Light-absorbing anisotropic layer, method for producing light-absorbing anisotropic layer, laminate, and image display device
By using dichroic substances and liquid crystal compounds in the light absorption anisotropic layer, and performing in-plane diffraction measurement and ultraviolet irradiation under specific conditions, the haze problem in the image display device is solved, and higher transparency is achieved and durability.
Patent Information
- Application Number
- CN202380025961.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-22
- Publication Date
- 2024-11-15
AI Technical Summary
The conventional light absorption anisotropic layer has a haze problem in the image display device, and it is difficult to effectively suppress its occurrence.
By using dichroic substances and liquid crystal compounds in the light absorption anisotropic layer and in-plane diffraction method to measure the X-ray diffraction pattern under specific conditions, the light absorption anisotropic layer structure that meets the specific peak intensity relationship, combined with ultraviolet rays The irradiation formation and curing process suppresses the occurrence of haze.
The haze generation of the light-absorbing anisotropic layer is effectively suppressed, the transparency and durability of the laminated body are improved, and the precipitation of dichromatic substances is reduced.
Smart Images

Figure CN118974608A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a light absorption anisotropic layer, a method for manufacturing the light absorption anisotropic layer, a laminate and an image display device. Background Art
[0002] In the past, when the attenuation function, polarization function, scattering function or light shielding function of the irradiated light including laser beam or natural light was required, a device operating according to a different principle for each function was used. Therefore, the products corresponding to the above functions were also manufactured through different manufacturing processes for each function.
[0003] For example, in image display devices (eg, liquid crystal display devices), linear polarizers or circular polarizers are used to control optical rotation or birefringence in display, and in organic light emitting diodes (OLEDs), circular polarizers are also used to prevent reflection of external light.
[0004] Conventionally, iodine has been widely used as a dichroic substance in these polarizers, but studies have been conducted on polarizers using an organic dye as a dichroic substance instead of iodine.
[0005] For example, Patent Document 1 describes a polarizing layer (light absorption anisotropic layer) formed of a composition containing a polymerizable smectic liquid crystal compound and a dichroic dye (see [Claim 1]).
[0006] Previous technical literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2019-049758 Summary of the invention
[0009] Technical issues to be solved by the invention
[0010] The present inventors have studied the light absorption anisotropic layer described in Patent Document 1 and have found that haze occurs and there is room for improvement.
[0011] Therefore, an object of the present invention is to provide a light absorption anisotropic layer in which the generation of haze is suppressed, a method for producing the same, a laminate using the light absorption anisotropic layer, and an image display device.
[0012] Means for solving technical problems
[0013] As a result of intensive research conducted by the present inventors to solve the above-mentioned problems, it was discovered that when the X-ray diffraction pattern is measured using the in-plane diffraction method, a light absorption anisotropic layer whose peak intensity value of the diffracted X-rays at specified positions (2 places) satisfies a specific relationship can suppress the generation of haze, thereby completing the present invention.
[0014] That is, the present inventors have found that the above-mentioned problems can be solved by the following configuration.
[0015] [1] A light absorption anisotropic layer comprising a dichroic substance and a liquid crystal compound, wherein:
[0016] When the light absorbing anisotropic layer is irradiated with X-rays and the X-ray diffraction pattern is measured using the in-plane diffraction method, the diffracted X-rays are measured in the following measurement area to determine the diffraction angle 2θmax and the rotation angle φmax at which the peak intensity becomes maximum. When the peak intensity of the diffraction X-rays at the diffraction angle 2θmax and the rotation angle φmax is set to I(φmax) and the peak intensity of the diffraction X-rays at the diffraction angle 2θmax and the rotation angle φmax-10° is set to I(φmax-10), the relationship of the following formula (1) is satisfied.
[0017] Measurement area:
[0018] · Rotation angle φ of the in-plane direction of the light absorption anisotropic layer: 0 to 180°
[0019] Diffraction angle 2θ: 0~10°
[0020] Formula (1):
[0021] I(φmax) / I(φmax-10)≥1.6
[0022] [2] The light absorption anisotropic layer according to [1], wherein
[0023] When the light absorption anisotropic layer is fixed at a rotation angle of φmax-90° and the diffraction angle 2θ is measured in a range of more than 10° and less than 30°, a peak of diffracted X-rays showing a peak intensity of I(φmax)×0.2 or more is observed.
[0024] [3] The light absorption anisotropic layer according to [1] or [2], wherein
[0025] The light absorption anisotropic layer is formed using a liquid crystal composition containing a dichroic substance, a liquid crystal compound and a monofunctional compound.
[0026] The molecular length of the long axis of the liquid crystal compound The molecular length in the direction of the long axis of the monofunctional compound The relationship of the following formula (2) is satisfied.
[0027] Formula (2):
[0028] 0.2×D1≤D2≤0.45×D1
[0029] [4] The light absorption anisotropic layer according to any one of [1] to [3], wherein
[0030] The dichroic substance includes at least two dichroic substances having maximum absorption wavelengths in the wavelength range of 550 to 700 nm.
[0031] [5] A method for producing a light absorption anisotropic layer, which is the method for producing the light absorption anisotropic layer according to any one of [1] to [4], comprising:
[0032] In the light absorption anisotropic layer forming step, a liquid crystal composition layer including a dichroic substance, a liquid crystal compound, and a monofunctional compound is irradiated with ultraviolet rays in air to form a light absorption anisotropic layer.
[0033] [6] The method for producing a light absorption anisotropic layer according to [5], comprising the following steps:
[0034] The optically anisotropic layer after the light absorption anisotropic layer forming step was irradiated with ultraviolet rays under nitrogen.
[0035] [7] A laminate comprising the light absorption anisotropic layer according to any one of [1] to [4] and a λ / 4 plate provided on the light absorption anisotropic layer.
[0036] [8] An image display device comprising the light absorption anisotropic layer according to any one of [1] to [4] or the laminate according to [7].
[0037] Effects of the Invention
[0038] According to the present invention, it is possible to provide a light absorption anisotropic layer in which generation of haze is suppressed, a method for producing the same, a laminate using the light absorption anisotropic layer, and an image display device. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a schematic conceptual diagram for explaining a measurement region when measuring an X-ray diffraction pattern of a light absorption anisotropic layer by an in-plane diffraction method. DETAILED DESCRIPTION
[0040] Hereinafter, the present invention will be described in detail.
[0041] The description of the constituent elements described below is based on typical embodiments of the present invention, but the present invention is not limited to these embodiments.
[0042] In addition, in this specification, the numerical range expressed using "to" means a range including the numerical values described before and after "to" as the lower limit and the upper limit.
[0043] In addition, in this specification, regarding each component, one substance corresponding to each component can be used alone, or two or more substances can be used simultaneously. Here, regarding each component, when two or more substances are used simultaneously, unless otherwise specified, the content of the component refers to the total content of the substances used simultaneously.
[0044] [Light absorption anisotropic layer]
[0045] The light absorption anisotropic layer of the present invention is a light absorption anisotropic layer containing a dichroic substance and a liquid crystal compound.
[0046] Furthermore, when the light absorption anisotropic layer of the present invention is irradiated with X-rays and the X-ray diffraction pattern is measured by the in-plane diffraction method, first, the diffracted X-rays are measured in the following measurement area to determine the diffraction angle 2θmax and the rotation angle φmax at which the peak intensity becomes the maximum, and then, when the peak intensity of the diffracted X-rays at the diffraction angle 2θmax and the rotation angle φmax is set to I(φmax) and the peak intensity of the diffracted X-rays at the diffraction angle 2θmax and the rotation angle φmax-10° is set to I(φmax-10), the relationship of the following formula (1) is satisfied. In addition, the peak value at which the peak intensity becomes the maximum is also simply referred to as "peak P1".
[0047] Measurement area:
[0048] · Rotation angle φ of the in-plane direction of the light absorption anisotropic layer: 0 to 180°
[0049] Diffraction angle 2θ: 0~10°
[0050] Formula (1):
[0051] I(φmax) / I(φmax-10)≥1.6
[0052] Figure 1 2 is a schematic conceptual diagram for explaining a measurement region when measuring an X-ray diffraction pattern of a light absorption anisotropic layer by an in-plane diffraction method.
[0053] like Figure 1As shown, in the measurement of the X-ray diffraction pattern based on the in-plane diffraction method, the incident X-ray 4 is made to be incident at an angle of incidence that is approximately parallel (greater than 0° and less than 1°) to the surface of the light absorption anisotropic layer 1, and the diffraction angle 2θ (the angle formed by the reflected X-ray 5 and the diffracted X-ray) of the diffracted X-ray 6 is measured using a detector, thereby evaluating the regularity of the arrangement structure (diffraction plane 2) of the liquid crystal compound 2.
[0054] In the present invention, in the measurement of the diffracted X-rays in the above-mentioned measurement area, the value of the peak intensity when measured under the following conditions is adopted. In addition, in the measurement of the diffracted X-rays in the above-mentioned measurement area, the measurement range of the diffraction angle 2θ (0 to 10°) may be measured at intervals of 0.008° while the rotation angle φ in the in-plane direction of the light absorption anisotropic layer is fixed at any angle from 0 to 180°, or the measurement range of the diffraction angle 2θ (0 to 180°) may be measured at intervals of 1° while the rotation angle φ in the in-plane direction of the light absorption anisotropic layer is fixed at any angle from 0 to 10°.
