Transition metal phosphide nano material as well as preparation method and application thereof

The N-doped porous carbon-loaded NiCoP electrode material derived from the ZIF-67 nanoparticle framework solves the problem of low charge and discharge capacity of lithium-ion battery anode materials at high charge and discharge rates, and achieves higher cycle capacity retention and stability and environmentally friendly materials and low cost.

CN118970036APending Publication Date: 2024-11-15GEM WUXI ENERGY MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411007350.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing lithium-ion battery anode materials have low charge and discharge capacity and short cycle life at high charge and discharge rates, and cannot effectively overcome the problems of volume expansion and limited conductivity.

Method used

Using ZIF-67 nanoparticles as the skeleton, N-doped porous carbon-supported transition metal phosphide nanomaterials were prepared through phosphating, nitriding and recarbonization reactions, forming an N-doped porous carbon-supported NiCoP electrode material derived from ZIF-67 as the skeleton. , improve the battery's cycle capacity retention rate and charge and discharge performance.

Benefits of technology

Maintaining stable charge and discharge performance at high charge and discharge rates improves the battery's cycle capacity retention rate, and the materials are environmentally friendly, low cost, and meet the requirements of sustainable development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970036A_ABST
    Figure CN118970036A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of metal phosphide materials, in particular to a transition metal phosphide nanometer material and a preparation method and application thereof. The preparation method of the N-doped porous carbon loaded transition metal phosphide nano material derived by taking ZIF-67 as a framework comprises the following steps: S1, mixing a nickel source, a carbon source, a nitrogen source and ZIF-67 nano particles, and heating to obtain an intermediate; s2, in the presence of inert gas, carrying out phosphating reaction on a phosphorus source and the intermediate to obtain a precursor; and S3, reacting the precursor at a first temperature for a first time, and reacting at a second temperature for a second time to obtain the transition metal phosphide nano material. According to the invention, the NiCoP electrode material is finally obtained through phosphorization, nitridation and carbonization, so that the cycle capacity retention rate of a battery when the NiCoP electrode material is used as a negative electrode material is improved, and stable charge-discharge performance can be maintained at a relatively high charge-discharge rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal phosphide materials, and in particular to a transition metal phosphide nanomaterial and a preparation method and application thereof. Background Art

[0002] In order to meet the human demand for energy use, break the barriers of the electric vehicle industry and enable it to develop better, the development of a new generation of lithium-ion batteries (LIBs) with excellent performance has attracted the attention of more and more researchers. As an important component of lithium-ion batteries, negative electrode materials affect the electrochemical performance of the entire battery. At present, most negative electrode materials choose traditional graphite negative electrode materials, but graphite materials have poor compatibility with solvents, low reversible capacity for the first charge and discharge, and short cycle life. Therefore, transition metal phosphides with advantages such as high theoretical capacity, low redox potential, high thermal stability and chemical stability have good application prospects. Transition metal phosphides are ideal choices for battery negative electrodes.

[0003] The prior art discloses a method for preparing a composite material of NiCoP nanoparticles encapsulated in a carbon nanobox, wherein nickel nitrate hexahydrate is used as a nickel source, cobalt nitrate hexahydrate is used as a cobalt source, sodium hypophosphite is used as a phosphorus source, a hollow carbon nanobox is used as a carbon source, and deionized water is used as a solvent, and the reaction is carried out under hydrothermal conditions to sequentially prepare α-Fe 2 O 3 Nanocubes, hollow carbon nanoboxes, and composites of hollow carbon nanoboxes encapsulating NiCoP nanoparticles improve the rate performance of batteries. However, due to the Li + The large volume expansion and limited conductivity during the insertion / extraction process result in a low charge / discharge specific capacity, especially at high charge / discharge rates. Summary of the invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the problem that the battery in the prior art has low charge and discharge capacity when the charge and discharge rate is high, thereby providing a transition metal phosphide nanomaterial and a preparation method and application thereof.

