Tungsten oxide coating material for electrochromic element, tungsten oxide thin film, and dimming member

By combining tungsten oxide nanoparticle coatings with controlled crystallinity and particle size with metal cyano complex films, the problems of low cost and insufficient durability of tungsten oxide and metal cyano complex combinations in electrochromic materials have been solved, achieving high-speed response and high-contrast color changes, which are suitable for fields such as smart glass.

CN118974645APending Publication Date: 2024-11-15NATIONAL INSTITUTE OF ADVANCED INDUSTRIAL SCIENCE & TECHNOLOGY +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380026946.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-11
Filing Date
2023-03-08
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing technology, electrochromic materials composed of tungsten oxide and metal cyano complexes have shortcomings in terms of low cost, mass production, durability and energy consumption. They are difficult to achieve high-speed response and high-contrast color changes, and their light resistance is insufficient, which affects their application in fields such as smart glass.

Method used

By preparing tungsten oxide nanoparticle coatings, controlling their crystallinity and particle size, and combining them with binders and pH adjusters, a tungsten oxide film suitable for electrochromic elements is formed. This film is then combined with a metal cyano complex film, and an electrochromic element is prepared using a coating method.

Benefits of technology

High contrast and high-speed switching between tungsten oxide thin film and metal cyano complex film were achieved, solving the problems of low cost and durability in the prior art, and improving the response speed and color change contrast of electrochromic elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974645A_ABST
    Figure CN118974645A_ABST
Patent Text Reader

Abstract

A tungsten oxide coating material for an electrochromic element, which is a coating material for forming a tungsten oxide thin film having electrochromic properties, and which is characterized in that: the tungsten oxide coating material for an electrochromic element contains a solvent, tungsten oxide nanoparticles dispersed in the solvent, and a binder; the tungsten oxide nanoparticles have a half width of 2 DEG or less of a peak detected at 29 DEG + / -1 DEG when X-ray diffraction analysis (2 [theta]) is performed, and the tungsten oxide nanoparticles have a primary particle diameter of 5-25 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a technology of a tungsten oxide thin film used for an electrochromic element that changes color through an electrochemical redox reaction. Background Art

[0002] An electrochromic device (hereinafter, also referred to as "ECD") is a color-changing device that uses an electrochromic material (hereinafter, also referred to as "EC material") that changes color through an electrochemical redox reaction. The use of ECD (electrochromic device) in vehicle-mounted reflectors that control reflectivity through color change and windows of vehicles or buildings that can control light transmittance to improve air conditioning efficiency have been studied. Furthermore, the use of ECD in displays, sunglasses, etc. has also been studied. ECD, for example, has an EC material and a solid electrolyte.

[0003] In recent years, research on the application of ECD in dimming glass, especially for buildings or vehicles, has been actively conducted. EC materials for dimming glass include, for example, metal oxides represented by tungsten oxide (Patent Document 1), small molecules represented by viologen (Patent Document 2), polymers represented by PEDOT-PSS (poly(3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) (Patent Document 3), and coordination polymers represented by metal cyano complex nanoparticles (Patent Document 4).

[0004] In addition, ECDs using organic polymer materials and silver nanoparticles have recently been developed. However, organic polymer materials often have problems with light resistance and are not suitable for use in light-adjusting glass. In addition, the development of ECDs using silver nanoparticles has just begun, and the evaluation of light resistance and other aspects is not sufficient.

[0005] As described above, inorganic materials are considered to have certain advantages from the viewpoint of light resistance, etc. Among inorganic materials, metal oxide and metal cyano complex nanoparticles are already commercialized.

[0006] However, in applications using tungsten oxide as a main EC material, various materials including solid electrolytes are mainly produced by physical processes using magnetron sputtering, etc. That is, since it is a batch process using glass as a substrate, there are problems in mass production.

[0007] In addition, from the perspective of convenience, portability, flexibility, cost, etc., a flexible dimming film using a resin or the like as a transparent substrate has been developed (Patent Document 4). However, in the technology of Patent Document 4, in particular, a cooling device is required to suppress damage to the resin substrate due to input heat during film formation by a solid electrolyte manufacturing method, and the cost is high due to the dependence on process equipment. Therefore, the flexible dimming film using a resin substrate is difficult to commercialize.

[0008] For example, smart glass, a general term for dimming glass, is expanding its market size. However, smart glass, like low-emissivity glass, is manufactured using a batch process using evaporation or sputtering. Therefore, manufacturing costs and introduction and operation costs are obstacles to popularization, and there is a strong desire to achieve cost reduction through material and process development (Non-Patent Document 1).

[0009] An electrochromic element has been reported, in which, from the viewpoint of achieving low cost, an electrode in which a dispersion liquid in which Prussian blue-type metal cyano complex nanoparticles are dispersed in water is formed by a coating method or the like, and an electrode in which a dispersion liquid in which tungsten oxide nanoparticles are dispersed in water is formed by a coating method or the like, are combined as inorganic EC materials to produce a color-transparency change (Patent Document 5).

[0010] Prior art literature

[0011] Patent Literature

[0012] Patent document 1: Japanese Patent Application Laid-Open No. 08-254717.

[0013] Patent document 2: Japanese Patent Application Laid-Open No. 2009-215166.

[0014] Patent document 3: Japanese Patent Publication No. 2005-519316.

[0015] Patent document 4: Japanese Patent Application Laid-Open No. 2011-180469.

[0016] Patent document 5: Japanese Patent Application Publication No. 2018-021113.

[0017] Non-patent literature

[0018] Non-patent document 1: QUADRENNIAL TECHNOLOGY REVIEW, Chapter 5, p. 160, DOE, 2015. Summary of the invention

[0019] Problems to be solved by the invention

[0020] The combination of tungsten oxide and metal cyano complex as a dimming material has attracted attention. However, in order to popularize various applications using the combination of tungsten oxide and metal cyano complex, productivity (low cost, mass production), durability (number of times, usage environment), simplicity of introduction / control system, and reduction of energy usage that can meet the needs of various uses are listed as issues. In particular, EC materials that can achieve high-contrast color changes and high-speed responses between colored and colorless and transparent are desired, and electrochromic elements that utilize such EC materials are desired. Furthermore, in the application of energy-saving window materials, it is desired to achieve high-efficiency controllability of imparting thermal energy from the perspective of light resistance, etc. in the form of new EC materials.

[0021] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an electrochromic film capable of high-speed response and high-contrast color change by providing a new EC material, and a light-adjusting component as an electrochromic element using the electrochromic film.

[0022] Means for solving problems

[0023] The inventors have conducted intensive research, and as a result, have studied the production method and physical properties of tungsten oxide nanoparticles having various characteristics such as crystallinity, non-crystallinity, and oxygen defect introduction for EC materials. In addition, they found that the half-peak width of the peak detected at 29°±1° during X-ray diffraction analysis (2θ) is less than 2°, and that a binder is added to a dispersion obtained by dispersing tungsten oxide nanoparticles having a primary particle size of 5 to 25 nm in a solvent to form a coating, and that a thin film formed using the coating has physical properties suitable for application to electrochromic elements, thereby completing the present invention.

[0024] [1] A tungsten oxide coating for an electrochromic element, which is a coating for forming a tungsten oxide thin film having electrochromic properties, characterized in that the tungsten oxide coating for an electrochromic element comprises a solvent, tungsten oxide nanoparticles dispersed in the solvent, and a binder, the half-peak width of the peak detected at 29°±1° of the tungsten oxide nanoparticles during X-ray diffraction analysis (2θ) is less than 2°, and the primary particle size of the tungsten oxide nanoparticles is 5 to 25 nm.

[0025] [2] The tungsten oxide coating material for an electrochromic element according to claim 1, wherein the content of the tungsten oxide nanoparticles is 5 mass % or more and 30 mass % or less relative to the mass of the coating material.

[0026] [3] The tungsten oxide coating for electrochromic elements as described in [1] or [2] is characterized in that the binder is one or more selected from polyvinyl alcohol (PVA), sodium carboxymethyl cellulose (CMC), hydroxypropyl cellulose (HPC) and hydroxyethyl cellulose (HEC), and the content of the binder is greater than 0.1% by mass and less than 10% by mass relative to the mass of the coating.

[0027] [4] The tungsten oxide coating material for an electrochromic element according to any one of [1] to [3], wherein the tungsten oxide coating material for an electrochromic element contains a pH adjuster.

[0028] [5] The tungsten oxide coating for an electrochromic element as described in [4] is characterized in that the pH adjuster is one or more selected from potassium chloride (KCl), sodium chloride (NaCl), lithium chloride (LiCl), potassium hydroxide (KOH), sodium hydroxide (NaOH), and lithium hydroxide (LiOH).

[0029] [6] The tungsten oxide coating for an electrochromic element according to [4] or [5], wherein the pH is 5 to 7.

[0030] [7] The tungsten oxide coating for an electrochromic element as described in [1] to [6] is characterized in that the tungsten oxide coating for an electrochromic element can form a tungsten oxide thin film by a coating method.

[0031] [8] A tungsten oxide thin film having electrochromic properties and comprising tungsten oxide nanoparticles and a binder, wherein the half-width of a peak detected at 29°±1° of the tungsten oxide nanoparticles during X-ray diffraction analysis (2θ) is less than 2°, and the primary particle size of the tungsten oxide nanoparticles is 5 to 25 nm.

