Positive electrode for power storage element, power storage element

By using particle-like and fibrous conductive agents in the positive electrode active material layer of the power storage element, the problem of increasing DC resistance during the charge and discharge cycle is solved, and the battery life is extended and performance is maintained.

CN118974961APending Publication Date: 2024-11-15GS YUASA INT LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030363.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-01
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The positive electrode of existing power storage components is prone to increase in DC resistance during the charge and discharge cycle, which affects the life and performance of the battery.

Method used

A positive electrode active material layer containing a positive electrode active material, a particle-like conductive agent and a fibrous conductive agent is used to control the dispersion and pore capacity distribution of the fibrous conductive agent to ensure uniform penetration and maintenance of the electrolyte, thereby reducing the increase in DC resistance.

Benefits of technology

It effectively reduces the increase rate of DC resistance during the charge and discharge cycle, extends the battery life and maintains good performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974961A_ABST
    Figure CN118974961A_ABST
Patent Text Reader

Abstract

A positive electrode for a power storage element according to one aspect of the present invention is provided with a positive electrode active material layer containing a positive electrode active material, a particulate conductive agent, and a fibrous conductive agent, the diameter of the fibrous conductive agent being 60 nm or less, and the median pore diameter in the pore volume distribution of the positive electrode active material layer being 100 nm or more. In a Log differential pore volume distribution curve obtained from the pore volume distribution, a first peak appears in a pore diameter range of 10 nm or more and less than 100 nm, a second peak appears in a pore diameter range of 100 nm or more and less than 2000 nm, and the ratio of the height of the second peak to the height of the first peak (second peak / first peak) is 1.20 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive electrode for an electricity storage element, an electricity storage element, and an electricity storage device. Background Art

[0002] Non-aqueous electrolyte secondary batteries represented by lithium ion secondary batteries are widely used in electronic devices such as personal computers, communication terminals, automobiles, etc. due to their high energy density. Generally speaking, non-aqueous electrolyte secondary batteries are composed of a pair of electrodes electrically isolated by a separator and a non-aqueous electrolyte between the electrodes, and are charged and discharged by the transfer of charge transport ions between the two electrodes. In addition, as storage elements other than non-aqueous electrolyte secondary batteries, capacitors such as lithium ion capacitors and double electric layer capacitors, storage elements using electrolytes other than non-aqueous electrolytes, etc. have also been widely popularized.

[0003] The positive electrode of the storage element generally has a structure in which a positive electrode active material layer including a positive electrode active material and a conductive agent is provided on a conductive substrate. As the conductive agent, carbon materials such as acetylene black are widely used. Patent document 1 describes a storage element in which acetylene black and carbon nanotubes are used in combination as the conductive agent of the positive electrode.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2012-221672 Summary of the invention

[0007] Conventional positive electrodes for electric storage devices and electric storage devices have the disadvantage that the DC resistance is easily increased with charge and discharge cycles.

[0008] An object of the present invention is to provide a positive electrode for an electric storage element, an electric storage element, and an electric storage device capable of reducing the rate of increase in direct current resistance accompanying a charge and discharge cycle.

[0009] The positive electrode for a storage element involved in one aspect of the present invention comprises a positive electrode active material layer containing a positive electrode active material, a particulate conductive agent and a fibrous conductive agent, the diameter of the above-mentioned fibrous conductive agent is less than 60nm, the median pore diameter in the pore volume distribution of the above-mentioned positive electrode active material layer is greater than 100nm, in the Log differential pore volume distribution curve calculated from the above-mentioned pore volume distribution, a first peak appears in the range of pore diameter greater than 10nm and less than 100nm, a second peak appears in the range of pore diameter greater than 100nm and less than 2000nm, and the ratio of the height of the above-mentioned second peak to the height of the above-mentioned first peak (second peak / first peak) is less than 1.20.

[0010] An electric storage device according to another aspect of the present invention includes the positive electrode for an electric storage device according to the first aspect of the present invention.

[0011] A power storage device according to another aspect of the present invention includes two or more power storage elements, and includes one or more power storage elements including the positive electrode for the power storage element according to the above-mentioned aspect of the present invention.

[0012] According to one aspect of the present invention, a positive electrode for an electric storage element and an electric storage element capable of reducing the rate of increase in direct current resistance accompanying a charge and discharge cycle can be provided.

[0013] According to another aspect of the present invention, it is possible to provide a power storage device capable of reducing the rate of increase in DC resistance accompanying a charge and discharge cycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a perspective view showing an embodiment of an electric storage element.

[0015] Figure 2 This is a schematic diagram showing one embodiment of an electric storage device constituted by combining a plurality of electric storage elements. DETAILED DESCRIPTION

[0016] First, the outline of the positive electrode for an electric storage element, the electric storage element, and the electric storage device disclosed in this specification will be described.

[0017] (1) A positive electrode for a storage element according to one aspect of the present invention comprises a positive electrode active material layer containing a positive electrode active material, a particulate conductive agent and a fibrous conductive agent, wherein the diameter of the fibrous conductive agent is 60 nm or less, the median pore diameter in the pore volume distribution of the positive electrode active material layer is 100 nm or more, and in a Log differential pore volume distribution curve obtained from the pore volume distribution, a first peak appears in a pore diameter range of 10 nm or more and less than 100 nm, and a second peak appears in a pore diameter range of 100 nm or more and less than 2000 nm, and the ratio of the height of the second peak to the height of the first peak (second peak / first peak) is 1.20 or less.

[0018] The positive electrode for the storage element described in (1) above can reduce the rate of increase of the DC resistance accompanying the charge and discharge cycle. The reason is still uncertain, but it is speculated to be the following reason. The above-mentioned first peak is a peak corresponding to the gap between the particles of the particulate conductive agent, and the above-mentioned second peak is a peak corresponding to the gap between the particles of the positive electrode active material. Moreover, when the gap between the particles of the positive electrode active material is fully formed, the median pore size in the pore volume distribution of the positive electrode active material layer becomes larger. Here, when a particulate conductive agent and a fibrous conductive agent are used together, if the fibrous conductive agent with low dispersibility agglomerates, the agglomerated fibrous conductive agent occupies the gap between the particles of the positive electrode active material, and the electrolyte (typically an electrolyte solution) is difficult to evenly penetrate between the particles of the positive electrode active material, which easily leads to an increase in the DC resistance accompanying the charge and discharge cycle. In addition, if the fibrous conductive agent covers the particulate conductive agent, the gaps between the particles of the particulate conductive agent are occupied by the fibrous conductive agent, and the electrolyte (typically an electrolyte solution) is difficult to maintain in the gaps between the particles of the particulate conductive agent, which easily leads to an increase in the DC resistance accompanying the charge and discharge cycle. In addition, when only the particulate conductive agent is used as the conductive agent, the contact between the particles of the positive electrode active material and the particles of the conductive agent or between the particles of the conductive agent becomes a point contact, and it is difficult to fully form an electron conduction path using the conductive agent. In addition, when only the fibrous conductive agent is used as the conductive agent, the electrolyte is difficult to maintain in the gaps between the particles of the fibrous conductive agent, which easily leads to an increase in the DC resistance accompanying the charge and discharge cycle. On the other hand, in the positive electrode for the storage element described in (1) above, since the median pore size in the pore volume distribution of the positive electrode active material layer is larger than 100nm, it is inferred that the fibrous conductive agent is fully dispersed and the gaps between the particles of the positive electrode active material are fully formed. In addition, in the positive electrode for the storage element described in (1), since the ratio of the height of the second peak to the height of the first peak (second peak / first peak) is 1.20 or less, that is, the first peak corresponding to the gaps between the particles of the particulate conductive agent is relatively large enough, it is estimated that the gaps between the particles of the particulate conductive agent are almost not occupied by the fibrous conductive agent. Therefore, it is estimated that in the positive electrode for the storage element described in (1), the electrolyte can be uniformly infiltrated between the particles of the positive electrode active material, and the electrolyte is easily retained in the gaps between the particles of the particulate conductive agent, so that the increase rate of the DC resistance accompanying the charge and discharge cycle can be reduced.

[0019] "Particulate conductive agent" refers to a granular conductive agent. The ratio of the major diameter to the minor diameter of the particulate conductive agent is greater than 1 and less than 10. The minor diameter and major diameter of the particulate conductive agent are based on a scanning electron microscope (SEM) or transmission electron microscope (TEM) image of a cross-section of the positive electrode active material layer. It should be noted that the shortest diameter passing through the center of the smallest circumscribed circle of the particulate conductive agent is taken as the minor diameter, and the diameter passing through the above center and orthogonal to the minor diameter is taken as the major diameter. When there are two or more shortest diameters, the longest orthogonal diameter is taken as the minor diameter. The particulate conductive agent can be a substantially undeformed granular conductive agent.