[0005] On the one hand, the present invention provides a method for preparing a transition metal phosphide nanomaterial, comprising the following steps: S1, mixing a nickel source, a carbon source and a nitrogen source with ZIF-67 nanoparticles, and heating to obtain an intermediate; S2, in the presence of an inert gas, allowing a phosphorus source to react with the intermediate to obtain a precursor; S3, allowing the precursor to react at a first temperature for a first time, and then allowing the precursor to react at a second temperature for a second time to obtain a transition metal phosphide nanomaterial.

[0006] In some embodiments, the step S1 comprises grinding and mixing the nickel source, the carbon source and the nitrogen source with the ZIF-67 nanoparticles.

[0007] In some of the embodiments, the heating temperature of the phosphating reaction in step S2 is 320-350° C., the time of the phosphating reaction is 2-3 h, and the heating rate during the phosphating reaction is 2-5° C. / min.

[0008] In some of the embodiments, in step S1, the mixture obtained by grinding and mixing the nickel source, carbon source and nitrogen source with ZIF-67 nanoparticles in the presence of a solvent is heated, and the heating temperature is 70 to 90° C. and the heating time is 10 to 30 min.

[0009] In some embodiments, the first reaction temperature is 500-600° C., and the first reaction time is 1-2 h.

[0010] In some embodiments, the second reaction temperature is 800-900° C. and the second reaction temperature is 1-2 hours.

[0011] In some of the embodiments, the mass ratio of the ZIF-67, nickel source, carbon source and nitrogen source is (0.1-0.2):(0.1-0.2):(0.8-1.5):(0.1-0.3).

[0012] In some of the embodiments, the mass ratio of the phosphorus source to the intermediate is (1-2):(0.1-0.3).

[0013] In some embodiments, the solvent is water.

[0014] In some embodiments, step S3 further comprises cooling, washing and drying the obtained transition metal phosphide nanomaterial.

[0015] Optionally, the nickel source is at least one of nickel nitrate, nickel chloride, nickel acetate and nickel sulfate. Preferably, the particle size of the nickel source is 50 to 600 nm.

[0016] Optionally, the phosphorus source is at least one of sodium hypophosphite and phytic acid.

[0017] Optionally, the carbon source is at least one of glucose, sucrose and citric acid.

[0018] Optionally, the nitrogen source is at least one of dicyandiamide, polyaniline and melamine.

[0019] In some of the embodiments, the preparation method of the ZIF-67 nanoparticles is to mix a cobalt source, a surfactant and 2-methylimidazole in the presence of an organic solvent, react at 20-30° C. for 8-12 hours, separate the solid from the liquid, wash and dry.

[0020] Optionally, the cobalt is at least one of cobalt nitrate, cobalt chloride, cobalt sulfate and cobalt acetate.

[0021] Optionally, the surfactant is hexadecyltrimethylammonium bromide.

[0022] Optionally, the organic solvent includes an alcohol solvent, preferably, the alcohol solvent is methanol.

[0023] In some of the embodiments, the mass ratio of the cobalt source, the surfactant and 2-methylimidazole is (2-4):(2-4):(1-2).

[0024] In some of the embodiments, the ratio of the cobalt source to the organic solvent in the ZIF-67 nanoparticle solution is (2-4):500, expressed in g:mL.

[0025] On the other hand, the present invention provides a transition metal phosphide nanomaterial prepared by the above-mentioned method for preparing the transition metal phosphide nanomaterial, and the transition metal phosphide nanomaterial can be used in catalysis, electrocatalysis or preparation of negative electrode materials.

