Dip-molded article, chloroprene polymer, and method for producing dip-molded article

By adding 2,3-dichloro-1,3-butadiene monomer and metal oxide to the chloroprene-based polymer, using impregnation solidification method and thermal drying treatment, a superior feel of hand and wearable feeling was prepared by using impregnation and solidification method and thermal drying treatment. The impregnated molded product solves the shortcomings of the chloroprene-based polymer in the prior art in terms of mechanical properties and feel, and realizes a high-performance impregnated molded product suitable for a variety of applications.

CN118974159APending Publication Date: 2024-11-15DENKA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030825.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-24
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In medical gloves and other applications, it is difficult to achieve the same mechanical properties and feel advantages as natural rubber and polyisoprene, especially in terms of wearable and fitting. insufficient.

Method used

By adding 2,3-dichloro-1,3-butadiene monomer to the chloroprene-based polymer, and using impregnation solidification method and thermal drying treatment, the energy storage modulus E' is 3.2MPa or less. The impregnated molded substance with a loss modulus E” is less than 0.37 MPa, and components such as calcium-based solidified liquid and metal oxide are used during the molding process to optimize the molecular weight distribution and combination formula of the polymer.

Benefits of technology

The impregnated molded product has achieved sufficient tensile strength of breakage and excellent feel and wearable feeling. It is suitable for industrial and medical gloves, balloons, catheters and other applications, and can achieve good mechanical characteristics without adding vulcanizing agents and vulcanizing accelerators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005061972410000021
    Figure BDA0005061972410000021
  • Figure BDA0005061972410000171
    Figure BDA0005061972410000171
  • Figure BDA0005061972410000261
    Figure BDA0005061972410000261
Patent Text Reader

Abstract

The purpose of the present invention is to provide a dip-molded article containing a chloroprene polymer, the dip-molded article having sufficient tensile strength at break and having excellent texture of a dip-molded article (film) and excellent wearing feel when made into gloves. According to the present invention, provided is a dip-molded article which contains a chloroprene polymer, and which has a storage modulus E'of 3.2 MPa or less and a loss modulus E ''of 0.37 MPa or less at a frequency range of 10 Hz as measured by a non-resonant forced vibration method under conditions of a static tension of 5 gf, a temperature of 25 DEG C, a strain of 0.75%, and an amplitude of 0.15 mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a dip-molded article of a chloroprene polymer, a chloroprene polymer, and a method for producing the dip-molded article. More specifically, the present invention relates to a dip-molded article obtained using a chloroprene polymer latex composition containing a chloroprene polymer. Background Art

[0002] Chloroprene-based polymers are known as materials for dip-molded products such as medical surgical gloves, medical examination gloves, industrial gloves, balloons, catheters, rubber boots, and the like.

[0003] Various technologies have been proposed for chloroprene polymer latex for dip-molded products with improved flexibility of chloroprene polymers and dip-molded products of chloroprene polymers. Patent Document 1 describes a polychloroprene latex for use in dip-molded products, which contains 100 parts by mass of modified polychloroprene obtained by copolymerizing chloroprene and methacrylic acid, 90 to 150 parts by mass of water, 1 to 5 parts by mass of an emulsifier, and 0.5 to 2.5 parts by mass of potassium ions, and has a pH of 7 to 14. Patent Document 2 describes a mercaptan-modified polychloroprene latex for use in dip-molded products, wherein chloroprene and 2,3-dichloro-1,3-butadiene are copolymerized, and in the 13C-solid NMR spectrum of the polychloroprene, the peak area (A) of 126.2 to 127.6 ppm, the peak area (B) of 122.0 to 126.2 ppm, and the peak area (C) of 129.9 to 130.3 ppm are in the ranges shown by the following general formula (I). Patent Document 3 describes a chloroprene polymer latex for use in dip-molded products, which contains a high molecular weight polymer and a low molecular weight polymer, and can achieve both excellent softness and mechanical properties in a vulcanized rubber prepared by dip molding. Patent Document 4 describes a chloroprene polymer latex, which has excellent flexibility and exhibits mechanical properties even under mild vulcanization conditions by copolymerizing chloroprene monomers with isoprene monomers as raw materials of isoprene rubber. Patent Document 5 describes an isoprene / chloroprene polymer dip-molded product, which exhibits excellent flexibility even without containing a diphenylguanidine reagent as a vulcanization accelerator by mixing isoprene polymer latex and chloroprene polymer latex. Patent Document 6 describes a dip-molded product, which exhibits excellent mechanical properties by mixing nitrile-butadiene polymer (NBR) latex and isoprene polymer latex with chloroprene polymer latex as a base.

[0004] [Number 1]

[0005]

[0006] [Prior art documents]

[0007] [Patent Document]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 2014-114342

[0009] [Patent Document 2] International Publication No. 2019 / 009038

[0010] [Patent Document 3] Japanese Patent Application Publication No. 2019-143002

[0011] [Patent Document 4] International Publication No. 2021-132460

[0012] [Patent Document 5] Japanese Patent Publication No. 2017-508840

[0013] [Patent Document 6] Japanese Patent Application Publication No. 2020-189963 Summary of the invention

[0014] Problem that the invention aims to solve

[0015] As dip-molded products, dip-molded articles containing chloroprene-based polymers have been widely used in applications such as gloves, balloons, boots, and catheters. On the other hand, in particular, in medical rubber gloves, there is a tendency to seek excellent mechanical properties similar to those of dip-molded articles obtained using natural rubber and polyisoprene, and it is also desired to develop a dip-molded article containing chloroprene-based polymers that can improve the feel of the dip-molded article (dip-molded film) and the wearing feeling (fitting feeling) when the gloves are made.

[0016] Therefore, the present invention aims to provide a dip-molded product containing a chloroprene-based polymer, which has sufficient tensile strength at break and has excellent hand feel of the dip-molded product (film) and excellent wearing feeling when made into gloves.

[0017] Solutions for solving problems

[0018] That is, according to the present invention, there is provided a dip-molded product comprising a chloroprene-based polymer, wherein the dip-molded product has a storage modulus E' of 3.2 MPa or less and a loss modulus E" of 0.37 MPa or less in a frequency region of 10 Hz, as measured by a tensile dynamic viscoelasticity measurement using a non-resonant forced vibration method under the conditions of a static tension of 5 gf, a temperature of 25° C., a strain of 0.75% and an amplitude of 0.15 mm.

[0019] Various embodiments of the present invention are described below. The embodiments described below can be combined with each other.

[0020] Preferably, the chloroprene-based polymer contains monomer units derived from 2,3-dichloro-1,3-butadiene.

[0021] Preferably, when the dip-molded product is dissolved in tetrahydrofuran and the soluble component is measured by gel permeation chromatography, at least a peak having a weight average molecular weight of 3,000 to 80,000 is detected.

[0022] Preferably, the dip-molded product contains at least a metal oxide.

[0023] Preferably, the aforementioned dip-molded article is industrial / general household gloves, medical gloves, balloons, catheters or boots.

[0024] According to another aspect of the present invention, a chloroprene-based polymer is provided, wherein:

[0025] The storage modulus E' of the chloroprene polymer dip-molded article in the frequency region of 10 Hz is 3.2 MPa or less, and the loss modulus E" is 0.37 MPa or less, when the tensile dynamic viscoelasticity is measured by a non-resonant forced vibration method under the conditions of a static tension of 5 gf, a temperature of 25°C, a strain of 0.75%, and an amplitude of 0.15 mm.

[0026] The dip-molded product is obtained by molding a chloroprene polymer latex composition containing the chloroprene polymer by a dip coagulation method and then performing a heat drying treatment at 150° C. for 60 minutes.

[0027] According to another aspect of the present invention, there is provided a method for manufacturing a dip-molded article, which is a method for manufacturing a dip-molded article containing a chloroprene-based polymer, comprising: a molding step, wherein a chloroprene-based polymer latex composition containing a chloroprene-based polymer is molded by an immersion coagulation method and using a calcium-based coagulation liquid to obtain a dip-molded article; and a drying step, wherein the obtained dip-molded article is subjected to a heat drying treatment to obtain a dip-molded article.

[0028] Furthermore, in the present invention, "JIS" means Japanese Industrial Standards.

[0029] Effects of the Invention

[0030] According to the present invention, there is provided a dip-molded product containing a chloroprene-based polymer, which has sufficient tensile strength at break and has excellent hand feel of the dip-molded product (film) and excellent wearing feeling when made into gloves. DETAILED DESCRIPTION

[0031] Hereinafter, the mode for implementing the present invention will be described in detail. In addition, the present invention is not limited to the embodiment described below.

[0032] 1. Chloroprene polymers

[0033] First, a chloroprene-based polymer according to one embodiment of the present invention will be described.

[0034] The chloroprene polymer described in this embodiment is a polymer containing monomer units from 2-chloro-1,3-butadiene (hereinafter, also referred to as chloroprene). In addition, the chloroprene polymer of one embodiment of the present invention may also be a copolymer of chloroprene and other monomers copolymerizable with chloroprene, and as other monomers, 1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, isoprene, styrene, methacrylic acid, acrylonitrile, sulfur, etc. can be listed, and other monomers may also be used in combination with two or more of them. The chloroprene polymer of one embodiment of the present invention preferably contains monomer units from 2,3-dichloro-1,3-butadiene. The chloroprene polymer of one embodiment of the present invention may not contain sulfur, and the chloroprene polymer of one embodiment of the present invention may also be a polymer that does not have a -SS- structure derived from sulfur in the main chain.

