Fiber for artificial hair and hair ornament
By attaching cationic polymers and surfactants to the surface of artificial hair fibers, the problem of contaminant adhesion is solved, and high pollution resistance and softness is achieved, which is suitable for hair decorations.
Patent Information
- Application Number
- CN202380030640.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-06
- Filing Date
- 2023-03-15
- Publication Date
- 2024-11-15
AI Technical Summary
During use, fibers for artificial hair are easily adhered to contaminated substances, resulting in dirt problems. The prior art is difficult to effectively solve the pollution resistance.
Using a fiber treatment agent including base fibers, cationic polymers, cationic surfactants and nonionic surfactants, the fibers are adhered to the fibers by attaching cationic polymers, cationic surfactants and nonionic surfaces. Active agent to improve the pollution resistance of fibers.
It achieves high pollution resistance of fibers, with dust removal rate of more than 40%, while maintaining softness and reducing stickiness, suitable for hair decorations.
Smart Images

Figure BDA0005061334710000021 
Figure BDA0005061334710000111 
Figure BDA0005061334710000131
Abstract
Description
Technical Field
[0001] The present invention relates to fibers for artificial hair, hair accessories, etc. Background Art
[0002] Fibers for artificial hair (fibers for artificial hair) can be used for hair accessories. Patent Document 1 below discloses a technique for treating base fibers with a fiber treating agent.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2002-285470 Summary of the invention
[0006] Problem that the invention aims to solve
[0007] Users of hair accessories are troubled by dirt and the like caused by the adhesion of pollutants (dandruff, hair oil, etc.) to artificial hair fibers during use. Therefore, artificial hair fibers are required to have excellent stain resistance.
[0008] An object of one aspect of the present invention is to provide a fiber for artificial hair having excellent stain resistance. Another object of the present invention is to provide a hair accessories including such a fiber for artificial hair.
[0009] Solutions for solving problems
[0010] The present invention relates to the following [1] to
[11] etc. in several aspects.
[0011] [1] An artificial hair fiber comprising a base fiber, a cationic polymer, a cationic surfactant and a nonionic surfactant, wherein the cationic polymer, the cationic surfactant and the nonionic surfactant are present on at least a portion of the surface of the base fiber, the cationic polymer comprises a monomer as a monomer unit, the monomer having at least one selected from the group consisting of a primary amino group, a secondary amino group, a tertiary amino group, an acid-neutralizing group thereof and a quaternary ammonium group, the cationic surfactant has a carbon chain having 12 to 22 carbon atoms, the nonionic surfactant has a carbon chain having 10 to 20 carbon atoms, the HLB value of the nonionic surfactant is 13.0 or more, and the content of the cationic polymer is 0.005% by mass or more based on the total amount of the artificial hair fiber.
[0012] [2] The fiber for artificial hair according to [1], wherein the base fiber comprises at least one selected from the group consisting of a homopolymer of vinyl chloride, a vinyl chloride-acrylonitrile copolymer, polyethylene terephthalate, a polyamide-based resin, polypropylene, and an acrylonitrile-styrene copolymer.
[0013] [3] The fiber for artificial hair according to [1] or [2], wherein the cationic polymer further comprises an alkyl (meth)acrylate as a monomer unit.
[0014] [4] The fiber for artificial hair according to any one of [1] to [3], wherein the cationic surfactant comprises a quaternary ammonium salt of a cation having a structure represented by the following general formula (1).
[0015]
[0016] [In formula (1), R 11 represents a group containing a carbon chain having 12 to 22 carbon atoms, R 12 , R 13 and R 14 Each independently represents a monovalent group.]
[0017] [5] The fiber for artificial hair according to any one of [1] to [4], wherein the carbon number of the carbon chain of the cationic surfactant is 18 to 22.
[0018] [6] The fiber for artificial hair according to any one of [1] to [5], wherein the HLB value of the nonionic surfactant is 13.0 to 19.0.
[0019] [7] The fiber for artificial hair according to any one of [1] to [6], wherein the nonionic surfactant comprises a polyoxyalkylene alkyl ether.
[0020] [8] The fiber for artificial hair according to any one of [1] to [7], wherein the content of the cationic polymer is 0.005 to 0.2% by mass based on the total amount of the fiber for artificial hair.
[0021] [9] The fiber for artificial hair according to any one of [1] to [8], wherein the mass ratio of the total amount of the cationic surfactant and the nonionic surfactant to the content of the cationic polymer is 3 to 160.
[0022]
[10] The fiber for artificial hair according to any one of [1] to [9], wherein the total amount of the cationic polymer, the cationic surfactant and the nonionic surfactant is 0.1 to 4% by mass based on the total amount of the fiber for artificial hair.
[0023]
[11] A hair accessories comprising the fiber for artificial hair according to any one of [1] to
[10] .
[0024] Effects of the Invention
[0025] According to one aspect of the present invention, a fiber for artificial hair having excellent stain resistance can be provided. According to another aspect of the present invention, a hair accessories including such a fiber for artificial hair can be provided. DETAILED DESCRIPTION
[0026] Hereinafter, embodiments of the present invention will be described in detail.
[0027] "Above A" in the numerical range refers to A and the range exceeding A. "Below A" in the numerical range refers to A and the range less than A. In the numerical ranges recorded in stages in this specification, the upper limit or lower limit of the numerical range of a certain stage can be arbitrarily combined with the upper limit or lower limit of the numerical range of other stages. In the numerical ranges recorded in this specification, the upper limit or lower limit of the numerical range can also be replaced by the values shown in the embodiments. "A or B" can include either A or B, or both. Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of more than two. In the case where there are multiple substances equivalent to each component in the composition, the content of each component in the composition refers to the total amount of the multiple substances present in the composition unless otherwise specified. The term "process" is not only an independent process, but also included in this term as long as the desired effect of the process can be achieved even if it cannot be clearly distinguished from other processes. "(Meth)acrylic acid" refers to at least one of acrylic acid and its corresponding methacrylic acid. The same is true for other similar expressions such as "(meth)acrylamide". "Polyoxyalkylene group" and "oxyalkylene group" are collectively described as "(poly)oxyalkylene group." The same applies to other expressions including "(poly)".
[0028] The fiber for artificial hair of the present embodiment comprises a base fiber, a cationic polymer, a cationic surfactant and a nonionic surfactant, and the cationic polymer, the cationic surfactant and the nonionic surfactant are present on at least a part of the surface of the base fiber.
[0029] The cationic polymer comprises, as a monomer unit, a monomer having at least one selected from the group consisting of a primary amino group, a secondary amino group, a tertiary amino group, an acid neutralizing group thereof, and a quaternary ammonium group, the cationic surfactant has a carbon chain having 12 to 22 carbon atoms, the nonionic surfactant has a carbon chain having 10 to 20 carbon atoms, the HLB value of the nonionic surfactant is 13.0 or more, and the content of the cationic polymer is 0.005% by mass or more based on the total amount of the artificial hair fiber.
[0030] Hereinafter, depending on the circumstances, the above-mentioned cationic polymer will be referred to as "cationic polymer P", the above-mentioned cationic surfactant having a carbon chain with a carbon number of 12 to 22 will be referred to as "cationic surfactant A", and the above-mentioned nonionic surfactant having a carbon chain with a carbon number of 10 to 20 and an HLB value of 13.0 or more will be referred to as "nonionic surfactant B".
[0031] The fiber for artificial hair of the present embodiment is excellent in stain resistance. According to the fiber for artificial hair of the present embodiment, in the evaluation of the examples described later, for example, 40% or more can be obtained as the dust release rate.
[0032] One aspect of the fiber for artificial hair of the present embodiment is excellent in softness. Another aspect of the fiber for artificial hair of the present embodiment is excellent in anti-stickiness (it is possible to reduce stickiness).
[0033] The fiber treatment agent of the present embodiment is a fiber treatment agent for obtaining the artificial hair fiber of the present embodiment, and contains a cationic polymer P, a cationic surfactant A, and a nonionic surfactant B. According to the fiber treatment agent of the present embodiment, the artificial hair fiber of the present embodiment can be obtained, and the artificial hair fiber excellent in stain resistance can be obtained.
[0034] The fiber for artificial hair of this embodiment can be used as artificial hair, and can also be used to obtain artificial hair. The fiber for artificial hair of this embodiment can be a fiber after a stretching treatment, or it can be an unstretched fiber. The single fineness of the fiber for artificial hair of this embodiment can be 20 dtex to 100 dtex after a stretching treatment.
[0035] As the material of the base fiber in the artificial hair fiber of the present embodiment, vinyl chloride resin, polyester resin, polyamide resin, polyolefin resin, ethylene-vinyl acetate copolymer (EVA), acrylonitrile-butadiene rubber (NBR), thermoplastic polyurethane (TPU), polyester thermoplastic elastomer (TPEE), methyl methacrylate-butadiene-styrene resin (MBS), acrylonitrile-butadiene-styrene resin (ABS), acrylonitrile-styrene copolymer (AS), polymethyl methacrylate (PMMA), etc. can be cited. In the case where a material that can be equivalent to a material other than vinyl chloride resin has a monomer unit of vinyl chloride, it is defined that the material is equivalent to vinyl chloride resin. The base fiber can contain at least one of these materials as a main component (main resin raw material). That is, based on the total amount of the base fiber, the content of at least one of these materials can be 50% by mass or more, or it can exceed 50% by mass.
