the surface of the secondary particles and in the grain boundaries formed between the primary particles, and the mass fraction of the boron element in the grain boundaries is greater than or equal to 1%.

[0144] At the same time, the ternary positive electrode materials prepared in Examples 1-10 and Comparative Examples 1-9 were respectively prepared into corresponding positive electrode sheets. The specific preparation method was as follows: the ternary positive electrode material, the conductive agent Super-P, and the binder PVDF were mixed in a mass ratio of 96.5:1.5:2 and added to the NMP solvent to mix evenly to obtain a positive electrode slurry with a solid content of 30%-40%. The positive electrode slurry was heated to about 20 mg / cm 2 The surface density of the film is coated on the positive electrode current collector aluminum foil, and the positive electrode sheet is obtained through drying-punching-rolling in sequence.

[0145] The above-mentioned positive electrode sheet, PP separator, and metal lithium sheet were stacked in sequence, and 1.0M LiPF6 electrolyte was added to assemble the corresponding LR2430 button batteries, and the discharge specific capacity and rate performance of the button batteries obtained above were tested. The test results are shown in Table 2, wherein the test method is as follows:

[0146] The button cell obtained above was tested at room temperature according to the following steps, and the discharge capacity at the corresponding rate was recorded:

[0147] (1) 0.2C charge to cut-off voltage, 0.2C discharge to termination voltage; (2) 0.5C charge to cut-off voltage, 0.5C discharge to termination voltage; (3) 0.5C charge to cut-off voltage, 1C discharge to termination voltage; (4) 0.5C charge to cut-off voltage, 2C discharge to termination voltage; (5) 0.5C charge to cut-off voltage, 3C discharge to termination voltage, where 1C = 200mA / g.

[0148] The positive electrode sheet, PP separator, and commercially available graphite negative electrode sheet obtained above were stacked in sequence, packaged in an aluminum plastic film, injected with 1.0M LiPF6 electrolyte, packaged and allowed to stand for formation to obtain a full battery, and the obtained full battery was tested for cycle performance in a 45°C constant temperature box according to the following steps. The test results are shown in Table 2, wherein the test method is as follows:

[0149] The test method for capacity retention rate after 200 cycles is as follows: charge to 4.25V at a constant current of 0.2C, and then charge to a cut-off current of 0.05C at a constant voltage of 4.25V; after standing for 2 minutes, discharge to 2.8V at a constant current of 0.2C, record the initial discharge capacity a1 of the battery, and then perform a charge and discharge cycle of 0.2C charge / 0.2C discharge; after 200 cycles, record the discharge capacity of the battery as a2, and the capacity retention rate is a2 / a1×100%, where 1C=200mA / g.

[0150] Table 2

[0151]

[0152]

[0153] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0154] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A ternary positive electrode material, characterized in that: The ternary positive electrode material includes a core and a coating layer coated on at least a portion of the surface of the core, the coating layer includes an electron-conducting compound and a lithium-ion-conducting compound, the electron-conducting compound is selected from nickel boride and / or cobalt boride, and the ternary positive electrode material is a secondary particle formed by the accumulation of primary particles, wherein the electron-conducting compound exists on the surface of the secondary particles and in the grain boundaries formed between the primary particles, and the mass fraction of the boron element in the grain boundaries is greater than or equal to 1%.

2. The ternary cathode material according to claim 1, characterized in that: The coating layer also satisfies at least one of the following conditions: (1) The mass fraction of boron in the grain boundary is 1.2%-5%; (2) The mass fraction of the coating layer in the ternary positive electrode material is 0.05%-0.5%; (3) The mass ratio of the electron-conducting compound to the lithium-ion-conducting compound is 1:10-1:1; (4) The lithium ion conductive compound is selected from compounds containing at least one element of Al, B, Ti, La, Zr, P, and Si.