[0035] The chloroprene polymer of one embodiment of the present invention can be obtained by mixing two or more different chloroprene polymers. The chloroprene polymer preferably includes at least one selected from the group consisting of a homopolymer of chloroprene (2-chloro-1,3-butadiene), a copolymer of chloroprene and 1-chloro-1,3-butadiene, a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene, and a copolymer of chloroprene and 1-chloro-1,3-butadiene and 2,3-dichloro-1,3-butadiene, and more preferably includes at least one of a homopolymer of chloroprene and a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene.

[0036] The chloroprene polymer of one embodiment of the present invention may contain 50 to 100% by mass of monomer units derived from chloroprene, preferably 70 to 100% by mass, based on 100% by mass of the chloroprene polymer contained in the chloroprene polymer latex composition. The content of the monomer units derived from chloroprene may be, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100% by mass, and may be within a range between any two of the values ​​exemplified herein.

[0037] The chloroprene polymer of one embodiment of the present invention may contain 0 to 30% by mass of a monomer unit derived from 2,3-dichloro-1,3-butadiene, based on 100% by mass of the chloroprene polymer contained in the chloroprene polymer latex composition. The content of the monomer unit derived from 2,3-dichloro-1,3-butadiene may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30% by mass, and may be within a range between any two of the values ​​exemplified herein.

[0038] The chloroprene polymer of one embodiment of the present invention may contain monomer units derived from chloroprene and monomer units derived from 2,3-dichloro-1,3-butadiene. In this case, when the total of monomer units derived from chloroprene and monomer units derived from 2,3-dichloro-1,3-butadiene contained in the chloroprene polymer is 100% by mass, the chloroprene polymer preferably contains 0 to 30% by mass of monomer units derived from 2,3-dichloro-1,3-butadiene, and more preferably contains 5 to 25% by mass.

[0039] When the chloroprene polymer is a mixture of two or more different chloroprene polymers, the content of each monomer unit refers to the total of each monomer unit in all chloroprene polymers contained in the chloroprene polymer latex composition.

[0040] Regarding the chloroprene polymer of one embodiment of the present invention, when the chloroprene polymer contained in the chloroprene polymer latex composition is set to 100% by mass, the content of the sulfur-modified chloroprene polymer contained in the chloroprene polymer latex composition is preferably 20% by mass or less. The content of the sulfur-modified chloroprene polymer is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20% by mass, and may be within the range between any two of the values ​​exemplified here. The chloroprene polymer of one embodiment of the present invention may not contain the sulfur-modified chloroprene polymer.

[0041] The chloroprene polymer of one embodiment of the present invention preferably has a peak with a weight average molecular weight of 3,000 to 80,000 detected in the molecular weight distribution obtained when a sol component soluble in tetrahydrofuran in the chloroprene polymer is measured by gel permeation chromatography. The peak position of the peak detected in the weight average molecular weight range of 3,000 to 80,000 is, for example, 3,000, 4,000, 5,000, 6,000, 7,000, 8,000, 9,000, 10,000, 11,000, 12,000, 13,000, 14,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, 21,000, 22,000, 23,000, 24,000, 25,000, 26,000, 27,000, 28,000, 29,000, 30,000, 31,000, 32,000, 33,000, 34,000, 35,000, 36,000, 37,000, 38,000, 39,000, 40,000, 41,000, 42,000, 43,000, 44,000 The amount may be within a range between any two of the values ​​exemplified herein.

[0042] The chloroprene polymer according to one embodiment of the present invention may be a mixture of two or more different chloroprene polymers, and preferably contains a chloroprene polymer having a weight average molecular weight of 3,000 to 80,000.

[0043] The chloroprene polymer of one embodiment of the present invention may further include a chloroprene polymer having a weight average molecular weight of 500,000 to 1,500,000. That is, the chloroprene polymer of one embodiment of the present invention may have a peak having a weight average molecular weight of 500,000 to 1,500,000 detected in the molecular weight distribution obtained when the sol component soluble in tetrahydrofuran in the chloroprene polymer is measured by gel permeation chromatography. The peak position of the peak detected within the weight average molecular weight range of 500,000 to 1,500,000 is, for example, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,200,000, 1,300,000, 1,500,000, or may be within the range between any two of the values ​​exemplified herein.

[0044] The molecular weight distribution of the sol component soluble in tetrahydrofuran in the chloroprene polymer can be obtained by measuring the weight average molecular weight using gel permeation chromatography (GPC). The measuring conditions of GPC can be described in the examples. The weight average molecular weight of the chloroprene polymer can be controlled by adjusting the formula such as the type and amount of the chain transfer agent in the polymerization of each chloroprene polymer, the polymerization temperature, the polymerization time, the polymerization conversion rate, etc. In addition, as described later, by adjusting the weight average molecular weight of the chloroprene polymer and the mixing ratio of the chloroprene polymers with different weight average molecular weights, the storage modulus E', the loss modulus E'' and the tensile strength at break can be adjusted.

[0045] The chloroprene polymer according to one embodiment of the present invention preferably has a peak with a weight average molecular weight of 3,000 to 80,000 and a peak with a weight average molecular weight of 500,000 to 1,000,000 detected in the molecular weight distribution obtained when the sol component soluble in tetrahydrofuran in the chloroprene polymer is measured by gel permeation chromatography. That is, the chloroprene polymer according to one embodiment of the present invention preferably contains a chloroprene polymer with a weight average molecular weight of 3,000 to 80,000 and a chloroprene polymer with a weight average molecular weight of 500,000 to 1,500,000.

[0046] The chloroprene polymer of one embodiment of the present invention preferably contains 5 to 40% by mass of a chloroprene polymer having a weight average molecular weight of 3,000 to 80,000, based on 100% by mass of the chloroprene polymer. The chloroprene polymer of one embodiment of the present invention may contain, for example, 5, 10, 15, 20, 25, 30, 35, or 40% by mass of a chloroprene polymer having a weight average molecular weight of 5,000 to 50,000, based on 100% by mass of the chloroprene polymer, or may be within the range between any two of the values ​​exemplified herein.

[0047] The chloroprene polymer of one embodiment of the present invention preferably contains 60 to 95% by mass of a chloroprene polymer having a weight average molecular weight of 500,000 to 1,500,000, based on 100% by mass of the chloroprene polymer. The chloroprene polymer of one embodiment of the present invention may contain, for example, 60, 65, 70, 75, 80, 85, 90, or 95% by mass of a chloroprene polymer having a weight average molecular weight of 500,000 to 1,500,000, based on 100% by mass of the chloroprene polymer, or may be within a range between any two of the values ​​exemplified herein.

[0048] By adjusting the content of the chloroprene polymers having different weight average molecular weights within the above numerical range, the storage modulus and the loss modulus can be more appropriately adjusted.

[0049] The chloroprene polymer according to one embodiment of the present invention has a storage modulus E' of 3.2 MPa or less and a loss modulus E" of 0.37 MPa or less in the frequency range of 10 Hz, obtained when a dip-molded article containing the chloroprene polymer is measured for tensile dynamic viscoelasticity by a non-resonant forced vibration method under the conditions of a static tension of 5 gf, a temperature of 25° C., a strain of 0.75% and an amplitude of 0.15 mm.

[0050] Here, the dip-molded article is a dip-molded article obtained by molding a chloroprene polymer latex composition containing the chloroprene polymer by a dip coagulation method, and then heat-drying the mixture at 150° C. for 60 minutes. That is, the dip-molded article containing the chloroprene polymer may be a dip-molded article obtained by dip-molding a chloroprene polymer latex composition containing a chloroprene polymer by a dip coagulation method, and then heat-drying the obtained dip-molded article at 150° C. for 60 minutes. In addition, the dip-molded article may contain a chloroprene polymer as a base polymer, and may contain 70% by mass or more of the chloroprene polymer, preferably 80% by mass or more, and more preferably 90% by mass or more of the chloroprene polymer, when the dip-molded article is taken as 100% by mass. When the dip molded product is taken as 100 mass %, the content of the chloroprene polymer in the dip molded product is, for example, 70, 75, 80, 85, 90, 95, 96, 97, 98, 99, or 100 mass %, and may be within the range between any two of the values ​​exemplified here.

[0051] The storage modulus E' of the dip molded product containing the chloroprene polymer is 3.2 MPa or less, and more preferably 3.0 or less. The storage modulus E' is, for example, 3.2, 3.1, 3.0, 2.9, 2.8, 2.7, 2.6, 2.5, 2.4, 2.3, 2.2, 2.1, 2.0, 1.9, 1.8, 1.7, 1.6, 1.5 MPa, and may be within the range of any of the values ​​exemplified herein.

[0052] The loss modulus E" of the dip-molded product containing the chloroprene polymer is 0.37 MPa or less, and more preferably 0.35 or less. The loss modulus E" is, for example, 0.37, 0.35, 0.33, 0.32, 0.31, 0.30, 0.29, 0.28, 0.27, 0.26, 0.25, 0.24, 0.23, 0.22, 0.21, 0.20, 0.19, or 0.18 MPa, and may be within the range between any two of the values ​​exemplified here.