[0036] The vinyl chloride resin is a polymer having a structural unit derived from vinyl chloride (monomer unit of vinyl chloride), and is a polymer having vinyl chloride as a monomer unit. The vinyl chloride resin can be obtained by bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, etc., and can be obtained by suspension polymerization from the viewpoint of excellent initial colorability of the fiber. The base fiber may contain a mixture of a vinyl chloride resin and a component (e.g., acrylonitrile-styrene copolymer) that can form a polymer alloy with the vinyl chloride resin.
[0037] As the vinyl chloride resin, homopolymers of vinyl chloride (homopolymers, polyvinyl chloride), copolymers of vinyl chloride with other monomers, etc. can be mentioned, and mixtures thereof can also be used. As copolymers of vinyl chloride with other monomers, copolymers of vinyl chloride with vinyl esters (vinyl chloride-vinyl acetate copolymers, vinyl chloride-vinyl propionate copolymers, etc.); copolymers of vinyl chloride with (meth) acrylic acid compounds ((meth) acrylic acid, (meth) acrylic acid esters, etc.) (vinyl chloride-butyl acrylate copolymers, vinyl chloride-2-ethylhexyl acrylate copolymers, etc.); copolymers of vinyl chloride with olefins (vinyl chloride-ethylene copolymers, vinyl chloride-propylene copolymers, etc.); vinyl chloride-acrylonitrile copolymers, etc. The vinyl chloride resin may not have a structural unit derived from a (meth) acrylic acid compound (monomer unit of a (meth) acrylic acid compound). In the copolymer, the content of monomers different from vinyl chloride can be determined according to the required quality such as molding processability and line characteristics. From the viewpoint of easily obtaining excellent stain resistance, flexibility and anti-stickiness, the vinyl chloride resin may contain at least one selected from the group consisting of a homopolymer of vinyl chloride and a vinyl chloride-acrylonitrile copolymer.
[0038] Examples of the polyester resin include polyethylene terephthalate (PET), polybutylene terephthalate, polyethylene-2,6-naphthalate, polyethylene terephthalate, and glycol-modified polyethylene terephthalate (PETG).
[0039] Examples of the polyamide-based resin include nylon 6, nylon 66, nylon 11, nylon 12, nylon 6 / 10, and nylon 6 / 12.
[0040] Examples of the polyolefin-based resin include polyethylene (PE) and polypropylene (PP).
[0041] From the viewpoint of easily obtaining excellent stain resistance, softness and stickiness resistance, the base fiber may include at least one selected from the group consisting of vinyl chloride resins, polyester resins, polyamide resins, polyolefin resins and acrylonitrile-styrene copolymers, or may include at least one selected from the group consisting of homopolymers of vinyl chloride, vinyl chloride-acrylonitrile copolymers, polyethylene terephthalate, polyamide resins, polypropylene and acrylonitrile-styrene copolymers.
[0042] The content of the vinyl chloride resin, polyester resin, polyamide resin, polyolefin resin or acrylonitrile-styrene copolymer in the substrate fiber may be 50% by mass or more, more than 50% by mass, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, 98% by mass or more or 99% by mass or more, based on the total mass of the substrate fiber. The substrate fiber may be composed only of the vinyl chloride resin, polyester resin, polyamide resin, polyolefin resin or acrylonitrile-styrene copolymer (substantially 100% by mass of the substrate fiber is the vinyl chloride resin, polyester resin, polyamide resin, polyolefin resin or acrylonitrile-styrene copolymer).
[0043] From the viewpoint of easily reducing the stretching ratio to obtain fine-fine artificial hair fibers, the average fineness of the base fiber when not stretched may be 300 dtex or less, 200 dtex or less, or 100 dtex or less.
[0044] The fiber for artificial hair of the present embodiment comprises a cationic polymer P present on at least a part of the surface of a base fiber, a cationic surfactant A and a nonionic surfactant B. The cationic polymer P, the cationic surfactant A and the nonionic surfactant B may be present at the same position or at different positions on the surface of the base fiber.
[0045] The cationic polymer P comprises as a monomer unit a monomer having at least one selected from the group consisting of a primary amino group, a secondary amino group, a tertiary amino group, an acid neutralizing group thereof, and a quaternary ammonium group (quaternary ammonium salt group). The cationic polymer P may not have a carbon chain having 12 to 22 carbon atoms.
[0046] In the artificial hair fiber and the fiber treatment agent of the present embodiment, at least one of the cationic polymers P is present. In the case where the cationic polymer P and a cationic polymer other than the cationic polymer P are present in the artificial hair fiber and the fiber treatment agent of the present embodiment, the content of the cationic polymer P may be 50% by mass or more, or may exceed 50% by mass, based on the total amount of the cationic polymer (the total amount of the cationic polymer P and the cationic polymer other than the cationic polymer P).
[0047] The primary amino group, the secondary amino group and the tertiary amino group may have a hydrocarbon group bonded to the nitrogen atom. The hydrocarbon group may be linear, branched or cyclic. Examples of the hydrocarbon group include alkyl, alkenyl, and aryl groups. The number of carbon atoms in the hydrocarbon group may be 1 to 12, 1 to 10, 1 to 8, 1 to 5, 1 to 3, or 1 to 2. From the viewpoint of easily obtaining excellent stain resistance, flexibility, and anti-tackiness, the tertiary amino group may have two hydrocarbon groups with carbon atoms in the above range.
[0048] The acid-neutralizing group of the primary amino group, the secondary amino group, and the tertiary amino group is an acid addition base formed by adding a hydrogen ion (proton) and an anion to the amino group. The quaternary ammonium group is a group formed by adding an anion to an ammonium cation. Examples of the acid addition base and the anion in the quaternary ammonium group include halide ions such as chloride ion, bromide ion, and iodide ion; alkyl sulfate ions such as methyl sulfate ion; ions of organic acids such as acetate ion, etc.
[0049] Examples of the monomer P1 include (dialkylamino)alkyl (meth)acrylates, acid neutralized products and quaternized products thereof; (dialkylamino)alkyl (meth)acrylamides, acid neutralized products and quaternized products thereof; (monoalkylamino)alkyl (meth)acrylates, acid neutralized products thereof; (monoalkylamino)alkyl (meth)acrylamides, acid neutralized products thereof, and the like. Examples of (dialkylamino)alkyl (meth)acrylates include (dimethylamino)ethyl (meth)acrylate, (diethylamino)ethyl (meth)acrylate, (dimethylamino)propyl (meth)acrylate, and (diethylamino)propyl (meth)acrylate. Examples of (dialkylamino)alkyl (meth)acrylamides include (dimethylamino)ethyl (meth)acrylamide, (diethylamino)ethyl (meth)acrylamide, (dimethylamino)propyl (meth)acrylamide, and (diethylamino)propyl (meth)acrylamide. Examples of the (monoalkylamino)alkyl (meth)acrylate include (monomethylamino)ethyl (meth)acrylate, (monoethylamino)ethyl (meth)acrylate, (monomethylamino)propyl (meth)acrylate, (monoethylamino)propyl (meth)acrylate, and 2-(tert-butylamino)ethyl (meth)acrylate. Examples of the (monoalkylamino)alkyl (meth)acrylamide include (monomethylamino)ethyl (meth)acrylamide, (monoethylamino)ethyl (meth)acrylamide, (monomethylamino)propyl (meth)acrylamide, and (monoethylamino)propyl (meth)acrylamide.
[0050] From the viewpoint of easily obtaining excellent stain resistance, flexibility and anti-tackiness, the cationic polymer P may have a monomer having a tertiary amino group as a monomer unit, may have a (dialkylamino)alkyl (meth)acrylate as a monomer unit, and may have a (dimethylamino)ethyl (meth)acrylate as a monomer unit.
[0051] The content of the monomer unit of the monomer P1 in the cationic polymer P can be in the following ranges based on the total amount of the monomer units constituting the cationic polymer P, from the viewpoint of easily obtaining excellent stain resistance, flexibility and anti-tackiness. The content of the monomer unit of the monomer P1 can be 10% by mass or more, 20% by mass or more, 30% by mass or more, 35% by mass or more, 40% by mass or more, 45% by mass or more, or 50% by mass or more. The content of the monomer unit of the monomer P1 can be 100% by mass or less, less than 100% by mass, 99% by mass or less, 98% by mass or less, 96% by mass or less, or 95% by mass or less. From these viewpoints, the content of the monomer unit of the monomer P1 may be 10 to 100% by mass, 10% to less than 100% by mass, 10 to 99% by mass, 10 to 95% by mass, 30 to 100% by mass, 30% to less than 100% by mass, 30% to 99% by mass, 30% to 95% by mass, 50 to 100% by mass, 50% to less than 100% by mass, 50% to 99% by mass, or 50% to 95% by mass.