[0055] <Measurement Conditions>
[0056] Source of incident X-rays: CuK α rays
[0057] Reference (0°) position of the rotation angle φ: Position of the optically anisotropic layer when X-rays are first incident
[0058] Reference (180°) position of the rotation angle φ: the position where the light absorption anisotropic layer is rotated 180° clockwise from the position of 0°
[0059] Measurement interval of rotation angle φ: 1°
[0060] Diffraction angle 2θ measurement interval: 0.008°
[0061] As described above, the light absorption anisotropic layer of the present invention can suppress the generation of haze by satisfying the above formula (1) when an X-ray diffraction pattern is measured by an in-plane diffraction method.
[0062] Although the details of why this effect is achieved are not clear, the present inventors speculate as follows.
[0063] First, in the measurement of the X-ray diffraction pattern by the in-plane diffraction method, as described above, the light absorption anisotropic layer is rotated to a predetermined position in the in-plane direction, and the diffraction angle 2θ of the diffracted X-ray is measured using a detector to evaluate the regularity of the structure.
[0064] Therefore, the presence of a regular structure that does not diffract incident X-rays (i.e., the disorder of the orientation of the liquid crystal compound) cannot be correctly evaluated based on the rotation position of the light absorption anisotropic layer. Furthermore, the present inventors speculate that the disorder of the orientation of the liquid crystal compound is the cause of the haze in the light absorption anisotropic layer.
[0065] In contrast, it is considered that in the present invention, I(φmax-10) is measured at a position where the rotation angle and diffraction angle representing the maximum intensity I(φmax) are shifted by only 10°, and I(φmax) and I(φmax-10) satisfy the above formula (1), that is, I(φmax-10) originating from the regular structure caused by the disorder of the orientation of the liquid crystal compound is reduced to a certain extent, thereby suppressing the generation of haze of the light absorption anisotropic layer.
[0066] In the present invention, for the reason of further suppressing the generation of haze, it is preferred that the light absorption anisotropic layer is fixed at a position of rotation angle φmax-90° (i.e., the light absorption anisotropic layer is rotated 90° counterclockwise from the position of rotation angle φmax) and when the diffraction angle 2θ is measured in the range of more than 10° and less than 30°, a peak value of diffracted X-rays showing a peak intensity of I(φmax)×0.2 times or more is observed (hereinafter, also referred to as “peak P2”). In addition, in the measurement of the diffracted X-rays of the peak P2, the value of the peak intensity when measured under the following conditions is adopted.
[0067] <Measurement Conditions>
[0068] The source of incident X-rays: CuKα rays
[0069] Diffraction angle 2θ measurement interval: 0.008°
[0070] As described above, the light absorption anisotropic layer of the present invention is a layer containing a dichroic substance and a liquid crystal compound, and is preferably a layer in which the alignment states of the liquid crystal compound and the dichroic substance are fixed.
[0071] Hereinafter, the dichroic substance, the liquid crystal compound, and the optional components contained in the light absorption anisotropic layer of the present invention will be described.
[0072] <Dichroic substances>
[0073] In the present invention, a dichroic substance refers to a pigment whose absorbance differs depending on the direction. A dichroic substance may or may not exhibit liquid crystallinity.
[0074] There is no particular limitation on dichroic substances, and examples thereof include visible light absorbing substances (dichroic pigments), luminescent substances (fluorescent substances, phosphorescent substances), ultraviolet absorbing substances, infrared absorbing substances, nonlinear optical substances, carbon nanotubes and inorganic substances (such as quantum rods), etc. Conventionally known dichroic substances (dichroic pigments) can be used.
[0075] Specifically, for example, paragraphs
[0067] to
[0071] of Japanese Patent Application Laid-Open No. 2013-228706, paragraphs
[0008] to
[0026] of Japanese Patent Application Laid-Open No. 2013-227532, paragraphs
[0008] to
[0015] of Japanese Patent Application Laid-Open No. 2013-209367, paragraphs
[0045] to
[0058] of Japanese Patent Application Laid-Open No. 2013-14883, paragraphs
[0012] to
[0029] of Japanese Patent Application Laid-Open No. 2013-109090, paragraphs
[0009] to
[0017] of Japanese Patent Application Laid-Open No. 2013-101328, and paragraphs
[0051] to
[0065] of Japanese Patent Application Laid-Open No. 2013-37353. , paragraphs
[0049] to
[0073] of Japanese Patent Application Laid-Open No. 2012-63387, paragraphs
[0016] to
[0018] of Japanese Patent Application Laid-Open No. 11-305036, paragraphs
[0009] to
[0011] of Japanese Patent Application Laid-Open No. 2001-133630, paragraphs
[0030] to
[0169] of Japanese Patent Application Laid-Open No. 2011-215337, paragraphs
[0021] to
[0075] of Japanese Patent Application Laid-Open No. 2010-106242, paragraphs
[0011] to
[0025] of Japanese Patent Application Laid-Open No. 2010-215846, paragraphs
[0017] to
[0069] of Japanese Patent Application Laid-Open No. 2011-048311, paragraphs
[0018] to
[0069] of Japanese Patent Application Laid-Open No. 2011- 213610, paragraphs
[0013] to
[0133] of Japanese Patent Application Publication No. 2011-237513, paragraphs
[0074] to
[0246] of Japanese Patent Application Publication No. 2016-006502, paragraphs
[0005] to
[0051] of Japanese Patent Application Publication No. 2018-053167, paragraphs
[0014] to
[0032] of Japanese Patent Application Publication No. 2020-11716, paragraphs
[0005] to
[0041] of International Publication No. 2016 / 060173, paragraphs
[0008] to
[0062] of International Publication No. 2016 / 136561, International Publication No. 2017 / 154835 paragraphs
[0014] to
[0033] of International Publication No. 2017 / 154695, paragraphs
[0014] to
[0033] of International Publication No. 2017 / 195833, paragraphs
[0014] to
[0034] of International Publication No. 2018 / 164252, paragraphs
[0021] to
[0030] of International Publication No. 2018 / 186503, paragraphs
[0043] to
[0063] of International Publication No. 2019 / 189345, paragraphs
[0043] to
[0085] of International Publication No. 2019 / 225468, paragraphs
[0050] to
[0074] of International Publication No. 2020 / 004106,The contents described in paragraphs
[0015] to
[0038] of International Publication No. 2021 / 044843.
[0076] As the dichroic substance, a dichroic azo dye compound is preferred.
[0077] A dichroic azo dye compound refers to an azo dye compound whose absorbance varies according to the direction. A dichroic azo dye compound may or may not exhibit liquid crystallinity. When a dichroic azo dye compound exhibits liquid crystallinity, it may exhibit either nematicity or smecticity. The temperature range in which the liquid crystal phase is exhibited is preferably room temperature (about 20 to 28° C.) to 300° C., and more preferably 50 to 200° C. from the viewpoint of operability and manufacturing applicability.
[0078] In the present invention, it is preferred to use at least two dichroic substances having maximum absorption wavelengths in the range of 550 to 700 nm because the precipitation of the dichroic substance over time in the light absorption anisotropic layer-forming composition described later can be suppressed.
[0079] The upper limit of the content of the dichroic substance contained in the light absorption anisotropic layer is preferably 30 mass % or less, more preferably 20 mass % or less, and further preferably 15 mass % or less, relative to the total mass of the light absorption anisotropic layer. Furthermore, the lower limit is preferably 0.1 mass % or more, more preferably 1 mass % or more, and further preferably 3 mass % or more.
[0080] Furthermore, the content of the dichroic substance contained in the light absorption anisotropic layer is preferably 20 to 400 mg / cm because the orientation degree of the formed light absorption anisotropic layer becomes high. 3 , more preferably 30 to 200 mg / cm 3 , more preferably 40 to 150 mg / cm 3 In addition, when a plurality of dichroic substances are used simultaneously, the total amount of the plurality of dichroic substances is preferably within the above range.
[0081] Here, the content of dichroic substances (mg / cm 3) can be obtained by measuring a solution obtained by dissolving a laminate having a light absorption anisotropic layer or an extract obtained by impregnating an optical laminate with a solvent using high-speed liquid chromatography (HPLC), but is not limited to the above method. In addition, quantification can be performed by using the dichroic substance contained in the light absorption anisotropic layer as a standard sample. And, as an example of a method for calculating the content of the dichroic substance, the following method can be cited: the volume is calculated by the product of the thickness of the light absorption anisotropic layer obtained from the microscope observation image of the cross section of the laminate and the area of the laminate used to measure the amount of pigment, and the amount of pigment measured by HPLC is divided by the volume, thereby calculating the pigment content.
[0082] <Liquid Crystalline Compound>
[0083] As the liquid crystal compound contained in the light absorption anisotropic layer, any of a high molecular weight liquid crystal compound and a low molecular weight liquid crystal compound can be used.
[0084] Here, the "polymer liquid crystal compound" refers to a liquid crystal compound having a repeating unit in its chemical structure.
[0085] Here, the "low-molecular liquid crystal compound" refers to a liquid crystal compound having no repeating unit in the chemical structure.
[0086] Examples of the polymer liquid crystal compound include the thermotropic liquid crystal polymer described in JP-A-2011-237513 and the polymer liquid crystal compound described in paragraphs
[0012] to
[0042] of WO-2018 / 199096.
[0087] Examples of the low-molecular liquid crystal compound include the liquid crystal compounds described in paragraphs
[0072] to
[0088] of JP-A-2013-228706, and among these, liquid crystal compounds showing smecticity are preferred.