[0020] The "fibrous conductive agent" refers to a conductive agent in a deformable elongated shape. The ratio of the length to the diameter (fiber diameter) of the fibrous conductive agent is greater than 10. The diameter and length of the fibrous conductive agent are based on a SEM or TEM image of a cross section of the positive electrode active material layer.

[0021] The "pore volume distribution" of the positive electrode active material layer is measured by mercury intrusion under the following conditions using a pore distribution measuring device ("AutoPore9400" manufactured by Micromeritics). The contact angle of mercury is set to 130°, and the surface tension is set to 484 dynes / cm. The pore size range for measurement is 5.5 nm to 20 μm. The number of measurement points in the pore size range for measurement is set to 40 points. The cumulative pore volume curve is obtained by plotting the pore size (pore diameter) as the horizontal axis and the pore volume as the vertical axis. The median pore diameter is obtained from the cumulative pore volume curve. Next, the value obtained by dividing the volume difference dV between the measurement points by the logarithmic difference d (logD) of the pore size is obtained, and this value is plotted relative to the average pore size of each interval to obtain the Log differential pore volume curve. It should be noted that “in the Log differential pore volume curve, a first peak appears in the range of pore diameters greater than 10 nm and less than 100 nm, and a second peak appears in the range of pore diameters greater than 100 nm and less than 2000 nm” means that the Log differential pore volume curve has a maximum value within the range of each pore diameter. It should be noted that, when the positive electrode for the storage element is set on the storage element, the sample of the positive electrode active material layer for the measurement of the pore volume distribution is prepared by the following method. The storage element is discharged at a current of 0.1 C to the discharge end voltage during normal use, which is taken as the discharged state. Here, “normal use” refers to the case where the storage element is used under the discharge conditions recommended or specified in the storage element. The storage element in the discharged state is disassembled and the positive electrode is taken out as the working electrode, and a half-cell is assembled using metal Li as the counter electrode, and the battery is discharged at a current of 0.1 C until the positive electrode potential becomes 3.0 V (vs. Li / Li +). The half-cell is disassembled, the positive electrode is removed and thoroughly washed with dimethyl carbonate, and then dried under reduced pressure at room temperature for 24 hours. A sample of a specified size (e.g., 2×2 cm) is cut from the dried positive electrode as a sample for the measurement of pore volume distribution. The operation from disassembly of the storage element to the preparation of the sample for the measurement of pore volume distribution is carried out in a dry air atmosphere with a dew point below -40°C.

[0022] (2) In the positive electrode for a storage element described in (1), the height of the first peak may be 0.054 mL / g or more. In the positive electrode for a storage element described in (2), the electrolyte is more easily retained in the gaps between particles of the particulate conductive agent, further reducing the increase rate of the DC resistance accompanying the charge and discharge cycle.

[0023] (3) In the positive electrode for storage element described in (1) or (2), the content of the fibrous conductive agent relative to the positive electrode active material may be 0.10 mass % to 2 mass %. In the positive electrode for storage element described in (3), the fibrous conductive agent can fully cover the surface of each particle of the positive electrode active material, resulting in the formation of a good electron conduction path. In addition, the excessive presence of the fibrous conductive agent can suppress the reduction of the gap between each particle of the positive electrode active material, thereby further reducing the increase rate of the DC resistance accompanying the charge and discharge cycle.

[0024] (4) In the positive electrode for an electric storage element described in any one of (1) to (3), the particulate conductive agent may be carbon black, and the fibrous conductive agent may be fibrous carbon. In the positive electrode for an electric storage element described in (4), the electrolyte is particularly easily retained in the gaps between the carbon black particles, and the fibrous carbon can form a particularly good electron conduction path, thereby further reducing the increase rate of the DC resistance accompanying the charge and discharge cycle.

[0025] "Fibrous carbon" refers to a fibrous conductive agent of a carbonaceous material. A carbonaceous material refers to a material whose main component element (the element with the largest content based on mass) is carbon. The content of carbon in the carbonaceous material is, for example, 70% by mass or more, preferably 90% by mass or more, and more preferably 95% by mass or more. As elements other than carbon that may be contained in the carbonaceous material, for example, oxygen, hydrogen, etc. may be cited.

[0026] (5) Another aspect of the present invention is an electric storage element having a positive electrode for an electric storage element as described in any one of (1) to (4). The electric storage element described in (5) can reduce the rate of increase of DC resistance accompanying charge and discharge cycles. Therefore, the electric storage element described in (5) has a long charge and discharge cycle life and can maintain good performance for a long time.

[0027] (6) A power storage device according to another aspect of the present invention includes two or more power storage elements, and includes one or more power storage elements including the power storage element positive electrode according to any one of (1) to (4) above.

[0028] The power storage device described in (6) above has a power storage element that can reduce the rate of increase of DC resistance accompanying the charge and discharge cycle, has a long charge and discharge cycle life, and can maintain good performance for a long time. Therefore, it can reduce the rate of increase of DC resistance accompanying the charge and discharge cycle, has a long charge and discharge cycle life, and can maintain good performance for a long time.

[0029] A positive electrode for a storage element, a method for manufacturing a positive electrode for a storage element, a storage element, a storage device, a method for manufacturing a storage element, and other embodiments of the present invention are described in detail. It should be noted that the names of the components (components) used in each embodiment are sometimes different from the names of the components (components) used in the background art.

[0030] <Positive electrode for energy storage device>

[0031] A positive electrode for an electric storage device (hereinafter also simply referred to as a “positive electrode”) according to an embodiment of the present invention includes a positive electrode substrate and a positive electrode active material layer disposed on the positive electrode substrate directly or via an intermediate layer.

[0032] The positive electrode substrate has electrical conductivity. Whether it has "electrical conductivity" is determined by measuring the volume resistivity 10 -2 Ω·cm is used as the threshold value for judgment. As the material of the positive electrode substrate, metals such as aluminum, titanium, tantalum, stainless steel, or their alloys can be used. Among these, aluminum or aluminum alloys are preferred from the viewpoints of potential resistance, high conductivity and cost. As the positive electrode substrate, foil, vapor-deposited film, mesh, porous material, etc. can be cited. From the viewpoint of cost, foil is preferred. Therefore, as the positive electrode substrate, aluminum foil or aluminum alloy foil is preferred. As aluminum or aluminum alloy, A1085, A3003, A1N30, etc. specified in JIS-H-4000 (2014) or JIS-H-4160 (2006) can be exemplified.

[0033] The average thickness of the positive electrode substrate is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, further preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By setting the average thickness of the positive electrode substrate to the above range, the strength of the positive electrode substrate can be increased, and the energy density per unit volume of the storage element can be increased.

[0034] The intermediate layer is a layer disposed between the positive electrode substrate and the positive electrode active material layer. The intermediate layer reduces the contact resistance between the positive electrode substrate and the positive electrode active material layer by including a conductive agent such as carbon particles. The composition of the intermediate layer is not particularly limited, and for example, includes a binder and a conductive agent.

[0035] The positive electrode active material layer contains a positive electrode active material, a particulate conductive agent, and a fibrous conductive agent. The positive electrode active material layer contains optional components such as a binder, a thickener, and a filler as needed.

[0036] As the positive electrode active material, it can be appropriately selected from known positive electrode active materials. As the positive electrode active material for lithium ion secondary batteries, materials that can absorb and release lithium ions can generally be used. As the positive electrode active material, for example, lithium transition metal composite oxides having an α-NaFeO2 type crystal structure, lithium transition metal composite oxides having a spinel type crystal structure, polyanion compounds, chalcogen compounds, sulfur, etc. can be cited. As the lithium transition metal composite oxide having an α-NaFeO2 type crystal structure, for example, Li[Li x Ni (1-x) ]O2(0≤x<0.5), Li[Li x Ni γ Co (1-x-γ) ]O2 (0≤x<0.5, 0<γ<1, 0<1-x-γ), Li[Li x Co (1-x) ]O2(0≤x<0.5), Li[Li x Ni γ Mn (1-x-γ) ]O2 (0≤x<0.5, 0<γ<1, 0<1-x-γ), Li[Li x Ni γ Mn β Co (1-x-γ-β) ]O2 (0≤x<0.5, 0<γ, 0<β, 0.5<γ+β<1, 0<1-x-γ-β), Li[Li x Ni γ Co β Al (1-x-γ-β) ]O2 (0≤x<0.5, 0<γ, 0<β, 0.5<γ+β<1, 0<1-x-γ-β), etc. As lithium transition metal composite oxides having a spinel crystal structure, Li x Mn2O4、Li x Ni γ Mn (2-γ)O4, etc. As polyanion compounds, LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, Li3V2(PO4)3, Li2MnSiO4, Li2CoPO4F, etc. can be mentioned. As chalcogen compounds, titanium disulfide, molybdenum disulfide, molybdenum dioxide, etc. can be mentioned. Atoms or part of polyanions in these materials can be replaced by atoms or anions composed of other elements. The surfaces of these materials can be coated with other materials. In the positive electrode active material layer, one of these materials can be used alone, or two or more of them can be mixed and used.