[0026] The technical solution of the present invention has the following advantages:

[0027] The present invention provides a method for preparing a N-doped porous carbon-loaded transition metal phosphide nanomaterial derived from ZIF-67 as a skeleton, comprising the following steps: S1, mixing a nickel source, a carbon source and a nitrogen source with ZIF-67 nanoparticles, heating to obtain an intermediate; S2, in the presence of an inert gas, a phosphorus source and the intermediate undergo a phosphating reaction to obtain a precursor; S3, reacting the precursor at a first temperature for a first time, and then reacting at a second temperature for a second time to obtain a transition metal phosphide nanomaterial. The present invention finally obtains an N-doped porous carbon-loaded NiCoP electrode material derived from ZIF-67 as a skeleton through phosphating, nitriding and then carbonizing. Among them, due to the reducing property of glucose, during the heating process, Ni salt can be reduced to Ni element, and then Ni element and cobalt element on ZIF-67 form stable Ni-Co-O metal oxide, and a precursor is formed through phosphating reaction. After nitridation and carbonization reactions, N-doped porous carbon-loaded transition metal phosphide nanomaterials are obtained, which improves the battery cycle capacity retention rate when used as a negative electrode material, and can maintain stable charge and discharge performance at a higher charge and discharge rate.

[0028] The transition metal phosphide nanomaterial prepared by the preparation method of the transition metal phosphide nanomaterial provided by the invention is environmentally friendly, meets the requirements of sustainable development, and has low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 is a scanning electron microscope image of ZIF-67 nanoparticles prepared in Example 1 of the present invention;

[0031] Figure 2 This is a scanning electron microscope image of the transition metal phosphide nanomaterial prepared in Example 1 of the present invention;

[0032] Figure 3 It is a graph showing the capacity retention rate of batteries formed by the negative electrode materials obtained in Example 1 of the present invention and Comparative Example 1 after 50 cycles. DETAILED DESCRIPTION

[0033] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0034] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0035] Example 1

[0036] This embodiment provides a method for preparing a transition metal phosphide nanomaterial, and the specific steps and parameters are as follows:

[0037] (1) 2.9gCo(NO 3 ) 2 6H 2 O is mixed with 3.6 g of hexadecyltrimethylammonium bromide (CTAB), 1.5 g of 2-methylimidazole (2-Melm) and 500 ml of methanol to obtain a mixed solution;

[0038] The mixed solution was reacted at 25°C for 8 h to obtain a solution containing ZIF-67 nanoparticles;

[0039] The above solution was placed in a centrifuge for centrifugation (normal temperature, 8000 rpm, 5 min), the obtained precipitate was washed twice with ethanol to remove unreacted impurities and then vacuum dried to obtain ZIF-67 nanoparticles.

[0040] (2) Take 0.1 g ZIF-67 nanoparticles and 0.1 g Ni(NO 3 ) 2 6H 2 O, 1g glucose, 0.2g dicyandiamide, and grind in a mortar;

[0041] Take 0.4 g of the ground powder, mix it evenly with 100 ml of water, react it in a rotary evaporator at 80° C. for 20 min, and dry the sample to obtain an intermediate.

[0042] (3) Transfer 0.2 g of the intermediate into a porcelain boat and place it downstream of the quartz tube. 2 PO 2 ·H 2 O was placed upstream of the quartz tube, and argon was introduced as a protective gas. The heating rate was set to 2°C / min, and the phosphating reaction was carried out at 320°C for 3h.

[0043] (4) continuing to carry out nitridation reaction at 550°C for 1 hour at a heating rate of 2°C / min, then raising the temperature to 850°C at a heating rate of 2°C / min, carrying out carbonization reaction for 2 hours, and obtaining nitrogen-doped porous carbon-supported transition metal phosphide nanomaterials after cooling;

[0044] After cooling, the transition metal phosphide nanomaterials were washed twice with ethanol to remove unreacted impurities and then dried in vacuum.

[0045] The scanning electron microscopy image of the ZIF-67 nanoparticles obtained in step (1) is shown in Figure 1 The scanning electron microscope image of the transition metal phosphide nanomaterial after cooling and washing in step (4) is shown in Figure 2 .