[0052] The cationic polymer P may have a monomer other than the monomer P1 (hereinafter referred to as "monomer P2") as a monomer unit, or may be a copolymer having the monomer P1 and the monomer P2 as monomer units. Examples of the monomer P2 include (meth)acrylates; unsaturated monocarboxylic acids and salts thereof such as (meth)acrylic acid, crotonic acid, and α-allyloxyacrylic acid; aromatic vinyl monomers such as styrene; olefin monomers such as ethylene and propylene; halogenated vinyls such as vinyl chloride; alkyl vinyl ethers such as methyl vinyl ether and ethyl vinyl ether; cyclic vinyl monomers such as N-vinyl pyrrolidone, etc. Examples of salts of unsaturated monocarboxylic acids include alkali metal salts (lithium salts, sodium salts, potassium salts, etc.).
[0053] The (meth)acrylate may or may not have a substituent. Examples of the substituent include hydroxyl groups; alkoxy groups having 1 to 18 carbon atoms such as methoxy and ethoxy groups; oxygen-containing groups such as oxyalkylene groups, sulfonic acid groups, and phosphoric acid groups; halogenated groups such as fluoro groups; epoxy groups such as glycidyl groups; and carbonyl groups such as aldehyde groups.
[0054] From the viewpoint of easily obtaining excellent stain resistance, flexibility and anti-tackiness, the cationic polymer P may have an alkyl (meth)acrylate as a monomer unit. Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, sec-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, tridecyl (meth)acrylate, cycloalkyl (meth)acrylate (cyclohexyl (meth)acrylate, etc.), n-lauryl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and isobornyl (meth)acrylate.
[0055] The content of the monomer unit of the monomer P2 in the cationic polymer P can be the following ranges based on the total amount of the monomer units constituting the cationic polymer P, from the viewpoint of easily obtaining excellent stain resistance, flexibility and anti-tackiness. The content of the monomer unit of the monomer P2 can be 90% by mass or less, 80% by mass or less, 70% by mass or less, 65% by mass or less, 60% by mass or less, 55% by mass or less, or 50% by mass or less. The content of the monomer unit of the monomer P2 can be more than 0% by mass, 1% by mass or more, 2% by mass or more, 4% by mass or more, or 5% by mass or more. From these viewpoints, the content of the monomer unit of the monomer P2 can be more than 0% by mass and less than 90% by mass, more than 0% by mass and less than 70% by mass, more than 0% by mass and less than 50% by mass, 1 to 90% by mass, 1 to 70% by mass, 1 to 50% by mass, 5 to 90% by mass, 5 to 70% by mass, or 5 to 50% by mass.
[0056] From the viewpoint of being easy to obtain excellent stain resistance, flexibility and anti-tackiness, the weight average molecular weight of the cationic polymer P can be the following range. The weight average molecular weight can be 1000 or more, 3000 or more, 5000 or more, 8000 or more, 10,000 or more, 12,000 or more, 15,000 or more, 18,000 or more, or 20,000 or more. The weight average molecular weight can be 500,000 or less, 300,000 or less, 200,000 or less, 150,000 or less, 100,000 or less, 90,000 or less, 80,000 or less, 70,000 or less, 60,000 or less, or 50,000 or less. From these viewpoints, the weight average molecular weight can be 1000-500,000, 1000-100,000, 1000-80,000, 1000-50,000, 10,000-100,000, 10,000-80,000, 10, ...20,000-500,000, 20,000-100,000, 20,000-80,000, or 20,000-50,000.
[0057] The weight average molecular weight (Mw) of the cationic polymer P can be measured by GPC (gel permeation chromatography) under the following conditions.
[0058] Device: Waters e2695
[0059] Detector: Differential refractometer (RI) detector
[0060] Column: TSKgel α-M, α-2500 manufactured by Tosoh Corporation
[0061] Column temperature: 40°C
[0062] Flow rate: 0.8 mL / min
[0063] Injection volume: 10 μL (sample concentration 0.4 mass % eluent preparation solution)
[0064] Standard curve: Polyethylene glycol manufactured by GL Science Co., Ltd.
[0065] GPC software: EMPOWER3 manufactured by Waters
[0066] Eluent: 0.5M acetic acid + 0.2M sodium nitrate / acetonitrile = 50 / 50 (v / v)
[0067] Cationic surfactant A has a carbon chain with 12 to 22 carbon atoms (hereinafter referred to as "carbon chain A"), and nonionic surfactant B has a carbon chain with 10 to 20 carbon atoms (hereinafter referred to as "carbon chain B"). "Carbon chain" is a molecular chain formed by continuous bonding of carbon atoms. For example, "carbon chain with 12 to 22 carbon atoms" is a molecular chain formed by continuous bonding of 12 to 22 carbon atoms. "Carbon chain" can be any of linear, branched or cyclic. "Carbon chain" may or may not have unsaturated bonds.
[0068] In the artificial hair fiber and the fiber treatment agent of the present embodiment, at least one of the cationic surfactants A and at least one of the nonionic surfactants B are present. When the cationic surfactant A and a cationic surfactant other than the cationic surfactant A are present in the artificial hair fiber and the fiber treatment agent of the present embodiment, the content of the cationic surfactant A may be 50% by mass or more, or may exceed 50% by mass, based on the total amount of the cationic surfactants (the total amount of the cationic surfactant A and the cationic surfactants other than the cationic surfactant A). When the nonionic surfactant B and a nonionic surfactant other than the nonionic surfactant B are present in the artificial hair fiber and the fiber treatment agent of the present embodiment, the content of the nonionic surfactant B may be 50% by mass or more, or may exceed 50% by mass, based on the total amount of the nonionic surfactants (the total amount of the nonionic surfactant B and the nonionic surfactants other than the nonionic surfactant B).
[0069] When the carbon number of carbon chain A is 22 or less, excellent stain resistance can be obtained, and excellent anti-sticking property can be easily obtained. When the carbon number of carbon chain B is 10 or more, excellent stain resistance can be obtained, and excellent flexibility and anti-sticking property can be easily obtained. When the carbon number of carbon chain B is 20 or less, excellent stain resistance can be obtained, and excellent anti-sticking property can be easily obtained.
[0070] From the viewpoint of easily obtaining excellent stain resistance, flexibility and tack resistance, the carbon number of the carbon chain A in the cationic surfactant A may be 12 or more, 13 or more, 14 or more, 15 or more, 16 or more, 17 or more, 18 or more, 19 or more, 20 or more, or 21 or more. From the viewpoint of adjusting stain resistance, flexibility and tack resistance, the carbon number of the carbon chain A may be 21 or less, 20 or less, 19 or less, 18 or less, 17 or less, 16 or less, 15 or less, 14 or less, or 13 or less. From these viewpoints, the carbon number of the carbon chain A may be 12 to 20, 12 to 18, 12 to 16, 12 to 14, 16 to 22, 16 to 20, 16 to 18, 18 to 22, 18 to 20, or 20 to 22.
[0071] Cationic surfactant A is a surfactant having a cationic hydrophilic group, and is a surfactant having a hydrophilic group that dissociates into ions in water and becomes a cation. Examples of cationic surfactant A include quaternary ammonium salts, amine salts, pyridinium salts, imidazolinium salts, etc. Examples of salts include halide salts, chloride salts, bromide salts, iodide salts, etc.
[0072] Examples of the quaternary ammonium salt include aliphatic quaternary ammonium salts, aromatic quaternary ammonium salts (excluding compounds corresponding to heterocyclic quaternary ammonium salts), heterocyclic quaternary ammonium salts, etc. Examples of the amine salt include aliphatic amine salts, monoalkylamine salts, dialkylamine salts, trialkylamine salts, etc.
[0073] From the viewpoint of easily obtaining excellent stain resistance, flexibility, and anti-tackiness, the cationic surfactant A may contain a quaternary ammonium salt or a quaternary ammonium salt that is a chloride salt (a quaternary ammonium salt having a chloride ion as a counter anion).
[0074] From the viewpoint of easily obtaining excellent stain resistance, flexibility and anti-tackiness, the cationic surfactant A may contain a compound having a cation having a structure represented by the following general formula (1) or a quaternary ammonium salt of a cation having a structure represented by the following general formula (1).
[0075]
[0076] [In formula (1), R 11represents a group containing a carbon chain having 12 to 22 carbon atoms, R 12 , R 13 and R 14 Each independently represents a monovalent group.]
[0077] As R 11 , and examples thereof include an alkyl group having 12 to 22 carbon atoms. 12 , R 13 and R 14 The monovalent group of R includes hydrogen atoms, groups containing carbon atoms (which may contain atoms other than carbon atoms), etc. 12 , R 13 and R 14 Each independently may be a group containing carbon atoms.
[0078] Examples of the group containing carbon atoms include alkyl groups, aryl groups, carboxyl groups, carboxylate groups, alkoxy groups, etc. From the viewpoint of easily obtaining excellent stain resistance, flexibility, and anti-tackiness, the number of carbon atoms in the alkyl group may be 1 to 10, 1 to 8, 1 to 6, 1 to 5, 1 to 4, 1 to 3, or 1 to 2. Examples of the aryl group include benzyl groups, phenyl groups, naphthyl groups, etc.
[0079] From the viewpoint of easily obtaining excellent stain resistance, flexibility, and anti-tackiness, the cationic surfactant A may satisfy at least one of the following conditions.
[0080] The cationic surfactant A may include R selected from the group consisting of 12 and R 13 The quaternary ammonium salt of at least one of the groups consisting of an alkyl group may also contain R selected from the group consisting of 12 , R 13 and R 14 At least one of the group consisting of is a quaternary ammonium salt of an alkyl group.