[0032] [9] The tungsten oxide thin film according to [8], wherein the tungsten oxide thin film contains a pH adjuster.

[0033]

[10] The tungsten oxide film as described in [8] or [9] is characterized in that an electrochromic reaction occurs in an electrolyte containing any one or more (trifluoromethanesulfonyl)imide salts of bis(trifluoromethanesulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, potassium bis(trifluoromethanesulfonyl)imide, and sodium bis(trifluoromethanesulfonyl)imide.

[0034]

[11] A dimming component, characterized in that the dimming component comprises: the tungsten oxide thin film described in [8] to

[10] ; a metal cyano complex thin film containing metal cyano complex nanoparticles whose coloration and bleaching changes caused by redox reactions are opposite to those of tungsten oxide, or an oxide thin film containing oxide nanoparticles whose coloration and bleaching changes caused by redox reactions are opposite to those of tungsten oxide; and an electrolyte layer, the electrolyte layer being located between the tungsten oxide thin film and the metal cyano complex thin film or between the tungsten oxide thin film and the oxide thin film.

[0035] The dispersion is a dispersion obtained by mixing tungsten oxide nanoparticles and a solvent. In contrast, the coating of the present invention is a substance obtained by adding a binder to the dispersion. Therefore, there is a difference between the dispersion and the coating.

[0036] Effects of the Invention

[0037] According to the present invention, by appropriately combining a thin film using the tungsten oxide nanoparticles and a thin film using metal cyano complex nanoparticles, an electrochromic element capable of switching between coloring and decoloring with high contrast and high speed can be manufactured and provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a cross-sectional view showing an example of the electrochromic element according to the embodiment.

[0039] Figure 2 This is a diagram showing the X-ray diffraction results of tungsten oxide nanoparticles used in Examples.

[0040] Figure 3 This is a transmission electron microscope photograph of tungsten oxide nanoparticles used in Examples.

[0041] Figure 4 These are field emission scanning electron microscope photographs of the tungsten oxide thin films of Examples and Comparative Examples.

[0042] Figure 5 1 is a cyclic voltammogram of the tungsten oxide thin film of the example and the comparative example.

[0043] Figure 6 Graphs 1 and 2 show changes in visible light transmission spectra of the tungsten oxide thin films of the examples and comparative examples.

[0044] Figure 7 It is a comparison of the cyclic voltammograms of the tungsten oxide thin films of Examples.

[0045] Figure 8 It is the cyclic voltammogram of ECD1 of Example.

[0046] Fig. 9 : is the visible light transmission spectrum of ECD1 of the example.

[0047] Fig.10 This is a photograph of the color change of ECD1 of the example.

[0048] Fig.11 is the total light transmission spectrum of ECD1 of the embodiment.

[0049] Fig.12 This is a photograph of the color change of ECD2 of the example.

[0050] Fig.13 : is the total light transmission spectrum of ECD2 of the embodiment.

[0051] Fig.14 : is the total light transmission spectrum of ECD3 of the example.

[0052] Fig.15 : is the total light transmission spectrum of ECD4 of the embodiment.

[0053] Fig.16 This is a graph showing the relationship between the amount of tungsten oxide nanoparticles 1 added and the pH of the coating material of the example.

[0054] Fig.17 This is a graph showing the relationship between the amount of 0.1 M NaOH added and the pH of the coating material of the Examples.

[0055] Fig.18 The figure shows the change in the visible light transmission spectrum of the tungsten oxide thin film of the example.

[0056] Fig.19 It is a graph showing the results of the cycle test of ECD5 of the example.

[0057] Fig. 20 It is a graph showing the results of the cycle test of ECD5 of the example.

[0058] Fig.21 The diagram shows changes in the visible light transmission spectrum when measuring the withstand voltage characteristics for ECD5 and ECD6 of Examples.

[0059] Fig. 22 It is a graph showing the results of the cycle test of ECD7 of the example. DETAILED DESCRIPTION

[0060] [Tungsten oxide coating for electrochromic elements]

[0061] The tungsten oxide (WO3) coating for electrochromic elements of the present invention is described. The tungsten oxide coating for electrochromic elements of the present invention (hereinafter, also referred to as "coating") is a coating for forming a tungsten oxide thin film having electrochromic properties, and is used for electrochromic elements. Specifically, the coating of the present invention includes a solvent, tungsten oxide nanoparticles dispersed in the solvent, and a binder.

[0062] In addition, in the following description, "A to B" which shows a numerical range has the same meaning as A or more and B or less.

[0063] The tungsten oxide nanoparticles for coating materials are characterized in that the half-value width of the peak detected at 29°±1° in X-ray diffraction analysis (2θ) is 2° or less, and the primary particle size is 5 to 25 nm.

[0064] X-ray diffraction analysis (2θ) can be performed using, for example, Cu-Kα radiation (wavelength ) was performed with a tube voltage of 40 kV, a tube current of 40 mA, an operating axis of 2θ / θ, a scanning range (2θ) of 10° to 60°, a scanning speed of 0.1° / sec, and a step width of 0.02°.

[0065] The peak detected at 29°±1° used for determining the half-peak width typically uses the strongest peak within the range of 29°±1°. The strongest peak refers to the peak with the largest intensity ratio. The half-peak width is determined using the smaller value of the root portion of the two ends of the peak as the reference value. The position from the reference value to the peak top is taken as the peak height. In addition, the width of the peak at half the peak height is taken as the half-peak width. It should be noted that when there are two peaks at 29°±1° and the bottoms of the peaks overlap, the half-peak width can also be obtained by analyzing the software of the X-ray diffraction device.

[0066] X-ray diffraction indicates the crystallinity of tungsten oxide nanoparticles. If the crystallinity is good, a sharp peak with a small half-width can be obtained. The half-width of the peak detected at 29°±1° during X-ray diffraction analysis (2θ) is 2° or less, indicating that crystal defects are suppressed. Crystal defects refer to the disorder of crystal arrangement. Due to the presence of crystal defects, there are defects at the lower end of the conductor with a band gap, and the apparent band gap is narrow. As a result, absorption occurs in the visible light region. Based on the above reasons, the upper limit of the half-width of the peak detected at 29°±1° during X-ray diffraction analysis (2θ) is 2° or less.

[0067] The lower limit of the half-peak width is not particularly limited, preferably 0.1 ° or more. When the half-peak width is less than 0.1 °, it means that the repeatability of crystallization is high. This shows that the primary particle size of the primary particle is greater than 25nm. If the primary particle size becomes larger, the transmitted light will scatter, and therefore, the transmittance is reduced under full wavelength conditions. Therefore, when performing X-ray diffraction analysis (2θ), the lower limit of the half-peak width of the peak detected at 29 ° ± 1 ° is preferably 0.1 ° or more.

[0068] The primary particle size of tungsten oxide nanoparticles refers to the diameter of the primary particles, which can be identified, for example, based on structural analysis using a transmission electron microscope (TEM). It should be noted that, in the case where a ligand or the like is adsorbed on the surface of the tungsten oxide nanoparticles, the primary particle size is derived by removing the ligand from the particles as primary particles. The primary particle size is the length of the longest diagonal line of the particle. The longest diagonal line of the primary particles present in the TEM image with a field of view of 60nm×60nm is measured. In addition, only particles whose outlines of the primary particles are known are counted. In addition, for primary particles, more than 10 particles are observed. For example, particles whose outlines cannot be observed due to overlap between primary particles are not counted.

[0069] From the viewpoint of increasing the specific surface area to increase the electrochemical response speed (i.e., the color change speed of switching coloring and decolorization) and the viewpoint of forming a smooth film, the upper limit of the primary particle size in the tungsten oxide nanoparticles is below 25nm. The lower limit of the primary particle size in the tungsten oxide nanoparticles is not particularly limited, for example, above 5nm.

[0070] Relative to the coating mass (that is, when all coatings are set to 100 mass %), the lower limit of the content of tungsten oxide nanoparticles is more than 5 mass %, preferably more than 10 mass %. Relative to the coating mass, the upper limit of the content of tungsten oxide nanoparticles is less than 30 mass %, preferably less than 25 mass %. By setting the content of tungsten oxide nanoparticles to the above-mentioned range, a homogeneous tungsten oxide film can be manufactured.

[0071] As for the method for producing the tungsten oxide nanoparticles used in the coating material of the present invention, any known production technology may be adopted. An example of the method for producing the tungsten oxide nanoparticles is shown below.

[0072] The method for producing tungsten oxide (WO3) particles includes a sublimation step. The sublimation step is a step of producing tungsten oxide nanoparticles by sublimating a precursor or a precursor solution of tungsten oxide nanoparticles in an oxygen environment. The precursor of tungsten oxide nanoparticles is metal tungsten powder or tungsten compound powder, and the precursor solution of tungsten oxide nanoparticles is a solution formed by dissolving these precursors in a solvent (e.g., water, alcohol).

[0073] As the tungsten compound, known compounds capable of producing tungsten oxide (WO 3 ) particles can be used, and examples thereof include various tungsten oxides (eg, WO 3 , WO 2 ), tungsten carbide, ammonium tungstate, calcium tungstate, tungstic acid, and the like.