[0088] Examples of such liquid crystal compounds include those described in paragraphs
[0019] to
[0140] of International Publication No. 2022 / 014340, and these descriptions are incorporated into this specification by reference.
[0089] In the present invention, the liquid crystal compound contained in the light absorption anisotropic layer is preferably a liquid crystal compound showing a liquid crystal state of a smectic phase (hereinafter, also simply referred to as a "smectic liquid crystal compound").
[0090] Here, as the smectic phase, for example, smectic A phase, smectic C phase, etc. can be mentioned, but it can also be a higher-order smectic phase (for example, smectic B phase, smectic E phase, smectic F phase, smectic G phase, smectic H phase, smectic I phase, smectic J phase, smectic K phase, smectic L phase, etc.).
[0091] Furthermore, in addition to the smectic phase, a nematic phase may also appear.
[0092] Furthermore, in the present invention, because the orientation degree of the light absorption anisotropic layer is improved, the liquid crystal compound is preferably a liquid crystal compound showing any liquid crystal state of smectic B phase, E phase, F phase, G phase, H phase, I phase, J phase, K phase and L phase.
[0093] As the smectic liquid crystal compound, a compound represented by the following formula (I) or (II) is preferred, and a compound represented by the following formula (I) and (II) is more preferably used together.
[0094] Formula (I)
[0095] Q1-V1-SP1-X1-(Ma-La)na-X2-SP2-V2-Q2
[0096] Formula (II)
[0097] Q1-V1-SP1-X1-(Ma-La)na-Q3
[0098] In the above formulae (I) and (II), Q1 and Q2 each independently represent a polymerizable group, and Q3 represents a hydrogen atom or a substituent.
[0099] Furthermore, V1, V2, X1 and X2 each independently represent a single bond or a divalent linking group.
[0100] Furthermore, SP1 and SP2 each independently represent a divalent spacer group.
[0101] Furthermore, na represents an integer of 2-10.
[0102] Furthermore, Ma represents an aromatic ring, an aliphatic ring or a heteroatom-containing ring which may have a substituent. A plurality of Ma may be the same or different.
[0103] Furthermore, La represents a single bond or a divalent linking group. A plurality of La's may be the same or different.
[0104] The polymerizable group represented by one embodiment of Q1 and Q2 is preferably a radically polymerizable group (radical polymerizable group) or a cationically polymerizable group (cationically polymerizable group).
[0105] As the free radical polymerizable group, a known free radical polymerizable group can be used, and as a preferred free radical polymerizable group, an acryloyloxy group or a methacryloyloxy group can be mentioned. At this time, it is known that an acryloyloxy group generally has a fast polymerization rate, and from the viewpoint of improving productivity, an acryloyloxy group is preferred, but a methacryloyloxy group can also be used as a polymerizable group.
[0106] As the cationically polymerizable group, a known cationically polymerizable group can be used, and specifically, an alicyclic ether group, a cyclic acetal group, a cyclic lactone group, a cyclic thioether group, a spirocyclic orthoester group, and a vinyloxy group can be mentioned, among which an alicyclic ether group or a vinyloxy group is preferred, and an epoxy group, an oxetanyl group, or a vinyloxy group is particularly preferred.
[0107] As particularly preferred examples of the polymerizable group, there can be mentioned a polymerizable group represented by any of the following formulae (P-1) to (P-20).
[0108] [Chemical formula 1]
[0109]
[0110] In the above formulae (I) and (II), examples of the divalent linking group represented by one embodiment of V1, V2, X1, X2, and La include -O-, -(CH 2 ) g -、-(CF 2 ) g -、-Si(CH 3 ) 2 -、-(Si(CH 3 ) 2 O) g -、-(OSi(CH 3 ) 2 ) g -〔g represents an integer of 1 to 10.〕, -N(Z)-, -C(Z)=C(Z')-, -C(Z)=N-, -N=C(Z)-, -C(Z) 2 -C(Z') 2-, -C(O)-, -OC(O)-, -C(O)O-, -OC(O)O-, -N(Z)C(O)-, -C(O)N(Z)-, -C(Z)=C(Z')-C(O)O-, -OC(O)-C(Z)=C(Z') -, -C(Z)=N-, -N=C(Z)-, -C(Z)=C(Z')-C(O)N(Z”)-, -N(Z”)-C(0)-C(Z)=C(Z’)-, -C(Z)=C(Z’)-C(O)-S-, -SC(O) -C(Z)=C(Z')-, -C(Z)=NN=C(Z')-〔Z, Z' and Z" each independently represent a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a cycloalkyl group, an aryl group, a cyano group or a halogen atom.〕, -C≡C-, -N=N-, -S-, -S(O)-, --S(O)(O)--, -(O)S(O)O-, -O(O)S(O)O-, -SC(O)- and -C(O)S-, etc. V1, V2, X1, X2 and La can be a group formed by combining two or more of these groups.
[0111] Among these divalent linking groups, -CO-, -O-, -S-, -C(=S)-, -C(Z)(Z')-, -C(Z)=C(Z')-, -N(Z)-, or a divalent linking group consisting of a combination of two or more of these is preferred.
[0112] In the above formulae (I) and (II), the divalent spacer groups represented by SP1 and SP2 include, for example, linear, branched or cyclic alkylene groups having 1 to 50 carbon atoms, and heterocyclic groups having 1 to 20 carbon atoms.
[0113] The carbon atoms of the alkylene group and the carbon atoms of the heterocyclic group may be replaced by -O-, -Si(CH 3 ) 2 -、-(Si(CH 3 ) 2 O) g -、-(OSi(CH 3 ) 2 ) g -〔g represents an integer of 1 to 10.〕, -N(Z)-, -C(Z)=C(Z')-, -C(Z)=N-, -N=C(Z)-, -C(Z) 2 -C(Z') 2-, -C(O)-, -OC(O)-, -C(O)O-, -OC(O)O-, -N(Z)C(O)-, -C(O)N(Z)-, -C(Z)=C(Z')-C(O)O -, -OC(O)-C(Z)=C(Z')-, -C(Z)=N-, -N=C(Z)-, -C(Z)=C(Z')-C(0)N(Z”)-, -N(Z”)-C(O)- C(Z)=C(Z')-, -C(Z)=C(Z')-C(O)-S-, -SC(O)-C(Z)=C(Z')-, -C(Z)=NN=C(Z')-(Z, Z' and Z" independently represent a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a cycloalkyl group, an aryl group, a cyano group or a halogen atom. 〕, -C≡C-, -N=N-, -S-, -C(S)-, -S(O)-, -SO 2 -, -(O)S(O)O-, -O(O)S(O)O-, -SC(O)- and -C(O)S-, or a group consisting of two or more of these.
[0114] The hydrogen atoms of the above alkylene group and the hydrogen atoms of the heterocyclic group may be substituted by halogen atoms, cyano groups, -Z H 、-OH、-OZ H 、-COOH、-C(O)Z H 、-C(O)OZ H 、-OC(O)Z H 、-OC(O)OZ H 、-NZ H Z H '、-NZ H C(O)Z H '、-NZ H C(O)OZ H '、-C(O)NZ H Z H '、-OC(O)NZ H Z H '、-NZ H C(O)NZ H 'OZ H ”、-SH、-SZ H 、-C(S)Z H 、-C(O)SZ H 、-SC(0)Z H Replace. Among them, Z H , Z H' and Z" independently represent an alkyl group having 1 to 10 carbon atoms, a halogenated alkyl group, -LQ (L represents a single bond or a divalent linking group. Specific examples of the divalent linking group are the same as those of V1 described above. Q represents a crosslinking group, and a polymerizable group that is a preferred embodiment of Q1 or Q2 described above can be cited, preferably a polymerizable group represented by the above formulae (P-1) to (P-20)].
[0115] Furthermore, the divalent spacer groups represented by SP1 and SP2 are preferably linear alkylene groups having 1 to 12 carbon atoms, branched alkylene groups having 3 to 12 carbon atoms, or -CH 2 - is a divalent linking group in which at least one of - is substituted with -O-, -S-, -NH-, -N(Z)- or -CO-.
[0116] In the above formulae (I) and (II), Ma represents an aromatic ring, an aliphatic ring or a heteroatom-containing ring which may have a substituent, and is preferably a 4- to 15-membered ring. Ma may be a single ring or a condensed ring, and a plurality of Ma may be the same or different.
[0117] Examples of the aromatic ring represented by Ma include phenylene, naphthylene, fluorene-diyl, anthracene-diyl, and naphthacene-diyl. From the viewpoint of the diversity of design of the mesogen skeleton and the availability of raw materials, phenylene and naphthylene are preferred.
[0118] Examples of the aliphatic ring represented by Ma include cyclopentylene and cyclohexylene. The carbon atom may be replaced by -O-, -Si(CH 3 ) 2 -, -N(Z)- (Z represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a cycloalkyl group, an aryl group, a cyano group, or a halogen atom.), -C(O)-, -S-, -C(S)-, -S(O)-, and -SO 2 -, or a group formed by combining two or more of these groups.