[0046] Example 2

[0047] This embodiment provides a method for preparing a transition metal phosphide nanomaterial, and the specific steps and parameters are as follows:

[0048] (1) Mix 2 g of cobalt chloride, 2 g of hexadecyltrimethylammonium bromide (CTAB), 1.5 g of 2-methylimidazole (2-Melm) and 500 ml of methanol to obtain a mixed solution;

[0049] The mixed solution was reacted at 20°C for 12 h to obtain a solution containing ZIF-67 nanoparticles;

[0050] The above solution was placed in a centrifuge for centrifugation (normal temperature, 8000 rpm, 5 min), the obtained precipitate was washed twice with ethanol to remove unreacted impurities and then vacuum dried to obtain ZIF-67 nanoparticles.

[0051] (2) Take 0.1 g ZIF-67 nanoparticles, 0.1 g nickel chloride, 1 g sucrose, and 0.2 g melamine and grind them in a mortar;

[0052] Take 0.4 g of the ground powder, mix it evenly with 100 ml of water, react it in a rotary evaporator at 70° C. for 30 min, and dry the sample to obtain an intermediate.

[0053] (3) 0.2 g of the intermediate was transferred to a porcelain boat and placed downstream of the quartz tube. 2.0 g of phytic acid was placed upstream of the quartz tube. With argon as the protective gas, the heating rate was set to 3°C / min and the phosphating reaction was carried out at 350°C for 2 h.

[0054] (4) After the nitridation reaction was carried out at 500°C for 2 h at a heating rate of 3°C / min, the temperature was raised to 900°C at a heating rate of 3°C / min, and the carbonization reaction was carried out for 1 h. After cooling, nitrogen-doped porous carbon-supported transition metal phosphide nanomaterials were obtained;

[0055] After cooling, the transition metal phosphide nanomaterials were washed twice with ethanol to remove unreacted impurities and then dried in vacuum.

[0056] Example 3

[0057] This embodiment provides a method for preparing a transition metal phosphide nanomaterial, and the specific steps and parameters are as follows:

[0058] (1) 4 g of cobalt sulfate, 4 g of hexadecyltrimethylammonium bromide (CTAB), 1.5 g of 2-methylimidazole (2-Melm) and 500 ml of methanol were mixed to obtain a mixed solution;

[0059] The mixed solution was reacted at 30°C for 8 h to obtain a solution containing ZIF-67 nanoparticles;

[0060] The above solution was placed in a centrifuge for centrifugation (normal temperature, 8000 rpm, 5 min), the obtained precipitate was washed twice with ethanol to remove unreacted impurities and then vacuum dried to obtain ZIF-67 nanoparticles.

[0061] (2) Take 0.1 g ZIF-67 nanoparticles, 0.1 g nickel acetate, 1 g citric acid, and 0.2 g dicyandiamide and grind them in a mortar;

[0062] Take 0.4 g of the ground powder, mix it evenly with 100 ml of water, react it in a rotary evaporator at 90° C. for 10 min, and dry the sample to obtain an intermediate.

[0063] (3) Transfer 0.2 g of the intermediate into a porcelain boat and place it downstream of the quartz tube. 2 PO 2 ·H 2 O was placed upstream of the quartz tube, and argon was introduced as a protective gas, the heating rate was set to 5°C / min, and the phosphating reaction was carried out at 340°C for 2.5h.

[0064] (4) After the nitridation reaction was carried out at 600°C for 1 hour at a heating rate of 5°C / min, the temperature was raised to 800°C at a heating rate of 5°C / min, and the carbonization reaction was carried out for 2 hours. After cooling, nitrogen-doped porous carbon-supported transition metal phosphide nanomaterials were obtained;

[0065] After cooling, the transition metal phosphide nanomaterials were washed twice with ethanol to remove unreacted impurities and then dried in vacuum.