[0037] As the positive electrode active material, a lithium transition metal composite oxide is preferred, more preferably a lithium transition metal composite oxide containing nickel, cobalt and manganese or aluminum, and further preferably a lithium transition metal composite oxide containing nickel, cobalt and manganese. The lithium transition metal composite oxide preferably has an α-NaFeO2 type crystal structure. By using such a lithium transition metal composite oxide, energy density, etc. can be improved.

[0038] The material of the positive electrode active material may be used alone or in combination of two or more. The positive electrode active material preferably contains a lithium transition metal composite oxide in a proportion of 50% by mass or more (preferably 70 to 100% by mass, more preferably 80 to 100% by mass) of the total positive electrode active material used, and more preferably a positive electrode active material substantially consisting of only a lithium transition metal composite oxide is used.

[0039] The positive electrode active material is usually a particle (powder). The average particle size of the positive electrode active material is preferably, for example, 0.1 μm to 20 μm. By making the average particle size of the positive electrode active material above the above lower limit, it is easy to manufacture or handle the positive electrode active material. By making the average particle size of the positive electrode active material below the above upper limit, the electronic conductivity of the positive electrode active material layer is improved. It should be noted that when a composite of the positive electrode active material and other materials is used, the average particle size of the composite is taken as the average particle size of the positive electrode active material. "Average particle size" refers to the particle size distribution obtained by measuring a dilution obtained by diluting particles with a solvent by a laser diffraction and scattering method based on JIS-Z-8825 (2013), and the volume-based cumulative distribution calculated according to JIS-Z-8819-2 (2001) is 50%.

[0040] In order to obtain a powder with a predetermined particle size, a pulverizer, a classifier, etc. can be used. As a pulverization method, for example, a mortar, a ball mill, a sand mill, a vibrating ball mill, a planetary ball mill, a jet mill, a reverse jet mill, a cyclonic jet mill, or a sieve can be used. During pulverization, wet pulverization coexisting with water or an organic solvent such as hexane can also be used. As a classification method, a sieve, a wind classifier, etc., dry or wet, can be used as needed.

[0041] The content of the positive electrode active material in the positive electrode active material layer is sometimes preferably 50% to 99% by mass, more preferably 70% to 98% by mass, further preferably 80% to 97% by mass, further preferably 90% to 96% by mass, and further preferably 92% or more by mass or 94% or more by mass. By making the content of the positive electrode active material the above range, the high energy density and manufacturability of the positive electrode active material layer can be taken into account. In particular, in the positive electrode involved in the present embodiment, since a particulate conductive agent and a fibrous conductive agent are used as conductive agents, a good electron conduction path can be formed even if the content of the conductive agent is small. Therefore, in the positive electrode, the content of the positive electrode active material can be increased, and high energy density can be achieved.

[0042] As particulate conductive agents, particulate metals, particulate conductive resins, particulate conductive ceramics, particulate carbon, etc. can be mentioned, and particulate carbon is preferred among these. Particulate carbon refers to a particulate conductive agent that is a carbonaceous material. As particulate carbon (a particulate conductive agent that is a carbonaceous material), particulate conductive agents such as graphite, non-graphite carbon, and graphene-based carbon can be mentioned. As particulate non-graphite carbon, carbon black, etc. can be mentioned. As carbon black, furnace black, acetylene black, Ketjen black, etc. can be mentioned. As particulate graphene-based carbon, fullerene, etc. can be mentioned. Among these, non-graphite carbon is preferred, and carbon black is more preferred.

[0043] The particulate conductive agent is preferably composed of primary particles and exists in a state of aggregation of the primary particles. The average particle size of the primary particles of the particulate conductive agent is, for example, 10nm to 500nm, and more preferably 20nm to 100nm. By using a particulate conductive agent of such a size, the electronic conductivity of the positive electrode active material layer can be improved, and the electrolyte can be fully maintained in the gaps between the particles of the particulate conductive agent. The "average particle size" of the primary particles of the particulate conductive agent refers to the average value of the particle sizes of any 10 primary particles of the particulate conductive agent observed by SEM or TEM. The particle size of the primary particles of the particulate conductive agent is the average value of the major diameter and the minor diameter.

[0044] The average aspect ratio of the particulate conductive agent is 1 or more and less than 10, for example, preferably 6 or less, 3 or less, 2 or less, or 1.5 or less. The "average aspect ratio" of the particulate conductive agent refers to the average value of the aspect ratios (ratio of the major diameter to the minor diameter) of any 10 particulate conductive agents observed by SEM or TEM. In addition, when the particulate conductive agent exists in a state of primary particle aggregation, the average aspect ratio of the particulate conductive agent is the average aspect ratio of the primary particles.

[0045] As the content of the particulate conductive agent in the positive electrode active material layer, for example, it is sometimes preferably 0.1 mass% to 10 mass%, more preferably 0.5 mass% to 6 mass%, further preferably 1 mass% to 5 mass%, and further preferably 2 mass% to 4 mass%. By making the content of the particulate conductive agent above the above lower limit, the electronic conductivity of the positive electrode active material layer can be improved, and the increase rate of the DC resistance accompanying the charge and discharge cycle can be further reduced. On the other hand, by making the content of the particulate conductive agent below the above upper limit, the increase rate of the DC resistance accompanying the charge and discharge cycle can be fully reduced, and the content of the positive electrode active material can be relatively increased to improve the energy density.

[0046] As the fibrous conductive agent, fibrous metal, fibrous conductive resin, fibrous carbon, etc. can be cited, among which fibrous carbon is preferred. As the fibrous carbon (fibrous conductive agent of carbonaceous material), carbon fiber, pitch-based carbon fiber, carbon nanotube (CNT), etc. can be cited, and CNT can be preferably used.

[0047] The average diameter (average fiber diameter) of the fibrous conductive agent is, for example, preferably 0.5 nm to 60 nm, more preferably 1 nm to 55 nm, further preferably 2 nm to 50 nm, further preferably 3 nm to 45 nm, and further preferably 4 nm to 40 nm. By making the average diameter of the fibrous conductive agent within the above range, the electronic conductivity of the positive electrode active material layer becomes better, and the increase rate of the DC resistance accompanying the charge and discharge cycle can be further reduced. It should be noted that the "average diameter" of the fibrous conductive agent refers to the average value of the diameters of any 10 fibrous conductive agents observed by SEM or TEM.

[0048] The average aspect ratio (ratio of average length to average diameter) of the fibrous conductive agent is 10 or more, for example, preferably 10 to 10000, more preferably 100 or more, and further preferably 1000 or more. By using a fibrous conductive agent with an average aspect ratio in the above range, the electron conductivity of the positive electrode active material layer can be made better. It should be noted that the "average length" of the fibrous conductive agent refers to the average value of the lengths of any 10 fibrous conductive agents observed by SEM or TEM. When calculating the average aspect ratio, the 10 fibrous conductive agents used to determine the average diameter and the 10 fibrous conductive agents used to determine the average length are preferably the same particles, but the average diameter and average length can be obtained for different 10 fibrous conductive agents, and the ratio is taken as the average aspect ratio. That is, the average aspect ratio refers to the average value of the aspect ratios of any 10 fibrous conductive agents observed by SEM or TEM, or the ratio of the average length of any 10 fibrous conductive agents observed by SEM or TEM to the average diameter of any 10 different fibrous conductive agents.

[0049] When the fibrous conductive agent is fibrous carbon, the average interplanar spacing (d 002 ), preferably less than 0.340 nm. 002 ) is small and the crystallinity is high, the electron conductivity of the positive electrode active material layer is further improved. It should be noted that the average interplanar spacing (d 002 ) can be, for example, 0.330 nm. In addition, the half-peak width (002) of the peak corresponding to the (002) plane determined by the X-ray diffraction method using CuKα rays of the fibrous carbon is, for example, 0.5° or more. The half-peak width (002) of the fibrous carbon is preferably less than 0.7°.