[0074] In the sublimation process, the precursor or precursor solution of the tungsten oxide nanoparticles is sublimated in an oxygen environment using any known technique. For example, in the sublimation process, any one of plasma treatment, arc discharge treatment, laser treatment, and electron beam treatment is used, and inductively coupled plasma treatment is preferably used.

[0075] By appropriately setting the various conditions of the treatment (plasma treatment, arc discharge treatment, laser treatment or electron beam treatment) performed in the sublimation process, and the average particle size of the metal tungsten powder and the tungsten compound powder, it is possible to produce tungsten oxide nanoparticles having a half-peak width of less than 2° and a primary particle size of 5 to 25 nm when performing X-ray diffraction analysis (2θ) at 29°±1°.

[0076] It should be noted that the manufacturing method may also include other steps besides the sublimation step. For example, in order to increase the ratio of tungsten oxide (WO3) in the powder after the sublimation step, a heat treatment step may be included after the sublimation step.

[0077] As the solvent used in the coating, any solvent that can disperse the tungsten oxide nanoparticles and does not affect the tungsten oxide nanoparticles can be used. For example, water or alcohol is used as the solvent. As the alcohol, one or more alcohols can be selected from isopropyl alcohol, ethanol, methanol, n-propyl alcohol, isobutyl alcohol, n-butyl alcohol, etc. From the viewpoint of improving the dispersibility of the tungsten oxide nanoparticles, for example, water is preferably used alone.

[0078] The binder used in the coating is not particularly limited, and one or more binders selected from organic binders or inorganic binders can be used arbitrarily. As the organic binder, for example, cellulose derivatives, vinyl resins, fluorine resins, silicone resins, acrylic resins, epoxy resins, polyester resins, melamine resins, urethane resins, alkyd resins, etc. are used. As the inorganic binder, for example, products obtained by decomposing hydrolyzable silicon compounds such as alkyl silicates, silicon halides, and partial hydrolyzates thereof, organic polysiloxane compounds and polycondensates thereof, silicon dioxide, colloidal silicon dioxide, water glass, silicon compounds, phosphates such as zinc phosphate, metal oxides such as zinc oxide and zirconium oxide, hydrogen phosphates, cement, gypsum, lime, glass frit for enamel, etc. are used.

[0079] From the viewpoint of producing a homogeneous tungsten oxide thin film, for example, one or more selected from polyvinyl alcohol (PVA), sodium carboxymethylcellulose (CMC), hydroxypropylcellulose (HPC), and hydroxyethylcellulose (HEC) are preferably used as the binder.

[0080] The lower limit of the content of the binder is 0.1% by mass or more, preferably 0.15% by mass or more, relative to the mass of the coating (i.e., when the total coating is 100% by mass). The upper limit of the content of the binder is 10% by mass or less, preferably 5% by mass or less, and more preferably 2% by mass or less, relative to the mass of the coating. By setting the content of the binder within the above range, the coating has a longer shelf life, and even though the film-forming tungsten oxide thin film contains a binder, coarse agglomerates cannot be observed.

[0081] The coating material of the present invention may further contain a pH adjuster.

[0082] The pH adjuster used in the coating is not particularly limited, and one or more pH adjusters selected from pH adjusters that do not hinder electrochemical reactions can be used arbitrarily. The electrochromic element of the present invention is driven by, for example, a redox reaction related to lithium, potassium, and sodium, and therefore, the pH adjuster is one or more selected from potassium chloride (KCl), sodium chloride (NaCl), lithium chloride (LiCl), potassium hydroxide (KOH), sodium hydroxide (NaOH), and lithium hydroxide (LiOH).

[0083] The content of the pH adjuster in the coating is appropriately controlled according to the solid amount of the tungsten oxide nanoparticles. The pH of the coating containing the pH adjuster is, for example, 2 to 8. However, from the viewpoint of achieving good durability, the pH of the coating is preferably 3 or more, more preferably 5 to 7, and further preferably about 5.

[0084] In addition to the binder and pH adjuster, the coating may also contain various other additives, such as defoamers, crosslinking agents, curing catalysts, pigment dispersants, emulsifiers, film-forming aids, thickeners, neutralizers, preservatives, and the like.

[0085] [ECD]

[0086] Hereinafter, the electrochromic element (hereinafter referred to as "ECD") of the present invention is described. The electrochromic element is used as a light control member capable of adjusting light.

[0087] Figure 1 1 is a cross-sectional view showing an example of ECD 100 according to the present embodiment. Figure 1As shown, ECD100 includes a first electrochromic layer 10 (an example of a "tungsten oxide thin film"), a second electrochromic layer 20 (an example of a "metal cyano complex thin film"), an electrolyte layer 30, a first transparent electrode layer 40, a second transparent electrode layer 50, a first insulating layer 60, and a second insulating layer 70. These layers (10, 20, 30, 40, 50, 60, 70) are stacked to form ECD100.

[0088] The electrolyte layer 30 is located between the first electrochromic layer 10 and the second electrochromic layer 20. The first transparent electrode layer 40 is located on the surface of the first electrochromic layer 10 opposite to the electrolyte layer 30. The second transparent electrode layer 50 is located on the surface of the second electrochromic layer 20 opposite to the electrolyte layer 30. The first insulating layer 60 is located on the surface of the first transparent electrode layer 40 opposite to the first electrochromic layer 10. The second insulating layer 70 is located on the surface of the second transparent electrode layer 50 opposite to the second electrochromic layer 20.

[0089] The first electrochromic layer 10 and the second electrochromic layer 20 are layers having electrochromic properties, and the colors are reversibly changed (the colored state and the decolorized state are reversibly changed) by redox reaction. The first electrochromic layer 10 is colored in the reduced state and decolorized in the oxidized state. On the other hand, the second electrochromic layer 20 is decolorized in the reduced state and colored in the oxidized state.

[0090] In general, the ECD 100 is driven by applying a voltage between the first transparent electrode layer 40 and the second transparent electrode layer 50. Specifically, when a voltage is applied between the first transparent electrode layer 40 and the second transparent electrode layer 50, the ECD 100 changes between a first state and a second state.

[0091] In the first state, the first electrochromic layer 10 is in an oxidized state (i.e., a decolorized state), and the second electrochromic layer 20 is in a reduced state (i.e., a decolorized state). On the other hand, in the second state, the first electrochromic layer 10 is in a reduced state (i.e., a colored state), and the second electrochromic layer 20 is in an oxidized state (i.e., a colored state). It can be understood from the above description that the color change in the ECD 100 can be controlled according to the application of voltage.

[0092] (1) First electrochromic layer 10

[0093] The first electrochromic layer 10 includes the above-mentioned tungsten oxide (WO3) particles and a binder. That is, the first electrochromic layer 10 is a tungsten oxide thin film. Tungsten oxide nanoparticles are colorless (almost colorless and transparent) in an oxidized state and are colored blue in a reduced state.

[0094] The thickness of the first electrochromic layer 10 is appropriately set according to the purpose, and is, for example, 500 to 1500 nm. It should be noted that the thickness of the first electrochromic layer 10 may be constant or may not be constant (ie, may vary depending on the position in the plane direction).

[0095] The present invention is a film having electrochromic properties and comprising tungsten oxide nanoparticles and a binder, and can also be considered as a tungsten oxide film in which the half-peak width of the peak detected at 29°±1° of the tungsten oxide nanoparticles during X-ray diffraction analysis (2θ) is less than 2° and the primary particle size is 5 to 25 nm. Furthermore, the tungsten oxide film of the present invention may also contain the above-mentioned pH adjuster.

[0096] (2) Second electrochromic layer 20

[0097] The second electrochromic layer 20 includes a material whose coloring and color-removing changes caused by redox reactions are opposite to those of tungsten oxide used in the first electrochromic layer 10, and is preferably a metal cyano complex nanoparticle or an oxide nanoparticle. It should be noted that the second electrochromic layer 20 including the metal cyano complex nanoparticles is an example of a metal cyano complex thin film, and the second electrochromic layer 20 including the oxide nanoparticles is an example of an oxide thin film.

[0098] When metal cyano complex nanoparticles or oxide nanoparticles are used in the second electrochromic layer 20, any type of metal cyano complex nanoparticles may be used as long as they can reversibly undergo redox reactions. Metal cyano complex nanoparticles or oxide nanoparticles are materials that are colored in an oxidized state and decolorized in a reduced state.

[0099] The following is a detailed description of the use of metal cyano complex nanoparticles in the second electrochromic layer 20. As the metal cyano complex nanoparticles, it is suitable to use a metal cyano complex nanoparticle represented by the general formula "AxM α [M β Prussian blue type metal cyano complex particles represented by "(CN)6]y·zH2O".

[0100] A is an atom selected from the group consisting of hydrogen, lithium, sodium, and potassium.

[0101] As M α , is one or more metal atoms selected from the group consisting of vanadium, chromium, manganese, iron, ruthenium, cobalt, rhodium, nickel, palladium, platinum, copper, silver, zinc, lanthanum, europium, gadolinium, lutetium, barium, strontium, and calcium.