[0066] Example 4

[0067] This embodiment provides a method for preparing a transition metal phosphide nanomaterial, and the specific steps and parameters are as follows:

[0068] (1) 2.9 g of cobalt acetate, 3.6 g of hexadecyltrimethylammonium bromide (CTAB), 1.5 g of 2-methylimidazole (2-Melm) and 500 ml of methanol were mixed to obtain a mixed solution;

[0069] The mixed solution was reacted at 25°C for 8 h to obtain a solution containing ZIF-67 nanoparticles;

[0070] The above solution was placed in a centrifuge for centrifugation (normal temperature, 8000 rpm, 5 min), the obtained precipitate was washed twice with ethanol to remove unreacted impurities and then vacuum dried to obtain ZIF-67 nanoparticles.

[0071] (2) Take 0.1 g ZIF-67 nanoparticles, 0.1 g nickel sulfate, 1 g glucose, and 0.2 g dicyandiamide and grind them in a mortar;

[0072] Take 0.4 g of the ground powder, mix it evenly with 100 ml of water, react it in a rotary evaporator at 80° C. for 20 min, and dry the sample to obtain an intermediate.

[0073] (3) Transfer 0.2 g of the intermediate into a porcelain boat and place it downstream of the quartz tube. 2 PO 2 ·H2 O was placed upstream of the quartz tube, and argon was introduced as a protective gas. The heating rate was set to 2°C / min, and the phosphating reaction was carried out at 320°C for 3h.

[0074] (4) continuing to carry out nitridation reaction at 550°C for 1 hour at a heating rate of 2°C / min, then raising the temperature to 850°C at a heating rate of 2°C / min, carrying out carbonization reaction for 2 hours, and obtaining nitrogen-doped porous carbon-supported transition metal phosphide nanomaterials after cooling;

[0075] After cooling, the transition metal phosphide nanomaterials were washed twice with ethanol to remove unreacted impurities and then dried in vacuum.

[0076] Example 5

[0077] This embodiment provides a method for preparing a transition metal phosphide nanomaterial. The specific steps and parameters are the same as those in Example 1, except that an equal mass of polyaniline (molecular weight 2500) is used to replace dicyandiamide in step (2).

[0078] Example 6

[0079] This embodiment provides a method for preparing a transition metal phosphide nanomaterial. The specific steps and parameters are the same as those in Example 1, except that an equal mass of polyaniline (molecular weight 9000) is used to replace dicyandiamide in step (2).

[0080] Example 7

[0081] This embodiment provides a method for preparing a transition metal phosphide nanomaterial. The specific steps and parameters are the same as those in Example 1, except that an equal mass of polyaniline (molecular weight 65,000) is used to replace dicyandiamide in step (2).

[0082] Example 8

[0083] This embodiment provides a method for preparing a transition metal phosphide nanomaterial. The specific steps and parameters are the same as those in Example 1, except that in step (2), ZIF-67, Ni(NO 3 ) 2 6H 2 The mass ratio of O, glucose and dicyandiamide is 0.2:0.2:0.8:0.1.

[0084] Example 9

[0085] This embodiment provides a method for preparing a transition metal phosphide nanomaterial. The specific steps and parameters are the same as those in Example 1, except that in step (2), ZIF-67, Ni(NO 3 ) 2 6H 2The mass ratio of O, glucose and dicyandiamide is 0.2:0.2:1.5:0.3.

[0086] Example 10

[0087] This embodiment provides a method for preparing a transition metal phosphide nanomaterial. The specific steps and parameters are the same as those in Example 1, except that in step (3), the mass ratio of the phosphorus source to the intermediate is 2:0.1.

[0088] Embodiment 11

[0089] This embodiment provides a method for preparing a transition metal phosphide nanomaterial. The specific steps and parameters are the same as those in Example 1, except that in step (3), the mass ratio of the phosphorus source to the intermediate is 1:0.3.