[0053] The storage modulus E' and loss modulus E" of the impregnated article containing the chloroprene polymer can be controlled by adjusting the type (weight average molecular weight and the type and content of the monomer units contained, etc.) and amount of the chloroprene polymer contained in the impregnated article. In addition, the method for measuring the storage modulus E' and loss modulus E" of the impregnated article is described later, and can be measured using the method described in the Examples, etc.

[0054] Regarding the chloroprene polymer of one embodiment of the present invention, the tensile strength at break of the dip-molded article containing the chloroprene polymer measured in accordance with JIS K6251 is, for example, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, or 40 MPa, and may be within the range between any two of the values ​​exemplified herein.

[0055] The tensile strength at break of the dip molded article containing the chloroprene polymer can be controlled by adjusting the type (weight average molecular weight and type and content of monomer units contained, etc.) and amount of the chloroprene polymer contained in the dip molded article. In addition, the method for measuring the tensile strength at break can be as described in the Examples.

[0056] 2. Chloroprene polymer latex

[0057] The chloroprene polymer latex of one embodiment of the present invention contains the chloroprene polymer of the present invention. In addition, the dip molded article of one embodiment of the present invention can be obtained using a chloroprene polymer latex composition containing the chloroprene polymer latex. The chloroprene polymer latex may be a latex obtained by dispersing a chloroprene polymer in water, or a latex obtained by dispersing at least one selected from the group consisting of a homopolymer of chloroprene, a copolymer of chloroprene and 1-chloro-1,3-butadiene, a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene, and a copolymer of chloroprene and 1-chloro-1,3-butadiene and 2,3-dichloro-1,3-butadiene in water, or a latex obtained by dispersing a homopolymer of chloroprene or a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene in water.

[0058] 3. Method for producing chloroprene polymer latex

[0059] Next, a method for producing the chloroprene polymer latex contained in the chloroprene polymer latex composition for obtaining the chloroprene polymer dip-molded product of the present invention will be described.

[0060] The method for producing chloroprene polymer latex may include a polymerization step of polymerizing a monomer containing chloroprene to obtain the chloroprene polymer latex. In addition, the method for producing chloroprene polymer latex may also include a mixing step of mixing two or more chloroprene polymer latexes having different weight average molecular weights.

[0061] In the polymerization step, the monomer includes chloroprene and may include other monomers copolymerizable with chloroprene. Examples of other monomers copolymerizable with chloroprene include 1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, isoprene, styrene, methacrylic acid, acrylonitrile, sulfur, and the like. The monomer may also include chloroprene and 2,3-dichloro-1,3-butadiene.

[0062] It is preferred to adjust the type and amount of each monomer so that the content of each monomer unit in the obtained chloroprene polymer falls within the above numerical range. As an example, the copolymerization amount of 2,3-dichloro-1,3-butadiene in the chloroprene polymer contained in the chloroprene polymer latex may be in the range of 0 to 30% by mass relative to 100% by mass of the total of the chloroprene monomer and 2,3-dichloro-1,3-butadiene contained in the chloroprene polymer. In this case, the amount of 2,3-dichloro-1,3-butadiene added before the start of emulsion polymerization is preferably in the range of 0 to 30 parts by mass relative to 100 parts by mass of the total of the chloroprene monomer and the 2,3-dichloro-1,3-butadiene monomer. From the viewpoint of controlling polymerization, the amount of 2,3-dichloro-1,3-butadiene added is more preferably 5 to 25 parts by mass relative to 100 parts by mass of the total of the chloroprene monomer and the 2,3-dichloro-1,3-butadiene monomer.

[0063] When producing chloroprene-based polymers, the raw monomers are polymerized by polymerization methods such as emulsion polymerization, solution polymerization, suspension polymerization, and bulk polymerization. Among these polymerization methods, emulsion polymerization is preferred because it has various advantages such as easy control, easy extraction of the polymer from the polymerization-completed solution, and high polymerization speed.

[0064] Emulsion polymerization is a type of free radical polymerization, in which raw monomers are put into a reaction tank together with a chain transfer agent, water, an alkali (for example, metal hydroxides such as potassium hydroxide and sodium hydroxide), an emulsifier (dispersant), a reducing agent (for example, sodium bisulfite), a polymerization initiator, etc. for polymerization.

[0065] The type of chain transfer agent used in emulsion polymerization is not particularly limited, and for example, long-chain alkyl mercaptans such as n-dodecyl mercaptan and tert-dodecyl mercaptan, dialkyl xanthogen disulfides such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide, and known chain transfer agents commonly used in emulsion polymerization of chloroprene such as iodoform can be used. The chain transfer agent is preferably a long-chain alkyl mercaptan, and more preferably n-dodecyl mercaptan.

[0066] By adjusting the type and amount of the chain transfer agent, the weight average molecular weight of the obtained chloroprene polymer latex can be adjusted.

[0067] For example, in order to obtain a latex containing a chloroprene polymer having a weight average molecular weight of 500,000 or more, that is, in order to obtain a chloroprene polymer latex in which a peak having a weight average molecular weight of 500,000 or more is detected in the molecular weight distribution, the amount of the chain transfer agent added before the start of emulsion polymerization is preferably 0.01 parts by mass or more relative to 100 parts by mass of the monomer (for example, 100 parts by mass of the total of chloroprene and 2,3-dichloro-1,3-butadiene). From the viewpoint of obtaining a chloroprene polymer latex in which a peak having a weight average molecular weight of 500,000 or more is detected, the amount of the chain transfer agent added is more preferably 0.02 to 0.05 parts by mass, for example, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09 parts by mass, or less than 0.10 parts by mass, and may also be within the range between any two of the numerical values ​​exemplified here. When the amount of the chain transfer agent, especially the long-chain alkyl mercaptan, added is 0.01 parts by mass or more, the storage stability of the latex is further improved, and when the amount added is less than 0.10 parts by mass, especially less than 0.05 parts by mass, the toluene insoluble matter increases, and the breaking strength of the dip-molded product containing the obtained chloroprene polymer latex increases.

[0068] In order to obtain a chloroprene polymer latex having a weight average molecular weight of 3,000 to 80,000, that is, to obtain a chloroprene polymer latex having a peak of a weight average molecular weight of 3,000 to 80,000 detected in the molecular weight distribution, the amount of the chain transfer agent added before the start of the emulsion polymerization is preferably 0.5 to 10.0 parts by mass relative to 100 parts by mass of the monomer. In this case, the amount added is, for example, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, and may be within the range between any two of the values ​​exemplified here.

[0069] Emulsifiers include anionic emulsifiers, nonionic emulsifiers, and the like. Examples of anionic emulsifiers include fatty acid salts such as potassium tallow fatty acid, partially hydrogenated potassium tallow fatty acid, potassium oleate, and sodium oleate; resin acid salts such as potassium rosinate, sodium rosinate, hydrogenated potassium rosinate, and hydrogenated sodium rosinate; alkylbenzene sulfonates such as sodium dodecylbenzene sulfonate; sodium salt of β-naphthalenesulfonic acid formalin condensate, and the like. Examples of nonionic emulsifiers include polyethylene glycol ester emulsifiers and polyvinyl alcohol. Among them, anionic emulsifiers are preferred, resin acid salts are preferred, rosin acids such as rosin acid and rosin acid salts are preferred, and at least one selected from the group consisting of potassium rosinate and sodium rosinate is more preferred. These emulsifiers may be used alone or in combination of two or more. The amount of the emulsifier used is preferably 1.0 to 6.5 parts by mass relative to 100 parts by mass of the monomer.

[0070] The emulsifier used in the emulsion polymerization preferably contains an anionic emulsifier, more preferably contains a resinate, particularly rosin acids, which can prevent the aggregation of the rubber solid component and pH fluctuation when blended with the base chloroprene polymer latex. Rosin acids include disproportionated rosin acid, conjugated resin acid, alkali metal salts of disproportionated rosin acid, alkali metal salts of conjugated resin acid, and the like.

[0071] In addition, in the method for producing the chloroprene polymer latex according to one embodiment of the present invention, in addition to the rosin acids, other commonly used emulsifiers and fatty acids may also be used in combination. As other emulsifiers, for example, an anionic emulsifier is preferably contained, and in addition to the above-mentioned anionic emulsifiers, metal salts of aromatic sulfinic acid formalin condensates, sodium dodecylbenzene sulfonate, potassium dodecylbenzene sulfonate, sodium alkyl diphenyl ether sulfonate, potassium alkyl diphenyl ether sulfonate, sodium polyoxyethylene alkyl ether sulfonate, sodium polyoxypropylene alkyl ether sulfonate, potassium polyoxyethylene alkyl ether sulfonate, potassium polyoxypropylene alkyl ether ether sulfonate, etc. may be cited.

[0072] The content of the anionic emulsifier other than rosin acid is preferably 0.2 to 1.0 mass % relative to 100 mass % of the chloroprene polymer contained in the chloroprene polymer latex. Therefore, the amount of the anionic emulsifier other than rosin acid added before the start of emulsion polymerization is preferably in the range of 0.2 to 0.9 mass parts relative to 100 mass parts of the monomers (for example, the total of chloroprene and 2,3-dichloro-1,3-butadiene).

