Method for recovering active material from electricity storage device

By processing the lithium-ion battery electrodes in a wave-like manner and using airflow, water flow, or shock waves for stripping, the problem of difficult separation of active materials in existing lithium-ion battery recycling has been solved, achieving efficient and low-cost recycling of active materials.

CN118975016APending Publication Date: 2024-11-15CENTRAL RESEARCH INSTITUTE OF ELECTRIC POWER INDUSTRY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031108.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In existing lithium-ion battery recycling methods, the roasting and melting processes suffer from resource waste, environmental pollution, and difficulty in separating active materials due to high-temperature treatment. Furthermore, existing non-roasting processes are difficult to efficiently strip active materials.

Method used

By processing the electrodes into a wavy shape and then peeling them off under external stimulation such as airflow, water flow, or shock waves, electrode deformation is avoided, thereby improving the recovery rate and purity of active materials.

Benefits of technology

It achieves efficient and low-cost recovery of active substances, reduces the introduction of impurities, improves recovery rate and purity, and reduces environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118975016A_ABST
    Figure CN118975016A_ABST
Patent Text Reader

Abstract

A recovery method for recovering an active material from a power storage device includes a processing step of performing processing so that at least a portion of an electrode in a power storage device including the electrode to which the active material adheres has a wavy shape.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for recovering active materials from an electricity storage device. Background Art

[0002] As vehicles become more electric and renewable energy is used more and more, lithium-ion batteries, which are one type of power storage devices, have excellent power storage performance and are therefore used in increasing amounts. The value of resources such as cobalt and nickel used in these lithium-ion batteries fluctuates greatly, and it is expected that supply can be ensured through recycling.

[0003] Compared with conventional nickel-metal hydride batteries, lithium-ion batteries have a lower resource value as a whole, so a recycling process that requires less energy is ideal. Examples of such recycling processes include a roasting process in which the batteries are burned in a roasting furnace, a melting process in which the batteries are melted, and a non-roasting process in which the batteries are not burned in a roasting furnace. However, the roasting process is the main recycling process for lithium-ion batteries in China.

[0004] However, the calcination process and the melting process have the problems of consuming fossil fuels such as natural gas and heavy oil, electric energy, and generating a large amount of carbon dioxide due to the thermal decomposition of organic electrolyte and plastic constituting the battery due to the high temperature treatment of the battery. In addition, the calcination process and the melting process have the problems of oxidizing and mixing the raw materials recovered from the battery due to the high temperature treatment of the materials, making it difficult to separate each raw material, and the types of recyclable active materials are less than those of non-calcination processes, and the value of the raw materials is reduced.

[0005] On the other hand, overseas, with Europe as the center, which seeks to avoid the incineration of batteries, various studies are being conducted on recycling technologies for non-baked lithium-ion batteries that do not rely on incineration. For example, there is a known method of using a milling cutter or the like to cut the electrodes of a lithium-ion battery, applying airflow to the cut electrodes, causing the electrodes to collide in a container, thereby stripping the active material from the electrodes (e.g., non-patent document 1, etc.).

[0006] In addition, there is known a method in which the above-mentioned electrode is dispersed in water and stirred in a water flow to remove the active material from the electrode (for example, Non-Patent Document 2).

[0007] However, the method described in non-patent document 1 has the following problems: in order to efficiently peel off the active material, the electrode needs to be cut into pieces of about 10 mm; the peeling rate of the active material is low when the active material is firmly in contact with the electrode; and during long-term treatment, the electrodes will deform and become miniaturized each time they collide, making it impossible to efficiently recover the active material (due to the mixing of impurities such as aluminum and copper, separation requires a complicated process).

[0008] In addition, in the method described in non-patent document 2, although there is no restriction on the size of the cut electrode, the electrode will not be deformed or miniaturized during the peeling process and the active material with less impurities can be efficiently recovered, but when the active material is firmly in contact with the electrode, there are the following problems: the peeling rate of the active material is low; and the cost caused by the use of water in the process.

[0009] <Prior Art Literature>

[0010] <Patent Documents>

[0011] Non-patent literature 1: https: / / www.duesenfeld.com / recycling_en.html

[0012] Non-patent document 2: Ministry of the Environment, 2011, CO2 Recycling and Other Equipment Technology Demonstration Project, "Electric Vehicle Driving Battery Reuse and Recycling Technology Development Demonstration Project (Chubu Electric Power Co., Ltd.)", Ministry of the Environment, February 28, 2011 Summary of the invention

[0013] <Problems to be Solved by the Invention>

[0014] The present invention aims to solve the above-mentioned various conventional problems and achieve the following objectives: Specifically, the present invention aims to provide a method for recovering active materials from a power storage device, which can recover active materials from the power storage device with high efficiency and high purity.

[0015] In the present invention, the active material can be easily peeled off from the electrode by processing the electrode into a corrugated shape.

[0016] In addition, by processing the electrode into a shape that is difficult to deform even if a collision occurs, the electrode does not deform during the airflow treatment, so even if it is a relatively large electrode larger than the 10 mm used in the past, the active material attached to the center of the electrode can be peeled off, and the recovery rate of the active material is improved. In addition, since the miniaturization of the metal foil can be suppressed, the mixing of impurities in the recovered active material can be reduced.