[0119] As atoms other than carbon constituting the heteroatom ring represented by Ma, nitrogen atoms, sulfur atoms and oxygen atoms can be mentioned. When the heteroatom ring has a plurality of atoms constituting the ring other than carbon, these atoms can be the same or different. As specific examples of heteroatom rings, for example, pyridylene (pyridine-diyl), pyridazine-diyl, imidazole-diyl, thiophene (thiophene-diyl), quinolylene (quinoline-diyl), isoquinolylene (isoquinoline-diyl), oxazole-diyl, thiazole-diyl, oxadiazole-diyl, benzothiazole-diyl, benzothiadiazole-diyl, phthalimide-diyl, thienothiazole-diyl, thiazolothiazole-diyl, thienothiophene-diyl and thienothiazole-diyl, the following structures (II-1) to (II-4), etc. can be mentioned.
[0120] [Chemical formula 2]
[0121]
[0122] In formulas (II-1) to (II-4), D 1 Indicates -S-, -O- or NR 11 -, R 11 It represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.
[0123] Y 1 It represents an aromatic hydrocarbon group having 6 to 12 carbon atoms or an aromatic heterocyclic group having 3 to 12 carbon atoms.
[0124] Z 1 , Z 2 , and Z 3 each independently represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 20 carbon atoms, an alicyclic hydrocarbon group having 3 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms, a halogen atom, a cyano group, a nitro group, -NR 12 R 13 or -SR 12 Here, Z 1 and Z 2 can be bonded to each other to form an aromatic ring or an aromatic heterocyclic ring, R 12 and R 13 Each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.
[0125] A 1 and A 2 Each independently represents a group consisting of -O-, -NR 21 -(R 21 represents a hydrogen atom or a substituent. ), a group in the group of -S- and -CO-.
[0126] E represents a hydrogen atom or a non-metal atom of Groups 14 to 16 to which a substituent may be bonded.
[0127] Ax represents an organic group having 2 to 30 carbon atoms and having at least one aromatic ring selected from the group consisting of aromatic hydrocarbon rings and aromatic heterocyclic rings,
[0128] Ay represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms which may have a substituent, or an organic group having 2 to 30 carbon atoms which has at least one aromatic ring selected from the group consisting of an aromatic hydrocarbon ring and an aromatic heterocyclic ring. The aromatic rings possessed by Ax and Ay may have a substituent, and Ax and Ay may be bonded to form a ring.
[0129] D 2 It represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms which may have a substituent.
[0130] In formula (II-2), when Y 1 When Y is an aromatic hydrocarbon group having 6 to 12 carbon atoms, it may be a monocyclic or polycyclic ring. 1 In the case of an aromatic heterocyclic group having 3 to 12 carbon atoms, it may be a monocyclic or polycyclic group.
[0131] In formula (II-2), when A 1 and A 2 Indicates -NR 21 -, as R 21 For the substituents of, for example, reference can be made to the description in paragraphs 0035 to 0045 of JP-A-2008-107767, the contents of which are incorporated into the present specification.
[0132] In formula (II-2), when X is a non-metal atom of Groups 14 to 16 to which a substituent may be bonded, it is preferably =O, =S, =NR', or =C(R')R'. R' represents a substituent, and as a substituent, for example, reference can be made to paragraphs
[0035] to
[0045] of Japanese Patent Application Laid-Open No. 2008-107767, and is preferably a nitrogen atom.
[0133] As for MA in the above formulae (I) and (II), examples of the substituent that the aromatic ring, aliphatic ring or heteroatom-containing ring may have include a halogen atom, an alkyl group having 1 to 20 carbon atoms, a haloalkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkenyl group having 1 to 20 carbon atoms, an alkynyl group having 1 to 20 carbon atoms, an aryl group having 1 to 20 carbon atoms, a heterocyclic group (also referred to as a heteroatom-containing cyclic group), a cyano group, a hydroxyl group, a nitro group, a carboxyl group, an aryloxy group, a silyloxy group, a heterocyclicoxy group, an acyloxy group, and a carbamoyloxy group. , alkoxycarbonyloxy, aryloxycarbonyloxy, amino (including aniline), ammonium, acylamino, aminocarbonylamino, alkoxycarbonylamino, aryloxycarbonylamino, sulfamoylamino, alkyl or arylsulfonylamino, mercapto, alkylthio, arylthio, heterocyclic thio, sulfamoyl, sulfo, alkyl or arylsulfinyl, alkyl or arylsulfonyl, acyl, aryloxycarbonyl, alkoxycarbonyl, carbamoyl, aryl or heterocyclic azo, imide, phosphino, phosphinyl, phosphinyloxy, phosphinylamino, phosphono, silyl, hydrazine, urea, boronic acid (-B(OH) 2 ), phosphate group (-OPO(OH) 2 ), sulfate group (-OSO 3 H), other known substituents, etc.
[0134] In addition, details of the substituents are described in paragraph
[0023] of JP-A-2007-234651.
[0135] In the above formulae (I) and (II), na represents an integer of 2-10, preferably an integer of 2-8, and more preferably an integer of 2-5.
[0136] In the above formula (II), as a substituent represented by one mode of Q3, there can be mentioned the same substituents as the substituents that the aromatic ring, aliphatic ring or heteroatom-containing ring described in Ma in the above formula (I), among which an alkyl group having 1 to 20 carbon atoms or an alkoxy group having 1 to 20 carbon atoms is preferred.
[0137] As smectic liquid crystal compounds, for example, there can be mentioned the smectic liquid crystal compounds described in paragraphs
[0033] to
[0039] of Japanese Patent Publication No. 2008-19240, paragraphs
[0037] to
[0041] of Japanese Patent Publication No. 2008-214269, and paragraphs
[0033] to
[0040] of Japanese Patent Publication No. 2006-215437, and these descriptions are incorporated into this specification by reference.
[0138] In the present invention, the content of the liquid crystal compound is preferably 50 to 99% by mass, more preferably 75 to 95% by mass, based on the total mass of the light absorption anisotropic layer.
[0139] <Liquid Crystal Composition>
[0140] The light absorption anisotropic layer of the present invention is preferably formed using a liquid crystal composition containing the above-mentioned dichroic substance and a liquid crystal compound (hereinafter, also simply referred to as a "light absorption anisotropic layer forming composition").
[0141] (Monofunctional Compounds)
[0142] In order to further suppress the generation of haze, the composition for forming anisotropic light-absorbing layer preferably contains a monofunctional compound that satisfies the relationship of the following formula (2) with the above-mentioned liquid crystal compound. That is, the molecular length of the long axis direction of the above-mentioned liquid crystal compound is preferably The molecular length in the direction of the long axis of the monofunctional compound The relationship of the following formula (2) is satisfied. It is believed that by satisfying the following formula (2), free volume is created between the molecules of the liquid crystal compound, and the presence of the free volume can suppress the alignment disorder that may occur when the light absorption anisotropic layer-forming composition is cured, and as a result, the generation of haze can be further suppressed.
[0143] Formula (2):
[0144] 0.2×D1≤D2≤0.45×D1
[0145] Here, the molecular length in the long axis direction of the liquid crystal compound is and the molecular length of the long axis of the monofunctional compound This is the value calculated by following the steps below.
[0146] (1) The structure of a compound to be calculated (target compound) is identified.
[0147] (2) Save the ChemDraw file containing the chemical formula of the target compound in the "MDLMolfile format".
[0148] (3) Open the saved MDLMolfile file using a molecular modeling application (such as Winmostar) and perform structural optimization using a simplified molecular force field method.
[0149] (4) The interatomic distance between both ends of the target compound after structure optimization is calculated as the molecular length.
[0150] Such a monofunctional compound is preferably a non-liquid crystal compound, more preferably a compound having a polymerizable group, and still more preferably a compound having a polymerizable group and having a molecular weight of 500 or less.
[0151] Here, the polymerizable group includes the same polymerizable groups as those described for Q1 in the above formula (I), and among them, the polymerizable group represented by any one of the above formulae (P-1) to (P-20) is preferred.
[0152] (Solvent)
[0153] From the viewpoint of workability, the composition for forming a light absorption anisotropic layer preferably contains a solvent.
[0154] Examples of the solvent include organic solvents such as ketones, ethers, aliphatic hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, halogenated carbons, esters, alcohols, cellosolves, cellosolve acetates, sulfoxides, amides, and heteroatom-containing ring compounds, and water.
[0155] These solvents may be used alone or in combination of two or more.
[0156] Among these solvents, organic solvents are preferred, and halogenated carbons or ketones are more preferred.
[0157] When the composition for forming anisotropic light absorbing layer contains a solvent, the content of the solvent is preferably 80 to 99% by mass, more preferably 83 to 97% by mass, and further preferably 85 to 95% by mass based on the total mass of the composition for forming anisotropic light absorbing layer.
[0158] (Polymerization initiator)
[0159] The composition for forming a light absorption anisotropic layer may contain a polymerization initiator.
[0160] The polymerization initiator is not particularly limited, but is preferably a photosensitivity compound, ie, a photopolymerization initiator.
[0161] As such a photopolymerization initiator, commercially available products can be used, and examples thereof include Irgacure 184, Irgacure 907, Irgacure 369, Irgacure 651, Irgacure 819, Irgacure OXE-01, and Irgacure OXE-02 manufactured by BASF.
[0162] The polymerization initiator may be used alone or in combination of two or more.
[0163] When the composition for forming anisotropic light absorbing layer contains a polymerization initiator, the content of the polymerization initiator is preferably 0.01 to 30% by mass, more preferably 0.1 to 15% by mass, based on the total solid content of the composition for forming anisotropic light absorbing layer.