[0073] The pH of the aqueous emulsion at the start of emulsion polymerization is preferably 10.5 to 13.5. The aqueous emulsion refers to a mixed solution of a chain transfer agent and monomers (chloroprene, 2,3-dichloro-1,3-butadiene, etc.) immediately before the start of emulsion polymerization, and also includes the case where the composition is changed by adding each component later or adding it in batches. If the pH of the aqueous emulsion at the start of emulsion polymerization is 10.5 or more, the polymerization reaction can be controlled more stably. If the pH is below 13.5, the excessive increase in viscosity during polymerization can be suppressed, and the polymerization reaction can be controlled more stably.

[0074] The polymerization temperature of the emulsion polymerization is preferably in the range of 5 to 55° C. It is more preferred that the temperature is 5° C. or higher because the emulsion does not freeze, and that the temperature is 55° C. or lower because the chloroprene monomer does not evaporate or boil.

[0075] As the polymerization initiator, potassium persulfate, benzoyl peroxide, ammonium persulfate, hydrogen peroxide, etc., which are generally used for radical polymerization, can be used.

[0076] The polymerization conversion rate is preferably in the range of 50 to 95%. The polymerization reaction is terminated by adding a polymerization terminator. When the polymerization conversion rate is 50% or more, the toluene insoluble matter tends to increase, and the strength of the obtained dip-molded film tends to increase. In addition, it is also advantageous in terms of production cost. When the polymerization conversion rate is lower than 95%, the decrease in polymerization reactivity due to the decrease in unreacted monomers can be avoided, and the decrease in productivity can be avoided.

[0077] Examples of the polymerization terminator include diethylhydroxylamine, thiodiphenylamine, 4-tert-butylcatechol, 2,2'-methylenebis-4-methyl-6-tert-butylphenol, etc. After the emulsion polymerization, unreacted monomers can be removed by a conventional method such as reduced pressure distillation.

[0078] Furthermore, to the chloroprene polymer latex obtained by the production method of one embodiment of the present invention, a freeze stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, a preservative, etc. may be optionally added after polymerization within a range that does not impair the effects of the present invention.

[0079] The method for producing a chloroprene polymer latex according to an embodiment of the present invention may further include a mixing step of mixing two or more chloroprene polymer latexes having different weight average molecular weights after the polymerization step. In the mixing step, the two or more chloroprene polymer latexes may be mixed by a known method. In the mixing step, for example, the chloroprene polymer latex may be obtained by stirring and mixing at 30 to 300 rpm using a paddle for 20 seconds to 3 minutes, for example, at 100 rpm for 2 minutes.

[0080] 4. Chloroprene polymer latex composition

[0081] The chloroprene polymer latex composition of one embodiment of the present invention includes a chloroprene polymer latex containing the chloroprene polymer of the present invention. The chloroprene polymer latex composition of one embodiment of the present invention may contain a metal oxide, an antioxidant, and other necessary agents in addition to the chloroprene polymer latex. The types and amounts of the metal oxide, antioxidant, and other necessary agents that the chloroprene polymer latex composition may contain will be described later as components that may be contained in the dip molded article.

[0082] 5. Method for producing chloroprene polymer latex composition

[0083] The method for producing the chloroprene polymer latex composition may include a raw material mixing step of mixing raw materials containing the chloroprene polymer latex, a metal oxide, an antioxidant, and other necessary reagents.

[0084] In the mixing step, an aqueous dispersion containing a metal oxide, an antioxidant, and other necessary reagents may be prepared in advance, and then the chloroprene polymer latex and the aqueous dispersion may be mixed.

[0085] The mixing step can be performed using a known mixing device such as a ball mill.

[0086] 6. Dip-molded products (dip-molded films and films)

[0087] The dip-molded article of one embodiment of the present invention is obtained using a chloroprene polymer latex composition containing the above-mentioned chloroprene polymer latex. The dip-molded article of this embodiment can be obtained by dip-molding the above-mentioned chloroprene polymer latex composition alone or after blending with other chloroprene polymer latex compositions. The dip-molded article of the present invention can be a dip-molded article obtained by heat drying at 150°C for 60 minutes on a dip-molded article obtained by dip-molding a chloroprene polymer latex composition containing a chloroprene polymer latex containing a chloroprene polymer by a dip coagulation method. The dip-molded article of the present invention has low values ​​of storage modulus and loss modulus, and excellent mechanical properties such as tensile strength at break. The dip-molded article can be suitably used as industrial / general household gloves, medical gloves, balloons, catheters, and boots.

[0088] The dip molded article of the present invention may have the components contained in the above-mentioned chloroprene polymer latex. In addition, the dip molded article may contain a chloroprene polymer as a base polymer, and when the dip molded article is set to 100 mass%, it may contain 70 mass% or more of the chloroprene polymer, preferably 80 mass% or more, and more preferably 90 mass% or more. When the dip molded article is set to 100 mass%, the content of the chloroprene polymer in the dip molded article is, for example, 70, 75, 80, 85, 90, 95, 96, 97, 98, 99, 100 mass%, and may also be within the range between any two of the values ​​exemplified here.

[0089] The dip-molded article containing the chloroprene polymer of the present invention has an excellent hand feel regardless of whether a vulcanizing agent and a vulcanization accelerator are added, and has an excellent wearing feel when made into gloves. In addition, the chloroprene polymer latex composition of one embodiment of the present invention may not contain a vulcanizing agent and a vulcanization accelerator, and may not contain sulfur and a vulcanization accelerator such as a thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthate-based, thiazole-based, etc. The components that may be contained in the dip-molded article of the present invention are described in detail below.

[0090] 6.1 Metal oxides

[0091] The dip-molded product of the chloroprene polymer of the present invention may contain a metal oxide.

[0092] The metal oxide contained in the chloroprene polymer latex composition for obtaining the dip-molded product is not particularly limited, and examples thereof include zinc oxide, lead oxide, lead tetraoxide, magnesium oxide, aluminum oxide, iron oxide, beryllium oxide, titanium oxide, etc. The metal oxide preferably contains zinc oxide. Zinc oxide is generally considered to function as a supplement for the dechlorination atoms of the chloroprene polymer. In addition, these metal oxides may be used alone or in combination of two or more.

[0093] The amount of the metal oxide added is preferably 0.5 to 15.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer latex contained in the chloroprene polymer latex composition used to obtain the dip-molded product. If the amount of the metal oxide added is 0.5 parts by mass or more, an improvement in the breaking strength can be expected due to the cross-linking effect between the polymers. If the amount of the metal oxide added is 15.0 parts by mass or less, a dip-molded product with excellent softness can be obtained. In addition, from the viewpoint of the physical property balance between the softness and the breaking strength of the obtained dip-molded product, the amount of the metal oxide added is more preferably 0.5 to 5.0 parts by mass.

[0094] 6.2 Antioxidants

[0095] The dip-molded product of the chloroprene polymer of the present invention may contain an antioxidant.

[0096] The antioxidant is not particularly limited, and phenolic antioxidants, amine antioxidants, heat-resistant antioxidants (aging) agents, ozone-resistant antioxidants, etc. can be used. When the obtained dip-molded product is used for medical gloves, phenolic antioxidants can be used from the perspective of color tone, texture, and hygiene of the dip-molded product. In particular, the above-mentioned effect of hindered phenolic antioxidants is stronger. Examples of hindered phenolic antioxidants include 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 4,4'-butylene(3-methyl-6-tert-butylphenol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), a butylation product of p-cresol and dicyclopentadiene, 2,5'-di-tert-butylhydroquinone, and 2,5'-di-tert-amylhydroquinone. Among them, generally, from the viewpoint of being dispersible in water-based materials, a butylation reaction product of p-cresol and dicyclopentadiene is preferred. In addition, these compounds may be used alone or in combination of two or more.

[0097] The amount of the antioxidant added is preferably 0.5 to 10.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer latex contained in the chloroprene polymer latex composition used to obtain the dip molded product. The amount of the antioxidant added is, for example, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0 parts by mass, and may also be within the range between any two of the numerical values ​​exemplified herein. If the amount of the antioxidant added is 0.5 parts by mass or more, the effect of suppressing the change in color tone of the dip molded product can be obtained. If the amount of the antioxidant added is 10.0 parts by mass or less, the stability of the chloroprene polymer latex composition can be ensured. In addition, from the viewpoint of the physical property balance between the softness and the breaking strength of the obtained dip molded product, the amount of the antioxidant added is more preferably 0.5 to 5.0 parts by mass.

[0098] 6.3 Vulcanizing agents and vulcanization accelerators

[0099] The dip-molded article of the chloroprene polymer of one embodiment of the present invention may also contain a vulcanizing agent and / or a vulcanization accelerator. In addition, the chloroprene polymer latex composition used to obtain the dip-molded article may also be free of sulfur and the above-mentioned thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthate-based, thiazole-based and other vulcanization accelerators. That is, the chloroprene polymer latex composition includes those containing a vulcanizing agent but not containing a vulcanization accelerator, those containing no vulcanizing agent but containing a vulcanization accelerator, those containing a vulcanizing agent and a vulcanization accelerator, and those containing no vulcanizing agent and a vulcanization accelerator. Whether to deploy a vulcanizing agent and a vulcanization accelerator can be determined according to the expected dip-molded article.