[0017] Furthermore, when the electrode of the power storage device is multi-layered, the layers can be peeled off from each other to form a single layer, and the subsequent steps (material separation step, etc.) can be performed more easily.

[0018] <Methods used to solve the problem>

[0019] The means for solving the above-mentioned problems are as follows.

[0020] <1> A method for recovering active material from an electricity storage device, comprising: a processing step of processing an electrode in an electricity storage device including an electrode to which the active material is attached so that at least a portion of the electrode has a corrugated shape.

[0021] <2> The method for recovering active material from an electric storage device according to <1>, further comprising a peeling step of applying an external stimulus to the electrode to peel the active material from the electrode after the processing step.

[0022] <3> The method for recovering active material from an electrical storage device according to <2> above, wherein the wavy shape is at least one of a wavy shape as a whole, a wavy shape only at the ends, and a wavy shape in one direction as a whole and in a direction different from the one direction.

[0023] <4> The method for recovering active material from a power storage device according to any one of <1> to <3>, wherein a radius of curvature of the wavy shape is greater than or equal to 0 mm and less than or equal to 5 mm.

[0024] <5> The method for recovering active material from a power storage device according to any one of <1> to <4>, wherein a radius of curvature of the wavy shape is greater than or equal to 0 mm and less than or equal to 0.5 mm.

[0025] <6> The method for recovering active material from a power storage device according to any one of <2> to <5>, wherein the stripping step is performed at 0° C. or higher and 200° C. or lower.

[0026] <7> The method for recovering active material from a power storage device according to any one of <2> to <6>, wherein the external stimulus is airflow.

[0027] <8> The method for recovering active material from a power storage device according to <7>, wherein the airflow is applied to the electrode at a wind speed of 5 m / s to 100 m / s and for a time of 0.5 minutes to 2.0 minutes.

[0028] <9> The method for recovering active material from a power storage device according to any one of <2> to <6>, wherein the external stimulus is a water flow.

[0029] <10> The method for recovering active material from an electrical storage device according to <9> above, wherein the water flow is applied to the electrode at a flow rate of 0.05 m / s to 10 m / s and for a time of 0.1 min to 5.0 min.

[0030] <11> The method for recovering active material from a power storage device according to any one of <2> to <6>, wherein the external stimulus is a shock wave.

[0031] <12> A method for recovering active materials from a power storage device according to <11> above, wherein the shock wave is applied to the electrode under the following conditions: an applied voltage of 10 kV to 200 kV, a distance from a counter electrode of an electric pulse device of 0.5 cm to 30 cm, and a pulse number of 1 to 100.

[0032] <Effects of the Invention>

[0033] According to the present invention, various conventional problems can be solved, and a recovery method for recovering active materials from a power storage device can be provided, the recovery method being capable of recovering active materials from the power storage device with high efficiency and high purity. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is an example of a flow chart for explaining the method for recovering the active material of the present invention.

[0035] Figure 2 This is a schematic diagram showing an example of an embodiment in which airflow is used as an external stimulus in the present invention.

[0036] Figure 3 This is a schematic diagram showing an example of an embodiment in which a water flow is used as an external stimulus in the present invention.

[0037] Figure 4 This is a schematic diagram showing an example of an embodiment in which a shock wave is used as an external stimulus in the present invention.

[0038] Figure 5 is a photograph showing the appearance of the active material recovered in Example 1, Figure 5 (a) is the electrode before the processing step. Figure 5 (b) is the electrode after the processing step.

[0039] Fig. 6A is a photograph showing the appearance of the active material recovered in Example 2-A, Fig. 6A (a) is the electrode before the processing step. Fig. 6A (b) is the electrode after the processing step.

[0040] Figure 6B is a photograph showing the appearance of the active material recovered in Example 2-B, Figure 6B (a) is the electrode before the processing step. Figure 6B (b) is the electrode after processing in one direction. Figure 6B (c) is an electrode that has been further processed in the above-mentioned 45-degree direction.

[0041] Figure 6C is a photograph showing the appearance of the active material recovered in Example 2-C, Figure 6C (a) is the electrode before the processing step. Figure 6C (b) is the electrode after processing in one direction. Figure 6C (c) is an electrode that has been further processed in the above 45-degree direction. Figure 6C (d) is an electrode that has been further processed in the above-mentioned 135-degree direction.

[0042] Figure 7 is a photograph showing the appearance of the active material recovered in Example 3, Figure 7 (a) is the electrode before the processing step. Figure 7 (b) is the electrode after the processing step.

[0043] Fig. 8A is a photograph showing the appearance of the active material recovered in Example 4-A, Fig. 8A (a) is the electrode before the processing step. Fig. 8A (b) is the electrode after the processing step.

[0044] Figure 8B is a photograph showing the appearance of the active material recovered in Example 4-B, Figure 8B (a) is the electrode before the processing step. Figure 8B (b) is the electrode after processing in one direction. Figure 8B (c) is an electrode that has been further processed in the above-mentioned 45-degree direction.