[0164] [Method for producing light absorption anisotropic layer]
[0165] The method for producing an anisotropic light absorption layer of the present invention is a method for producing the above-mentioned anisotropic light absorption layer of the present invention, which includes a step of forming an anisotropic light absorption layer by irradiating a liquid crystal composition layer containing a dichroic substance, a liquid crystal compound and a monofunctional compound with ultraviolet light (UV) in air to form the anisotropic light absorption layer.
[0166] Here, the "liquid crystal composition layer containing a dichroic substance, a liquid crystal compound and a monofunctional compound" is not particularly limited as long as it is a liquid crystal composition layer formed using a liquid crystal composition (a composition for forming a light-absorbing anisotropic layer) containing the above-mentioned dichroic substance, liquid crystal compound and monofunctional compound. For example, it can be a coating film formed by coating the above-mentioned light-absorbing anisotropic layer forming composition on an oriented film to be described later.
[0167] Examples of the coating method for the light-absorbing anisotropic layer-forming composition include known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spray coating, and inkjet.
[0168] The alignment film may be any film as long as it is a film that can align the liquid crystal component that can be contained in the composition for forming a light-absorbing anisotropic layer.
[0169] It can be set by friction treatment of the film surface with an organic compound (preferably a polymer), oblique evaporation of an inorganic compound, forming a layer with microgrooves, or accumulation of organic compounds (such as ω-tricosanoic acid, dioctadecyl methyl ammonium chloride, methyl stearate) based on the Langmuir-Blodgett method (LB film). In addition, it is also known that an alignment film that generates an alignment function by imparting an electric field, a magnetic field or light irradiation. Among them, in the present invention, from the viewpoint of the ease of controlling the pretilt angle of the alignment film, an alignment film formed by friction treatment is preferred, and from the viewpoint of alignment uniformity, a photo-aligned film formed by light irradiation is also preferred.
[0170] The photo-alignment compound used in the photo-alignment film is described in a plurality of documents. In the present invention, preferred examples include: azo compounds described in Japanese Patent Publication No. 2006-285197, Japanese Patent Publication No. 2007-76839, Japanese Patent Publication No. 2007-138138, Japanese Patent Publication No. 2007-94071, Japanese Patent Publication No. 2007-121721, Japanese Patent Publication No. 2007-140465, Japanese Patent Publication No. 2007-156439, Japanese Patent Publication No. 2007-133184, Japanese Patent Publication No. 2009-109831, Japanese Patent No. 3883848, and Japanese Patent No. 4151746. Compounds; aromatic ester compounds described in Japanese Patent Publication No. 2002-229039; maleimide and / or alkenyl-substituted naphthalene diimide compounds having photo-alignment units described in Japanese Patent Publication No. 2002-265541 and Japanese Patent Publication No. 2002-317013; photo-crosslinkable silane derivatives described in Japanese Patent No. 4205195 and Japanese Patent No. 4205198; and photo-crosslinkable polyimide, polyamide or ester described in Japanese Patent Table No. 2003-520878, Japanese Patent Table No. 2004-529220 or Japanese Patent No. 4162850. More preferably, azo compounds, photo-crosslinkable polyimide, polyamide or ester.
[0171] Among these, it is preferable to use a photosensitive compound having a photoreactive group that undergoes at least one of dimerization and isomerization by the action of light as the photo-alignment compound.
[0172] In addition, as the photoreactive group, for example, there can be mentioned a group having a cinnamic acid (cinnamoyl) structure (skeleton), a group having a coumarin structure (skeleton), a group having a chalcone structure (skeleton), a group having a benzophenone structure (skeleton), and a group having an anthracene structure (skeleton). Among these groups, a group having a cinnamoyl structure and a group having a coumarin structure are preferred, and a group having a cinnamoyl structure is more preferred.
[0173] Furthermore, the photosensitive compound having the above-mentioned photo-alignment group may further have a crosslinking group.
[0174] The crosslinkable group is preferably a thermal crosslinkable group that causes a curing reaction by heat or a photo crosslinkable group that causes a curing reaction by light, and may be a crosslinkable group having either a thermal crosslinkable group or a photo crosslinkable group.
[0175] Examples of the crosslinkable group include epoxy, oxetanyl, -NH-CH 2 At least one selected from the group consisting of -0-R (R represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms), a group having an ethylenically unsaturated double bond, and a blocked isocyanate group. Among them, an epoxy group, an oxetanyl group, and a group having an ethylenically unsaturated double bond are preferred.
[0176] In addition, a three-membered ring cyclic ether group is also called an epoxy group, and a four-membered ring cyclic ether group is also called an oxetanyl group.
[0177] Furthermore, specific examples of the group having an ethylenically unsaturated double bond include a vinyl group, an allyl group, a styryl group, an acryloyl group, and a methacryloyl group, and an acryloyl group or a methacryloyl group is preferred.
[0178] The photo-alignment film formed of the above-mentioned material is irradiated with linearly polarized light or non-polarized light to produce the photo-alignment film.
[0179] In this specification, "linearly polarized light irradiation" and "non-polarized light irradiation" are operations for causing a photoreaction in a photo-alignment material. The wavelength of the light used varies depending on the photo-alignment material used, and is not particularly limited as long as it is a wavelength required for the photoreaction. The peak wavelength of the light used for light irradiation is preferably 200nm to 700nm, and more preferably ultraviolet light with a peak wavelength of 400nm or less.
[0180] The light source used for light irradiation includes commonly used light sources, such as tungsten lamps, halogen lamps, xenon lamps, xenon flash lamps, mercury lamps, mercury-xenon lamps and carbon arc lamps, various lasers [for example, semiconductor lasers, helium-neon lasers, argon ion lasers, helium-cadmium lasers and YAG (yttrium aluminum garnet) lasers], light emitting diodes and cathode ray tubes, etc.
[0181] As a method of obtaining linearly polarized light, a method using a polarizing plate (e.g., an iodine polarizing plate, a dichroic dye polarizing plate, and a wire grid polarizing plate), a method using a prism element (e.g., a Glan-Thomson prism) or a reflective polarizer using the Brewster angle, or a method using light emitted from a laser light source having polarized light can be adopted. In addition, a filter or a wavelength conversion element can be used to selectively irradiate only light of a desired wavelength.
[0182] When the irradiated light is linearly polarized light, the method of irradiating the alignment film from the top or back in a direction perpendicular or oblique to the alignment film surface is adopted. The incident angle of light varies depending on the photo-alignment material, but is preferably 0 to 90° (perpendicular), preferably 40 to 90°.
[0183] In the case of non-polarized light, the alignment film is irradiated with non-polarized light from an oblique direction, and the incident angle is preferably 10 to 80°, more preferably 20 to 60°, and further preferably 30 to 50°.
[0184] The irradiation time is preferably 1 minute to 60 minutes, more preferably 1 minute to 10 minutes.
[0185] When patterning is required, a method of performing light irradiation using a photomask a number of times required for patterning, or a method of writing a pattern by laser scanning can be adopted.
[0186] The method for producing a light absorption anisotropic layer of the present invention is characterized by comprising a light absorption anisotropic layer forming step of irradiating the liquid crystal composition layer with ultraviolet rays in air to form the light absorption anisotropic layer. It is believed that by curing by irradiating with ultraviolet rays in air, a hard film can be formed while relieving the curing strain, so that the alignment disorder that may occur during curing can be suppressed, and as a result, the generation of haze can be suppressed.
[0187] Here, the method of ultraviolet irradiation is not particularly limited except that it is performed in air in the presence of oxygen, and the same method as conventionally known ultraviolet irradiation (exposure) can be employed.
[0188] From the perspective of improving the durability of the light absorption anisotropic layer, the method for producing a light absorption anisotropic layer of the present invention preferably includes a step of irradiating the optically anisotropic layer after the light absorption anisotropic layer forming step with ultraviolet rays under nitrogen.
[0189] The method for producing a light absorption anisotropic layer of the present invention preferably includes a step of orienting the liquid crystal components contained in the above-mentioned liquid crystal composition layer before irradiating the above-mentioned liquid crystal composition layer with ultraviolet rays in air in the above-mentioned light absorption anisotropic layer forming step (hereinafter also referred to as "orientation step").
[0190] The alignment step is a step of aligning the liquid crystal components (particularly, the dichroic substance) contained in the liquid crystal composition layer. In the alignment step, it is considered that the dichroic substance is aligned along the liquid crystal compound aligned by the alignment film.
[0191] The orientation process may include a drying process. By drying, components such as solvents can be removed from the coating film. The drying process may be performed by leaving the coating film at room temperature for a predetermined time (e.g., natural drying), or by heating and / or blowing air.
[0192] The orientation step preferably includes a heat treatment. This further orients the dichroic substance contained in the coating film, and the degree of orientation of the dichroic substance further increases.
[0193] From the viewpoint of production suitability, the heat treatment is preferably performed at 10 to 250° C., more preferably 25 to 190° C. The heating time is preferably 1 to 300 seconds, more preferably 1 to 60 seconds.
[0194] The orientation process may include a cooling process performed after the heating process. The cooling process is a process of cooling the heated coating film to about room temperature (20 to 25° C.). As a result, the orientation of the dichroic substance contained in the coating film is further fixed, and the degree of orientation of the dichroic substance is further increased. There is no particular limitation on the cooling method, and it can be performed by a known method.
[0195] [Laminated body]
[0196] The laminate of the present invention is a laminate having the above-mentioned light absorption anisotropic layer of the present invention and a λ / 4 plate provided on the light absorption anisotropic layer.