[0050] Fibrous carbon can be obtained, for example, by spinning a polymer into fibers and heat treating it in an inert atmosphere, or by vapor phase growth of an organic compound reacting at high temperature in the presence of a catalyst. Fibrous carbon and other fibrous conductive agents can be commercially available products.

[0051] As the content of the fibrous conductive agent in the positive electrode active material layer, for example, it is sometimes preferably 0.05% by mass to 5% by mass, more preferably 0.1% by mass to 3% by mass, further preferably 0.2% by mass to 2% by mass, further preferably 0.4% by mass to 1.0% by mass, and further preferably 0.5% by mass to 0.8% by mass. By making the content of the fibrous conductive agent above the above lower limit, the electronic conductivity of the positive electrode active material layer can be further improved, and the rate of increase of the DC resistance accompanying the charge and discharge cycle can be further reduced. On the other hand, by making the content of the fibrous conductive agent below the above upper limit, the rate of increase of the DC resistance accompanying the charge and discharge cycle can be fully reduced, and the content of the positive electrode active material can be relatively increased to improve the energy density. In addition, by making the content of the fibrous conductive agent below the above upper limit, the production cost can also be suppressed.

[0052] As the content of the fibrous conductive agent relative to the positive electrode active material (fibrous conductive agent / positive electrode active material), it is preferably 0.10 mass% to 2 mass%, more preferably 0.2 mass% to 1.5 mass%, further preferably 0.3 mass% to 1.2 mass%, further preferably 0.4 mass% to 1.0 mass%, and further preferably 0.5 mass% to 0.8 mass%. By making the content of the fibrous conductive agent relative to the positive electrode active material above the above lower limit, the fibrous conductive agent can fully cover the surface of the particles of the positive electrode active material, and as a result, a good electron conduction path can be formed, further reducing the increase rate of the DC resistance accompanying the charge and discharge cycle. On the other hand, by making the content of the fibrous conductive agent relative to the positive electrode active material below the above upper limit, it is possible to suppress the space between the particles of the positive electrode active material from being occupied by the fibrous conductive agent in excess, etc., further reducing the increase rate of the DC resistance accompanying the charge and discharge cycle.

[0053] The content of the fibrous conductive agent relative to the total content of the fibrous conductive agent and the particulate conductive agent in the positive electrode active material layer is preferably 1% by mass to 90% by mass, more preferably 3% by mass to 70% by mass, further preferably 5% by mass to 50% by mass, and further preferably 10% by mass to 30% by mass. By making the content of the fibrous conductive agent relative to the total content of the fibrous conductive agent and the particulate conductive agent within the above range, the mixing ratio of the fibrous conductive agent and the particulate conductive agent can be optimized, so that the electronic conduction path formed in the positive electrode active material layer becomes a better state, and as a result, the rate of increase of the DC resistance accompanying the charge and discharge cycle can be further reduced.

[0054] The total content of the particulate conductive agent and the fibrous conductive agent in the positive electrode active material layer is preferably 0.3% to 10% by mass, more preferably 1% to 8% by mass, further preferably 2% to 6% by mass, and further preferably 3% to 5% by mass. By making the total content of the particulate conductive agent and the fibrous conductive agent in the positive electrode active material layer above the above lower limit, the electronic conductivity of the positive electrode active material layer can be further improved, and the increase rate of the DC resistance accompanying the charge and discharge cycle can be further reduced. On the other hand, by making the total content of the particulate conductive agent and the fibrous conductive agent below the above upper limit, the increase rate of the DC resistance accompanying the charge and discharge cycle can be fully reduced, and the content of the positive electrode active material is relatively increased, thereby improving the energy density.

[0055] The positive electrode active material layer may further contain a conductive agent other than a particulate conductive agent and a fibrous conductive agent. The conductive agent in the positive electrode active material layer is preferably substantially composed of a particulate conductive agent and a fibrous conductive agent. For example, the total content of the particulate conductive agent and the fibrous conductive agent in the positive electrode active material layer relative to the total conductive agent is preferably 90% by mass or more, and more preferably 99% by mass or more.

[0056] The content of all conductive agents in the positive electrode active material layer is preferably 0.3% to 10% by mass, more preferably 1% to 8% by mass, further preferably 2% to 6% by mass, and further preferably 3% to 5% by mass. By making the content of all conductive agents in the positive electrode active material layer above the above lower limit, the electronic conductivity of the positive electrode active material layer can be further improved, and the rate of increase of the DC resistance accompanying the charge and discharge cycle can be further reduced. On the other hand, by making the content of all conductive agents below the above upper limit, the rate of increase of the DC resistance accompanying the charge and discharge cycle can be fully reduced, and the content of the positive electrode active material can be relatively increased to improve the energy density.

[0057] As the binder, for example, fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), thermoplastic resins such as polyethylene, polypropylene, polyacrylic acid, and polyimide; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber; polysaccharide polymers, etc. Among these, fluororesins are preferred, and PVDF is more preferred.

[0058] The content of the binder in the positive electrode active material layer is sometimes preferably 0.3 mass % to 10 mass %, more preferably 0.5 mass % to 8 mass %, further preferably 1 mass % to 5 mass %, and further preferably 3 mass % or less or 2 mass % or less. By making the content of the binder above the lower limit, the positive electrode active material can be stably maintained. In addition, by making the content of the binder below the upper limit, the content of the positive electrode active material can be increased to improve the energy density.

[0059] As a thickener, for example, polysaccharide polymers such as carboxymethyl cellulose (CMC) and methyl cellulose can be cited. When the thickener has a functional group that reacts with lithium or the like, the functional group can be deactivated in advance by methylation or the like. When a thickener is used, the content of the thickener in the positive electrode active material layer is preferably 5% by mass or less, and more preferably 1% by mass or less. The technology disclosed herein is preferably implemented in a manner that the positive electrode active material layer does not contain a thickener.

[0060] The filler is not particularly limited. As fillers, polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, aluminum oxide, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicates, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, calcium fluoride, barium fluoride, and barium sulfate are insoluble ionic crystals, nitrides such as aluminum nitride and silicon nitride, talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, mica, etc., or their man-made products. When using a filler, the content of the filler in the positive electrode active material layer is preferably less than 5% by mass, and more preferably less than 1% by mass. The technology disclosed herein is preferably implemented in a manner where the positive electrode active material layer does not contain a filler.

[0061] The positive electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, I, typical metal elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, Ba, and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material, conductive agent, binder, thickener, and filler.

[0062] The lower limit of the median pore size in the pore volume distribution of the positive electrode active material layer is 100nm, sometimes preferably 105nm, more preferably 110nm, 115nm or 120nm. By making the above-mentioned median pore size above the above-mentioned lower limit, the gaps between the particles of the positive electrode active material can be fully formed, and the electrolyte can be uniformly infiltrated between the particles of the positive electrode active material, resulting in a reduction in the rate of increase of the DC resistance accompanying the charge and discharge cycle. The upper limit of the above-mentioned median pore size can be, for example, 200nm, 150nm, or 130nm. By making the above-mentioned median pore size below the above-mentioned upper limit, the distance between the particles of the positive electrode active material is appropriately close, and the content of the positive electrode active material in the positive electrode active material layer can be increased to achieve high energy density. In addition, it is possible to suppress the situation where it is difficult to fully form an electron conduction path using a particulate conductive agent and a fibrous conductive agent because the distance between the particles of the positive electrode active material is too far, and the rate of increase of the DC resistance accompanying the charge and discharge cycle can be further reduced. The above-mentioned median pore size can be above any of the above-mentioned lower limits and below any of the above-mentioned upper limits. The median pore size can be controlled by the composition ratio of each component constituting the positive electrode active material layer, the shape of each component, the dispersion state of each component, etc. It should be noted that even when the same components are used, as described below, if the fibrous conductive agent is fully dispersed, the median pore size tends to become larger.

[0063] In the Log differential pore volume distribution curve obtained from the pore volume distribution of the positive electrode active material layer, a first peak appears in the pore diameter range of 10 nm to less than 100 nm, and a second peak appears in the pore diameter range of 100 nm to less than 2000 nm.

[0064] The first peak is a peak corresponding to the gaps between particles of the particulate conductive agent. The range (peak position) in which the first peak appears is preferably in the range of 30nm to 90nm, and more preferably in the range of 40nm to 80nm. As the height of the first peak, it is preferably 0.054mL / g to 0.100mL / g, more preferably 0.056mL / g to 0.080mL / g, and further preferably 0.060mL / g to 0.070mL / g. When the height of the first peak is within the above range, the electrolyte is more easily maintained in the gaps between particles of the particulate conductive agent, and the rate of increase of the DC resistance with the charge and discharge cycle is further reduced.