[0090] Comparative Example 1

[0091] This comparative example provides a method for preparing a transition metal phosphide nanomaterial, and the specific steps and parameters are as follows:

[0092] (1) 2.9gCo(NO 3 ) 2 6H 2 O is mixed with 3.6 g of hexadecyltrimethylammonium bromide (CTAB), 1.5 g of 2-methylimidazole (2-Melm) and 500 ml of methanol to obtain a mixed solution;

[0093] The mixed solution was reacted at 25°C for 8 h to obtain a solution containing ZIF-67 nanoparticles;

[0094] The above solution was placed in a centrifuge for centrifugation (normal temperature, 8000 rpm, 5 min), the obtained precipitate was washed twice with ethanol to remove unreacted impurities and then vacuum dried to obtain ZIF-67 nanoparticles.

[0095] (2) Take 0.2 g ZIF-67 nanoparticles and 0.2 g Ni(NO 3 ) 2 6H 2 O was ground in a mortar, the ground powder was mixed evenly with 100 ml of water, reacted at 80° C. for 20 min in a rotary evaporator, and the sample was dried to obtain an intermediate.

[0096] (3) Transfer 0.2 g of the intermediate into a porcelain boat and place it downstream of the quartz tube. 2 PO 2 ·H 2 O was placed upstream of the quartz tube, and argon was introduced as a protective gas. The heating rate was set to 2°C / min, and the phosphating reaction was carried out at 320°C for 3h.

[0097] (4) continuing to carry out nitridation reaction at 550°C for 1 hour at a heating rate of 2°C / min, then raising the temperature to 850°C at a heating rate of 2°C / min, carrying out carbonization reaction for 2 hours, and obtaining nitrogen-doped porous carbon-supported transition metal phosphide nanomaterials after cooling;

[0098] After cooling, the transition metal phosphide nanomaterials were washed twice with ethanol to remove unreacted impurities and then dried in vacuum.

[0099] Comparative Example 2

[0100] This comparative example provides a method for preparing a transition metal phosphide nanomaterial, and the specific steps and parameters are as follows:

[0101] (1) 2.9gCo(NO 3 ) 2 6H 2 O is mixed with 3.6 g of hexadecyltrimethylammonium bromide (CTAB), 1.5 g of 2-methylimidazole (2-Melm) and 500 ml of methanol to obtain a mixed solution;

[0102] The mixed solution was reacted at 25°C for 8 h to obtain a solution containing ZIF-67 nanoparticles;

[0103] The above solution was placed in a centrifuge for centrifugation (normal temperature, 8000 rpm, 5 min), the obtained precipitate was washed twice with ethanol to remove unreacted impurities and then vacuum dried to obtain ZIF-67 nanoparticles.

[0104] (2) Take 0.2g ZIF-67 nanoparticles and 0.2g Ni(NO 3 ) 2 6H 2 O. Grind 2 g glucose in a mortar;

[0105] Take 0.4 g of the ground powder, mix it evenly with 100 ml of water, react it in a rotary evaporator at 80° C. for 20 min, and dry the sample to obtain an intermediate.

[0106] (3) Transfer 0.2 g of the intermediate into a porcelain boat and place it downstream of the quartz tube. 2 PO 2 ·H 2 O was placed upstream of the quartz tube, and argon was introduced as a protective gas. The heating rate was set to 2°C / min, and the phosphating reaction was carried out at 320°C for 3h.

[0107] (4) continuing to carry out nitridation reaction at 550°C for 1 hour at a heating rate of 2°C / min, then raising the temperature to 850°C at a heating rate of 2°C / min, carrying out carbonization reaction for 2 hours, and obtaining nitrogen-doped porous carbon-supported transition metal phosphide nanomaterials after cooling;

[0108] After cooling, the transition metal phosphide nanomaterials were washed twice with ethanol to remove unreacted impurities and then dried in vacuum.