[0081] The cationic surfactant A may include R selected from the group consisting of 12 and R 13 The quaternary ammonium salt of at least one of the group consisting of methyl may also contain R selected from the group consisting of 12 , R 13 and R 14 At least one of the group consisting of is a quaternary ammonium salt of methyl.
[0082] The cationic surfactant A may include R 12 and R 13 A quaternary ammonium salt of methyl may also contain R in the general formula (1): 12 , R 13 and R 14 It is a quaternary ammonium salt of methyl.
[0083] From the viewpoint of easily obtaining excellent stain resistance, flexibility and anti-tackiness, the cationic surfactant A may contain at least one selected from the group consisting of hexadecyltrimethylammonium chloride, stearyltrimethylammonium chloride, oleyltrimethylammonium chloride, nonadecyltrimethylammonium chloride, eicosyltrimethylammonium chloride, heneicosyltrimethylammonium chloride and behenyltrimethylammonium chloride, and may also contain at least one selected from the group consisting of hexadecyltrimethylammonium chloride, stearyltrimethylammonium chloride and behenyltrimethylammonium chloride.
[0084] The molecular weight of the cationic surfactant A may be 10,000 or less, less than 10,000, 8,000 or less, less than 8,000, 5,000 or less, less than 5,000, 3,000 or less, less than 3,000, 1,000 or less, or less than 1,000.
[0085] The nonionic surfactant B is a surfactant that does not have a group that dissociates into ions in water. From the viewpoint of easily obtaining excellent stain resistance and flexibility, the carbon number of the carbon chain B in the nonionic surfactant B may be 12 or more, 14 or more, or 16 or more. From the viewpoint of easily obtaining excellent flexibility, the carbon number of the carbon chain B may be 18 or more. From the viewpoint of easily obtaining excellent stain resistance and tack resistance, the carbon number of the carbon chain B may be 18 or less or 16 or less. From the viewpoint of easily obtaining excellent tack resistance, the carbon number of the carbon chain B may be 14 or less or 12 or less. From these viewpoints, the carbon number of the carbon chain B may be 10 to 18, 10 to 16, 10 to 14, 10 to 12, 12 to 20, 12 to 18, 12 to 16, or 12 to 14.
[0086] From the viewpoint of easily obtaining excellent stain resistance and softness, the nonionic surfactant B may include at least one selected from the group consisting of ether compounds, ester compounds, amide compounds and amine compounds, and may also include a compound having at least one selected from the group consisting of a structure represented by the following general formula (2a), a structure represented by the following general formula (2b), a structure represented by the following general formula (2c) and a structure represented by the following general formula (2d).
[0087]
[0088] [Where R 21a , R 21b , R 21c and R 21d Each independently represents a hydrophobic portion comprising a carbon chain having 10 to 20 carbon atoms (carbon chain B), and R 22a , R 22b , R 22c , R 23c and R22d Each independently represents a hydrophilic part, R 23d Indicates the hydrophobic part or the hydrophilic part. ]
[0089] Examples of the hydrophobic part including a carbon chain (carbon chain B) having 10 to 20 carbon atoms include hydrocarbon groups such as alkyl groups. The hydrocarbon group (alkyl group, etc.) may be linear, branched, or cyclic.
[0090] The hydrophilic part may be a group having a hydrophilic group or a hydrophilic group. Examples of the hydrophilic group include (poly)oxyalkylene groups, hydroxyl groups, carboxyl groups, carboxylate groups, phosphoric acid groups, phosphate groups, sulfonic acid groups, and sulfonate groups. Examples of the (poly)oxyalkylene groups include (poly)oxyethylene groups and (poly)oxypropylene groups.
[0091] From the viewpoint of easily obtaining excellent stain resistance and softness, the nonionic surfactant B may include at least one selected from the group consisting of polyoxyalkylene alkyl ethers, fatty acid monoalkanolamides, fatty acid dialkanolamides, polyoxyalkylene dialkylamines, dipolyoxyalkylene alkylamines and polyoxyalkylene fatty acid esters, may include polyoxyalkylene alkyl ethers, and may include at least one selected from the group consisting of polyoxyethylene decyl ether, polyoxyethylene cetyl ether and polyoxyethylene stearyl ether.
[0092] The HLB value of the nonionic surfactant B is 13.0 or more. That is, in the artificial hair fiber and the fiber treatment agent of the present embodiment, at least one nonionic surfactant B having an HLB value of 13.0 or more is present. By setting the HLB value of the nonionic surfactant B to be 13.0 or more, excellent stain resistance can be obtained, and excellent softness and anti-tackiness can be easily obtained. In the artificial hair fiber and the fiber treatment agent of the present embodiment, a plurality of nonionic surfactants B having different HLB values may be present.
[0093] From the viewpoint of easily obtaining excellent stain resistance, softness and stickiness resistance, the HLB value of the nonionic surfactant B may be 13.5 or more, 14.0 or more, 14.5 or more, 15.0 or more, 15.5 or more, 16.0 or more, 16.5 or more, or 16.7 or more. From the viewpoint of easily obtaining excellent softness, the HLB value of the nonionic surfactant B may be 17.0 or more, 17.5 or more, 18.0 or more, 18.5 or more, or 19.0 or more. From the viewpoint of easily obtaining excellent stain resistance and stickiness resistance, the HLB value of the nonionic surfactant B may be 19.0 or less, 18.5 or less, 18.0 or less, 17.5 or less, 17.0 or less, or 16.7 or less. The HLB value of the nonionic surfactant B may be 16.5 or less, 16.0 or less, 15.5 or less, 15.0 or less, 14.5 or less, or 14.0 or less. From these viewpoints, the HLB value of the nonionic surfactant B may be 13.0 to 19.0, 14.0 to 19.0, 15.0 to 19.0, 16.0 to 19.0, 13.0 to 17.0, 14.0 to 17.0, 15.0 to 17.0, 16.0 to 17.0, 13.0 to 16.0 or 14.0 to 16.0. The HLB value of the nonionic surfactant B can be calculated based on the Griffin method using the formula weight of the hydrophilic part and the molecular weight of the nonionic surfactant B. For example, after extracting the nonionic surfactant B to be measured, it can be calculated based on the Griffin method after molecular weight measurement based on GPC, structural determination based on NMR, etc. The HLB value of the nonionic surfactant B can be adjusted, for example, by the length of the hydrophilic part ((poly)oxyalkylene group, etc.).
[0094] In the fiber for artificial hair of the present embodiment, the content of the cationic polymer P is 0.005 mass % or more based on the total amount of the fiber for artificial hair. When the content of the cationic polymer P is 0.005 mass % or more, excellent stain resistance can be obtained.
[0095] The content of the cationic polymer P may be in the following ranges based on the total amount of the fiber for artificial hair. From the viewpoint of easily obtaining excellent stain resistance and softness, the content of the cationic polymer P may be 0.001% by mass or more, 0.002% by mass or more, 0.005% by mass or more, 0.008% by mass or more, 0.01% by mass or more, 0.02% by mass or more, 0.05% by mass or more, 0.08% by mass or more, 0.1% by mass or more, or 0.12% by mass or more. The content of the cationic polymer P may be 0.15% by mass or more or 0.2% by mass or more. From the viewpoint of easily obtaining excellent stain resistance, softness and anti-tackiness, the content of the cationic polymer P may be 1% by mass or less, 0.8% by mass or less, 0.6% by mass or less, 0.5% by mass or less, 0.4% by mass or less, 0.3% by mass or less, 0.25% by mass or less, 0.2% by mass or less, or 0.15% by mass or less. From the viewpoint of easily obtaining excellent anti-tackiness, the content of the cationic polymer P may be 0.12% by mass or less, 0.1% by mass or less, 0.08% by mass or less, 0.05% by mass or less, 0.02% by mass or less, 0.01% by mass or less, 0.008% by mass or less, or 0.005% by mass or less. From these viewpoints, the content of the cationic polymer P may be 0.001 to 1% by mass, 0.001 to 0.3% by mass, 0.001 to 0.2% by mass, 0.001 to 0.15% by mass, 0.001 to 0.05% by mass, 0.005 to 1% by mass, 0.005 to 0.3% by mass, 0.005 to 0.2% by mass, 0.005 to 0.15% by mass, 0.005 to 0.05% by mass, 0. % by mass, 0.01-0.3% by mass, 0.01-0.2% by mass, 0.01-0.15% by mass, 0.01-0.05% by mass, 0.1-1% by mass, 0.1-0.3% by mass, 0.1-0.2% by mass, 0.1-0.15% by mass, 0.15-1% by mass, 0.15-0.3% by mass, 0.15-0.2% by mass, 0.2-1% by mass or 0.2-0.3% by mass.