[0102] As M β , is one or more metal atoms selected from the group consisting of vanadium, chromium, molybdenum, tungsten, manganese, iron, ruthenium, cobalt, nickel, platinum, and copper. It should be noted that x is 0 to 3, y is 0.3 to 1.5, and z is 0 to 30.

[0103] As the metal cyano complex, one species represented by the above general formula may be used alone, or a plurality of species may be mixed and used.

[0104] From the viewpoint that improves electrochemical response speed, form the viewpoint of smooth film from improving specific surface area, the upper limit value of the primary particle diameter in the metal cyano complex nanoparticle is below 300nm, is preferably below 100nm, more preferably below 50nm.The lower limit value of the primary particle diameter in the metal cyano complex nanoparticle is not particularly limited, for example, is more than 4nm, is preferably more than 5nm, more preferably more than 6nm.It should be noted that, for the assay method of the primary particle diameter in the metal cyano complex nanoparticle, is identical with the assay method of the primary particle diameter of above-mentioned tungsten oxide nanoparticle.

[0105] The thickness of the second electrochromic layer 20 is appropriately set according to the purpose, and is, for example, 500 to 3000 nm. It should be noted that the thickness of the second electrochromic layer 20 may be constant or may not be constant (ie, may vary depending on the position in the plane direction).

[0106] (3) Electrolyte layer 30

[0107] The electrolyte layer 30 is a layer containing an electrolyte. The first electrochromic layer 10 and the second electrochromic layer 20 undergo an electrochromic reaction in the electrolyte.

[0108] As the electrolyte used for the electrolyte layer 30, it is preferred to include a (trifluoromethanesulfonyl)imide salt. As the (trifluoromethanesulfonyl)imide salt, one or more of bis(trifluoromethanesulfonyl)imide, bis(trifluoromethanesulfonyl)imide lithium, bis(trifluoromethanesulfonyl)imide potassium, and bis(trifluoromethanesulfonyl)imide sodium are included. Among them, bis(trifluoromethanesulfonyl)imide potassium is preferred.

[0109] The content of the electrolyte in the electrolyte layer 30 is not particularly limited, but is, for example, 0.1 to 1.5 mol / kg, preferably 0.5 to 1.5 mol / kg, from the viewpoint of increasing the electrochemical response speed in the ECD 100 .

[0110] In addition, the electrolyte layer 30 may contain a solvent and a resin in addition to the electrolyte. As the solvent contained in the electrolyte layer 30, a known solvent that can dissolve the electrolyte contained in the electrolyte layer 30 can be used, for example, a chain carbonate such as dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate, a cyclic carbonate such as ethylene carbonate, propylene carbonate, and butylene carbonate, aliphatic carboxylates such as methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, methyl butyrate, methyl isobutyrate, and trimethyl methyl acetate, aromatic carboxylates such as methyl benzoate and ethyl benzoate, lactones such as γ-butyrolactone and γ-valerolactone, and ε-caprolactam. , lactams such as N-methylpyrrolidone, tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, cyclic ethers such as 1,3-dioxolane, chain ethers such as 1,2-diethoxyethane and ethoxymethoxyethane, sulfones such as methyl ethyl sulfone, cyclopentane, 3-methylcyclopentane, 2,4-dimethylcyclopentane, nitriles such as acetonitrile, propionitrile, methoxypropionitrile, phosphate esters such as trimethyl phosphate, ethyl dimethyl phosphate, diethyl methyl phosphate, triethyl phosphate, alcohols such as ethanol and 2-propanol, glycols such as ethylene glycol, propylene glycol, polyethylene glycol, and water, etc.

[0111] The resin contained in the electrolyte layer 30 is not particularly limited, and one or more kinds of resins can be selected from known resins such as acrylic resin, urethane resin, silicone resin, epoxy resin, vinyl chloride resin, vinyl resin, melamine resin, phenolic resin, methyl methacrylate resin, polyvinyl alcohol resin, polyvinyl acetal resin, polyethylene oxide resin, etc. The electrolyte layer 30 contains a resin, so that the mechanical strength of the electrolyte layer 30 can be improved.

[0112] The electrolyte layer 30 may contain any other various additives within the range not impairing the function of the electrolyte layer 30. Examples of known additives include ultraviolet absorbers, antioxidants, lubricants, plasticizers, mold release agents, tackifiers, coloring inhibitors, flame retardants, antistatic agents, and the like.

[0113] The thickness of the electrolyte layer 30 is appropriately set according to the purpose, and is, for example, 50 μm to 0.3 mm. The thickness of the electrolyte layer 30 may be constant or may not be constant (ie, may vary depending on the position in the plane direction).

[0114] It should be noted that the electrolyte layer 30 may be colored or colorless (transparent). The color of the electrolyte layer 30 can be appropriately changed according to the purpose.

[0115] (4) First transparent electrode layer 40 and second transparent electrode layer 50

[0116] The first transparent electrode layer 40 and the second transparent electrode layer 50 are layers made of transparent conductive materials. As the conductive material constituting the first transparent electrode layer 40 and the second transparent electrode layer 50, there is no particular limitation as long as it is a material that does not corrode or deteriorate to a level that is problematic in practical use when used as an electrochemical element. For example, conductive oxides such as indium tin oxide (ITO), zinc oxide, and materials doped with metals such as aluminum, silver, and titanium, precious metals such as gold and platinum, alloys or metals with corrosion resistance due to a passivation film such as stainless steel and aluminum, and carbon materials such as graphene or carbon nanotubes can be used. From the viewpoint of durability, FTO (fluorine-doped tin) and TCO (transparent conductive oxide) are particularly preferred as transparent electrode layers (40, 50).

[0117] The thickness of the first transparent electrode layer 40 and the second transparent electrode layer 50 is appropriately set according to the purpose, for example, 100 to 300 nm. It should be noted that the thickness of the first transparent electrode layer 40 and the second transparent electrode layer 50 may be constant or not constant (that is, it may be different according to the position in the surface direction).

[0118] However, from the viewpoint of increasing the contact area between the first electrochromic layer 10 and the first transparent electrode layer 40 and improving the electrochemical response speed, the thickness of the first transparent electrode layer 40 may not be constant. Specifically, the surface of the first transparent electrode layer 40 is formed with concavoconvexity (i.e., the smoothness of the surface is reduced). The convex portion in the surface of the first transparent electrode layer 40 is formed of, for example, a conductive material. Similarly, from the viewpoint of increasing the contact area between the second electrochromic layer 20 and the second transparent electrode layer 50 to improve the response speed, the thickness of the second transparent electrode layer 50 may not be constant.

[0119] The first transparent electrode layer 40 may also contain known additives for the purpose of improving the adhesion with the first electrochromic layer 10 and inhibiting corrosion. Similarly, the second transparent electrode layer 50 may also contain known additives for the purpose of improving the adhesion with the second electrochromic layer 20 and inhibiting corrosion. Examples of known additives include ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, tackifiers, coloring inhibitors, flame retardants, antistatic agents, and the like.

[0120] (5) First insulation layer 60 and second insulation layer 70

[0121] The first insulating layer 60 and the second insulating layer 70 are layers made of a transparent insulating material. For example, the first insulating layer 60 and the second insulating layer 70 are formed of a resin, glass, etc. As the resin, for example, polyethylene terephthalate (PET), polycarbonate, polyethylene naphthalate (PEN), etc. can be cited. It should be noted that the first insulating layer 60 and the second insulating layer 70 may also contain known additives such as ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, tackifiers, coloring inhibitors, flame retardants, antistatic agents, etc.

[0122] The thickness of the first insulating layer 60 and the second insulating layer 70 is, for example, 50 μm to 1.1 mm. It should be noted that the thickness of the first insulating layer 60 and the second insulating layer 70 may be constant or may not be constant (ie, may be different depending on the position in the plane direction).

[0123] As described above, ECD100 changes between the first state and the second state due to the application of voltage. Here, it is assumed that Prussian blue type metal complex particles (e.g., iron-ferrocyanide complex particles) are used as metal cyanide complex nanoparticles in the second electrochromic layer 20 and a transparent material is used in the electrolyte layer 30. In the above configuration, the color of ECD100·BR> changes from dark blue to colorless and transparent. Tungsten oxide is almost colorless and transparent in an oxidized state, and iron-ferrocyanide complex particles are almost colorless and transparent in a reduced state. Therefore, ECD100 becomes colorless and transparent in the first state. On the other hand, tungsten oxide is colored blue in a reduced state, and iron-ferrocyanide complex nanoparticles are colored blue in an oxidized state. Therefore, ECD100 is dark blue in the second state.

[0124] The ECD100 of the present invention is not limited to the above configuration. For example, the first insulating layer 60 and the second insulating layer 70 may be omitted in the ECD100. In addition, the ECD100 may also include layers other than the layers (10, 20, 30, 40, 50, 60, 70) described above. For example, other layers (e.g., insulating layers) may be provided between the first transparent electrode and the first insulating layer 60. Similarly, other layers may be provided between the second transparent electrode and the second insulating layer 70.

[0125] According to the ECD of this embodiment, by combining the first electrochromic layer 10 containing tungsten oxide (WO3) nanoparticles and the second electrochromic layer 20 containing metal cyano complex nanoparticles, a high-speed response can be achieved, and a color change with high contrast can be obtained.