[0109] Comparative Example 3

[0110] This comparative example provides a method for preparing a transition metal phosphide nanomaterial, and the specific steps and parameters are as follows:

[0111] (1) 2.9gCo(NO 3 ) 2 6H 2 O is mixed with 3.6 g of hexadecyltrimethylammonium bromide (CTAB), 1.5 g of 2-methylimidazole (2-Melm) and 500 ml of methanol to obtain a mixed solution;

[0112] The mixed solution was reacted at 25°C for 8 h to obtain a solution containing ZIF-67 nanoparticles;

[0113] The above solution was placed in a centrifuge for centrifugation (normal temperature, 8000 rpm, 5 min), the obtained precipitate was washed twice with ethanol to remove unreacted impurities and then vacuum dried to obtain ZIF-67 nanoparticles.

[0114] (2) Take 0.1 g ZIF-67 nanoparticles and 0.1 g Ni(NO 3 ) 2 6H 2 O, 0.2g of dicyandiamide, and grind it in a mortar. Take the ground powder and mix it evenly with 100ml of water. React it in a rotary evaporator at 80°C for 20min, dry the sample, and obtain an intermediate.

[0115] (3) Transfer 0.2 g of the intermediate into a porcelain boat and place it downstream of the quartz tube. 2 PO 2 ·H 2 O was placed upstream of the quartz tube, and argon was introduced as a protective gas. The heating rate was set to 2°C / min, and the phosphating reaction was carried out at 320°C for 3h.

[0116] (4) continuing to carry out nitridation reaction at 550°C for 1 hour at a heating rate of 2°C / min, then raising the temperature to 850°C at a heating rate of 2°C / min, carrying out carbonization reaction for 2 hours, and obtaining nitrogen-doped porous carbon-supported transition metal phosphide nanomaterials after cooling;

[0117] After cooling, the transition metal phosphide nanomaterials were washed twice with ethanol to remove unreacted impurities and then dried in vacuum.

[0118] Experimental example

[0119] The transition metal phosphide nanomaterials and commercial graphite prepared in Examples 1-11 and Comparative Examples 1-3 were used as negative electrode materials, and button cells were assembled in the order of negative electrode shell, gasket, washer, negative electrode material, diaphragm, NCM811 electrode sheet and positive electrode shell. The NCM811 electrode sheet was used as the counter electrode, Celgard 2400 polypropylene (PP) film was used as the diaphragm, and the electrolyte was 1 mol / L LiPF 6 Dissolved in ethylene carbonate (EC) and diethyl carbonate (DEC) (EC:DEC = 1:1, volume ratio), the synthesized material is used as the negative electrode material of the battery. The button battery is assembled in a glove box with an argon atmosphere, sealed with a sealing machine, and left to stand for 12 hours before conducting relevant tests.

[0120] The specific test method is to put the button battery into the blue electric test system for electrical performance testing. The test voltage range is 2.5-4.25V. The discharge specific capacity of the button battery at different discharge rates and the capacity retention rate of 50 cycles are tested. The test results are shown in Table 1.

[0121] Table 1 Electrochemical performance of button cell

[0122]

[0123]

[0124] According to Table 1, the batteries formed by the negative electrode materials prepared in Examples 1-11 of the present invention can obtain a high discharge specific capacity at different discharge rates, and the capacity retention rate after 50 cycles is good, especially at a discharge rate of 1C, the discharge specific capacity decrease is low. Comparative Example 1 uses negative electrode materials obtained by not coating the surface of ZIF-67 nanoparticles with carbon source and nitrogen source, Comparative Example 2 only with carbon coating, and Comparative Example 3 only with nitrogen coating, and the battery formed by using graphite as the negative electrode, and the cycle capacity retention rate is poor, especially at a discharge rate of 1C, the discharge specific capacity can only reach a maximum of 178.1mAh / g.

[0125] The battery formed by the negative electrode materials prepared in Example 1 and Comparative Example 1 was cycled 50 times at a voltage of 4.25 V and a charge / discharge rate of 1C / 1C, and the battery capacity retention rate at each cycle was measured to obtain Figure 3 It can be seen that within 50 cycles, the battery formed by the negative electrode material prepared in Example 1 has better cycle stability than the negative electrode material prepared in Comparative Example 1.