[0100] Examples of the vulcanizing agent include sulfur, but are not limited thereto. The amount of the vulcanizing agent added may be 0 to 10.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer latex contained in the chloroprene polymer latex composition. The amount of the vulcanizing agent added may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass, or may be within the range between any two of the values ​​exemplified herein.

[0101] Vulcanization accelerator refers to a reagent added during the vulcanization of raw rubber to increase the vulcanization rate by reacting with the vulcanizing agent, shorten the vulcanization time, lower the vulcanization temperature, reduce the vulcanizing agent, and improve the physical properties of the vulcanized rubber. It usually refers to a reagent that promotes sulfur vulcanization reaction.

[0102] Examples of vulcanization accelerators commonly used in the vulcanization of chloroprene polymer latex include, but are not limited to, thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthate-based, and thiazole-based accelerators, and these may be used alone or in combination of two or more as needed.

[0103] Examples of the thiuram-based vulcanization accelerator include tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide, and bis(pentamethylene)thiuram tetrasulfide.

[0104] Examples of the dithiocarbamate-based vulcanization accelerator include sodium dibutyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, copper dimethyldithiocarbamate, iron (III) dimethyldithiocarbamate, tellurium diethyldithiocarbamate, and the like. Zinc dibutyldithiocarbamate is particularly preferably used.

[0105] Examples of the thiourea-based vulcanization accelerator include ethylenethiourea, N,N′-diethylthiourea, trimethylthiourea, and N,N′-diphenylthiourea.

[0106] Examples of the guanidine-based vulcanization accelerator include 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, and di-o-tolylguanidine salt of dicatechol borate.

[0107] Examples of the xanthate-based vulcanization accelerator include butyl zinc xanthate and isopropyl zinc xanthate.

[0108] Examples of the thiazole vulcanization accelerator include 2-mercaptobenzothiazole, di-2-benzothiazole disulfide, 2-mercaptobenzothiazole zinc salt, cyclohexylamine salt of 2-mercaptobenzothiazole, and 2-(4′-morpholinodithio)benzothiazole.

[0109] The amount of the vulcanization accelerator added may be 0 to 5.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer latex contained in the chloroprene polymer latex composition. The amount of the vulcanization accelerator added may be, for example, 0, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, or may be within the range between any two of the values ​​exemplified herein.

[0110] 6.4 Other reagents (aromatic heterocyclic compounds)

[0111] The dip-molded product of the chloroprene polymer of the present invention may contain an aromatic heterocyclic compound in the chloroprene polymer.

[0112] The aromatic heterocyclic compound contained in the chloroprene polymer latex composition for obtaining the dip-molded product can be represented by the chemical formula (1) and has a benzimidazole structure. In addition, the compound having this structure is sometimes mainly used as a secondary antioxidant in the preparation of the rubber composition.

[0113] [Chemistry 1]

[0114]

[0115] In the chemical formula (1), X of the mercapto group represents a hydrogen atom or a metal atom. X may be a group having a thiol group and a hydrogen atom. In addition, X may be a metal atom, and examples of the metal atom include zinc, sodium, copper, nickel, and tellurium, and zinc is preferred.

[0116] R in the chemical formula (1) 1 ~R 4 Each of R represents a hydrogen atom, an alkyl group which may have a substituent, an ether group which may have a substituent, a nitro group, an amino group, or a carboxyl group. 1 ~R 4 The aromatic heterocyclic compounds may be used alone or in combination of two or more.

[0117] As aromatic heterocyclic compounds, for example, 2-mercaptobenzimidazole, 5-methyl-2-mercaptobenzimidazole, 4-methyl-2-mercaptobenzimidazole, 5-methoxy-2-mercaptobenzimidazole, 4-methoxy-2-mercaptobenzimidazole, 5-nitro-2-mercaptobenzimidazole, 5-amino-2-mercaptobenzimidazole, 5-carboxyl-2-mercaptobenzimidazole, or zinc salts of 2-mercaptobenzimidazole can be cited. Among them, 2-mercaptobenzimidazole, 5-methyl-2-mercaptobenzimidazole, 4-methyl-2-mercaptobenzimidazole, 5-methoxy-2-mercaptobenzimidazole, 4-methoxy-2-mercaptobenzimidazole, and zinc salts of 2-mercaptobenzimidazole are preferred.

[0118] The amount of the aromatic heterocyclic compound added is preferably 0.2 to 10.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer latex contained in the chloroprene polymer latex composition. The amount of the aromatic heterocyclic compound added is, for example, 0.2, 0.3, 0.4, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0 parts by mass, and may also be within the range between any two of the values ​​exemplified herein. If the amount added is 0.2 parts by mass or more, the dip-molded article obtained using the composition can exhibit very high breaking strength. If the amount added is 10.0 parts by mass or less, the stability of the chloroprene polymer latex composition can be ensured. In addition, from the viewpoint of the physical property balance between the softness and breaking strength of the obtained dip-molded article, the amount added is more preferably 0.3 to 5.0 parts by mass.

[0119] 6.5 Characteristics of Dip-molded Products

[0120] The dip-molded article of one embodiment of the present invention is made into a strip test piece (width: 4.5 mm, length: 30 mm), and the storage modulus E' in the frequency region of 10 Hz is 3.2 MPa or less, and more preferably 3.0 MPa or less when the tensile dynamic viscoelasticity is measured (inter-chuck distance: 20 mm) by a non-resonant forced vibration method under the conditions of static tension 5 gf, temperature 25°C, and strain 0.75% (amplitude: 0.15 mm). The storage modulus is, for example, 3.2, 3.1, 3.0, 2.9, 2.8, 2.7, 2.6, 2.5, 2.4, 2.3, 2.2, 2.1, 2.0, 1.9, 1.8, 1.7, 1.6, 1.5 MPa, and may also be within the range between any of the numerical values ​​exemplified herein.

[0121] The dip-molded product of the present invention is made into a strip test piece (width: 4.5 mm, length: 30 mm). When the tensile dynamic viscoelasticity is measured by the non-resonant forced vibration method (between chucks: 20 mm) under the conditions of static tension 5 gf, temperature 25°C, and strain 0.75% (amplitude: 0.15 mm), the loss modulus E" in the frequency region of 10 Hz is 0.37 MPa or less, and more preferably 0.35 MPa or less. The loss modulus E" is, for example, 0.37, 0.35, 0.33, 0.32, 0.31, 0.30, 0.29, 0.28, 0.27, 0.26, 0.25, 0.24, 0.23, 0.22, 0.21, 0.20, 0.19, and 0.18 MPa, and can also be within the range between any two of the values ​​exemplified here.

[0122] The two physical properties of the storage modulus E' and the loss modulus E" affect the feel and wearing feeling in the glove application which is the main application of the dip-molded product. By making the storage modulus E' below the above upper limit and the loss modulus E" below the above upper limit, a dip-molded product having excellent feel and excellent wearing feeling when molded into a glove shape can be obtained.

[0123] The breaking strength of the dip-molded product of the present invention measured in accordance with JIS K6251 is preferably 17 MPa or more. In particular, the ASTM standard "D3577" for surgical gloves stipulates that the breaking strength is 17 MPa or more, and if it is 20 MPa, it can be said that more sufficient mechanical properties are exhibited. As described above, the dip-molded product of the chloroprene polymer according to one embodiment of the present invention has sufficient tensile strength at break, and the feel of the dip-molded product (film) and the wearing feeling when made into gloves are excellent.

[0124] The dip-molded article contains a chloroprene polymer and may also contain an antioxidant and a metal oxide. In addition, the dip-molded article may also contain a vulcanizing agent, a vulcanization accelerator and other reagents. The manufacturing method of the dip-molded article, and the determination method of the storage modulus E', the loss modulus E", and the breaking strength may be described in the examples.

[0125] In addition, as described above, the storage modulus E', loss modulus E", and breaking strength of the dip-molded article containing the chloroprene polymer latex composition can be controlled by adjusting the type and amount of the chloroprene polymer latex composition, the polymerization formula / conditions of the chloroprene polymer latex used, the heat drying treatment conditions in the preparation of the dip-molded article, and adjusting the weight average molecular weight and the degree of crosslinking.

[0126] 6.6 Weight average molecular weight of impregnated product

[0127] The dip molded product according to one embodiment of the present invention may have a peak with a weight average molecular weight of 3,000 to 80,000 in the molecular weight distribution of a sol component soluble in tetrahydrofuran in the dip molded product measured by gel permeation chromatography, and the weight average molecular weight of the peak is preferably 5,000 to 50,000.

[0128] In the molecular weight distribution, when the peak weight average molecular weight is greater than the lower limit, more excellent breaking strength can be obtained. From the viewpoint of obtaining a better impregnation molded body, the peak weight average molecular weight may be 10,000 or more, or 15,000 or more.

[0129] In the above molecular weight distribution, if the peak weight average molecular weight is below the above upper limit, better flexibility can be obtained. From the viewpoint of easily obtaining better flexibility, the peak weight average molecular weight of the dip molded product of the chloroprene polymer may be 80,000 or less, 70,000 or less, 50,000 or less, or 30,000 or less.