[0096] In the fiber for artificial hair of the present embodiment, the content of the cationic surfactant A exceeds 0% by mass based on the total amount of the fiber for artificial hair, and may be in the following ranges. From the viewpoint of easily obtaining excellent stain resistance, softness and stickiness resistance, the content of the cationic surfactant A may be 0.001% by mass or more, 0.005% by mass or more, 0.01% by mass or more, 0.015% by mass or more, 0.02% by mass or more, 0.025% by mass or more, 0.03% by mass or more, 0.035% by mass or more, 0.038% by mass or more, 0.04% by mass or more, or 0.042% by mass or more. From the viewpoint of easily obtaining excellent stickiness resistance, the content of the cationic surfactant A may be 0.045% by mass or more or 0.05% by mass or more. From the viewpoint of easily obtaining excellent stain resistance and softness, the content of cationic surfactant A can be 1% by mass or less, 0.5% by mass or less, 0.1% by mass or less, 0.08% by mass or less, 0.05% by mass or less, 0.045% by mass or less, or 0.042% by mass or less. The content of cationic surfactant A can be 0.04% by mass or less, 0.038% by mass or less, or 0.035% by mass or less. From these viewpoints, the content of the cationic surfactant A can be 0.001 to 1 mass%, 0.001 to 0.1 mass%, 0.001 to 0.05 mass%, 0.001 to 0.045 mass%, 0.001 to 0.04 mass%, 0.01 to 1 mass%, 0.01 to 0.1 mass%, 0.01 to 0.05 mass%, 0.01 to 0.045 mass%, 0.01 to 0.04 mass%, 0.04 to 1 mass%, 0.04 to 0.1 mass%, 0.04 to 0.05 mass%, 0.04 to 0.045 mass%, 0.05 to 1 mass% or 0.05 to 0.1 mass%.
[0097] In the fiber for artificial hair of the present embodiment, the content of the nonionic surfactant B exceeds 0% by mass based on the total amount of the fiber for artificial hair, and may be in the following ranges. From the viewpoint of easily obtaining excellent stain resistance, softness and stickiness resistance, the content of the nonionic surfactant B may be 0.01% by mass or more, 0.05% by mass or more, 0.1% by mass or more, 0.2% by mass or more, 0.3% by mass or more, 0.35% by mass or more, 0.4% by mass or more, 0.45% by mass or more, 0.5% by mass or more, 0.55% by mass or more, or 0.6% by mass or more. From the viewpoint of easily obtaining excellent stickiness resistance, the content of the nonionic surfactant B may be 0.65% by mass or more or 0.7% by mass or more. From the viewpoint of easily obtaining excellent stain resistance and softness, the content of nonionic surfactant B can be 5% by mass or less, 3% by mass or less, 1% by mass or less, 0.9% by mass or less, 0.8% by mass or less, 0.75% by mass or less, 0.7% by mass or less, or 0.65% by mass or less. The content of nonionic surfactant B can be 0.6% by mass or less or 0.55% by mass or less. From these viewpoints, the content of the nonionic surfactant B can be 0.01 to 5 mass%, 0.01 to 1 mass%, 0.01 to 0.8 mass%, 0.01 to 0.7 mass%, 0.01 to 0.6 mass%, 0.1 to 5 mass%, 0.1 to 1 mass%, 0.1 to 0.8 mass%, 0.1 to 0.7 mass%, 0.1 to 0.6 mass%, 0.6 to 5 mass%, 0.6 to 1 mass%, 0.6 to 0.8 mass%, 0.6 to 0.7 mass%, 0.7 to 5 mass%, 0.7 to 1 mass% or 0.7 to 0.8 mass%.
[0098] The content of each of the cationic polymer P, the cationic surfactant A and the nonionic surfactant B can be measured by NMR, GC-MS, HPLC, FT-IR, oil extraction, solvent extraction, etc. The relative amounts of the various components of the cationic polymer P, the cationic surfactant A and the nonionic surfactant B in the hair fiber tend to be the same as those in the fiber treatment agent.
[0099] In the fiber for artificial hair of the present embodiment, the total amount of the cationic surfactant A and the nonionic surfactant B based on the total amount of the fiber for artificial hair may be in the following ranges. From the viewpoint of easily obtaining excellent stain resistance, softness and stickiness resistance, the total amount may be 0.01% by mass or more, 0.05% by mass or more, 0.1% by mass or more, 0.2% by mass or more, 0.3% by mass or more, 0.4% by mass or more, 0.45% by mass or more, 0.5% by mass or more, 0.55% by mass or more, 0.6% by mass or more, or 0.65% by mass or more. From the viewpoint of easily obtaining excellent stickiness resistance, the total amount may be 0.7% by mass or more or 0.75% by mass or more. From the viewpoint of easily obtaining excellent stain resistance and flexibility, the total amount may be 5% by mass or less, 3% by mass or less, 1% by mass or less, 0.95% by mass or less, 0.9% by mass or less, 0.85% by mass or less, 0.8% by mass or less, 0.75% by mass or less, or 0.7% by mass or less. The total amount may be 0.65% by mass or less, or 0.6% by mass or less. From these viewpoints, the total amount may be 0.01 to 5 mass%, 0.01 to 1 mass%, 0.01 to 0.8 mass%, 0.01 to 0.7 mass%, 0.01 to 0.65 mass%, 0.1 to 5 mass%, 0.1 to 1 mass%, 0.1 to 0.8 mass%, 0.1 to 0.7 mass%, 0.1 to 0.65 mass%, 0.65 to 5 mass%, 0.65 to 1 mass%, 0.65 to 0.8 mass%, 0.65 to 0.7 mass%, 0.7 to 5 mass%, 0.7 to 1 mass% or 0.7 to 0.8 mass%.
[0100] In the fiber for artificial hair of the present embodiment, the total amount of the cationic polymer P, the cationic surfactant A and the nonionic surfactant B based on the total amount of the fiber for artificial hair may be in the following ranges. From the viewpoint of easily obtaining excellent stain resistance, softness and stickiness resistance, the total amount may be 0.02 mass% or more, 0.05 mass% or more, 0.1 mass% or more, 0.2 mass% or more, 0.3 mass% or more, 0.4 mass% or more, 0.5 mass% or more, 0.6 mass% or more, 0.7 mass% or more, or 0.8 mass% or more. From the viewpoint of easily obtaining excellent stain resistance and softness, the total amount may be 0.9 mass% or more, 1 mass% or more, more than 1 mass%, 2 mass% or more, 3 mass% or more, 4 mass% or more, or 5 mass% or more. From the viewpoint of easily obtaining excellent stain resistance, softness and stickiness resistance, the total amount may be 10 mass% or less, 8 mass% or less, 6 mass% or less, or 5 mass% or less. From the viewpoint of easily obtaining excellent anti-tackiness, the total amount may be 4% by mass or less, 3% by mass or less, 2% by mass or less, 1% by mass or less, less than 1% by mass, 0.9% by mass or less, or 0.8% by mass or less. The total amount may be 0.7% by mass or less, 0.6% by mass or less, 0.5% by mass or less, 0.4% by mass or less, 0.3% by mass or less, 0.2% by mass or less, or 0.1% by mass or less. From these viewpoints, the total amount may be 0.02 to 10 mass%, 0.02 to 4 mass%, 0.02 to 1 mass%, 0.02 to 0.8 mass%, 0.02 to 0.5 mass%, 0.1 to 10 mass%, 0.1 to 4 mass%, 0.1 to 1 mass%, 0.1 to 0.8 mass%, 0.1 to 0.5 mass%, 0.5 to 10 mass%, 0.5 to 4 mass%, 0.5 to 1 mass%, 0.5 to 0.8 mass%, 0.8 to 10 mass%, 0.8 to 4 mass%, 0.8 to 1 mass%, 1 to 10 mass% or 1 to 5 mass%.
[0101] In the fiber for artificial hair and the fiber treatment agent of the present embodiment, the mass ratio R1 of the content of the cationic polymer P to the content of the cationic surfactant A (content of the cationic polymer P / content of the cationic surfactant A) may be in the following ranges. From the viewpoint of easily obtaining excellent stain resistance and softness, the mass ratio R1 may be 0.01 or more, 0.05 or more, 0.1 or more, 0.5 or more, 1 or more, 1.5 or more, 2 or more, 2.5 or more, or 3 or more. The mass ratio R1 may be 3.5 or more, 4 or more, 4.5 or more, 5 or more, 5.5 or more, 6 or more, 6.5 or more, or 7 or more. From the viewpoint of easily obtaining excellent stain resistance, softness, and anti-tackiness, the mass ratio R1 may be 50 or less, 30 or less, 20 or less, 10 or less, 8 or less, 7 or less, 6.5 or less, 6 or less, 5.5 or less, 5 or less, 4.5 or less, 4 or less, 3.5 or less, or 3 or less. From the viewpoint of easily obtaining excellent anti-tackiness, the mass ratio R1 may be 2 or less, 1.5 or less, 1 or less, 0.5 or less, or 0.1 or less. From these viewpoints, the mass ratio R1 may be 0.01 to 50, 0.01 to 10, 0.01 to 5, 0.01 to 3, 0.01 to 1, 0.1 to 50, 0.1 to 10, 0.1 to 5, 0.1 to 3, 0.1 to 1, 1 to 50, 1 to 10, 1 to 5, 1 to 3, 3 to 50, 3 to 10, 3 to 5, 5 to 50, or 5 to 10.