[0126] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing a transition metal phosphide nanomaterial, characterized in that: The following steps are included: S1, mixing a nickel source, a carbon source, and a nitrogen source with ZIF-67 nanoparticles and heating to obtain an intermediate; S2, in the presence of an inert gas, a phosphorus source and an intermediate undergo a phosphating reaction to obtain a precursor; S3, reacting the precursor at a first temperature for a first time, and then reacting at a second temperature for a second time to obtain a transition metal phosphide nanomaterial.

2. The method for preparing the transition metal phosphide nanomaterial according to claim 1, characterized in that: Step S1 comprises mixing the nickel source, the carbon source and the nitrogen source with the ZIF-67 nanoparticles by grinding; and / or, The heating temperature of the phosphating reaction in step S2 is 320-350° C., the time of the phosphating reaction is 2-3 hours, and the heating rate during the phosphating reaction is 2-5° C. / min.

3. The method for preparing the transition metal phosphide nanomaterial according to claim 2, characterized in that: In the step S1, in the presence of a solvent, the nickel source, the carbon source and the nitrogen source are ground and mixed with the ZIF-67 nanoparticles to obtain a mixture which is heated at a temperature of 70 to 90° C. for a heating time of 10 to 30 min; and / or, The first reaction temperature is 500-600° C., and the first reaction time is 1-2 hours; and / or, The second reaction temperature is 800-900° C. and the second reaction time is 1-2 hours.

4. The method for preparing the transition metal phosphide nanomaterial according to claim 3, characterized in that: The mass ratio of the ZIF-67, the nickel source, the carbon source and the nitrogen source is (0.1-0.2):(0.1-0.2):(0.8-1.5):(0.1-0.3); and / or, The mass ratio of the phosphorus source to the intermediate is (1-2):(0.1-0.3); and / or, The solvent is water.

5. The method for preparing the transition metal phosphide nanomaterial according to claim 1, characterized in that: Step S3 also includes cooling, washing, and drying the obtained transition metal phosphide nanomaterial; and / or, The nickel source is at least one of nickel nitrate, nickel chloride, nickel acetate and nickel sulfate; and / or, The phosphorus source is at least one of sodium hypophosphite and phytic acid; and / or, The carbon source is at least one of glucose, sucrose and citric acid; and / or, The nitrogen source is at least one of dicyandiamide, polyaniline and melamine.

6. The method for preparing the transition metal phosphide nanomaterial according to claim 1, characterized in that: The preparation method of the ZIF-67 nanoparticles is as follows: in the presence of an organic solvent, a cobalt source, a surfactant and 2-methylimidazole are mixed, reacted at 20 to 30° C. for 8 to 12 hours, solid-liquid separation, washing and drying.

7. The method for preparing the transition metal phosphide nanomaterial according to claim 6, characterized in that: The cobalt is at least one of cobalt nitrate, cobalt chloride, cobalt sulfate and cobalt acetate; and / or, The surfactant is hexadecyltrimethylammonium bromide; and / or, The organic solvent includes an alcohol solvent, and optionally, the alcohol solvent is methanol.

8. The method for preparing the transition metal phosphide nanomaterial according to claim 7, characterized in that: The mass ratio of the cobalt source, the surfactant and the 2-methylimidazole is (2-4):(2-4):(1-2); The ratio of the cobalt source to the organic solvent in the ZIF-67 nanoparticle solution is (2-4):500, in units of g:mL.

9. A transition metal phosphide nanomaterial, characterized in that: The transition metal phosphide nanomaterial is prepared by the preparation method of the transition metal phosphide nanomaterial according to any one of claims 1 to 8.

10. Use of the transition metal phosphide nanomaterial according to claim 9 in catalysis, electrocatalysis or preparation of negative electrode materials.