[0130] The weight average molecular weight of the peak is, for example, 3,000, 4,000, 5,000, 6,000, 7,000, 8,000, 9,000, 10,000, 11,000, 12,000, 13,000, 14,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, 21 The amount may be within the range between any two of the values ​​exemplified herein.

[0131] The dip-molded product of the chloroprene-based polymer according to one embodiment of the present invention preferably has a peak within the above range in the above molecular weight distribution.

[0132] According to the dip-molded product of the chloroprene polymer of one embodiment of the present invention, by having the above molecular weight distribution, it is possible to obtain a dip-molded product having low values ​​of storage modulus E' and loss modulus E" in dynamic viscoelasticity measurement and excellent hand feel and wearing feel.

[0133] The dip molded product of one embodiment of the present invention may have a peak with a weight average molecular weight of 500,000 to 1,500,000 in the molecular weight distribution of the tetrahydrofuran-soluble sol component in the dip molded product measured by gel permeation chromatography. The peak position of the peak detected in the weight average molecular weight range of 500,000 to 1,500,000 is, for example, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,200,000, 1,300,000, 1,400,000, 1,500,000, or may be within the range between any two of the values ​​exemplified herein.

[0134] The dip molded product according to one embodiment of the present invention preferably has a peak with a weight average molecular weight of 3,000 to 80,000 and a peak with a weight average molecular weight of 500,000 to 1,500,000 detected in the molecular weight distribution of a sol component soluble in tetrahydrofuran in the dip molded product measured by gel permeation chromatography.

[0135] The dip molded article of one embodiment of the present invention preferably contains 5 to 40% by mass of a chloroprene polymer having a weight average molecular weight of 3,000 to 80,000, based on 100% by mass of the chloroprene polymer contained in the dip molded article. The dip molded article of one embodiment of the present invention may contain, for example, 5, 10, 15, 20, 25, 30, 35, or 40% by mass of a chloroprene polymer having a weight average molecular weight of 5,000 to 50,000, based on 100% by mass of the chloroprene polymer, or may be within the range between any two of the values ​​exemplified herein.

[0136] The dip molded article of one embodiment of the present invention preferably contains 60 to 95% by mass of a chloroprene polymer having a weight average molecular weight of 500,000 to 1,500,000, based on 100% by mass of the chloroprene polymer contained in the dip molded article. The dip molded article of one embodiment of the present invention may contain, for example, 60, 65, 70, 75, 80, 85, 90, or 95% by mass of a chloroprene polymer having a weight average molecular weight of 500,000 to 1,500,000, based on 100% by mass of the chloroprene polymer contained in the dip molded article, or may be within the range between any two of the values ​​exemplified herein.

[0137] The molecular weight distribution of the tetrahydrofuran-soluble sol component in the dip-molded product of the present invention can be obtained by cutting the dip-molded product into, for example, a specific size, immersing the product in tetrahydrofuran at 25° C. for 24 hours to prepare a 0.1% tetrahydrofuran solution, and measuring the weight average molecular weight of the solution by gel permeation chromatography. The measurement conditions of GPC can be as described in the Examples.

[0138] Furthermore, when the object of analysis is a chloroprene polymer latex or a chloroprene polymer latex composition, the molecular weight distribution of the sol component soluble in tetrahydrofuran in the chloroprene polymer latex or the chloroprene polymer latex composition can be determined by dissolving the chloroprene polymer latex or the chloroprene polymer latex composition in tetrahydrofuran and analyzing the chloroprene polymer latex by the same method.

[0139] The chloroprene polymer latex composition used in the production of the dip molded article of the present invention can be obtained by mixing the above two or more chloroprene polymer latexes having different weight average molecular weights. By using two or more chloroprene polymer latexes having different weight average molecular weights, a chloroprene polymer latex in which the above peak is detected in the molecular weight distribution can also be obtained. When two or more chloroprene polymer latexes are mixed, the weight average molecular weight of each chloroprene polymer latex can be controlled by adjusting the formulation such as the type and amount of the chain transfer agent in the polymerization of each chloroprene polymer latex, the polymerization temperature, the polymerization time, the polymerization conversion rate, etc.

[0140] 6.5 Shape of Dip Molded Product

[0141] The thickness of the dip-molded article (e.g., minimum thickness) may be 0.01 to 0.50 mm. The thickness of the dip-molded article may be, for example, 0.01, 0.05, 0.10, 0.20, 0.30, 0.40, or 0.50 mm, or may be within the range between any two of the values ​​exemplified herein. The thickness of the dip-molded article may be adjusted by the time the molding die is immersed in the polymer latex composition, the solid content concentration of the chloroprene polymer latex composition, and the like. When the thickness of the dip-molded article is to be reduced, the immersion time may be shortened or the solid content concentration of the chloroprene polymer latex composition may be reduced.

[0142] As described above, the dip-molded article according to one embodiment of the present invention has excellent hand feel and wearing feel, and has sufficient tensile strength at break regardless of whether a vulcanizing agent, a vulcanization accelerator, or a cross-linking agent is added.

[0143] Latex containing conventional chloroprene rubber has been used as a rubber latex raw material for dip-molded films of gloves, balloons, boots, catheters, etc. On the other hand, in particular for medical rubber gloves, there is a tendency to seek a dip-molded product of a chloroprene polymer having the same high softness as a dip-molded product obtained by using natural rubber or polyisoprene, and a dip-molded product of a chloroprene polymer having improved hand feeling of the dip-molded product (film) and wearing feeling (fitting feeling) when made into gloves. The dip-molded product of the present invention has mechanical properties equivalent to those of a dip-molded product containing conventional chloroprene polymers, has excellent hand feeling, and has excellent wearing feeling when made into gloves.

[0144] The dip-molded product obtained from the chloroprene polymer latex composition may contain sulfur or a vulcanization accelerator. However, even if the dip-molded product does not contain sulfur and a vulcanization accelerator, it has mechanical properties equivalent to or better than those of a vulcanized dip-molded product obtained from a conventional chloroprene polymer latex. Therefore, the chloroprene polymer latex composition is suitable for use as a raw material for the dip-molded product (dipping molded body) of the chloroprene polymer of the present embodiment.

[0145] 7. Method for producing dip-molded article

[0146] The method for producing the dip-molded article containing a chloroprene-based polymer of the present invention may include:

[0147] a molding step of molding the chloroprene polymer latex composition containing the chloroprene polymer by an immersion coagulation method using a calcium-based coagulation liquid to obtain an immersion molded body; and

[0148] In the drying step, the obtained impregnated body is subjected to a heat drying treatment to obtain an impregnated product.

[0149] The molding method when manufacturing the impregnation molded body of one embodiment of the present invention is not particularly limited, and molding can be performed according to a common method. As molding methods, for example, an impregnation coagulation method, a simple impregnation method, a thermosensitive impregnation method, an electrodeposition method, etc. can be cited. From the viewpoint of easy manufacture and easy acquisition of an impregnation molded body of a certain thickness, an impregnation coagulation method can be used. Specifically, a ceramic molding mold coated with a calcium-based coagulation liquid is immersed in a chloroprene polymer latex composition, and the chloroprene polymer latex composition is coagulated. Then, after removing water-soluble impurities by leaching, it is dried, and then a dip-molded film (rubber coating) is formed by heating and vulcanization, and then the dip-molded film is demoulded. Thus, a film-like impregnation molded body can be obtained.

[0150] In addition, the method for manufacturing an impregnated molded product of one embodiment of the present invention may include a step of subjecting the obtained impregnated molded product to a heat drying treatment and vulcanizing the unvulcanized impregnated molded product. The heat drying temperature may be appropriately set according to the composition of the chloroprene polymer latex composition, and may be 100 to 220°C, or 120 to 180°C. The heat drying temperature may be, for example, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, or 220°C, or may be within the range between any two of the values ​​exemplified herein. The heat drying time may be appropriately set according to the composition of the chloroprene polymer latex composition, the shape of the unvulcanized molded product, etc., and may be 10 to 300 minutes. The heat drying time is, for example, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300 minutes, and may be within the range between any two of the values ​​exemplified herein. As an example, the dip molded article of one embodiment of the present invention may be obtained by heat drying at 150° C. for 60 minutes.

[0151] [Example]

[0152] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to these examples. In the following examples relating to the synthesis of chloroprene polymer latex, unless otherwise specified, "parts by mass" refers to the amount relative to 100 parts by mass of the total of chloroprene monomer and 2,3-dichloro-1,3-butadiene monomer before the start of emulsion polymerization. In addition, "% by mass" refers to the amount relative to 100% by mass of the chloroprene polymer contained in the chloroprene polymer latex.

[0153] [Synthesis Example A1]

[0154] <Preparation of Chloroprene Polymer Latex>

[0155] In a polymerization tank having an internal volume of 40 liters, 91 parts by mass of chloroprene monomer, 9 parts by mass of 2,3-dichloro-1,3-butadiene monomer, 0.02 parts by mass of n-dodecyl mercaptan, 76.5 parts by mass of pure water, 18 parts by mass of gum rosin-based disproportionated rosin acid potassium (aqueous solution, solid content 25%) (manufactured by Arakawa Chemical Industries, Ltd., trade name: RONDIS K-25), 0.80 parts by mass of potassium hydroxide, and 0.50 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation) were added. The pH of the aqueous emulsion before the start of polymerization was 13.2. 0.1 parts by mass of potassium persulfate was added as a polymerization initiator, and polymerization was carried out at a polymerization temperature of 15° C. under a nitrogen gas stream. When the polymerization conversion rate reached 83%, 0.01 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, thereby obtaining a latex.