[0126] An example of a method for manufacturing an ECD is described below. For example, two commercially available substrates with transparent electrodes (e.g., ITO-coated glass) are used as the substrate. When ITO-coated glass is used as the substrate, ITO is equivalent to Figure 1 The first transparent electrode layer 40 and the second transparent electrode layer 50 in the same manner, the glass is equivalent to the first insulating layer 60 and the second insulating layer 70. The two substrates are respectively referred to as the first substrate (the second transparent electrode layer 50 + the second insulating layer 70) and the second substrate (the first transparent electrode layer 40 + the first insulating layer 60).

[0127] First, on the first substrate, a coating method such as a wet coating process such as slit coating, spin coating, rod coating, spray coating, etc. is used to form a second electrochromic layer 20 (metal cyano complex film) using a coating containing metal cyano complex nanoparticles, thereby manufacturing a first film-forming substrate. Similarly, on the second substrate, using this method, the tungsten oxide coating of the present invention is used to form a first electrochromic layer 10 (tungsten oxide film), thereby manufacturing a second film-forming substrate. An electrolyte layer 30 is formed on the first film-forming substrate using a dispenser. A UV curable resin is further used to form a sealing structure on the periphery. Alternatively, the sealing structure can be formed using a commercially available electronic equipment sealing tape, etc.

[0128] Then, the second film-forming substrate is covered on the first film-forming substrate from above, and stamped and bonded in a vacuum chamber. When a sealing tape is used, there is no problem even if bonding is performed under room temperature and atmospheric pressure. In the manner described above, an ECD consisting of a structure of a first insulating layer 60 / a first transparent electrode layer 40 / a first electrochromic layer 10 / an electrolyte layer 30 / a second electrochromic layer 20 / a second transparent electrode layer 50 / a second insulating layer 70 can be obtained.

[0129] Example

[0130] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples.

[0131] [Tungsten Oxide Nanoparticles]

[0132] Tungsten oxide nanoparticles 1 to 4 were produced as follows.

[0133] <Tungsten oxide nanoparticles 1>

[0134] Tungsten oxide nanoparticles are obtained by pulverizing tungsten oxide nanoparticles produced by a sublimation process using a dry bead mill.

[0135] <Tungsten oxide nanoparticles 2>

[0136] Tungsten oxide nanoparticles produced using a sublimation process.

[0137] <Tungsten oxide nanoparticles 3>

[0138] Tungsten oxide nanoparticles are produced by a sublimation process and then fired at 450°C in the air.

[0139] <Tungsten oxide nanoparticles 4>

[0140] Tungsten oxide nanoparticles are produced by a sublimation process and then fired at 550°C in the air.

[0141] Figure 2 The results of analyzing tungsten oxide nanoparticles 1 to 4 using powder X-ray diffraction are shown. X-ray diffraction uses Cu-Kα radiation (wavelength It should be noted that the diffraction information of tungsten oxide nanoparticles 1-4 is consistent with the diffraction information of tungsten oxide nanoparticles retrieved from the standard reagent database.

[0142] For tungsten oxide nanoparticles 1 to 4, the half-peak width of the peak (strongest peak) detected at 29°±1° in X-ray diffraction analysis (2θ) was determined. The determined half-peak width is as follows.

[0143] Tungsten oxide nanoparticles 1: 0.9°.

[0144] Tungsten oxide nanoparticles 2: 0.7°.

[0145] Tungsten oxide nanoparticles 3: 0.7°.

[0146] Tungsten oxide nanoparticles 4: 0.6°.

[0147] In particular, a broad peak was observed in tungsten oxide nanoparticle 1, indicating that the crystallinity was low.

[0148] Figure 3 : is a transmission electron microscope photograph of tungsten oxide nanoparticles 1 and tungsten oxide nanoparticles 4. It can be confirmed that the primary particle diameters of tungsten oxide nanoparticles 1 and tungsten oxide nanoparticles 4 are both within the range of 5 to 25 nm. Specifically, tungsten oxide nanoparticles 1 are aggregates of nanoparticles (primary particles) with a diameter of about 10 nm or less, and tungsten oxide nanoparticles 4 are aggregates of nanoparticles with a diameter of about 20 nm.

[0149] [Tungsten oxide coating for electrochromic elements]

[0150] The tungsten oxide coating material for an electrochromic element of the example and the dispersion liquid of the comparative example were prepared as follows.

[0151] <Example 1>

[0152] After 25 g of tungsten oxide nanoparticles 1 (powder sample) were suspended in 75 mL of water, PVA was added as a binder to reduce surface tension and stirred to obtain the coating of Example 1. PVA was added so that the PVA solid content relative to the entire coating became 0.63 mass %.

[0153] <Example 2>

[0154] The same procedure as in Example 1 was performed except that PVA was added so that the PVA solid content relative to the entire coating material became 0.15 mass %.

[0155] <Example 3>

[0156] The same procedure as in Example 1 was performed except that PVA was added so that the PVA solid content relative to the entire coating material became 1.29 mass %.

[0157] <Example 4>

[0158] The same procedure as in Example 1 was performed except that CMC was added as a binder instead of PVA. CMC was added so that the solid content of the whole coating material was 1.32% by mass.

[0159] <Example 5>

[0160] The same procedure as in Example 1 was performed except that HPC was added as a binder instead of PVA. HPC was added so that the solid content of the HPC relative to the entire coating material became 0.68% by mass.

[0161] <Example 6>

[0162] The same procedure as in Example 1 was performed except that HEC was added as a binder instead of PVA. HEC was added so that the solid content of HEC relative to the entire coating material became 0.83% by mass.

[0163] <Comparative Example 1>

[0164] Except that no binder was added, the same procedure as in Example 1 was performed. That is, Comparative Example 1 was not a coating but a simple dispersion.

[0165] [Tungsten oxide thin film]

[0166] The tungsten oxide thin films (first electrochromic layers) of Examples and Comparative Examples were produced as follows.

[0167] <Example 1-A>

[0168] A tungsten oxide thin film of Example 1-A was produced on an ITO-coated glass substrate composed of glass (first insulating layer) coated with ITO (first transparent electrode layer) using the coating material of Example 1. The tungsten oxide thin film was formed by spin coating.

[0169] First, the coating of Example 1 was filtered before use to adjust the viscosity to about 15 mPa·s. 2 mL was measured with a micropipette and dropped onto a 100 mm square ITO-coated glass substrate set in a spin coater, and then rotated at 400 rpm for 10 seconds and then at 800 rpm for 10 seconds to form a thin film. The film was naturally dried to obtain Example 1-A. The film thickness of the tungsten oxide thin film of Example 1-A was about 1000 nm.

[0170] <Example 1-B>

[0171] The tungsten oxide thin film of Example 1-B was formed on an ITO-coated polyethylene terephthalate (PET) substrate composed of polyethylene terephthalate (first insulating layer) coated with ITO (first transparent electrode layer) using the coating of Example 1. The tungsten oxide thin film was formed by spin coating.

[0172] First, the coating of Example 1 was filtered before use to adjust the viscosity to about 15 mPa·s. 500 μL was measured with a micropipette and dropped onto a 50 mm square ITO-coated PET substrate set in a spin coater, and then rotated at 400 rpm for 10 seconds and then at 800 rpm for 10 seconds to form a thin film. The film was naturally dried to obtain Example 1-B. The film thickness of the tungsten oxide thin film of Example 1-B was about 1000 nm.

[0173] <Example 1-C>

[0174] The same process as in Example 1-B was performed except that the tungsten oxide thin film of Example 1-C was formed on an ITO-coated polycarbonate substrate composed of polycarbonate (first insulating layer) coated with ITO (first transparent electrode layer). The film thickness of the tungsten oxide thin film of Example 1-C was about 1000 nm.

[0175] <Example 1-D>

[0176] The tungsten oxide thin film of Example 1-D was the same as Example 1-B except that it was formed on an ITO-coated polyethylene naphthalate (PEN) substrate composed of polyethylene naphthalate (first insulating layer) coated with ITO (first transparent electrode layer). The film thickness of the tungsten oxide thin film of Example 1-D was about 1000 nm.

[0177] <Example 2-A>

[0178] The tungsten oxide thin film of Example 2-A was formed on the same ITO-coated glass substrate as that used in Example 1-A using the coating material of Example 2. The tungsten oxide thin film was formed using a spin coating method.

[0179] First, the coating of Example 2 was filtered before use to adjust the viscosity to about 15 mPa·s. 500 μL was measured with a micropipette and dropped onto a 50 mm square ITO-coated glass substrate set in a spin coater, and then rotated at 400 rpm for 10 seconds and then at 800 rpm for 10 seconds to form a thin film. The film was naturally dried to obtain Example 2-A. The film thickness of the tungsten oxide thin film of Example 2-A was about 1000 nm.

[0180] <Example 3-A>

[0181] The same process as Example 2-A was performed except that the coating material of Example 3 was used. The film thickness of the tungsten oxide thin film of Example 3-A was about 1000 nm.

[0182] <Example 4-A>

[0183] A tungsten oxide thin film of Example 4-A was formed on the same ITO-coated glass substrate as that used in Example 1-A using the coating material of Example 4. The tungsten oxide thin film was formed using a spin coating method.