[0197] Furthermore, the laminated body of the present invention preferably has a substrate, and more preferably is a laminated body having a substrate, a light absorption anisotropic layer, and a λ / 4 plate in this order.
[0198] Furthermore, the laminate of the present invention preferably has a barrier layer, and more preferably is a laminate having a light absorption anisotropic layer, a barrier layer, and a λ / 4 plate in this order.
[0199] Furthermore, the laminated body of the present invention may have an alignment film between the substrate and the optically anisotropic layer.
[0200] Hereinafter, each layer constituting the laminate of the present invention will be described.
[0201] 〔Base material〕
[0202] The substrate can be appropriately selected according to the application of the optically anisotropic layer, and examples thereof include glass and polymer films. The light transmittance of the substrate is preferably 80% or more.
[0203] When a polymer film is used as a substrate, an optically isotropic polymer film is preferably used. The specific examples and preferred embodiments of the polymer can be described in paragraph
[0013] of Japanese Patent Application Laid-Open No. 2002-22942. In addition, a polymer that is known to be easy to show birefringence, such as polycarbonate or polysulfone, can also be used, which is a polymer whose showability is reduced by modifying the molecules described in International Publication No. 2000 / 26705.
[0204] [Optically anisotropic layer]
[0205] The optically anisotropic layer is as described above, and therefore the description thereof is omitted.
[0206] 〔λ / 4 plate〕
[0207] The so-called “λ / 4 plate” is a plate having a λ / 4 function, specifically, a plate having a function of converting linearly polarized light of a certain wavelength into circularly polarized light (or converting circularly polarized light into linearly polarized light).
[0208] For example, as a mode in which the λ / 4 plate is a single-layer structure, specifically, a phase difference film in which a stretched polymer film or an optically anisotropic layer having a λ / 4 function is provided on a support, etc., and as a mode in which the λ / 4 plate is a multi-layer structure, specifically, a broadband λ / 4 plate formed by stacking a λ / 4 plate and a λ / 2 plate can be mentioned.
[0209] The λ / 4 plate and the optically anisotropic layer may be provided in contact with each other, or another layer may be provided between the λ / 4 plate and the optically anisotropic layer. Examples of such a layer include an adhesive layer or a bonding layer for ensuring adhesion and a barrier layer.
[0210] 〔Barrier layer〕
[0211] When the laminate of the present invention has a barrier layer, the barrier layer is preferably provided between the optically anisotropic layer and the λ / 4 plate. In addition, when there is another layer (e.g., an adhesive layer or bonding layer) other than the barrier layer between the optically anisotropic layer and the λ / 4 plate, the barrier layer can be provided, for example, between the optically anisotropic layer and the other layer.
[0212] The barrier layer is also called a gas barrier layer (oxygen barrier layer), and has a function of protecting the optically anisotropic layer from gases such as oxygen in the atmosphere, moisture, or compounds contained in an adjacent layer.
[0213] Regarding the barrier layer, reference can be made to paragraphs
[0014] to
[0054] of Japanese Patent Publication No. 2014-159124, paragraphs
[0042] to
[0075] of Japanese Patent Publication No. 2017-121721, paragraphs
[0045] to
[0054] of Japanese Patent Publication No. 2017-115076, paragraphs
[0010] to
[0061] of Japanese Patent Publication No. 2012-213938, and paragraphs
[0021] to
[0031] of Japanese Patent Publication No. 2005-169994.
[0214] 〔Oriented film〕
[0215] The laminated body of the present invention may have an alignment film between the substrate and the optically anisotropic layer.
[0216] Examples of the alignment film include the same films as those described in the above-mentioned method for producing the light absorption anisotropic layer of the present invention.
[0217] [Image display device]
[0218] The image display device of the present invention comprises the above-mentioned optically anisotropic layer of the present invention or the above-mentioned laminated body of the present invention.
[0219] The display element used in the image display device of the present invention is not particularly limited, and examples thereof include a liquid crystal cell, an organic electroluminescent (hereinafter, abbreviated as "EL") display panel, and a plasma display panel.
[0220] Among these, a liquid crystal cell or an organic EL display panel is preferred, and a liquid crystal cell is more preferred. That is, as the image display device of the present invention, a liquid crystal display device using a liquid crystal cell as a display element and an organic EL display device using an organic EL display panel as a display element are preferred, and a liquid crystal display device is more preferred.
[0221] 〔Liquid crystal display device〕
[0222] As an example of the image display device of the present invention, a liquid crystal display device preferably includes the above-mentioned optically anisotropic layer and a liquid crystal cell. More preferably, a liquid crystal display device includes the above-mentioned laminate (excluding the λ / 4 plate) and a liquid crystal cell.
[0223] In addition, in the present invention, the optically anisotropic layer (laminate) of the present invention is preferably used as a polarizing element on the front side of the optically anisotropic layer (laminate) provided on both sides of the liquid crystal cell, and the optically anisotropic layer (laminate) of the present invention is more preferably used as a polarizing element on the front and rear sides.
[0224] Hereinafter, the liquid crystal cell constituting the liquid crystal display device will be described in detail.
[0225] <Liquid Crystal Unit>
[0226] The liquid crystal cell used in the liquid crystal display device is preferably a VA (Vertical Alignment) mode, an OCB (Optically Compensated Bend) mode, an IPS (In-Plane-Switching) mode, or a TN (Twisted Nematic) mode, but is not limited thereto.
[0227] In a TN mode liquid crystal cell, rod-shaped liquid crystal molecules are substantially horizontally oriented when no voltage is applied, and further twisted at 60 to 120 degrees. TN mode liquid crystal cells are most commonly used as color TFT (Thin Film Transistor) liquid crystal display devices and are described in many documents.
[0228] In a VA mode liquid crystal cell, rod-shaped liquid crystal molecules are substantially aligned vertically when no voltage is applied. VA mode liquid crystal cells include, in addition to (1) a narrow VA mode liquid crystal cell in which rod-shaped liquid crystal molecules are substantially aligned vertically when no voltage is applied and substantially aligned horizontally when voltage is applied (described in Japanese Patent Publication No. 2-176625), (2) a VA mode multi-domain (MVA mode) liquid crystal cell in order to widen the viewing angle (described in SID97, Digest of tech. Papers (Collection of Papers) 28 (1997) 845), (3) a liquid crystal cell in which rod-shaped liquid crystal molecules are substantially aligned vertically when no voltage is applied and twisted and multi-domain (n-ASM mode) when voltage is applied (described in the Collection of Papers of the Japanese Liquid Crystal Symposium 58-59 (1998)), and (4) a SURVIVAL mode liquid crystal cell (published at LCD International 98). Furthermore, it may be any of PVA (Patterned Vertical Alignment), optical alignment, and PSA (Polymer-Sustained Alignment). Details of these modes are described in Japanese Unexamined Patent Publication No. 2006-215326 and Japanese Translation of National Publication No. 2008-538819.
[0229] In the IPS mode liquid crystal unit, the rod-shaped liquid crystal molecules are substantially parallel to the substrate, and the liquid crystal molecules respond in plane by applying an electric field parallel to the substrate surface. In the IPS mode, a black display is obtained when no electric field is applied, and the absorption axes of the upper and lower polarizers are orthogonal. Japanese Patent Publication No. 10-54982, Japanese Patent Publication No. 11-202323, Japanese Patent Publication No. 9-292522, Japanese Patent Publication No. 11-133408, Japanese Patent Publication No. 11-305217, Japanese Patent Publication No. 10-307291, etc. disclose a method of using an optical compensation sheet to reduce light leakage during black display in an inclined direction to improve the viewing angle.
[0230] [Organic EL display device]
[0231] As an example of the image display device of the present invention, that is, an organic EL display device, for example, a preferred embodiment includes an optically anisotropic layer, a λ / 4 plate, and an organic EL display panel in this order from the viewing side.
[0232] More preferably, the laminated body including the λ / 4 plate and the organic EL display panel are provided in order from the visual recognition side. In this case, the laminated body is provided with a substrate, an alignment film provided as required, an optical anisotropic layer, a barrier layer provided as required, and the λ / 4 plate in order from the visual recognition side.
[0233] The organic EL display panel is a display panel formed by using an organic EL element in which an organic light emitting layer (organic electroluminescent layer) is sandwiched between electrodes (cathode and anode). There is no particular limitation on the structure of the organic EL display panel, and a known structure can be adopted.
[0234] Example
[0235] Hereinafter, the present invention will be described in further detail according to the examples. The materials, usage amounts, ratios, processing contents, processing steps etc. shown in the following examples can be appropriately changed without departing from the gist of the present invention. Therefore, the scope of the present invention should not be interpreted restrictively by the following examples.
[0236] [Example 1]
[0237] 〔Production of photo-alignment film〕
[0238] 2 parts by mass of the photo-alignment polymer PA1 described below and 98 parts by mass of o-xylene were mixed, and the obtained mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a photo-alignment film.
[0239] Next, the coating was performed by a bar coating method, and the coating was dried at 120° C. to obtain a dry film.
[0240] Next, the dried film was irradiated with polarized UV to obtain a photo-alignment film. The polarized UV treatment was performed using a UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Inc.) at an intensity of 100 mJ measured at a wavelength of 365 nm.
[0241] Photo-oriented polymer PA1:
[0242] [Chemical formula 3]
[0243]
[0244] [Fabrication of light-absorbing anisotropic layer]
[0245] The following components were mixed and stirred at 80° C. for 1 hour to obtain a composition 1 for forming a light absorption anisotropic layer.