[0156] The latex was subjected to reduced pressure distillation to remove unreacted monomers and a portion of water, thereby obtaining a chloroprene polymer latex having a solid content of 60%.

[0157] [Synthesis Examples A2 to A4]

[0158] Chloroprene polymer latex samples of Synthesis Examples A2 to A4 were prepared in the same manner as Synthesis Example A1 except that the addition amount of 2,3-dichloro-1,3-butadiene and n-dodecyl mercaptan as a chain transfer agent, the polymerization temperature, and the polymerization conversion rate were changed as shown in Table 1 below.

[0159] [Synthesis example B1]

[0160] <Preparation of Chloroprene Polymer Latex>

[0161] In a polymerization tank having an internal volume of 40 liters, 91 parts by mass of chloroprene monomer, 9 parts by mass of 2,3-dichloro-1,3-butadiene monomer, 3.0 parts by mass of n-dodecyl mercaptan, 76.5 parts by mass of pure water, 18 parts by mass of gum rosin-based disproportionated rosin acid potassium (aqueous solution) (manufactured by Arakawa Chemical Industries, Ltd., trade name: RONDIS K-25), 0.80 parts by mass of potassium hydroxide, and 0.50 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation) were added. The pH of the aqueous emulsion before the start of polymerization was 13.1. 0.1 parts by mass of potassium persulfate was added as a polymerization initiator, and polymerization was carried out at a polymerization temperature of 30° C. under a nitrogen gas flow. When the polymerization conversion rate reached 83%, 0.01 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, thereby obtaining a latex.

[0162] The latex was subjected to reduced pressure distillation to remove unreacted monomers, thereby obtaining a chloroprene polymer latex having a solid content of 60%.

[0163] [Synthesis Examples B2 to B8]

[0164] Chloroprene polymer latex samples of Synthesis Examples B2 to B8 were prepared in the same manner as Synthesis Example B1, except that the addition amount of 2,3-dichloro-1,3-butadiene and n-dodecyl mercaptan as a chain transfer agent, the polymerization temperature, and the polymerization conversion rate were changed as shown in Table 1 below.

[0165] The following analysis was performed using the obtained chloroprene polymer latex containing the chloroprene polymer.

[0166] <Measurement of Weight Average Molecular Weight of Each Chloroprene Polymer Latex>

[0167] The polymer precipitated from the obtained latex containing the chloroprene polymer with methanol was dissolved in tetrahydrofuran to prepare a 0.1% THF (tetrahydrofuran) solution, and the weight average molecular weight of the eluted component (sol component) was measured by gel permeation chromatography (GPC). The detected peak can be obtained as the weight average molecular weight converted to polystyrene, and the measurement was performed under the conditions described below.

[0168] <Weight Average Molecular Weight Measurement by Gel Permeation Chromatography>

[0169] GPC measurement was performed under the following conditions. The weight average molecular weight was determined in terms of polystyrene.

[0170] · Gel permeation chromatography (GPC) measuring device: Gel permeation chromatograph (HLC-8320) manufactured by Tosoh Corporation

[0171] ·Chromatographic column: TSKgel ALPHA-M manufactured by Tosoh Corporation

[0172] ·Eluent: Tetrahydrofuran (manufactured by Kanto Chemical)

[0173] Eluent flow rate: 1.0ml / min

[0174] Column temperature: 40℃

[0175] ·Detection method: Differential refractive index (RI) meter

[0176] Calibration curve: Prepared using standard polystyrene

[0177] <Determination of Copolymerization Amount of 2,3-Dichloro-1,3-butadiene>

[0178] The rubber sample of the chloroprene polymer obtained by freeze-drying the obtained chloroprene polymer latex was cut into a test piece of 0.05 mg, and measured by a pyrolysis gas chromatography-mass spectrometer to obtain the area ratio of the peak derived from chloroprene to the peak derived from 2,3-dichloro-1,3-butadiene. The content (mass %) of 2,3-dichloro-1,3-butadiene in the chloroprene polymer was obtained using the calibration curve of the area ratio of the peak derived from chloroprene to the peak derived from 2,3-dichloro-1,3-butadiene and the content of 2,3-dichloro-1,3-butadiene.

[0179] <Measurement by pyrolysis gas chromatography-mass spectrometry>

[0180] The measurement conditions of the pyrolysis gas chromatography-mass spectrometer are as follows.

[0181] Device name: HP5890-II

[0182] Chromatographic column: DB-5 (Film thickness 1.0μm)

[0183] Column temperature: 50℃(5min)→10℃ / min→150℃→25℃ / min→300℃

[0184] Inlet temperature: 250℃

[0185] Detector temperature: 280°C

[0186] Detector: FID [Table 1]

[0187]

[0188] [Example 1]

[0189] When the total amount of the chloroprene polymer latex of Synthesis Example A1 and the chloroprene polymer latex of Synthesis Example B1 was 100 parts by mass, 80 parts by mass of the sample of Synthesis Example A1 and 20 parts by mass of the sample of Synthesis Example B1 were stirred and mixed at 100 rpm for 2 minutes using a paddle to obtain the chloroprene polymer latex of Example 1.

[0190] <Measurement of Weight Average Molecular Weight of Chloroprene Polymer Latex>

[0191] The polymer precipitated from the latex containing the chloroprene polymer obtained by mixing with methanol was dissolved in tetrahydrofuran to prepare a 0.1% THF (tetrahydrofuran) solution, and the tetrahydrofuran-soluble component was measured by gel permeation chromatography (GPC). As a result, a peak with a weight average molecular weight (Mw) of 22,715 was confirmed. In addition, the conditions of the GPC measurement were the same as those for the weight average molecular weight measurement in the above-mentioned synthesis examples.

[0192] <Copolymerization Amount of 2,3-dichloro-1,3-butadiene in Chloroprene-Based Polymer Contained in Chloroprene-Based Polymer Latex>

[0193] The copolymerization amount of 2,3-dichloro-1,3-butadiene in the chloroprene polymer rubber obtained by freeze-drying the mixed chloroprene polymer latex was measured, and the result was 9.5% by mass. From this analysis value, it was confirmed that the copolymerization amount of 2,3-dichloro-1,3-butadiene in the chloroprene polymer was roughly related to the blending amount (addition amount) of 2,3-dichloro-1,3-butadiene. In addition, the conditions of this measurement were the same as those of the thermal decomposition gas chromatography measurement in each of the above-mentioned synthesis examples.

[0194] <Preparation of Dip-Molded Article (Dip-Molded Film Sample)>

[0195] (Preparation of Chloroprene-Based Polymer Latex Composition)

[0196] A chloroprene polymer latex composition was prepared by mixing 100 parts by mass of the solid content of the chloroprene polymer latex with an aqueous dispersion, and adding water to adjust the total solid content concentration of the formulation to 30% by mass. The aqueous dispersion was prepared by mixing 2 parts by mass of type 2 zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 2 parts by mass of dibutyl dithiocarbamic acid zinc salt (trade name "Nocceler BZ", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 1 part by mass of sulfur, 0.1 part by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), and 10.7 parts by mass of water at 20° C. for 16 hours using a ceramic ball mill. The obtained chloroprene polymer latex composition contained 2 parts by mass of type 2 zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 2 parts by mass of dibutyl dithiocarbamic acid (trade name "Nocceler BZ", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 1 part by mass of sulfur, 0.1 part by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), and water, based on 100 parts by mass of the solid content of the chloroprene polymer latex.

[0197] (Preparation of Dip-Molded Film of Chloroprene-Based Polymer)

[0198] A ceramic surgical glove mold (manufactured by Shinko Co., Ltd.) with a palm circumference of 7.5 inches was immersed in a coagulation solution prepared by mixing 62 parts by mass of water, 35 parts by mass of calcium nitrate tetrahydrate, and 3 parts by mass of calcium carbonate for 1 second and then taken out. After drying for 3 minutes, it was immersed in the chloroprene polymer latex composition prepared by the above steps for 2 minutes. Then, it was washed with running water at 45°C for 1 minute and dried at 150°C for 60 minutes to prepare an evaluation dip-molded product (glove-shaped film).

[0199] <Evaluation of Dip Molded Product>

[0200] (film thickness)

[0201] The thickness (film thickness) of three locations in the center of the evaluation film was measured using a test piece thickness meter (manufactured by Kobun Keiki Co., Ltd., trade name: ASKER SDA-12), and the minimum thickness was determined as the thickness of the evaluation film.

[0202] (Storage modulus E' and loss modulus E")

[0203] The dip-molded film sample was cut to make a strip test piece (width: 4.5 mm, length: 30 mm). The obtained strip test piece was used to carry out tensile dynamic viscoelasticity measurement according to the non-resonant forced vibration method (between chucks: 20 mm). The measurement conditions were set as static tension 5 gf, temperature 25°C, strain 0.75% (amplitude: 0.15 mm), and the storage modulus E' and loss modulus E" in the frequency range of 10 Hz were measured. The measurement apparatus used was DDV-25FP manufactured by ORIENTEC Co., Ltd. The results are shown in Tables 2 and 3. In addition, the thickness of the test piece can be 0.18 to 0.21 mm as described in Tables 2 and 3.