[0102] In the fiber for artificial hair and the fiber treatment agent of the present embodiment, the mass ratio R2 of the content of the cationic polymer P to the content of the nonionic surfactant B (content of the cationic polymer P / nonionic surfactant B) may be in the following ranges. From the viewpoint of easily obtaining excellent stain resistance and softness, the mass ratio R2 may be 0.001 or more, 0.005 or more, 0.01 or more, 0.05 or more, 0.1 or more, 0.15 or more, or 0.2 or more. The mass ratio R2 may be 0.25 or more, 0.3 or more, 0.33 or more, 0.35 or more, 0.4 or more, or 0.45 or more. From the viewpoint of easily obtaining excellent stain resistance, softness, and anti-tackiness, the mass ratio R2 may be 5 or less, 3 or less, 1 or less, 0.8 or less, 0.5 or less, 0.45 or less, 0.4 or less, 0.35 or less, 0.33 or less, 0.3 or less, 0.25 or less, or 0.2 or less. From the viewpoint of easily obtaining excellent anti-tackiness, the mass ratio R2 may be 0.15 or less, 0.1 or less, 0.05 or less, or 0.01 or less. From these viewpoints, the mass ratio R2 may be 0.001 to 5, 0.001 to 0.5, 0.001 to 0.3, 0.001 to 0.2, 0.001 to 0.1, 0.01 to 5, 0.01 to 0.5, 0.01 to 0.3, 0.01 to 0.2, 0.01 to 0.1, 0.1 to 5, 0.1 to 0.5, 0.1 to 0.3, 0.1 to 0.2, 0.2 to 5, 0.2 to 0.5, 0.2 to 0.3, 0.3 to 5, or 0.3 to 0.5.
[0103] In the artificial hair fiber and the fiber treatment agent of the present embodiment, the mass ratio R3 of the content of the cationic surfactant A to the content of the nonionic surfactant B (content of the cationic surfactant A / content of the nonionic surfactant B) can be in the following ranges from the viewpoint of easily obtaining excellent stain resistance, softness and anti-tackiness. The mass ratio R3 can be 0.01 or more, 0.03 or more, 0.05 or more, 0.06 or more, or 0.07 or more. The mass ratio R3 can be 1 or less, 0.5 or less, 0.1 or less, 0.09 or less, 0.08 or less, or 0.07 or less. From these viewpoints, the mass ratio R3 may be 0.01 to 1, 0.03 to 1, 0.05 to 1, 0.07 to 1, 0.01 to 0.1, 0.03 to 0.1, 0.05 to 0.1, 0.07 to 0.1, 0.01 to 0.07, 0.03 to 0.07, or 0.05 to 0.07.
[0104] In the fiber for artificial hair and the fiber treatment agent of the present embodiment, the mass ratio R4 of the total amount of the cationic surfactant A and the nonionic surfactant B to the content of the cationic polymer P ((total amount of the cationic surfactant A and the nonionic surfactant B) / content of the cationic polymer P) may be in the following ranges. From the viewpoint of easily obtaining excellent stain resistance, softness and stickiness resistance, the mass ratio R4 may be more than 0, 0.1 or more, 0.5 or more, 1 or more, 1.5 or more, 2 or more, 2.5 or more, 3 or more, 3.5 or more, 4 or more, 4.5 or more, 5 or more, or 5.3 or more. From the viewpoint of easily obtaining excellent stickiness resistance, the mass ratio R4 may be 5.5 or more, 6 or more, 8 or more, 10 or more, 50 or more, 100 or more, 150 or more, or 160 or more. From the viewpoint of easily obtaining excellent stain resistance and flexibility, the mass ratio R4 may be 300 or less, 250 or less, 200 or less, 160 or less, 150 or less, 100 or less, 50 or less, 10 or less, 8 or less, 6 or less, 5.5 or less, or 5.3 or less. The mass ratio R4 may be 5 or less, 4.5 or less, 4 or less, 3.5 or less, 3 or less, or 2.5 or less. From these viewpoints, the mass ratio R4 may be more than 0 and less than 300, more than 0 and less than 160, more than 0 and less than 10, more than 0 and less than 6, more than 0 and less than 4, more than 0 and less than 3, 1 to 300, 1 to 160, 1 to 10, 1 to 6, 1 to 4, 1 to 3, 3 to 300, 3 to 160, 3 to 10, 3 to 6, 3 to 4, 4 to 300, 4 to 160, 4 to 10, 4 to 6, 10 to 300, or 10 to 160.
[0105] In the fiber treatment agent of the present embodiment, the content of the cationic polymer P can be the following ranges based on the total amount of the fiber treatment agent. From the viewpoint of easily obtaining excellent stain resistance and softness, the content of the cationic polymer P can be 0.06% by mass or more, 0.1% by mass or more, 0.5% by mass or more, 1% by mass or more, 2% by mass or more, or 3% by mass or more. The content of the cationic polymer P can be 4% by mass or more, 5% by mass or more, 6% by mass or more, or 7% by mass or more. From the viewpoint of easily obtaining excellent stain resistance, softness, and anti-stickiness, the content of the cationic polymer P can be 20% by mass or less, 15% by mass or less, 10% by mass or less, 8% by mass or less, 7% by mass or less, 6% by mass or less, 5% by mass or less, 4% by mass or less, or 3% by mass or less. From the viewpoint of easily obtaining excellent anti-stickiness, the content of the cationic polymer P can be 2% by mass or less, 1% by mass or less, 0.5% by mass or less, or 0.1% by mass or less. From these viewpoints, the content of the cationic polymer P can be 0.06 to 20 mass%, 0.06 to 8 mass%, 0.06 to 5 mass%, 0.06 to 3 mass%, 0.06 to 1 mass%, 0.1 to 20 mass%, 0.1 to 8 mass%, 0.1 to 5 mass%, 0.1 to 3 mass%, 0.1 to 1 mass%, 1 to 20 mass%, 1 to 8 mass%, 1 to 5 mass%, 1 to 3 mass%, 3 to 20 mass%, 3 to 8 mass%, 3 to 5 mass%, 5 to 20 mass% or 5 to 8 mass%.
[0106] In the fiber treatment agent of the present embodiment, the content of the cationic surfactant A exceeds 0% by mass based on the total amount of the fiber treatment agent. From the viewpoint of easily obtaining excellent stain resistance, softness and stickiness resistance, it can be the following range. The content of the cationic surfactant A can be 0.1% by mass or more, 0.3% by mass or more, 0.4% by mass or more, 0.5% by mass or more, 0.8% by mass or more, or 1% by mass or more. The content of the cationic surfactant A can be 10% by mass or less, 8% by mass or less, 5% by mass or less, 3% by mass or less, 2% by mass or less, or 1% by mass or less. From these viewpoints, the content of the cationic surfactant A can be 0.1-10% by mass, 0.1-5% by mass, 0.1-3% by mass, 0.1-1% by mass, 0.5-10% by mass, 0.5-5% by mass, 0.5-3% by mass, 0.5-1% by mass, 1-10% by mass, 1-5% by mass, or 1-3% by mass.
[0107] In the fiber treatment agent of the present embodiment, the content of the nonionic surfactant B exceeds 0% by mass based on the total amount of the fiber treatment agent. From the viewpoint of easily obtaining excellent stain resistance, softness and stickiness resistance, it can be the following range. The content of the nonionic surfactant B can be 1% by mass or more, 3% by mass or more, 5% by mass or more, 6% by mass or more, 8% by mass or more, 10% by mass or more, 12% by mass or more, or 15% by mass or more. The content of the nonionic surfactant B can be 40% by mass or less, 35% by mass or less, 30% by mass or less, 25% by mass or less, 20% by mass or less, or 15% by mass or less. From these viewpoints, the content of the nonionic surfactant B can be 1 to 40% by mass, 1 to 20% by mass, 1 to 15% by mass, 5 to 40% by mass, 5 to 20% by mass, 5 to 15% by mass, 10 to 40% by mass, 10 to 20% by mass, or 10 to 15% by mass.
[0108] In the fiber treatment agent of the present embodiment, from the viewpoint of easily obtaining excellent stain resistance, softness and anti-tackiness, the water content can be in the following ranges based on the total amount of the fiber treatment agent. The water content can be 50% by mass or more, 55% by mass or more, 60% by mass or more, 65% by mass or more, 70% by mass or more, or 75% by mass or more. The water content can be 95% by mass or less, 90% by mass or less, 85% by mass or less, or 80% by mass or less. From these viewpoints, the water content can be 50-95% by mass, 50-90% by mass, 50-80% by mass, 70-95% by mass, 70-90% by mass, or 70-80% by mass.
[0109] The fiber for artificial hair of the present embodiment may have other additives (components not belonging to the cationic polymer P, the cationic surfactant A or the nonionic surfactant B) present on at least a part of the surface of the base fiber, and the fiber treatment agent of the present embodiment may have other additives (components not belonging to the cationic polymer P, the cationic surfactant A or the nonionic surfactant B). Examples of such additives include cationic polymers not belonging to the cationic polymer P, cationic surfactants not belonging to the cationic surfactant A, nonionic surfactants not belonging to the nonionic surfactant B, pH adjusters (e.g., citric acid), antibacterial agents, deodorizing agents, antifungal agents, UV blockers, softeners, SR agents, aromatic agents, flame retardants, defoaming agents, and fragrances. In the fiber for artificial hair of the present embodiment, at least one selected from the group consisting of zeolite and zirconium carbide may not be present on the surface of the base fiber, and the base fiber may not contain at least one selected from the group consisting of zeolite and zirconium carbide. In the artificial hair fiber of this embodiment, alcohol consisting only of carbon atoms, hydrogen atoms and oxygen atoms may not exist on the surface of the base fiber, and the fiber treatment agent of this embodiment may not contain alcohol consisting only of carbon atoms, hydrogen atoms and oxygen atoms.