3. The ternary cathode material according to claim 1, characterized in that: The ternary positive electrode material must also meet at least one of the following conditions: (1) The median particle size of the secondary particles is 5 μm-15 μm; (2) The average particle size of the primary particles is 150nm-800nm.

4. The ternary cathode material according to claim 1, characterized in that: The molecular formula of the core material is Li n Ni x Co y Mn 1-x-y-z M z O2, wherein 0.9<n<1.2, 0.6≤x<1, 0<y≤0.2, 0≤z≤0.02, and M is selected from at least one of B, Mg, Si, V, Cr, Zn, Sr, Y, Zr, Nb, Mo, Sn, Sb, Ba, W, and Ta.

5. A method for preparing a ternary positive electrode material according to any one of claims 1 to 4, characterized in that: The following steps are involved: The core material, polyvinyl pyrrolidone, solvent and transition metal salt solution are mixed, and then a borohydride solution is added at 0°C-10°C for reaction, followed by separation and drying to obtain an intermediate, wherein the transition metal salt solution is selected from a salt solution containing nickel and / or cobalt, the mass fraction of borohydride in the borohydride solution to the mass of the core material is greater than or equal to 0.01%, and the addition rate of the borohydride solution is 10mL / min-40mL / min based on 1kg-5kg of the core material; The intermediate and the lithium ion conductive source are mixed and sintered in an oxygen atmosphere to obtain a ternary positive electrode material.

6. The method for preparing the ternary cathode material according to claim 5, characterized in that: In the preparation method of the ternary positive electrode material, at least one of the following conditions must be met: (1) The mass ratio of the core material to the polyvinyl pyrrolidone is 1:0.01-1:0.05; (2) The mass ratio of the core material to the solvent is 1:0.5-1:1.2, and the solvent is selected from water and / or alcohol; (3) The mass of the transition metal salt in the transition metal salt solution is 0.03% to 1% of the mass of the core material; (4) The borohydride solution is selected from at least one of a sodium borohydride solution, a potassium borohydride solution, and a lithium borohydride solution; (5) adding the borohydride solution while stirring; (6) The mass of the lithium ion source is 0.025%-0.5% of the mass of the intermediate; (7) The lithium ion source is selected from a compound containing at least one element of Al, B, Ti, La, Zr, P, and Si; (8) The sintering temperature is 250℃-450℃, and the sintering time is 6h-20h.

7. The method for preparing the ternary cathode material according to claim 5, characterized in that: The method for preparing the core material comprises: mixing a ternary material precursor and a lithium source and sintering the mixture under an oxygen atmosphere to obtain the core material.

8. The method for preparing the ternary cathode material according to claim 7, characterized in that: In the method for preparing the core material, at least one of the following conditions is also met: (1) The molar ratio of the ternary material precursor to the lithium source is 1:1.01-1:1.2; (2) The ternary material precursor is selected from at least one of nickel cobalt manganese hydroxide, nickel cobalt manganese oxide, nickel cobalt manganese carbonate, and nickel cobalt manganese acetate, and the lithium source is selected from lithium hydroxide and / or lithium carbonate; (3) adding a dopant, wherein the mass of the dopant is 0.01% to 4% of the mass of the ternary material precursor, and the dopant is selected from a compound containing at least one element of B, Mg, Si, V, Cr, Zn, Sr, Y, Zr, Nb, Mo, Sn, Sb, Ba, W, and Ta; (4) The sintering temperature is 650℃-850℃, and the sintering time is 8h-15h.

9. A positive electrode sheet prepared using the ternary positive electrode material as claimed in any one of claims 1 to 4.

10. A lithium ion battery prepared using the positive electrode sheet as claimed in claim 9.

Citation Information

Patent Citations

  • High-nickel positive electrode material with embedded coating layer and preparation method of high-nickel positive electrode material

    CN114122377A

  • Positive electrode material, secondary battery and electric equipment

    CN116364891A

Cited By

  • Composite positive electrode material and preparation method thereof, positive plate and secondary battery

    CN119833595A