[0065] The second peak is a peak corresponding to the gap between the particles of the positive electrode active material. The range (peak position) where the second peak appears is preferably in the range of 150nm to 1000nm, more preferably in the range of 200nm to 500nm, and further preferably in the range of 250nm to 400nm. As the height of the second peak, for example, it can be 0.03mL / g to 0.10mL / g, or it can be 0.04mL / g to 0.08mL / g.

[0066] The upper limit of the ratio of the height of the second peak to the height of the first peak (hereinafter also referred to as "peak height ratio (second peak / first peak)") is 1.20, preferably 1.15, more preferably 1.10, and further preferably 1.05. When the peak height ratio (second peak / first peak) is below the above upper limit, the gaps between the particles of the particulate conductive agent are almost not occupied by the fibrous conductive agent, and the electrolyte is easily retained in the gaps between the particles of the particulate conductive agent, which can reduce the rate of increase of the DC resistance accompanying the charge and discharge cycle. The lower limit of the peak height ratio (second peak / first peak) can be, for example, 0.50, and can be 0.60, 0.70, 0.80, 0.90 or 1.00. The peak height ratio (second peak / first peak) can be above any of the above lower limits and below any of the above upper limits.

[0067] The positive electrode having a positive electrode active material layer having such a pore distribution can be effectively obtained by preparing a positive electrode mixture paste in a manner that the positive electrode active material is coated in a state where the fibrous conductive agent is fully dispersed and the particulate conductive agent is almost not coated by the fibrous conductive agent, and using such a positive electrode mixture paste to prepare the positive electrode active material layer. A preferred method for manufacturing the positive electrode is described below.

[0068] In the Log differential pore volume curve of the positive electrode active material layer, preferably, no peak higher than the first peak and the second peak appears within the pore diameter range of 5.5 nm or more and less than 20 μm, and more preferably, no peak higher than half the height of the first peak and half the height of the second peak appears.

[0069] The total pore volume of the positive electrode active material layer is preferably 0.05 mL / g to 0.20 mL / g, more preferably 0.06 mL / g to 0.15 mL / g, and further preferably 0.08 mL / g to 0.12 mL / g. When the total pore volume of the positive electrode active material layer is within the above range, the rate of increase of the DC resistance accompanying the charge and discharge cycle can be further reduced. The "total pore volume" of the positive electrode active material layer can be obtained by measuring the pore volume distribution of the above-mentioned positive electrode active material layer.

[0070] <Method for producing positive electrode for energy storage device>

[0071] The preparation of the positive electrode can be carried out, for example, by applying a positive electrode mixture paste directly or through an intermediate layer on the positive electrode substrate and drying it. The positive electrode mixture paste contains various components constituting the positive electrode active material layer, such as a positive electrode active material, a particulate conductive agent and a fibrous conductive agent, and a binder as an arbitrary component. The positive electrode mixture paste usually also contains a dispersion medium. As a dispersion medium, an organic solvent can be preferably used. As an organic solvent of a dispersion medium that can be used in the preparation of a positive electrode mixture paste, N-methylpyrrolidone (NMP), toluene, etc. can be cited.

[0072] When preparing a positive electrode mixture paste, for example, it is preferred to first prepare a dispersion containing a fibrous conductive agent, add a positive electrode active material to the dispersion, and then add a particulate conductive agent. That is, with respect to the order in which the positive electrode active material, the particulate conductive agent, and the fibrous conductive agent are mixed, it is preferred to first mix the positive electrode active material and the fibrous conductive agent, and then mix the particulate conductive agent. When prepared in this order, the fibrous conductive agent first coats the surface of the positive electrode active material, thereby suppressing the space between the particles of the particulate conductive agent from being occupied by the fibrous conductive agent, and there is a tendency to obtain a positive electrode active material layer having a peak height ratio (second peak / first peak) of less than 1.20.

[0073] In addition, by fully stirring the dispersion containing the fibrous conductive agent, the aggregation of the fibrous conductive agent can be suppressed, and there is a tendency to obtain a positive electrode active material layer with a median pore size of 100 nm or more. The stirring can be performed on a dispersion containing a positive electrode active material and a fibrous conductive agent, or on a dispersion containing a positive electrode active material, a fibrous conductive agent and a particulate conductive agent. The above stirring can be performed appropriately under stirring conditions of a rotation speed of 5000 rpm to 10000 rpm and a stirring time of 10 seconds to 30 seconds using a stirring device such as a thin film gyratory high-speed stirrer.

[0074] <Electrical storage element>

[0075] The storage element involved in one embodiment of the present invention comprises: an electrode body having a positive electrode, a negative electrode and a separator, an electrolyte, and a container for accommodating the electrode body and the electrolyte. The electrode body is usually a stacked type in which a plurality of positive electrodes and a plurality of negative electrodes are stacked with a separator, or a wound type in which the positive electrode and the negative electrode are wound in a state of being stacked with a separator. The electrolyte exists in a state of being impregnated in the positive electrode, the negative electrode and the separator. The electrolyte is preferably an electrolyte. The electrolyte refers to a liquid electrolyte. The electrolyte, for example, contains a solvent and an electrolyte salt dissolved in the solvent. The electrolyte can be an ionic liquid, etc. When the electrolyte is an electrolyte, the effect of the positive electrode and the storage element involved in one aspect of the present invention can be particularly significantly exerted.

[0076] As an example of an electric storage element, a nonaqueous electrolyte secondary battery (hereinafter, also simply referred to as a “secondary battery”) using a nonaqueous electrolyte as an electrolyte will be described.

[0077] (positive electrode)

[0078] The positive electrode included in the electric storage element is the positive electrode according to the above-mentioned embodiment of the present invention.

[0079] (negative electrode)

[0080] The negative electrode comprises a negative electrode substrate and a negative electrode active material layer disposed on the negative electrode substrate directly or via an intermediate layer. The structure of the intermediate layer is not particularly limited, and can be selected from the structures exemplified for the positive electrode described above.

[0081] The negative electrode substrate has conductivity. As the material of the negative electrode substrate, metals such as copper, nickel, stainless steel, nickel-plated steel, aluminum, or their alloys, carbonaceous materials, etc. can be used. Among these, copper or copper alloys are preferred. As the negative electrode substrate, foil, vapor-deposited film, mesh, porous material, etc. can be cited. From the perspective of cost, foil is preferred. Therefore, as the negative electrode substrate, copper foil or copper alloy foil is preferred. As examples of copper foil, rolled copper foil, electrolytic copper foil, etc. can be cited.

[0082] The average thickness of the negative electrode substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, further preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate to the above range, the strength of the negative electrode substrate can be increased, and the energy density per unit volume of the storage element can be increased.

[0083] The negative electrode active material layer contains a negative electrode active material. The negative electrode active material layer contains any components such as a conductive agent, a binder, a thickener, and a filler as needed. The conductive agent, the binder, the thickener, the filler, and any other components can be selected from the materials exemplified in the above-mentioned positive electrode. The conductive agent used in the negative electrode active material layer can be one or both of a particulate conductive agent and a fibrous conductive agent, or can be other conductive agents. The negative electrode active material layer can be a layer substantially composed only of a negative electrode active material such as metal Li.

[0084] The negative electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, I, typical metal elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, Ba, and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the negative electrode active material, conductive agent, binder, thickener, and filler.

[0085] The negative electrode active material can be appropriately selected from known negative electrode active materials. As the negative electrode active material for lithium ion secondary batteries, materials that can absorb and release lithium ions can generally be used. Examples of the negative electrode active material include metal Li; metals or semimetals such as Si and Sn; metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide; Li4Ti5O 12 , LiTiO2, TiNb2O7 and other titanium-containing oxides; polyphosphate compounds; silicon carbide; carbon materials such as graphite and non-graphite carbon (easily graphitized carbon or non-graphitized carbon). Among these materials, graphite and non-graphite carbon are preferred. In the negative electrode active material layer, one of these materials may be used alone, or two or more of them may be mixed and used.

[0086] “Graphite” refers to the average interplanar spacing (d) of the (002) plane determined by X-ray diffraction before charge or discharge or in a discharged state. 002 ) is a carbon material having a diameter of 0.33 nm or more and less than 0.34 nm. Examples of graphite include natural graphite and artificial graphite. From the perspective of obtaining a material with stable physical properties, artificial graphite is preferred.