[0110] In the method for producing the artificial hair fiber of the present embodiment, the fiber treatment agent of the present embodiment is brought into contact with the surface of the base fiber. That is, the method for producing the artificial hair fiber of the present embodiment includes a fiber treatment step of bringing the fiber treatment agent of the present embodiment into contact with the surface of the base fiber.
[0111] In the fiber treatment process, the fiber treatment agent may be applied to at least a portion of the surface of the substrate fiber. In this case, a conventionally known method of applying a liquid to the fiber may be used. For example, there may be mentioned: a method of applying the fiber treatment agent to the substrate fiber using a roller having a surface to which the fiber treatment agent is attached (roller transfer method); a method of immersing the substrate fiber in a liquid tank storing the fiber treatment agent (immersion method); a method of spreading the fiber treatment agent on the substrate fiber; a method of attaching the fiber treatment agent to the substrate fiber via an application tool such as a brush or bristles, etc. For example, in the immersion method, the amount of the fiber treatment agent applied may be adjusted by adjusting the number of applications, the content of the active ingredient in the fiber treatment agent, etc.
[0112] The method for producing the fiber for artificial hair of the present embodiment may include a spinning step of obtaining the base fiber by spinning the composition of the material containing the base fiber before the fiber treatment step. In the spinning step, the composition of the material containing the base fiber may be melt-spun (melt-deformed).
[0113] The manufacturing method of the fiber for artificial hair of the present embodiment can be provided with a kneading step of melt-kneading the composition of the material containing the base material fiber before the spinning step. As the device for melt-kneading, various general kneading machines can be used. As the kneading machine, single-screw extruder, twin-screw extruder, roller, Banbury mixer, kneading machine etc. can be cited.
[0114] The method for producing the fiber for artificial hair of the present embodiment may include a stretching step of stretching the yarn (unstretched yarn) obtained in the spinning step before the fiber treatment step.
[0115] From the viewpoint of easily showing the strength of the fiber, the stretching ratio in the stretching process may be 1.5 times or more or 2.0 times or more. From the viewpoint of not easily causing the breakage of the fiber during the stretching process, the stretching ratio may be 5.0 times or less or 4.0 times or less. From these viewpoints, the stretching ratio may be 1.5 to 5.0 times or 2.0 to 4.0 times.
[0116] The stretching treatment may be performed by a two-step method in which the unstretched yarn is temporarily wound on a bobbin and then stretched in a step not continuous with the spinning step, or by a direct spinning stretching method in which the unstretched yarn is not wound on a bobbin but stretched in a step continuous with the spinning step. The stretching treatment may be performed by a single-stage stretching method in which the unstretched yarn is stretched once to a target stretching ratio, or by a multi-stage stretching method in which the unstretched yarn is stretched twice or more to a target stretching ratio.
[0117] The temperature of the stretching treatment may be 80° C. to 120° C. When the temperature is 80° C. or higher, it is easy to ensure sufficient fiber strength and fiber breakage is unlikely to occur. When the temperature is 120° C. or lower, it is easy to obtain a suitable feel of the fiber.
[0118] The method for producing the fiber for artificial hair of the present embodiment may include a heat treatment step of heat-treating (annealing) the yarn (drawn yarn) obtained in the drawing step after the drawing step. The heat treatment step can reduce the thermal shrinkage of the drawn yarn. The heat treatment step may be performed before the fiber treatment step.
[0119] The heat treatment temperature may be 100° C. or higher or 110° C. or higher. The heat treatment temperature may be 200° C. or lower or 150° C. or lower. The heat treatment may be performed continuously after the stretching treatment or after temporary winding.
[0120] The method for producing the fiber for artificial hair of the present embodiment may include a step of processing the yarn (drawing the yarn) after the heat treatment step. In the processing step, for example, the yarn may be subjected to shaping. The heat treatment step may be performed before or after the fiber treatment step.
[0121] The hair accessories of this embodiment include the artificial hair fibers of this embodiment. The hair accessories of this embodiment are detachable from the head, and may be in a form composed of the artificial hair fibers of this embodiment (e.g., a fiber bundle of artificial hair fibers). Examples of the hair accessories include wigs, hair wigs, wig pieces, wig braids, extension pieces, artificial hair bundles, and the like.
[0122] Example
[0123] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited to these Examples.
[0124] <Preparation of base fiber>
[0125] As the base fiber, the following fibers were prepared.
[0126] Base fiber A: Polyvinyl chloride (Taiyo Vinyl Chloride Co., Ltd., trade name "TH-700") fiber, with a cross-sectional moment of 10 × 10 -4 mm 4 Fibers spun from a nozzle with an outlet cross-section of 100 mm (fibers produced by a solution spinning method), with an average fineness of 40 to 70 dtex (average fineness of 100 fibers)
[0127] Base fiber B: Fibers made of acrylonitrile-styrene copolymer (Denka Co., Ltd., trade name "GR-AT-6S"), with a cross-sectional moment of 10 × 10 -4 mm 4 Fibers spun from a nozzle with an outlet cross-section of 100 mm (fibers produced by a solution spinning method), with an average fineness of 40 to 70 dtex (average fineness of 100 fibers)
[0128] Base fiber C: PET (Mitsui Chemicals, Inc., trade name "J125S") fiber, with a cross-sectional moment of 10 × 10 -4 mm 4 Fibers spun from a nozzle with an outlet cross-section of 100 mm (fibers produced by melt spinning), with an average fineness of 40 to 70 dtex (average fineness of 100 fibers)
[0129] Base fiber D: A fiber made of a polyamide resin (Asahi Kasei Chemicals Corporation, trade name "Leona 1500") having a weak axis and a second moment of cross section of 10 × 10 -4 mm 4 Fibers spun from a nozzle with an outlet cross-section of 100 mm (fibers produced by a solution spinning method), with an average fineness of 40 to 70 dtex (average fineness of 100 fibers)
[0130] Base fiber E: Polypropylene (Sumitomo Chemical Co., Ltd., trade name "Sumitomo Noblen S131") fiber, with a second moment of cross section of 10 × 10 -4 mm 4 Fibers spun from a nozzle with an outlet cross-section of 100 mm (fibers produced by melt spinning), with an average fineness of 40 to 70 dtex (average fineness of 100 fibers)
[0131] Base fiber F: A fiber made of vinyl chloride-acrylonitrile copolymer (copolymerization ratio 50:50, weight average molecular weight 80,000 to 130,000) with a cross-sectional moment of 10 × 10 -4 mm 4 Fibers spun from a nozzle with an outlet cross section of 100 mm (fibers produced by a solution spinning method), with an average fineness of 40 to 70 dtex (average fineness of 100 fibers)
[0132] <Preparation of fiber treatment agent>
[0133] The fiber treatment agent was prepared by mixing a cationic polymer, a surfactant shown in Tables 1 to 3, citric acid and water. The contents of the cationic polymer, surfactant, citric acid and water in the fiber treatment agent are shown in each table as the content based on the total amount of the fiber treatment agent. The contents of the cationic polymer, cationic surfactant and nonionic surfactant are the contents as active ingredients. As the cationic polymer and surfactant, the following reagents were used.
[0134] (Cationic polymer)
[0135] A polymer having a weight average molecular weight of 20,000 to 50,000, 2-(dimethylamino)ethyl methacrylate 50 to 95% by mass and ethyl methacrylate 5 to 50% by mass as monomer units (the content of the monomer units is based on the total amount of the monomer units constituting the polymer)
[0136] (Cationic surfactant)
[0137] ·Tetradecyltrimethylammonium chloride: carbon number 24, our company's product
[0138] Mixture of behenyltrimethylammonium chloride and isopropyl alcohol: Toho Chemical Co., Ltd., trade name "CATINAL DC-80", carbon chain carbon number 22, active ingredient content about 80%
[0139] · A mixture of stearyl trimethyl ammonium chloride, isopropyl alcohol, and water: Carbon chain number 18, Toho Chemical Co., Ltd., trade name "Catinal STC-25W", active ingredient content about 25%
[0140] · Aqueous solution of hexadecyltrimethylammonium chloride: carbon number 16, Nikko Chemical Co., Ltd., trade name "CA-2330", active ingredient content about 29%
[0141] · Dodecyltrimethylammonium chloride aqueous solution: carbon chain carbon number 12, Toho Chemical Industry Co., Ltd., trade name "Catinal LTC-35A", active ingredient content about 35%
[0142] (Nonionic surfactant)
[0143] · Polyoxyethylene behenyl ether: carbon chain carbon number 22, HLB 16.1, Aoki Oil & Fats Industry Co., Ltd., trade name "BLAUNON BE-30"
[0144] · Polyoxyethylene stearyl ether: carbon number of the carbon chain is 18, HLB 16.0, prepared by our company
[0145] · Polyoxyethylene hexadecyl ether: carbon number of the carbon chain is 16, HLB 19.0, prepared by our company
[0146] · Polyoxyethylene cetyl ether: carbon number of the carbon chain is 16, HLB 16.7, Aoki Oil & Fats Industry Co., Ltd., trade name "BLAUNON CH-330L"
[0147] · Polyoxyethylene cetyl ether: carbon chain carbon number 16, HLB 14.3, Aoki Oil & Fats Industry Co., Ltd., trade name "BLAUNON CH-315L"
[0148] · Polyoxyethylene hexadecyl ether: carbon number of the carbon chain is 16, HLB 12.0, prepared by our company
[0149] · Polyoxyethylene decyl ether: carbon number of the carbon chain is 10, HLB 16.0, prepared by our company
[0150] ·Polyoxyethylene octyl ether: carbon number of carbon chain 8, HLB 16.0, prepared by our company
[0151] <Production of Evaluation Fiber>
[0152] After the above-mentioned base fiber is stretched at 100°C, the above-mentioned fiber treatment agent is applied to the base fiber by a roller transfer method. As the conditions for roller transfer, the radius of the roller is 125 mm, the roller is immersed in the fiber treatment agent from the lower end of the roller to a height of 20 mm, and the roller speed is 0.2 to 8 m / min. Then, annealing is performed at 110°C to obtain an evaluation fiber with a single fineness of 20 to 100 dtex. The stretching ratio is 3.25 times, and the relaxation rate during annealing is 25%. The relaxation rate during annealing is a value calculated by "(the circumference of the nearest part of the roller outlet of the annealing furnace) / (the circumference of the nearest part of the roller inlet of the annealing furnace)". The content of the active ingredient in the evaluation fiber is adjusted by the content of the active ingredient in the fiber treatment agent, the roller speed in the roller transfer method, etc.