[0184] First, the coating of Example 4 was filtered before use to adjust the viscosity to about 15 mPa·s. 400 μL was measured with a micropipette and dropped onto a 50 mm square ITO-coated glass substrate set in a spin coater, and then rotated at 350 rpm for 5 minutes and then at 1000 rpm for 5 seconds to form a thin film. The film was naturally dried to obtain Example 4-A. The film thickness of the tungsten oxide thin film of Example 4-A was about 1000 nm.

[0185] <Example 5-A>

[0186] A tungsten oxide thin film of Example 5-A was formed on the same ITO-coated glass substrate as that used in Example 1-A using the coating material of Example 5. The tungsten oxide thin film was formed using a spin coating method.

[0187] First, the coating of Example 5 was filtered before use to adjust the viscosity to about 15 mPa·s. 400 μL was measured with a micropipette and dropped onto a 50 mm square ITO-coated glass substrate set in a spin coater, and then rotated at 250 rpm for 5 minutes and then at 1000 rpm for 5 seconds to form a thin film. The film was naturally dried to obtain Example 5-A. The film thickness of the tungsten oxide thin film of Example 5-A was about 1000 nm.

[0188] <Example 6-A>

[0189] The same procedure as in Example 5-A was performed except that the coating material of Example 6 was used. The film thickness of the tungsten oxide thin film of Example 6-A was about 1000 nm.

[0190] <Comparative Example 1-A>

[0191] The same procedure as Example 2-A was performed except that the dispersion of Comparative Example 1 was used instead of the coating material. The film thickness of the tungsten oxide thin film of Comparative Example 1-A was about 1000 nm.

[0192] <Evaluation of physical properties of tungsten oxide thin films>

[0193] Figure 4 Figure 1 is a field emission scanning electron microscope photograph of Examples 1-A, 2-A, 3-A and Comparative Example 1-A. Figure 4 As shown, for Comparative Example 1-A in which no adhesive was added, the adhesion to the ITO-coated glass substrate was poor, and film peeling or large cracks were observed. In contrast, in Examples 1-A, 2-A, and 3-A in which PVA was added, the adhesion was good, and film peeling or large cracks were not observed.

[0194] In addition, for Examples 1-A, 2-A, 3-A and Comparative Example 1-A, the electrochromic properties were evaluated by cyclic voltammetry. Specifically, a platinum wire was used as the counter electrode, a saturated silver / silver chloride electrode was used as the reference electrode, and a potassium bis(trifluoromethanesulfonyl)imide (KTFSI)-propylene carbonate solution with a concentration of 1.5 mol / kg was used as the electrolyte, and the cyclic voltammogram was obtained at a scan rate of 5 mV / s. Figure 5 The cyclic voltammograms of Examples 1-A, 2-A, 3-A and Comparative Example 1-A are shown.

[0195] like Figure 5 As shown, it can be seen that Examples 1-A, 2-A, and 3-A produce good redox reactions compared to Comparative Example 1-A.

[0196] Furthermore, for Examples 1-A, 2-A, 3-A and Comparative Example 1-A, chronocoulometry was performed with end potentials of -1.2 V (reduction state) and +1.0 V (oxidation state), and visible light transmission spectra at the end were obtained. Figure 6 The visible light transmission spectra of Examples 1-A, 2-A, 3-A and Comparative Example 1-A are shown.

[0197] like Figure 6 As shown, it is colorless and transparent in the oxidation state of +1.0V, and dark blue in the reduction state of -1.2V. However, if the amount of PVA added increases, the amount of tungsten nanoparticles (WO3) decreases relatively, and the redox reaction is lacking. Therefore, from the perspective of achieving a higher contrast, the amount of PVA added is preferably 0.1 to 1.0 mass % relative to the total coating.

[0198] In addition, for Examples 4-A, 5-A, and 6-A, the electrochromic properties were evaluated. Specifically, a platinum wire was used as the counter electrode, a saturated silver / silver chloride electrode was used as the reference electrode, and a potassium bis(trifluoromethanesulfonyl)imide (KTFSI)-propylene carbonate solution with a concentration of 1.5 mol / kg was used as the electrolyte, and a cyclic voltammogram was obtained at a scan rate of 5 mV / s. Figure 7 The cyclic voltammograms of Examples 4-A, 5-A, and 6-A are shown. Figure 7 As shown, it can be seen that the tungsten oxide thin film undergoes a good redox reaction when any binder is used.

[0199] [Metal cyano complex film]

[0200] As described below, the coating material of metal cyano complex nanoparticles (Adjustment Example 1) was adjusted to produce the iron-ferrocyano complex thin films (second electrochromic layers) of Adjustment Examples 1-A to 1-D.

[0201] <Iron-ferrocyanide complex nanoparticles (Prussian blue)>

[0202] First, 30 mL of an aqueous solution prepared by dissolving 16.2 g of iron nitrate nonahydrate in water and 14.5 g of sodium ferrocyanide decahydrate in 60 mL of water were mixed and stirred for 5 minutes. The precipitated blue iron-ferrocyanide complex nanoparticles, i.e., the precipitate of Prussian blue, were centrifuged and washed three times with water, then washed once with methanol, and dried under reduced pressure to obtain iron-ferrocyanide complex nanoparticles. The yield at this time was 11.0 g, based on Fe[Fe(CN)6] 0.75 The yield of 3.75H2O was 97.4%. The precipitate of the iron-ferrocyanide complex nanoparticle AFe1 was analyzed by a powder X-ray diffraction device, and the result was consistent with the diffraction information of Prussian blue, namely Fe4[Fe(CN)6]3, retrieved from the standard reagent database. The transmission electron microscope was used to measure, and the result showed that the iron-ferrocyanide complex nanoparticle was an aggregate of nanoparticles (primary particles) with a diameter of 5 to 25 nm.

[0203] <Adjustment Example 1>

[0204] Then, 0.40 g of the iron-ferrocyanide complex nanoparticles were suspended in 8 mL of water, and 80 mg of sodium ferrocyanide decahydrate was added and stirred to form a blue transparent solution. In this manner, a coating material containing iron-ferrocyanide complex nanoparticles of Adjustment Example 1 was obtained.

[0205] <Adjustment Example 1-A>

[0206] Using the coating of Adjustment Example 1, the iron-ferrocyanide complex nanoparticle film of Adjustment Example 1-A was prepared on an ITO-coated glass substrate by spin coating. Specifically, a 50 mm square ITO-coated glass substrate was placed in a spin coater, 500 μL of a substance obtained by mixing 10% by mass of PVA as a binder with the coating of Adjustment Example 1 adjusted to 9% by mass was dropped, and the mixture was rotated at 400 rpm for 10 seconds and then at 900 rpm for 10 seconds to prepare Adjustment Example 1-A on the ITO-coated glass substrate. The film thickness of the iron-ferrocyanide complex nanoparticle film of Adjustment Example 1-A was about 1000 nm.

[0207] <Adjustment Example 1-B>

[0208] The same procedure as in Adjustment Example 1-A was performed except that an ITO-coated polyethylene naphthalate (PET) substrate was used instead of an ITO-coated glass substrate. The film thickness of the iron-ferrocyanide complex nanoparticle thin film of Adjustment Example 1-B was about 1000 nm.

[0209] <Adjustment Example 1-C>

[0210] The same procedure as in Adjustment Example 1-A was performed except that an ITO-coated polycarbonate substrate was used instead of an ITO-coated glass substrate. The film thickness of the iron-ferrocyanide complex nanoparticle thin film of Adjustment Example 1-C was about 1000 nm.

[0211] <Adjustment Example 1-D>

[0212] The same procedure as in Adjustment Example 1-A was performed except that an ITO-coated polyethylene terephthalate (PEN) substrate was used instead of an ITO-coated glass substrate. The film thickness of the iron-ferrocyanide complex nanoparticle thin film of Adjustment Example 1-D was about 1000 nm.

[0213] [ECD]

[0214] The tungsten oxide thin film (first electrochromic layer) and the metal cyano complex thin film (second electrochromic layer) were combined to produce ECDs 1 to 4 of Examples. Then, each of the produced ECDs was evaluated.

[0215] <ECD1>

[0216] As a dark blue-colorless and transparent ECD1, a tungsten oxide / iron-ferrocyanide complex nanoparticle ECD was produced. Specifically, an electrolyte layer was sandwiched between an ITO-coated glass substrate formed with a tungsten oxide thin film of Example 1-A and an ITO-coated glass substrate formed with an iron-ferrocyanide complex nanoparticle thin film of Adjustment Example 1-A, and ECD1 was produced. As an electrolyte layer, 30 parts by weight of a methyl methacrylate polymer was added to a 1.5 mol / kg potassium bis(trifluoromethanesulfonyl)imide (KTFSI)-propylene carbonate solution, and the viscosity was increased by heating at 60°C to 80°C for about 24 hours. The potential of ECD1 was set by using the working electrode as the tungsten oxide thin film side.

[0217] Figure 8 The cyclic voltammogram of ECD1 measured at a scan rate of 5 mV / s is shown. Figure 8 As shown, it was judged that ECD1 exhibited good redox reaction.