[0087] “Non-graphite carbon” refers to the average interplanar spacing (d ) of the (002) plane determined by X-ray diffraction before charge / discharge or in a discharged state. 002 ) is a carbon material having a particle size of 0.34 nm to 0.42 nm. Examples of non-graphite carbon include difficult-graphitization carbon and easy-graphitization carbon. Examples of non-graphite carbon include materials derived from resins, petroleum asphalt or materials derived from petroleum asphalt, petroleum coke or materials derived from petroleum coke, materials derived from plants, materials derived from alcohols, and the like.

[0088] Here, the "discharge state" of the carbon material refers to a state in which the lithium ions that can be stored and released accompanying the charge and discharge are fully released from the carbon material as the negative electrode active material. For example, in a half-cell using a negative electrode containing a carbon material as a negative electrode active material as a working electrode and using metal Li as a counter electrode, the open circuit voltage is 0.7V or more.

[0089] "Difficult to graphitize carbon" refers to the above-mentioned 002 It is a carbon material with a diameter of 0.36nm to 0.42nm.

[0090] "Easily graphitizable carbon" refers to the above-mentioned 002 A carbon material having a diameter of 0.34 nm or more and less than 0.36 nm.

[0091] The negative electrode active material is usually a particle (powder). The average particle size of the negative electrode active material can be, for example, 1 nm to 100 μm. When the negative electrode active material is a carbon material, a titanium-containing oxide or a polyphosphate compound, its average particle size can be 1 μm to 100 μm. When the negative electrode active material is Si, Sn, Si oxide or Sn oxide, etc., its average particle size can be 1 nm to 1 μm. By making the average particle size of the negative electrode active material above the above lower limit, it is easy to manufacture or handle the negative electrode active material. By making the average particle size of the negative electrode active material below the above upper limit, the electronic conductivity of the negative electrode active material layer is improved. In order to obtain a powder with a specified particle size, a pulverizer, a classifier, etc. can be used. The pulverization method and the classification method can be selected, for example, from the methods exemplified for the above-mentioned positive electrode. When the negative electrode active material is a metal such as metal Li, the negative electrode active material layer can be in the form of a foil.

[0092] The content of the negative electrode active material in the negative electrode active material layer is preferably 60% to 99% by mass, more preferably 90% to 98% by mass. When the content of the negative electrode active material is within the above range, both high energy density and manufacturability of the negative electrode active material layer can be achieved.

[0093] (Isolator)

[0094] The separator can be appropriately selected from known separators. As the separator, for example, a separator consisting only of a substrate layer, a separator in which a heat-resistant layer containing heat-resistant particles and a binder is formed on one or both sides of the substrate layer, etc. can be used. As the shape of the substrate layer of the separator, for example, woven fabrics, non-woven fabrics, porous resin films, etc. can be cited. Among these shapes, porous resin films are preferred from the viewpoint of strength, and non-woven fabrics are preferred from the viewpoint of liquid retention of non-aqueous electrolytes. As the material of the substrate layer of the separator, from the viewpoint of the shutdown function, for example, polyolefins such as polyethylene and polypropylene are preferred, and from the viewpoint of resistance to oxidative decomposition, for example, polyimides, aromatic polyamides, etc. are preferred. As the substrate layer of the separator, a material obtained by compounding these resins can be used.

[0095] The weight loss of the heat-resistant particles contained in the heat-resistant layer when the temperature is raised from room temperature to 500°C in an air atmosphere of 1 atmosphere is preferably 5% or less, and the weight loss when the temperature is raised from room temperature to 800°C is more preferably 5% or less. As materials with a weight loss below the prescribed value, inorganic compounds can be cited. As inorganic compounds, for example, oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminum silicate; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; insoluble ionic crystals such as calcium fluoride, barium fluoride, and barium titanate; covalent crystals such as organosilicon and diamond; talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, mica, etc., or their artificial products, etc. As inorganic compounds, monomers or composites of these substances can be used alone, or two or more can be mixed and used. Among these inorganic compounds, silicon oxide, aluminum oxide, or aluminosilicate is preferred from the viewpoint of safety of the electric storage element.

[0096] The porosity of the separator is preferably 80% by volume or less from the viewpoint of strength, and preferably 20% by volume or more from the viewpoint of discharge performance. Here, the "porosity" refers to a value based on volume, and is a value measured by a mercury porosimeter.

[0097] As the separator, a polymer gel composed of a polymer and a non-aqueous electrolyte can be used. Examples of the polymer include polyacrylonitrile, polyethylene oxide, polypropylene oxide, polymethyl methacrylate, polyvinyl acetate, polyvinyl pyrrolidone, and polyvinylidene fluoride. If a polymer gel is used, leakage can be suppressed. As the separator, a porous resin film or nonwoven fabric as described above can be used in combination with the polymer gel.

[0098] (Non-aqueous electrolyte)

[0099] The non-aqueous electrolyte can be appropriately selected from known non-aqueous electrolytes. The non-aqueous electrolyte can be a non-aqueous electrolyte solution. The non-aqueous electrolyte solution contains a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent.

[0100] As nonaqueous solvent, can suitably select from known nonaqueous solvent.As nonaqueous solvent, can enumerate cyclic carbonate, linear carbonate, carboxylate, phosphoric acid ester, sulfonic acid ester, ether, amides, nitrile etc.As nonaqueous solvent, can use the compound that the part of contained hydrogen atom in these compounds is replaced by halogen.

[0101] Examples of the cyclic carbonate include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), vinyl ethylene carbonate (VEC), chloroethylene carbonate, fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), styrene carbonate, 1-phenylvinylene carbonate, 1,2-diphenylvinylene carbonate, etc. Among these, EC is preferred.

[0102] Examples of the chain carbonate include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diphenyl carbonate, ethyl methyl trifluorocarbonate, bis(trifluoroethyl) carbonate, etc. Among these, EMC is preferred.

[0103] As the non-aqueous solvent, preferably a cyclic carbonate or a chain carbonate is used, and more preferably a cyclic carbonate and a chain carbonate are used in combination. By using a cyclic carbonate, the dissociation of the electrolyte salt can be promoted to improve the ionic conductivity of the non-aqueous electrolyte. By using a chain carbonate, the viscosity of the non-aqueous electrolyte can be suppressed to a low level. When a cyclic carbonate and a chain carbonate are used in combination, the volume ratio of the cyclic carbonate to the chain carbonate (cyclic carbonate: chain carbonate) is, for example, preferably in the range of 5:95 to 50:50.

[0104] As the electrolyte salt, it is possible to appropriately select from known electrolyte salts. Examples of the electrolyte salt include lithium salts, sodium salts, potassium salts, magnesium salts, Salts, etc. Among these, lithium salts are preferred.

[0105] As lithium salts, inorganic lithium salts such as LiPF6, LiPO2F2, LiBF4, LiClO4, and LiN(SO2F)2, lithium oxalate salts such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP), and lithium salts having halogenated hydrocarbon groups such as LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), LiC(SO2CF3)3, and LiC(SO2C2F5)3 can be cited. Among these, inorganic lithium salts are preferred, and LiPF6 is more preferred.

[0106] The content of the electrolyte salt in the non-aqueous electrolyte is preferably 0.1 mol / dm 3 ~2.5mol / dm 3 , more preferably 0.3 mol / dm 3 ~2.0mol / dm 3 , more preferably 0.5 mol / dm 3 ~1.7mol / dm 3 , particularly preferably 0.7 mol / dm 3 ~1.5mol / dm 3 By setting the content of the electrolyte salt to be within the above range, the ion conductivity of the non-aqueous electrolyte can be increased.

[0107] In addition to the non-aqueous solvent and the electrolyte salt, the non-aqueous electrolyte may contain additives. Examples of additives include halogenated carbonates such as fluoroethylene carbonate (FEC) and difluoroethylene carbonate (DFEC); oxalates such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP); imide salts such as lithium bis(fluorosulfonyl)imide (LiFSI); aromatic compounds such as biphenyl, alkylbiphenyl, terphenyl, partial hydride of terphenyl, cyclohexylbenzene, tert-butylbenzene, tert-amylbenzene, diphenyl ether, and dibenzofuran; partial halides of the above aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, 3,5-difluoro Anisole and other halogenated anisole compounds; vinylene carbonate, methyl vinylene carbonate, ethyl vinylene carbonate, succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, cyclohexanedicarboxylic anhydride; ethylene sulfite, propylene sulfite, dimethyl sulfite, methyl methanesulfonate, busulfan, methyl toluenesulfonate, dimethyl sulfate, ethylene sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-dioxo-1,3,2-dioxathiolane), 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, thioanisole, diphenyl disulfide, bipyridine disulfide, 1,3-propylene sultone, 1,3-propane sultone, 1,4-butane sultone, 1,4-butene sultone, perfluorooctane, tris(trimethylsilyl)borate, tris(trimethylsilyl)phosphate, tetrakis(trimethylsilyl)titanate, monofluorolithium phosphate, difluorolithium phosphate, etc. These additives may be used alone or in combination of two or more.