[0153] As the content of the effective ingredients in the evaluation fiber, the amount of cationic polymer and surfactant attached to the surface of the evaluation fiber was calculated (unit: mass %). The relative amounts of the various components of the cationic polymer, cationic surfactant and nonionic surfactant in the evaluation fiber tend to be the same as the relative amounts in the fiber treatment agent, so the attachment amount was calculated by the following formula based on the solid content extracted from the evaluation fiber using the warm water extraction method. The mass ratio of the total amount of effective ingredients (the total amount of cationic polymer, cationic surfactant and nonionic surfactant), the total amount of surfactants (the total amount of cationic surfactant and nonionic surfactant) to the content of cationic polymer, and the content of cationic polymer are shown in each table.
[0154] Adhesion amount [mass %] = (mass of extracted solid content [g] / mass of evaluation fiber before extraction [g]) × (effective ingredient amount of evaluation item in fiber treatment agent [mass %] / effective ingredient amount of all components in fiber treatment agent [mass %]) × 100
[0155] In the above-mentioned warm water extraction method, first, weigh 20g of the evaluation fiber into a 300mL beaker, and then add 200mL of pure water. Next, place the beaker in a constant temperature bath at 80°C, stir and mix with a glass rod every hour, and perform the extraction operation for a total of 4 hours to obtain an evaluation sample. Then, filter the evaluation sample with No.5A filter paper, and wash the beaker, evaluation sample and filter paper twice with a total of 100mL of water. The moisture of the obtained filtrate is dried and solidified at 80°C. The mass of the dry solid after complete removal of moisture is obtained as the mass of the extracted solid component.
[0156] <Evaluation of Evaluation Fiber>
[0157] After the evaluation fibers were shaped into a wave shape, the stain resistance, flexibility and stickiness resistance were evaluated. As the shaping process, a gear machine (NEW YAKI BRAID CRIMPING M / C-2.5mm / SUNG JIN INDUSTRIAL CO., LTD.) was used to perform a buffing process under the conditions of a gear pitch of 2.5mm, preheating at 90°C, a gear roller temperature of 90°C, and a gear roller speed of 1m / m. The results are shown in the tables.
[0158] (Pollution resistance)
[0159] With reference to the pollen release test QTEC method of the Japan Fiber Products Quality Technology Center, the stain resistance was evaluated according to the following steps. First, the above-mentioned evaluation fibers (after shaping) were bundled to obtain a fiber bundle with a length of 40 mm and a mass of 0.4 g. Next, 0.25 g of dust (simulated dust, Riren Co., Ltd., trade name "Test (Cotton) Dust") was added to container A (cylindrical bottle) and stirred. Next, 5 of the above-mentioned fiber bundles and wooden balls were placed in container A. Then, container A was placed in the rotating box used in the JIS L1076A method, and the rotating box was rotated using a pilling tester, so that the dust adhered to the fiber filaments.
[0160] Next, after the fiber bundles are taken out from the container A, three fiber bundles are selected in which dust is visually uniformly attached. For the three fiber bundles, the ratio A (average value of the three fiber bundles) of the total area (projected area) of dust to the area (projected area) of the portion constituting the fiber bundle is visually calculated.
[0161] Next, the fiber bundle is held with a support mounted on a bracket with the longitudinal direction of the fiber bundle facing the vertical direction, thereby fixing the fiber bundle at a height of 20 cm from the support platform. Next, the fiber bundle is dropped by leaving the support. This operation is repeated for a total of 5 times for each of the 3 fiber bundles. For the 3 fiber bundles, the area ratio B (the average value of the 3 fiber bundles) is calculated in the same manner as above. As the pollution resistance, the dust detachment rate (unit: %) is calculated by the following formula. It can be judged that the greater the dust detachment rate, the easier the dust is to detach, and the better the pollution resistance.
[0162] Detachment rate = [(ratio A - ratio B) / ratio A] × 100
[0163] (Softness)
[0164] The above-mentioned evaluation fibers (after shaping) were bundled to obtain a fiber bundle having a length of 600 mm and a mass of 120 g. The softness was evaluated on two levels of "soft" and "hard" by the hand feel (softness felt when touching the fiber bundle in a compressed manner with the palm) of 10 hair fiber processing technicians (with more than 5 years of practical experience), and the softness was evaluated according to the following criteria.
[0165] A: More than 9 people rated it as soft
[0166] B: 5 to 8 people rated it as soft
[0167] C: 0 to 4 people rated it as soft
[0168] (Resistance to stickiness)
[0169] The above-mentioned evaluation fibers (after shaping) were bundled to obtain a fiber bundle having a length of 600 mm and a mass of 120 g. Ten hair fiber treatment technicians (with more than 5 years of practical experience) were asked to grade the fiber bundle by hand feel (the degree of stickiness felt when the fiber bundle was touched by hand compression) into two levels: "non-sticky" and "sticky", and then the stickiness resistance was evaluated according to the following criteria.
[0170] A: More than 9 people rated it as not sticky
[0171] B: 5 to 8 people rated it as not sticky
[0172] C: 0 to 4 people rated it as not sticky
[0173] [Table 1]
[0174]
[0175] [Table 2]
[0176]
[0177] [Table 3]
[0178]
Claims
1. A fiber for artificial hair, comprising a base fiber, a cationic polymer, a cationic surfactant and a nonionic surfactant, The cationic polymer, the cationic surfactant, and the nonionic surfactant are present on at least a portion of the surface of the base fiber. The cationic polymer comprises a monomer as a monomer unit, wherein the monomer has at least one selected from the group consisting of a primary amino group, a secondary amino group, a tertiary amino group, an acid neutralizing group thereof, and a quaternary ammonium group. The cationic surfactant has a carbon chain with 12 to 22 carbon atoms. The nonionic surfactant has a carbon chain with 10 to 20 carbon atoms. The HLB value of the nonionic surfactant is greater than 13.0, The content of the cationic polymer is 0.005 mass % or more based on the total amount of the fiber for artificial hair.
2. The fiber for artificial hair according to claim 1, in, The base fiber includes at least one selected from the group consisting of a homopolymer of vinyl chloride, a vinyl chloride-acrylonitrile copolymer, polyethylene terephthalate, a polyamide-based resin, polypropylene, and an acrylonitrile-styrene copolymer.
3. The fiber for artificial hair according to claim 1, in, The cationic polymer further comprises an alkyl (meth)acrylate as a monomer unit.
4. The fiber for artificial hair according to claim 1, in, The cationic surfactant comprises a quaternary ammonium salt of a cation having a structure represented by the following general formula (1): In formula (1), R 11 represents a group containing a carbon chain having 12 to 22 carbon atoms, R 12 , R 13 and R 14 Each independently represents a monovalent group.
5. The fiber for artificial hair according to claim 1, in, The carbon number of the carbon chain of the cationic surfactant is 18 to 22.
6. The fiber for artificial hair according to claim 1, in, The HLB value of the nonionic surfactant is 13.0 to 19.
0.
7. The fiber for artificial hair according to claim 1, in, The nonionic surfactant includes a polyoxyalkylene alkyl ether.
8. The fiber for artificial hair according to claim 1, in, The content of the cationic polymer is 0.005 to 0.2% by mass based on the total amount of the fiber for artificial hair.
9. The fiber for artificial hair according to claim 1, in, The mass ratio of the total amount of the cationic surfactant and the nonionic surfactant to the content of the cationic polymer is 3 to 160.
10. The fiber for artificial hair according to claim 1, in, The total amount of the cationic polymer, the cationic surfactant and the nonionic surfactant is 0.1 to 4% by mass based on the total amount of the artificial hair fiber.
11. A hair accessories comprising the fiber for artificial hair according to any one of claims 1 to 10.