[0218] Fig. 9 The results of obtaining the visible light transmission spectrum of ECD1 are shown. Fig. 9 As shown, ECD1 is in a dark colored state when a voltage of -0.8V is applied, and returns to a colorless and transparent state when a voltage of +1.2V is applied. Fig.10 A photograph showing the changing state of the color of ECD1.

[0219] Fig.11 The results of obtaining the total light transmission spectrum of ECD1 are shown. In this measurement, a dry cell with a voltage of + / - 1.5 V was used. Fig.11 As shown, ECD1 can switch the transmittance in a wide range of wavelength regions not only in the visible light region but also in the near infrared region. In addition, using JIS R 3106:1998 (ISO 9050:2003), the visible light transmittance and the solar light transmittance are calculated based on the obtained measurement data. The visible light transmittance is 71.71% in the transparent state and 7.73% in the colored state. The solar light transmittance is 55.13% in the transparent state and 6.12% in the colored state. Based on the above results, it can be seen that it has effective performance as a dimming glass.

[0220] <ECD2>

[0221] ECD2 is the same as ECD1 except that an ITO-coated PET substrate with a tungsten oxide thin film of Example 1-B and an ITO-coated PET substrate with an iron-ferrocyanide complex nanoparticle thin film of Adjustment Example 1-B are used. The potential of ECD2 is set at the tungsten oxide thin film side as the working electrode.

[0222] Fig.12 The photographs show the changing state of ECD 2. ECD 2 is in a dark colored state when a voltage of -0.8 V is applied, and returns to a colorless and transparent state when a voltage of +1.2 V is applied.

[0223] Fig.13 The results of obtaining the total light transmission spectrum of ECD2 are shown. In this measurement, a dry cell with a voltage of plus or minus 1.5 V was used. Fig.13 As shown, ECD2 can switch the transmittance in a wide range of wavelength regions not only in the visible light region but also in the near infrared region. In addition, based on the obtained measurement data, the visible light transmittance and the solar light transmittance are calculated using JIS R 3106:1998 (ISO 9050:2003). The visible light transmittance is 78.98% in the transparent state and 1.64% in the colored state. The solar light transmittance is 55.81% in the transparent state and 2.86% in the colored state. Based on the above results, it can be seen that it has effective performance as a dimming film.

[0224] <ECD3>

[0225] ECD3 is the same as ECD1 except that an ITO-coated polycarbonate substrate with a tungsten oxide thin film of Example 1-C and an ITO-coated polycarbonate substrate with an iron-ferrocyanide complex nanoparticle thin film of Adjustment Example 1-C are used. The potential of ECD3 is set at the tungsten oxide thin film side as the working electrode.

[0226] Fig.14 The results of obtaining the total light transmission spectrum of ECD3 are shown. In this measurement, a dry cell with a voltage of plus or minus 1.5 V was used. Fig.14 As shown, ECD3 can switch the transmittance in a wide range of wavelength regions not only in the visible light region but also in the near infrared region. In addition, based on the obtained measurement data, the visible light transmittance and the solar light transmittance are calculated using JIS R 3106:1998 (ISO 9050:2003). The visible light transmittance is 72.63% in the transparent state and 6.75% in the colored state. The solar light transmittance is 67.49% in the transparent state and 4.80% in the colored state. Based on the above results, it can be seen that it has effective performance as a dimming film.

[0227] <ECD4>

[0228] ECD4 is the same as ECD1 except that an ITO-coated PEN substrate with a tungsten oxide thin film of Example 1-D and an ITO-coated PEN substrate with an iron-ferrocyanide complex nanoparticle thin film of Adjustment Example 1-D are used. The potential of ECD4 is set at the tungsten oxide thin film side as the working electrode.

[0229] Fig.15 The results of obtaining the total light transmission spectrum of ECD4 are shown. In this measurement, a dry cell with a voltage of plus or minus 1.5 V was used. Fig.15 As shown, ECD4 can switch the transmittance in a wide range of wavelength regions not only in the visible light region but also in the near infrared region. In addition, based on the obtained measurement data, the visible light transmittance and the solar light transmittance are calculated using JIS R 3106:1998 (ISO 9050:2003). The visible light transmittance is 67.90% in the transparent state and 4.47% in the colored state. The solar light transmittance is 47.81% in the transparent state and 3.19% in the colored state. Based on the above results, it can be seen that it has effective performance as a dimming film.

[0230] In the following description, an experiment was conducted regarding the relationship between the pH of the coating material of the present invention and the physical properties of the coating material.

[0231] <Example 7>

[0232] After suspending tungsten oxide nanoparticles 1 (powder sample) in water in an amount of 0.10 mass % relative to the total coating, PVA is added as a binder to reduce surface tension in an amount of 0.01 mass %, and stirred to obtain a coating. Similarly, a coating is obtained in an amount of 1 mass % relative to the total coating and 0.1 mass % of PVA. Similarly, a coating is obtained in an amount of 10 mass % relative to the total coating and 1 mass % of PVA. Similarly, a coating is obtained in an amount of 20 mass % relative to the total coating and 2 mass % of PVA. Here, the case where the amount of tungsten oxide nanoparticles 1 added is 0 mass % represents pure water manufactured by Milli-Q (registered trademark).

[0233] Fig.16 : is a graph showing the relationship between the amount (mass %) of tungsten oxide nanoparticles 1 added and the pH of the coating for Example 7. Fig.16 As shown, the pH of the coating material relatively decreases according to the addition amount of tungsten oxide nanoparticles 1. Specifically, when the addition amount of tungsten oxide nanoparticles 1 is 0.10 mass %, the pH is 4.83, when the addition amount is 1 mass %, the pH is 4.11, when the addition amount is 10 mass %, the pH is 3.15, and when the addition amount is 20 mass %, the pH is 2.87.

[0234] <Example 8>

[0235] The coating was prepared such that the solid content of tungsten oxide nanoparticles 1 was 0.1% by mass relative to the entire coating and PVA as a binder was 0.01% by mass. The pH of 20 mL of the coating was adjusted with HCl or NaOH to obtain a coating having a pH of 2 to 7.

[0236] Table 1 shows the types of pH adjusters used in Example 8, the amounts added, and the pH after adjustment.

[0237] Table 1

[0238] Target pH pH Adjuster Addition volume μL pH measurement value 2 1M HCL 130 2.00 3 1M HCL 13 3.00 4 0.1M HCl 120 4.00 5 0.001M NaOH 400 5.08 6 0.01M NaOH 300 6.06 7 0.1 M NaOH 300 7.18

[0239] As described in Example 7, the pH is relatively attenuated in accordance with the amount of tungsten oxide nanoparticles added. Specifically, when the amount of tungsten oxide nanoparticles added is 0.1 mass %, the pH is about 4.83. According to Table 1, it can be understood that the pH of the coating can be adjusted with a pH adjuster. Specifically, by adding an acidic solvent (HCL) or an alkaline solvent (NaOH) to the coating, the pH of the coating can be arbitrarily adjusted.

[0240] <Example 9>

[0241] The solid content of tungsten oxide nanoparticles 1 was adjusted to 7.9 mass % or 20 mass % relative to the total paint, 0.79 mass % and 2 mass % of PVA were added as a binder to prepare the paint, and the pH of 20 mL of the paint was adjusted with 0.1 M NaOH to prepare the paint of Example 9.

[0242] Fig.17 This is a graph showing the relationship between the amount of 0.1M NaOH added and the pH of the coating material of Example 9. Fig.16 Similarly, the pH becomes more acidic as the concentration of tungsten oxide nanoparticles increases. In addition, the pH can be adjusted by adjusting the amount of NaOH added for each concentration of tungsten oxide nanoparticles.

[0243] <Example 10>

[0244] The solid amount of tungsten oxide nanoparticles 1 is adjusted to 20% by mass relative to the total coating, 2% by mass of PVA is added as a binder to adjust the coating, 0.1M NaOH is added to 20mL of the coating to adjust the pH to make a coating, and the coating is used to make a tungsten oxide film. The amount of 0.1M NaOH added (i.e., pH) is changed to make multiple tungsten oxide films. 400μL is measured in the coating with a micropipette, and is dropped onto a 50mm square ITO-coated glass substrate set in a spin coater, rotated at 500rpm for 10 seconds, and then rotated at 1000rpm for 10 seconds to form a film. The tungsten oxide film of Example 10 is obtained by allowing the film to dry naturally. It can be confirmed that the film thickness of the tungsten oxide film of Example 10 is affected by the pH of the coating. Specifically, at pH 3 (1 mL of 0.1 M NaOH was added relative to 20 mL of paint), the film thickness was approximately 0.57 nm, at pH 4 (3 mL of 0.1 M NaOH was added relative to 20 mL of paint), the film thickness was approximately 0.43 nm, at pH 5 (6 mL of 0.1 M NaOH was added relative to 20 mL of paint), the film thickness was approximately 0.34 nm, and at pH 6 (10 mL of 0.1 M NaOH was added relative to 20 mL of paint), the film thickness was approximately 0.33 nm.

[0245] Fig.18 The visible light transmission spectrum of the tungsten oxide thin film of Example 10 is shown. Fig.18 In the figure, the dotted line shown in (1) is the change of the visible light transmission spectrum in the initial state, the solid line shown in (2) is the change of the visible light transmission spectrum when changing from the initial state to the colored state, and the dotted line shown in (3) is the change of the visible light transmission spectrum when returning from the colored state to the transparent state.