[0108] Relative to the mass of the entire nonaqueous electrolyte, the content of the additive contained in the nonaqueous electrolyte is preferably 0.01% by mass to 10% by mass, more preferably 0.1% by mass to 7% by mass, further preferably 0.2% by mass to 5% by mass, and particularly preferably 0.3% by mass to 3% by mass. By making the content of the additive within the above range, the capacity maintenance performance or cycle performance after high temperature storage can be improved, or the safety can be further improved.

[0109] The non-aqueous electrolyte may be used in combination with a non-aqueous electrolyte solution and a solid electrolyte.

[0110] The solid electrolyte can be selected from any material that has ion conductivity and is solid at room temperature (e.g., 15° C. to 25° C.), such as lithium, sodium, and calcium. Examples of the solid electrolyte include sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and polymer solid electrolytes.

[0111] As sulfide solid electrolytes, in the case of lithium ion secondary batteries, for example, Li2S-P2S5, LiI-Li2S-P2S5, Li 10 Ge-P2S 12 wait.

[0112] The shape of the electric storage element of the present embodiment is not particularly limited, and examples thereof include cylindrical batteries, square batteries, flat batteries, coin batteries, button batteries, and the like.

[0113] Figure 1 , a storage element 1 as an example of a square battery is shown. It should be noted that this figure is a perspective view of the inside of the container. An electrode body 2 having a positive electrode and a negative electrode wound with a separator sandwiched therebetween is housed in a square container 3. The positive electrode is electrically connected to a positive terminal 4 via a positive electrode lead 41. The negative electrode is electrically connected to a negative terminal 5 via a negative electrode lead 51.

[0114] <Electricity storage device>

[0115] The storage element of this embodiment can be installed as a storage unit (battery module) composed of a plurality of storage elements in a vehicle power source such as an electric vehicle (EV), a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), a power source for electronic devices such as a personal computer and a communication terminal, or a power source for power storage, etc. In this case, the technology of the present invention only needs to be applied to at least one storage element contained in the storage unit.

[0116] An electric storage device according to an embodiment of the present invention includes two or more electric storage elements, and includes one or more electric storage elements including the positive electrode for the electric storage element according to the embodiment of the present invention (hereinafter referred to as the "second embodiment"). The technology involved in the embodiment of the present invention can be applied to at least one electric storage element included in the electric storage device according to the second embodiment, and may include one electric storage element including the positive electrode for the electric storage element according to the embodiment of the present invention, and may include one or more electric storage elements not involved in the embodiment of the present invention, or may include two or more electric storage elements including the positive electrode for the electric storage element according to the embodiment of the present invention.

[0117] Figure 2, an example of a power storage device 30 according to the second embodiment is shown in which a power storage unit 20 formed by collecting two or more power storage elements 1 electrically connected is further collected. The power storage device 30 may include a bus bar (not shown) to which two or more power storage elements 1 are electrically connected, or a bus bar (not shown) to which two or more power storage units 20 are electrically connected. The power storage unit 20 or the power storage device 30 may include a state monitoring device (not shown) for monitoring the state of one or more power storage elements.

[0118] <Method for manufacturing energy storage device>

[0119] The manufacturing method of the storage element of this embodiment can be appropriately selected from known methods. The manufacturing method includes, for example, the steps of preparing an electrode body, preparing an electrolyte, and accommodating the electrode body and the electrolyte in a container. The step of preparing the electrode body includes the steps of preparing a positive electrode and a negative electrode, and stacking or winding the positive electrode and the negative electrode with a separator to form an electrode body.

[0120] The step of accommodating the electrolyte in the container can be appropriately selected from known methods. For example, when an electrolyte solution is used as the electrolyte, the electrolyte solution can be injected from an injection port formed in the container and then the injection port can be sealed.

[0121] <Other embodiments>

[0122] It should be noted that the storage element of the present invention is not limited to the above-mentioned embodiment, and various changes can be added within the scope of the main purpose of the present invention. For example, the structure of another embodiment can be added to the structure of a certain embodiment, and a part of the structure of a certain embodiment can be replaced with the structure of another embodiment or a known technology. In addition, a part of the structure of a certain embodiment can be deleted. In addition, a known technology can be added to the structure of a certain embodiment.

[0123] In the above embodiment, the case of using a storage element as a rechargeable non-aqueous electrolyte secondary battery (e.g., a lithium ion secondary battery) is described, but the type, shape, size, capacity, etc. of the storage element are arbitrary. The present invention can also be applied to capacitors such as various secondary batteries, double-layer capacitors or lithium ion capacitors. In addition, the storage element positive electrode and storage element of the present invention can also be applied to storage elements whose electrolyte is an electrolyte other than a non-aqueous electrolyte.

[0124] In the above embodiment, the positive electrode and the negative electrode are stacked with a separator, but the electrode body may not have a separator. For example, the positive electrode and the negative electrode may be in direct contact with each other with a non-conductive layer formed on the active material layer of the positive electrode or the negative electrode.

[0125] Example

[0126] The present invention will be described in more detail by way of examples below, but the present invention is not limited to the following examples.

[0127] [Example 1]

[0128] (Fabrication of the positive electrode)

[0129] Prepare a lithium transition metal composite oxide (NCM) represented by LiNi 0.6 Co 0.2 Mn 0.2 O2, carbon black (CB: average particle size 35 nm, average aspect ratio 1.1) as a particulate conductive agent, CNT (average diameter 7 nm, average length about 60 - 100 μm) as a fibrous conductive agent, and polyvinylidene fluoride (PVDF) as a binder.

[0130] First, prepare a dispersion containing CNT and PVDF with N - methylpyrrolidone (NMP) as the dispersion medium. Add the positive electrode active material (NCM) to this dispersion, and knead it for 20 seconds at a rotational speed of 7600 rpm using a thin - film spin - type high - speed mixer ("FILMIX" (registered trademark) manufactured by PRIMIX Corporation). Thereafter, further add CB to this dispersion, and use a mixing and kneading machine ("あわとり練太郎" (registered trademark) manufactured by THINKY Corporation) to knead it for 5 minutes at a rotational speed of 2000 rpm to prepare a positive electrode mixture paste. It should be noted that each component is used such that the mass ratio of the positive electrode active material, CB, CNT, and PVDF in the obtained positive electrode mixture paste is 94.5:3.4:0.6:1.5 in terms of solid components. The positive electrode active material layer is fabricated by coating the obtained positive electrode mixture paste on the surface of an aluminum foil serving as the positive electrode substrate and drying it. Thereafter, roll pressing is performed to obtain the positive electrode of Example 1.

[0131] (Fabrication of the negative electrode)

[0132] Prepare a negative electrode mixture paste containing graphite as the negative electrode active material, styrene - butadiene rubber (SBR) as the binder, and carboxymethyl cellulose (CMC) as the thickener in a mass ratio of 96:3:1 (in terms of solid components), with water as the dispersion medium. The negative electrode active material layer is fabricated by coating the obtained negative electrode mixture paste on the surface of a copper foil serving as the negative electrode substrate and drying it. Thereafter, roll pressing is performed to obtain the negative electrode.

[0133] (Preparation of the non - aqueous electrolyte)

[0134] Dissolve LiPF6 at 1.0 mol / dm 3The concentration of was dissolved in a non-aqueous solvent obtained by mixing ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) in a volume ratio of 30:35:35 to prepare a non-aqueous electrolyte.

[0135] (Assembly of energy storage elements)

[0136] The positive electrode and the negative electrode were stacked with a polyethylene separator interposed therebetween to produce an electrode assembly. The electrode assembly was housed in a container, and the nonaqueous electrolyte was injected into the container to obtain the electric storage element of Example 1.

[0137] [Example 2]

[0138] A positive electrode and an electric storage element of Example 2 were obtained in the same manner as in Example 1 except that the procedure for preparing the positive electrode mixture paste was as follows.