[0246]
[0247] Among these dichroic substances, the dichroic substance A3 and the dichroic substance A4 are dichroic substances having maximum absorption wavelengths in the wavelength range of 550 to 700 nm.
[0248] Next, the composition 1 for forming an anisotropic light absorbing layer was coated on the photo-alignment film PA1 using a slot die coater to form a coating film. The solvent was removed by conveying in a ventilation drying oven set at 110° C. for 2 minutes, and then rapidly cooled to form a dry film (liquid crystal composition layer).
[0249] Then, a high pressure mercury lamp was used in an air atmosphere at 500 mJ / cm 2 After irradiation with ultraviolet light (365 nm), the samples were further irradiated with a high-pressure mercury lamp at 500 mJ / cm 2 The film was irradiated with ultraviolet light (365 nm reference) to cure the polymerizable liquid crystal contained in the dried film, thereby producing a light absorption anisotropic layer. In addition, the curing step in Example 1 is also referred to as "air exposure => N2 exposure".
[0250] [Example 2]
[0251] In the curing step when forming the light absorption anisotropic layer, a high pressure mercury lamp was used in an air atmosphere at 1000 mJ / cm 2 A light absorption anisotropic layer was prepared in the same manner as in Example 1 except that the layer was cured by irradiating with ultraviolet light (365 nm standard). The curing step in Example 2 is also referred to as "air exposure".
[0252] [Example 3]
[0253] As the composition 1 for forming a light absorption anisotropic layer, a composition prepared by further preparing 6 parts by mass of the following monofunctional compound M1 was used. In the curing step for forming the light absorption anisotropic layer, a high pressure mercury lamp was used in a nitrogen atmosphere at 1000 mJ / cm 2 A light absorption anisotropic layer was prepared in the same manner as in Example 1 except that the layer was irradiated with ultraviolet light (365 nm reference) and cured. The curing step in Example 3 is also referred to as "N2 exposure".
[0254] [Example 4]
[0255] A light absorption anisotropic layer was prepared in the same manner as in Example 3 except that the monofunctional compound M2 described below was used instead of the monofunctional compound M1 described below.
[0256] [Example 5]
[0257] A light absorption anisotropic layer was produced in the same manner as in Example 1 except that 6 parts by mass of the following monofunctional compound M1 was further prepared as the light absorption anisotropic layer-forming composition 1.
[0258] [Example 6]
[0259] A light absorption anisotropic layer was prepared in the same manner as in Example 1 except that the composition 1 for forming a light absorption anisotropic layer was used in which the amount of the dichroic substance A3 was changed to 2 parts by mass and the dichroic substance A4 was not prepared.
[0260] [Examples 7 to 8]
[0261] A light absorption anisotropic layer was prepared in the same manner as in Example 1 except that the liquid crystal compounds shown in the following Table 1 were used instead of the liquid crystal compounds L1 and L2.
[0262] [Comparative Example 1]
[0263] The same photo-alignment film as in Example 1 was produced.
[0264] Next, the same composition 1 for forming a light absorption anisotropic layer as in Example 1 was prepared.
[0265] Next, the light absorption anisotropic layer-forming composition 1 prepared above was coated on the photo-alignment film prepared above by a rod coating method, and a light absorption anisotropic layer (polarizer layer) was prepared by the method described in paragraph
[0192] of Patent Document 1 (Japanese Patent Application Publication No. 2019-049758).
[0266] [evaluate]
[0267] (1) Diffraction angle 2θ and I(φmax) / I(φmax-10)
[0268] The X-ray diffraction pattern of the produced light absorption anisotropic layer was observed by the in-plane diffraction method using the above method. The measurement results of the diffraction angles 2θ of the peaks P1 and P2 and the calculation results of the left side of the above formula (1), i.e., "I(φmax) / I(φmax-10)", are shown in Table 1 below.
[0269] In addition, it was confirmed that the peak P2 observed in Examples 1 to 7 showed a peak intensity that was 0.2 times or more of the peak intensity of the peak P1, that is, I(φmax).
[0270] (2) Haze
[0271] The light scattering when a fluorescent lamp was passed through the produced light absorption anisotropic layer was observed. The haze performance was evaluated according to the following criteria. The evaluation results are shown in Table 1 below.
[0272] <Evaluation Criteria>
[0273] AA: Transparent, with no light scattering visually recognized at all.
[0274] A: There is very slight light scattering, but it cannot be visually identified.
[0275] B: Slight light scattering is visually recognized but is tolerable.
[0276] C: Light scattering is visually perceptible and is unacceptable.
[0277] (3) Durability
[0278] The transmittance change of the produced light absorption anisotropic layer after 500 hours in an environment of 80° C. was observed. The durability was evaluated based on the following criteria. The results are shown in Table 1 below.
[0279] <Evaluation Criteria>
[0280] A: The transmittance change is hardly visually recognized.
[0281] B: The transmittance changes slightly, but is tolerable.
[0282] C: The transmittance changes greatly and cannot be tolerated.
[0283] (4) Separation
[0284] The precipitation of the dichroic substance when the composition for forming anisotropic light absorption layer was left for a period of time at room temperature was evaluated according to the following criteria. The evaluation results are shown in the following Table 1. If it is C or higher, it is an acceptable level for practical use.
[0285] <Evaluation Criteria>
[0286] A: Even after 7 days, no pigmentation occurred.
[0287] B: After 3 days, no precipitation was observed, but after 7 days, precipitation was observed.
[0288] C: After 1 day, precipitation was not observed, but after 3 days, precipitation was observed.
[0289] D: After 1 day, precipitation was observed.
[0290]
[0291] The structures of the liquid crystal compounds, dichroic substances, and monofunctional compounds in Table 1 are shown below.
[0292] Liquid crystal compound L1
[0293] [Chemical formula 4]
[0294]
[0295] Liquid crystal compound L2
[0296] [Chemical formula 5]
[0297]
[0298] Liquid crystal compound L3
[0299] [Chemical formula 6]
[0300]
[0301] Liquid crystal compound L4
[0302] [Chemical formula 7]
[0303]
[0304] Liquid crystal compound L5
[0305] [Chemical formula 8]
[0306]
[0307] Liquid crystal compound L6
[0308] [Chemical formula 9]
[0309]
[0310] Dichroic substance A1
[0311] [Chemical formula 10]
[0312]
[0313] Dichroic substance A2
[0314] [Chemical formula 11]
[0315]
[0316] Dichroic substance A3
[0317] [Chemical formula 12]
[0318]
[0319] Dichroic substance A4
[0320] [Chemical formula 13]
[0321]
[0322] Monofunctional compound M1
[0323] [Chemical formula 14]
[0324]
[0325] Monofunctional compound M2
[0326] [Chemical formula 15]
[0327]
[0328] As shown in the results in Table 1, when the value of I(φmax) / I(φmax-10) is less than 1.6, haze is generated and the dichroic substance precipitation property of the composition for forming anisotropic light absorption layer is poor after a period of time at room temperature (Comparative Example 1)
[0329] On the other hand, it was found that when the value of I(φmax) / I(φmax-10) is 1.6 or more, the generation of haze can be suppressed (Examples 1 to 8).
[0330] In particular, from the comparison between Example 1 and Example 2, it can be seen that when ultraviolet irradiation (exposure) in air and ultraviolet irradiation (exposure) in nitrogen are sequentially performed in the curing step, the durability becomes good.
[0331] Furthermore, as can be seen from the comparison between Example 1 and Example 5, if a monofunctional compound satisfying the relationship of the above formula (2) is prepared, the generation of haze can be further suppressed.
[0332] Furthermore, from the comparison between Example 1 and Example 6, it can be seen that if at least two dichroic substances having maximum absorption wavelengths in the wavelength range of 550 to 700 nm are used, the precipitation of the dichroic substance over time in the composition for forming anisotropic light absorption layer can be suppressed.
[0333] Furthermore, as can be seen from the comparison between Example 1 and Example 8, when not only the peak P1 but also the peak P2 is observed, the generation of haze can be further suppressed.
[0334] 〔Production of positive A plate〕
[0335] After the coating liquid E1 for forming a photo-alignment film with the following composition was continuously applied by a wire bar, it was dried with hot air at 140° C. for 120 seconds, and then the coating film was irradiated with polarized ultraviolet light (10 mJ / cm 2, using an ultra-high pressure mercury lamp), thereby forming a photo-alignment film E1 with a thickness of 0.2 μm.
[0336]
[0337] Polymer PA-2
[0338] [Chemical formula 16]
[0339]
[0340] Acid Generator PAG-1
[0341] [Chemical formula 17]
[0342]
[0343] Acid Generator CPI-110TF
[0344] [Chemical formula 18]
[0345]
[0346] The composition F1 with the following composition was applied onto the photo-alignment film E1 using a bar coater. The coating formed on the photo-alignment film E1 was heated to 120°C with hot air, then cooled to 60°C, and then irradiated with 100 mJ / cm2 of mercury at a wavelength of 365 nm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film is irradiated with ultraviolet rays and then heated to 120°C while 500 mJ / cm 2 The coating film is irradiated with ultraviolet rays, thereby fixing the orientation of the liquid crystal compound, thereby producing a positive A plate F1.