[0246] like Fig.18 As shown, the tungsten oxide film was not negatively affected by the pH adjuster and showed a redox reaction. Within 60 seconds, it was in a dark colored state when a voltage of 1.0 V was applied, and became transparent when a voltage of -1.2 V was applied. On the other hand, it was shown that at pH 3, it did not completely return to the original colorless and transparent state in 60 seconds, and the difference in lightness between the colored state and the transparent state at around pH 5 was excellent.

[0247] An ECD having a tungsten oxide thin film composed of a coating having adjusted pH was produced according to the same procedure as ECD1. It should be noted that sodium glass and PET film were used as substrates, and ITO, FTO (fluorine-doped tin) and high-durability TCO (transparent conductive oxide) were used as transparent electrode materials, and the substrates were also compared.

[0248] <ECD5>

[0249] ECD5 is an electrochromic element (using a glass substrate) having a tungsten oxide thin film made of a coating having a pH of 2.2 (adjusted to a coating in which the solid amount of tungsten oxide nanoparticles 1 relative to the entire coating is 13.9% by mass and the amount of PVA added is 0.7% by weight). For ECD5, a cycle test was carried out under the measurement conditions of Table 2 to examine the changes in the transmittance of light at 550nm and 700nm. As shown in Table 2, a cycle of alternately applying a voltage of -1.2V (30 seconds) and a voltage of +1.0V (30 seconds) was repeated 1000 times (continuous measurement: about 16.6 hours). The results of the cycle test are shown in Fig.19 .

[0250] Table 2 (MPS cycle durability test conditions)

[0251]

[0252] like Fig.19 As shown, high-durability TCO and FTO showed stable cycle resistance, while rapid degradation was observed in ITO. It was shown that the acidic tungsten oxide film corroded ITO as the main cause. Compared with ITO, high-durability TCO and FTO as transparent electrode materials have excellent chemical resistance and corrosion resistance, high stability, and therefore good durability.

[0253] <ECD6>

[0254] ECD6 is an electrochromic element (using a glass substrate) having a tungsten oxide thin film made of a coating having a pH of 5.0 (a coating obtained by adding 5 mL of 0.1M NaOH to 20 mL of a coating adjusted to have a solid content of tungsten oxide nanoparticles 1 of 14.0% by mass and a PVA content of 0.7% by weight relative to the total coating). For ECD6, a cycle test was also conducted under the measurement conditions of Table 2 to examine changes in the transmittance of light at 550 nm and 700 nm. The results of the cycle test are shown in Fig. 20 .like Fig. 20 As shown, stable cycle resistance is shown in high-durability TCO and FTO, and slow degradation behavior is shown in ITO. However, for ITO, it is known that ECD6 has higher durability than ECD5. From the above description, it can be understood that the durability can be improved by adjusting the pH of the coating.

[0255] Fig.21The visible light transmission spectrum changes when the withstand voltage characteristics were measured under the conditions of Table 3 are shown for ECD5 and ECD6. It should be noted that here, the CV (cyclic voltammetry) measurement (high potential) was completed under each applied voltage condition. Low potential After the final potential), the coloring reaction was monitored by applying a negative potential while the voltage was raised and lowered in 0.5 V steps using the multi-potential step (MPS) method. The device color when a color-reducing reaction is carried out by applying a positive potential (color change of the transparent conductive film, color change state of the light-adjusting film).

[0256] Table 3

[0257]

[0258] like Fig.21 As shown, when using ITO, rapid degradation was observed in ECD5 (pH 2.2), especially under high voltage conditions, and degradation was also observed in ECD6 (pH 5.0), but it was suppressed to a certain extent. As mentioned above, the voltage resistance characteristics can also be improved by adjusting the pH of the coating. In addition, in the comparison of transparent electrode materials, not much degradation was observed in high-durability TCO and FTO under high voltage conditions, which also shows their advantages over ITO.

[0259] <ECD7>

[0260] Regarding the electrochromic element (using a PET substrate) having a tungsten oxide thin film made of a coating with adjusted pH, a cycle test was carried out under the conditions of Table 2 to examine the changes in the transmittance of light at 550nm and 700nm. By adding 0.1M NaOH to a coating adjusted to a solid amount of tungsten oxide nanoparticles 1 of 15% by mass and a PVA addition amount of 0.7% by weight relative to the entire coating, a tungsten oxide thin film was prepared using coatings adjusted to pH 2.4 and pH 4.9, respectively. The results of the cycle test are shown in Fig. 22 .like Fig. 22 As shown, when the substrate is changed from a glass substrate to a PET substrate, the electrochromic element using a tungsten oxide thin film composed of a coating having a pH of 2.4 also deteriorates rapidly, whereas the electrochromic element using a tungsten oxide thin film composed of a coating adjusted to a pH of 4.9 shows high durability. It can be understood from the above description that adjusting the pH of the coating is an effective method for improving durability.

[0261] As can be understood from the above description, it can be grasped that in the ECD of the present invention, the amplitude of change of the transmittance is large. The larger the amplitude of change of the transmittance, the higher the contrast. Therefore, according to the ECD of the present invention, without using an organic electrochromic material, an electrochromic element with high contrast coloring-decolorization can be realized. Assuming that the element is used for dimming glass / film, display, indicator, etc., and in particular, it also has the ability to control long wavelength components, it is also expected to be used as an energy-saving dimming component that can optimize the inflow of thermal components of solar energy, such as infrared rays, such as automobile window glass, building material window glass, etc.

[0262] Although the embodiments of the present invention have been described above, the present invention is not necessarily limited thereto, and a person skilled in the art can find various alternative embodiments without departing from the spirit of the present invention or the appended claims.

[0263] Description of Reference Numerals

[0264] 100:ECD.

[0265] 10: First electrochromic layer.

[0266] 20: Second electrochromic layer.

[0267] 30: Electrolyte layer.

[0268] 40: first transparent electrode layer. 50: second transparent electrode layer.

[0269] 60: First insulating layer.

[0270] 70: Second insulating layer.

Claims

1. A tungsten oxide coating for an electrochromic element, which is a coating for forming a tungsten oxide thin film having electrochromic properties, characterized in that: The tungsten oxide coating for an electrochromic element comprises a solvent, tungsten oxide nanoparticles dispersed in the solvent, and a binder. The half-peak width of the peak detected at 29°±1° when the tungsten oxide nanoparticles are subjected to X-ray diffraction analysis at 2θ is less than 2°, The primary particle size of the tungsten oxide nanoparticles is 5 to 25 nm.

2. The tungsten oxide coating for an electrochromic element according to claim 1, characterized in that: The content of the tungsten oxide nanoparticles is 5 mass % or more and 30 mass % or less relative to the mass of the coating material.

3. The tungsten oxide coating for an electrochromic element according to claim 1, characterized in that: The binder is one or more selected from polyvinyl alcohol (PVA), sodium carboxymethyl cellulose (CMC), hydroxypropyl cellulose (HPC) and hydroxyethyl cellulose (HEC). The content of the binder is 0.1% by mass or more and 10% by mass or less relative to the mass of the coating material.

4. The tungsten oxide coating for an electrochromic element according to claim 1, wherein: The tungsten oxide coating material for an electrochromic element contains a pH adjuster.

5. The tungsten oxide coating for an electrochromic element according to claim 4, characterized in that: The pH adjuster is one or more selected from potassium chloride KCl, sodium chloride NaCl, lithium chloride LiCl, potassium hydroxide KOH, sodium hydroxide NaOH, and lithium hydroxide LiOH.

6. The tungsten oxide coating for an electrochromic element according to claim 4, wherein: The pH is 5-7.

7. The tungsten oxide coating for an electrochromic element according to claim 1, characterized in that: The tungsten oxide coating material for the electrochromic element can form a tungsten oxide thin film by a coating method.

8. A tungsten oxide thin film having electrochromic properties and comprising tungsten oxide nanoparticles and a binder, characterized in that: The half-peak width of the peak detected at 29°±1° when the tungsten oxide nanoparticles are subjected to X-ray diffraction analysis at 2θ is less than 2°, The primary particle size of the tungsten oxide nanoparticles is 5 to 25 nm.

9. The tungsten oxide thin film according to claim 8, wherein: The tungsten oxide thin film contains a pH adjuster.

10. The tungsten oxide thin film according to claim 8, wherein An electrochromic reaction occurs in an electrolyte containing any one or more (trifluoromethanesulfonyl)imide salts of bis(trifluoromethanesulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, potassium bis(trifluoromethanesulfonyl)imide, and sodium bis(trifluoromethanesulfonyl)imide.

11. A dimming component, characterized in that: The dimming component has: The tungsten oxide thin film according to claim 8; A metal cyano complex film containing metal cyano complex nanoparticles whose coloration and decolorization changes caused by redox reaction are opposite to those of tungsten oxide, or an oxide film containing oxide nanoparticles whose coloration and decolorization changes caused by redox reaction are opposite to those of tungsten oxide; and An electrolyte layer is located between the tungsten oxide film and the metal cyano complex film or between the tungsten oxide film and the oxide film.

Citation Information

Cited By