[0139] First, a dispersion containing CNT and PVDF and using NMP as a dispersion medium is prepared. A positive electrode active material (NCM) is added to the dispersion, and CB is further added. After adding all the components, a thin film gyratory high-speed stirrer ("FILMIX" (registered trademark) manufactured by PRIMIX) is used to mix at a rotation speed of 7600 rpm for 20 seconds to prepare a positive electrode mixture paste.

[0140] [Comparative Example 1]

[0141] A positive electrode and a storage element of Comparative Example 1 were obtained in the same manner as in Example 1 except that a mixer ("Awato Ri Rentaro" (registered trademark) manufactured by THINKY Corporation) was used instead of the thin film rotary high-speed mixer and kneading was performed at a rotation speed of 2000 rpm for 5 minutes.

[0142] [Comparative Example 2]

[0143] A positive electrode and an electric storage element of Comparative Example 2 were obtained in the same manner as in Example 1 except that the procedure for preparing the positive electrode mixture paste was as follows.

[0144] First, a dispersion containing CB and PVDF and using NMP as a dispersion medium is prepared. A positive electrode active material (NCM) is added to the dispersion, and CNT and PVDF are further added. After adding all the components, a thin film gyratory high-speed stirrer ("FILMIX" (registered trademark) manufactured by PRIMIX) is used to mix at a rotation speed of 7600 rpm for 20 seconds to prepare a positive electrode mixture paste.

[0145] [Comparative Example 3]

[0146] A positive electrode and an electric storage element of Comparative Example 3 were obtained in the same manner as in Example 1 except that the procedure for preparing the positive electrode mixture paste was as follows.

[0147] The positive electrode mixture paste was prepared by adding a positive electrode active material (NCM), CB, and PVDF to NMP as a dispersion medium and kneading them for 5 minutes at a rotational speed of 2000 rpm using a mixing blender (“あわとり練太郎” (registered trademark) manufactured by THINKY Corporation). The mass ratio of the positive electrode active material, CB, and PVDF in terms of solid components was 94.5:4.0:1.5.

[0148] [Comparative Example 4]

[0149] The steps for preparing the positive electrode mixture paste were as follows. Otherwise, the same procedures as in Example 1 were carried out to obtain the positive electrode and the storage element of Comparative Example 4.

[0150] The positive electrode active material (NCM), CB, and PVDF were added to NMP as a dispersion medium, and a planetary mixer (“PVML-25” manufactured by Asada Iron Works Co., Ltd.) was used to knead them for 30 minutes at a rotational speed of 100 rpm to prepare the positive electrode mixture paste. The mass ratio of the positive electrode active material, CB, and PVDF in terms of solid components was 92.5:5.0:2.5.

[0151] [Measurement]

[0152] The pore volume distribution of the positive electrode active material layer of each obtained positive electrode was measured by the above method, and the total pore volume and the median pore diameter were determined. In addition, a Log differential pore volume distribution curve was obtained from the above pore volume distribution, and the positions and heights of the first peak and the second peak, and the peak height ratio (second peak / first peak) were determined. These measurement results are shown in Table 1.

[0153] [Evaluation]

[0154] (Initial charge and discharge)

[0155] Each obtained storage element was subjected to initial charge and discharge under the following conditions. In a thermostat at 25°C, it was charged at a constant current of 1.0C until the charge termination voltage of 4.20V, and then charged at a constant voltage of 4.20V. The end condition of the charge was that the total charge time reached 3 hours. Thereafter, a rest time of 10 minutes was set. It was discharged at a constant current of 1.0C until the discharge termination voltage of 2.50V.

[0156] (Initial DC resistance)

[0157] For each storage element after the initial charge and discharge, a constant current charge of 1.0C was performed in a thermostatic chamber at 25°C to make the SOC 50%. Thereafter, the discharge was performed in a thermostatic chamber at 25°C in the order of discharge current 0.2C, 0.5C, and 1.0C for 30 seconds each. After each discharge, a constant current charge was performed with a charge current of 0.05C to make the SOC 50%. The relationship between the discharge current in each discharge current and the voltage at 10 seconds after the start of discharge was plotted, and the DC resistance was calculated from the slope of the straight line obtained from the plot of the three points as the initial DC resistance.

[0158] (Charge and discharge cycle test)

[0159] Next, the following charge and discharge cycle test was performed. In a 60°C constant temperature chamber, the battery was charged at a constant current and constant voltage of 1.0C to a charge termination voltage of 4.20V. The charging termination condition was that the total charging time reached 3 hours. After that, a rest time of 10 minutes was set. The battery was discharged at a constant current of 1.0C to a discharge termination voltage of 2.50V, and then a rest time of 10 minutes was set. The charge and discharge were cycled 1000 times.

[0160] (Rate of increase in DC resistance)

[0161] After the charge-discharge cycle test, the DC resistance of each storage element was obtained by the same method as the above-mentioned "initial DC resistance" as the DC resistance after the charge-discharge cycle test. The increase rate of the DC resistance after the charge-discharge cycle test was obtained from the initial DC resistance and the DC resistance after the charge-discharge cycle test. The increase rate of the DC resistance (DCR increase rate) is shown in Table 1.

[0162]

[0163] The increase rate of the DC resistance of each storage element of Examples 1 and 2, in which the positive electrode active material layer contains a particulate conductive agent and a fibrous conductive agent, the median pore diameter is 100nm or more, and the peak height ratio (second peak / first peak) is 1.20 or less, is a low value of 28% or less. In contrast, the increase rate of the DC resistance of each storage element of Comparative Example 1 with a median pore diameter of less than 100nm, Comparative Example 2 with a peak height ratio (second peak / first peak) greater than 1.20, and Comparative Examples 3 and 4 in which the positive electrode active material layer does not contain a fibrous conductive agent is a high value of more than 28%.

[0164] In addition, in the preparation of the positive electrode mixture paste containing the positive electrode active material, the particulate conductive agent and the fibrous conductive agent, the comparative example 1 using the mixing and stirring machine was not mixed sufficiently, so the dispersion of the fibrous conductive agent was insufficient, etc., resulting in a small median pore size. In the comparative example 2 in which the fibrous conductive agent was added to the dispersion containing the positive electrode active material and the particulate conductive agent, most of the gaps between the particles of the particulate conductive agent were occupied by the fibrous conductive agent, etc., resulting in a large peak height ratio (second peak / first peak). On the other hand, in Examples 1 and 2, before adding the particulate conductive agent, the positive electrode active material was mixed with the fibrous conductive agent, and then the particulate conductive agent was added, and the mixing was fully performed with a thin film gyratory high-speed mixer. It is speculated that in Examples 1 and 2, the gaps between the particles of the particulate conductive agent are almost not occupied by the fibrous conductive agent, and the positive electrode active material is covered with the fibrous conductive agent in a state where the fibrous conductive agent is fully dispersed, so the median pore size is greater than 100nm and the peak height ratio is less than 1.20.

[0165] Industrial Applicability

[0166] The present invention is applicable to a storage element used as a power source for electronic devices such as personal computers and communication terminals, and automobiles, and a positive electrode included therein.

[0167] Explanation of symbols

[0168] 1 Storage element

[0169] 2 Electrode body

[0170] 3 Container

[0171] 4 Positive terminal

[0172] 41 Positive lead

[0173] 5 Negative terminal

[0174] 51 Negative lead

[0175] 20 Storage unit

[0176] 30 Power storage device

Claims

1. A positive electrode for a storage element, comprising a positive electrode active material layer containing a positive electrode active material, a particulate conductive agent and a fibrous conductive agent, The diameter of the fibrous conductive agent is less than 60 nm. The median pore diameter in the pore volume distribution of the positive electrode active material layer is greater than 100 nm. In the Log differential pore volume distribution curve obtained from the pore volume distribution, a first peak appears in the range of pore diameter greater than 10 nm and less than 100 nm, and a second peak appears in the range of pore diameter greater than 100 nm and less than 2000 nm, and the ratio of the height of the second peak to the height of the first peak, i.e., second peak / first peak, is less than 1.

20.

2. The positive electrode for an electric storage element according to claim 1, wherein The height of the first peak is greater than 0.054 mL / g.

3. The positive electrode for an electric storage element according to claim 1 or 2, wherein The content of the fibrous conductive agent relative to the positive electrode active material is 0.10 mass % to 2 mass %.

4. The positive electrode for an electric storage element according to claim 1 or 2, wherein The particulate conductive agent is carbon black, and the fibrous conductive agent is fibrous carbon. 5 . An electric storage element comprising the positive electrode for an electric storage element according to claim 1 . 6 . An electric storage device comprising two or more electric storage elements, wherein the electric storage device comprises one or more electric storage elements comprising the electric storage element positive electrode according to claim 1 or 2.