[0347] The thickness of the positive A plate F1 is 2.5 μm, and Re(550) is 144 nm. In addition, the positive A plate satisfies the relationship Re(450)≤Re(550)≤Re(650). Re(450) / Re(550) is 0.82.
[0348]
[0349]
[0350] Polymerizable liquid crystal compound LA-1 (tBu represents tert-butyl group)
[0351] [Chemical formula 19]
[0352]
[0353] Polymerizable liquid crystal compound LA-2
[0354] [Chemical formula 20]
[0355]
[0356] Polymerizable liquid crystal compound LA-3
[0357] [Chemical formula 21]
[0358]
[0359] Polymerizable liquid crystal compound LA-4 (Me represents methyl)
[0360] [Chemical formula 22]
[0361]
[0362] Polymerization initiator PI-1
[0363] [Chemical formula 23]
[0364]
[0365] Leveling agent T-1
[0366] [Chemical formula 24]
[0367]
[0368] [Production of TAC film with positive C plate H1]
[0369] After applying the photo-alignment film-forming coating liquid G1 having the following composition using a bar coater, the coating liquid was dried with hot air at 60° C. for 60 seconds and further dried with hot air at 100° C. for 120 seconds to form the photo-alignment film G1 .
[0370]
[0371] A coating liquid H1 for forming a positive C plate with the following composition was applied on the photo-alignment film G1, and the obtained coating film was aged at 60° C. for 60 seconds and then heated at 70 mW / cm in air. 2 An air-cooled metal halide lamp (manufactured by EYE GRAPHICS Co., Ltd.) was used to irradiate 1000 mJ / cm 2 The alignment state was fixed by ultraviolet rays, thereby vertically aligning the liquid crystal compound, thereby producing a positive C plate H1 with a thickness of 0.5 μm.
[0372] The Rth(550) of the obtained positive C plate was -60 nm.
[0373]
[0374]
[0375] Liquid crystal compound LC-1
[0376] [Chemical formula 25]
[0377]
[0378] Liquid crystal compound LC-2
[0379] [Chemical formula 26]
[0380]
[0381] Vertically aligned liquid crystal compound S01
[0382] [Chemical formula 27]
[0383]
[0384] Compound B03
[0385] [Chemical formula 28]
[0386]
[0387] [Preparation of adhesives N1 and N2]
[0388] Next, an acrylate polymer was prepared according to the following steps.
[0389] In a reaction vessel equipped with a condenser, a nitrogen inlet tube, a thermometer, and a stirring device, 95 parts by mass of butyl acrylate and 5 parts by mass of acrylic acid were polymerized by solution polymerization to obtain an acrylate polymer (NA1) having an average molecular weight of 2 million and a molecular weight distribution (Mw / Mn) of 3.0.
[0390] Next, the acrylate-based adhesives were prepared using the obtained acrylate polymer (NA1) according to the following composition. These compositions were coated on a release film surface-treated with a silicone-based release agent using a die coater, dried for 1 minute in an environment of 90 °C, and irradiated with ultraviolet rays (UV) under the following conditions to obtain the following acrylate-based adhesives N1 and N2 (adhesive layers). The composition and film thickness of the acrylate-based adhesives are shown below.
[0391] [UV irradiation conditions]
[0392] · Fusion's electrodeless lamp H bulb
[0393] · Illuminance 600 mW / cm 2 、 Light quantity 150 mJ / cm 2
[0394] UV illuminance and light quantity were measured using “UVPF-36” manufactured by EYE GRAPHICS Co., Ltd.
[0395]
[0396]
[0397]
[0398] (A) Multifunctional acrylate monomer: tris(acryloyloxyethyl)isocyanurate, molecular weight = 423, trifunctional type (manufactured by TOAGOSEI CO., LTD., product name "ARONIX M-315")
[0399] (B) Photopolymerization initiator: a mixture of benzophenone and 1-hydroxycyclohexyl phenyl ketone in a mass ratio of 1:1, "Irgacure 500" manufactured by Ciba Specialty Chemicals Co., Ltd.
[0400] (C) Isocyanate crosslinking agent: trimethylolpropane-modified toluene diisocyanate ("CORONATE L" manufactured by Nippon Polyurethane Industry Co., Ltd.)
[0401] (D) Silane coupling agent: 3-glycidyloxypropyltrimethoxysilane ("KBM-403" manufactured by Shin-Etsu Chemical Co., Ltd.)
[0402] [Production of UV Adhesive]
[0403] A UV adhesive composition having the following composition was prepared.
[0404]
[0405] CPI-100P
[0406] [Chemical formula 29]
[0407]
[0408] [Preparation of laminated body CPAC1]
[0409] The above-mentioned UV adhesive composition was used to pass 600mJ / cm 2The positive A plate F1 and the positive C plate H1 were bonded together by UV irradiation. The thickness of the UV adhesive layer was 3 μm. In addition, the surfaces bonded by the UV adhesive were subjected to corona treatment. Next, the support of the photo-alignment film E1 on the positive A plate F1 side was removed to prepare a phase difference plate AC1.
[0410] The light absorption anisotropic layer produced in Example 1 is bonded to the support side of the low-reflection surface film CV-LC5 (manufactured by FUJIFILM Corporation) using the above-mentioned adhesive N1. Next, the support contained in the light absorption anisotropic layer produced in Example 1 is removed, and the removed surface is bonded to the positive A plate F1 side of the above-mentioned phase difference plate AC1 using the above-mentioned adhesive N1. Next, the support on the positive C plate H1 side contained in the above-mentioned phase difference plate AC1 is removed, thereby producing the laminate CPAC1. At this time, the angle formed by the absorption axis of the light absorption anisotropic film C1 contained in the above-mentioned laminate CPAC1 and the slow axis of the positive A plate F1 becomes 45°. In addition, the layer structure of the laminate CPAC1 is a low-reflection surface film CV-LC5, an adhesive layer N1, an oxygen barrier layer D1, a light absorption anisotropic film C1, a photo-alignment film B1, an adhesive layer N1, a positive A plate F1, a UV adhesive layer and a positive C plate H1.
[0411] The GALAXY S5 manufactured by SAMSUNG equipped with an organic EL panel (organic EL display element) was disassembled, and the touch panel with a circular polarizer was peeled off from the organic EL display device, and then the circular polarizer was peeled off from the touch panel, so that the organic EL display element, the touch panel and the circular polarizer were separated. Then, the separated touch panel was again bonded to the organic EL display element, and then the positive C plate 1 side of the laminated body CPAC1 produced above was bonded to the touch panel in a way that air could not enter, thereby producing an image display device.
[0412] As a result of displaying images using the image display device produced as described above, no light scattering from the front surface or the oblique surface was visually recognized.
[0413] Explanation of symbols
[0414] 1-light absorption anisotropic layer, 2-liquid crystal compound, 3-diffraction plane, 4-incident X-ray, 5-reflected X-ray, 6-diffracted X-ray.
Claims
1. A light absorption anisotropic layer comprising a dichroic substance and a liquid crystal compound, wherein: When the light absorption anisotropic layer is irradiated with X-rays and the X-ray diffraction pattern is measured by an in-plane diffraction method, the diffracted X-rays are measured in the following measurement area, and the diffraction angle 2θmax and the rotation angle φmax at which the peak intensity becomes the maximum are determined. When the peak intensity of the diffracted X-rays at the diffraction angle 2θmax and the rotation angle φmax is set to I(φmax) and the peak intensity of the diffracted X-rays at the diffraction angle 2θmax and the rotation angle φmax-10° is set to I(φmax-10), the following relationship (1) is satisfied, Measurement area: · Rotation angle φ of the in-plane direction of the light absorption anisotropic layer: 0 to 180° Diffraction angle 2θ: 0~10° Formula (1): I(φmax) / I(φmax-10)≥1.
6.
2. The light absorption anisotropic layer according to claim 1, wherein: When the light absorption anisotropic layer is fixed at a rotation angle of φmax-90° and the diffraction angle 2θ is measured in a range of more than 10° and less than 30°, a peak of diffracted X-rays showing a peak intensity of I(φmax)×0.2 times or more is observed.
3. The light absorption anisotropic layer according to claim 1 or 2, wherein: The light absorption anisotropic layer is formed using a liquid crystal composition containing a dichroic substance, a liquid crystal compound and a monofunctional compound. The molecular length D1 of the long axis direction of the liquid crystal compound The molecular length D2 in the long axis direction of the monofunctional compound Satisfying the following relationship (2): Formula (2): 0.2×D1≤D2≤0.45×D1.
4. The light absorption anisotropic layer according to claim 1 or 2, wherein: The dichroic substance includes at least two dichroic substances having maximum absorption wavelengths in the range of 550 to 700 nm.
5. A method for manufacturing a light absorption anisotropic layer, which is a method for manufacturing the light absorption anisotropic layer according to claim 1 or 2, comprising: In the light absorption anisotropic layer forming step, a liquid crystal composition layer including a dichroic substance, a liquid crystal compound, and a monofunctional compound is irradiated with ultraviolet rays in air to form a light absorption anisotropic layer.
6. The method for manufacturing a light absorption anisotropic layer according to claim 5, wherein: Including the following processes: The optically anisotropic layer after the light absorption anisotropic layer forming step was irradiated with ultraviolet rays under nitrogen. 7 . A laminate comprising the light absorption anisotropic layer according to claim 1 or 2 and a λ / 4 plate provided on the light absorption anisotropic layer. 8 . An image display device comprising the light absorption anisotropic layer according to claim 1 .