[0204] (Tensile strength at break)

[0205] The tensile strength at break was measured using the dip molded film in accordance with JIS K 6251. The results are shown in Tables 2 and 3.

[0206] <Measurement of Weight Average Molecular Weight of Dip Molded Product>

[0207] The impregnation molded product containing the chloroprene polymer was cut into 2 mm squares, and the cut impregnation molded product was placed in 20 ml of tetrahydrofuran and dissolved for 24 hours to prepare a 0.1% solution. Afterwards, the obtained tetrahydrofuran soluble component was subjected to gel permeation chromatography (GPC) measurement. As a result, a peak with a weight average molecular weight (Mw) of 22,715 was confirmed. In addition, the conditions for GPC measurement were the same as those for the weight average molecular weight measurement in the above-mentioned synthesis examples. The results are shown in Tables 2 and 3.

[0208] <Evaluation of the feel of glove-like dip-molded products>

[0209] Five subjects were asked to touch the obtained dip-molded product (glove-like film) and evaluate the feel of the dip-molded product by touching the surface state and stretching and bending the film. The evaluation was performed according to the following criteria, and the average value of the evaluation of each subject was expressed as a rounded value.

[0210] (Hand feel evaluation criteria)

[0211] 3: Extremely soft, comfortable to touch, and has an excellent feel.

[0212] 2: Soft, no practical problems in touch, feels good.

[0213] 1: I can't feel the softness, it feels a bit hard and the feel is not good.

[0214] <Evaluation of wearing feeling of glove-like dip-molded article>

[0215] Five subjects actually wore the obtained glove-like dip-molded product, and evaluated the wearability by focusing on the close fit (fitting feeling) with the hand and the degree of deformation after peeling. The evaluation was performed according to the following criteria, and the average value of each subject's evaluation was expressed as a rounded value.

[0216] (Evaluation criteria for wearing comfort)

[0217] 3: Excellent fit when worn, good usability, and returns to its original shape immediately (within 5 minutes) after putting on and taking off, with excellent wearing feel.

[0218] 2: There is a certain sense of fit, and it takes time (more than 5 minutes) to return to its original state after putting on and taking off. It is practical and feels good to wear.

[0219] 1: There is no sense of fit, the dip-molded material is deformed after putting on and taking off, and the wearing feeling is not good.

[0220] [Examples 2 to 11, Comparative Examples 1 to 6]

[0221] Dip molded articles were prepared in the same manner as in Example 1 except that the formulation of the chloroprene polymer latex composition was changed to the conditions shown in Tables 2 and 3 below, and each dip molded film sample was produced and evaluated. Examples 2 to 3, 9 and 10, and Comparative Examples 1 to 3 and 6 did not contain a low molecular weight chloroprene polymer having a weight average molecular weight of 3,000 to 80,000, or the type of the low molecular weight chloroprene polymer having a weight average molecular weight of 3,000 to 80,000 contained in the dip molded article was changed, or the dip molded article contained only the low molecular weight chloroprene polymer. In Examples 4 and 5 and Comparative Examples 4 and 5, the type and mixing ratio of each chloroprene polymer latex contained in the dip molded article were changed. In Example 6, a dip molded article was obtained without using dibutyl dithiocarbamic acid as a vulcanization accelerator and sulfur as a vulcanizing agent contained in the chloroprene polymer latex composition of Examples 1 to 5, etc. In Example 7, no vulcanization accelerator and sulfur were used, and 1 part by mass of an aromatic heterocyclic compound represented by the following chemical formula (2) (2-mercaptobenzimidazole, trade name "Nocrac MB", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) was added as another reagent to 100 parts by mass of the chloroprene polymer. In Example 8 and Comparative Example 2, no vulcanization accelerator and sulfur were used, and a chloroprene polymer not copolymerized with 2,3-dichloro-1,3-butadiene was used as the chloroprene polymer contained in the composition. In Example 11, the amount of zinc oxide added having a crosslinking effect was changed.

[0222] [Chemistry 2]

[0223]

[0224] [Table 2]

[0225]

[0226] [Table 3]

[0227]

[0228] As can be seen from Tables 2 and 3, the dip-molded products (dip-molded films) of the chloroprene polymer of the present invention of Examples 1 to 11 have low values ​​of storage modulus E' and loss modulus E" in tensile dynamic viscoelasticity measurement, have sufficient tensile strength at break, and the dip-molded products (dip-molded films) have excellent hand feel and wearing feel when made into gloves.

[0229] The dip-molded product of Comparative Example 1 had no low molecular weight peak and had a high storage modulus, presumably because of the strong influence of the degree of crosslinking. As a result, the dip-molded film had a poor feel.

[0230] The dip-molded product of Comparative Example 2 had no low molecular weight peak and no copolymerization of 2,3-dichloro-1,3-butadiene. It is believed that even without the addition of a vulcanization accelerator and sulfur, the crosslinking degree and crystallinity of the chloroprene polymer strongly influenced the high storage modulus. As a result, the feel of the dip-molded film was poor.

[0231] In the dip-molded product of Comparative Example 3, the ratio of the chloroprene polymer having a low molecular weight peak was high, and it is considered that the loss modulus was high because the viscosity term was strongly affected. As a result, the wearing feeling was deteriorated.

[0232] The dip-molded product of Comparative Example 4 had no low molecular weight peak and had a high storage modulus, presumably because of the strong influence of the degree of crosslinking. As a result, the dip-molded film had a poor feel.

[0233] The dip-molded product of Comparative Example 5 has no low molecular weight peak and contains a high ratio of latex of a relatively low molecular weight chloroprene polymer. It is considered that the storage modulus is high due to the strong influence of the crosslinking degree, and the loss modulus is high due to the strong influence of the viscosity term. As a result, the hand feel and wearing feeling are deteriorated.

[0234] In Comparative Example 6, the chloroprene polymer in the chloroprene polymer latex composition used to obtain the dip-molded product was only a low-molecular-weight chloroprene polymer, so the dip-molded product was brittle and a dip-molded product having a strength sufficient for evaluating various physical properties could not be obtained.

[0235] In addition, from Examples 2 to 3 and Examples 9 and 10 using Synthesis Examples B2 to B3, B5, and B6, it can be seen that the value of the weight average molecular weight in the low molecular weight region affects the value of the storage modulus, and there is a tendency that the value of the storage modulus is higher as the weight average molecular weight is larger. In addition, as shown in Example 6, when no vulcanization accelerator or sulfur is contained, for example, the values ​​of the storage modulus and the loss modulus are slightly lower than those of Example 1, but a dip-molded product having sufficient strength and excellent hand feeling and wearing feeling can be obtained. From the above, it can be seen that the dip-molded product of the chloroprene polymer of the present invention has an excellent hand feeling regardless of whether a vulcanizing agent and a vulcanization accelerator are added, and exhibits an excellent wearing feeling when made into a glove.

Claims

1. A dip-molded article comprising a chloroprene polymer, The storage modulus E' of the dip-molded product in the frequency region of 10 Hz is 3.2 MPa or less, and the loss modulus E" is 0.37 MPa or less, as obtained when the tensile dynamic viscoelasticity is measured by the non-resonant forced vibration method under the conditions of static tension of 5 gf, temperature of 25°C, strain of 0.75%, and amplitude of 0.15 mm.

2. The dip-molded article according to claim 1, wherein The chloroprene-based polymer contains a monomer unit derived from 2,3-dichloro-1,3-butadiene.

3. The dip-molded article according to claim 1 or 2, wherein The dip-molded product is dissolved in tetrahydrofuran and the soluble component is measured by gel permeation chromatography, whereby at least a peak having a weight average molecular weight of 3,000 to 80,000 is detected.

4. The dip-molded article according to any one of claims 1 to 3, wherein The dip-molded product contains a metal oxide.

5. The dip-molded article according to any one of claims 1 to 4, These are industrial / general household gloves, medical gloves, balloons, catheters or boots.

6. A chloroprene polymer, wherein: The storage modulus E' of the dip-molded article containing the chloroprene polymer in the frequency region of 10 Hz obtained by measuring the tensile dynamic viscoelasticity by a non-resonant forced vibration method under the conditions of a static tension of 5 gf, a temperature of 25° C., a strain of 0.75%, and an amplitude of 0.15 mm is 3.2 MPa or less, and the loss modulus E" is 0.37 MPa or less, The dip-molded product is obtained by molding a chloroprene polymer latex composition containing the chloroprene polymer by a dip coagulation method and performing a heat drying treatment at 150° C. for 60 minutes.

7. A method for producing a dip-molded article, which is a method for producing a dip-molded article containing a chloroprene-based polymer, comprising: A molding step, molding the chloroprene polymer latex composition containing the chloroprene polymer according to claim 6 by an immersion coagulation method using a calcium-based coagulation liquid to obtain an immersion molded body; as well as In the drying step, the obtained impregnated body is subjected to a heat drying treatment to obtain an impregnated product.