[0045] Figure 8C is a photograph showing the appearance of the active material recovered in Example 4-C, Figure 8C (a) is the electrode before the processing step. Figure 8C (b) is the electrode after processing in one direction. Figure 8C (c) is an electrode that has been further processed in the above-mentioned 45-degree direction. Figure 8C (d) is an electrode that has been further processed in the above-mentioned 135-degree direction.

[0046] Fig. 9 is a photograph showing the appearance of the active material recovered in Example 5, Fig. 9 (a) is the electrode before the processing step. Fig. 9 (b) is the electrode after the processing step.

[0047] Fig. 10A is a photograph showing the appearance of the active material recovered in Example 6-A, Fig. 10A (a) is the electrode before the processing step. Fig. 10A (b) is the electrode after the processing step.

[0048] Fig. 10B is a photograph showing the appearance of the active material recovered in Example 6-B, Fig. 10B (a) is the electrode before the processing step. Fig. 10B (b) is the electrode after processing in one direction. Fig. 10B (c) is an electrode that has been further processed in the above-mentioned 45-degree direction.

[0049] Fig. 10C is a photograph showing the appearance of the active material recovered in Example 6-C, Fig. 10C (a) is the electrode before the processing step. Fig. 10C (b) is the electrode after processing in one direction. Fig. 10C (c) is an electrode that has been further processed in the above 45-degree direction. Fig. 10C (d) is an electrode that has been further processed in the above-mentioned 135-degree direction.

[0050] Fig.11 is a photograph showing the appearance of the active material recovered in Example 7, Fig.11 (a) is the electrode before the processing step. Fig.11 (b) is the electrode after the processing step.

[0051] Fig.12 is a photograph showing the appearance of the active material recovered in Example 8, Fig.12 (a) is the electrode before the processing step. Fig.12 (b) is the electrode after the processing step.

[0052] Fig.13 is a photograph showing the appearance of the active material recovered in Example 9, Fig.13 (a) is the electrode before the processing step. Fig.13 (b) is the electrode after the processing step.

[0053] Fig.14 is a photograph showing the appearance of the active material recovered in Example 10, Fig.14 (a) is the electrode before the processing step. Fig.14 (b) is the electrode after the processing step.

[0054] Fig.15 is a photograph showing the appearance of the active material recovered in Example 11, Fig.15 (a) is the electrode before the processing step. Fig.15 (b) is the electrode after the processing step.

[0055] Fig.16 is a photograph showing the appearance of the active material recovered in Example 12, Fig.16 (a) is the electrode before the processing step. Fig.16 (b) is the electrode after the processing step.

[0056] Fig.17 is a photograph showing the appearance of the active material recovered in Example 13, Fig.17 (a) is the electrode before the processing step. Fig.17 (b) is the electrode after the processing step.

[0057] Fig.18 is a photograph showing the appearance of the active material recovered in Example 14, Fig.18 (a) is the electrode before the processing step. Fig.18 (b) is the electrode after the processing step.

[0058] Fig.19 is a photograph showing the appearance of the active material recovered in Example 15, Fig.19 (a) is the electrode before the processing step. Fig.19 (b) is the electrode after the processing step.

[0059] Fig. 20 is a photograph showing the appearance of the active material recovered in Example 16, Fig. 20 (a) is the electrode before the processing step. Fig. 20 (b) is the electrode after the processing step.

[0060] Fig.21 is a photograph showing the appearance of the active material recovered in Example 17, Fig.21 (a) is the electrode before the processing step. Fig.21 (b) is the electrode after the processing step.

[0061] Fig. 22 is a photograph showing the appearance of the active material recovered in Example 18, Fig. 22 (a) is the electrode before the processing step. Fig. 22 (b) is the electrode after the processing step.

[0062] Fig.23is a photograph showing the appearance of the active material recovered in Example 19, Fig.23 (a) is the electrode before the processing step. Fig.23 (b) is the electrode after the processing step.

[0063] Fig.24A is a photograph showing the appearance of the active material recovered in Example 20-A, Fig.24A (a) is the electrode before the processing step. Fig.24A (b) is the electrode after the processing step.

[0064] Fig. 24B is a photograph showing the appearance of the active material recovered in Example 20-B, Fig. 24B (a) is the electrode before the processing step. Fig. 24B (b) is the electrode after processing in one direction. Fig. 24B (c) is an electrode that has been further processed in the above-mentioned 45-degree direction.

[0065] Fig.24C is a photograph showing the appearance of the active material recovered in Example 20-C, Fig.24C (a) is the electrode before the processing step. Fig.24C (b) is the electrode after processing in one direction. Fig.24C (c) is an electrode that has been further processed in the above-mentioned 45-degree direction. Fig.24C (d) is an electrode that has been further processed in the above-mentioned 135-degree direction.

[0066] Fig.25 is a photograph showing the appearance of the active material recovered in Example 21, Fig.25 (a) is the electrode before the processing step. Fig.25 (b) is the electrode after the processing step.

[0067] Fig.26A is a photograph showing the appearance of the active material recovered in Example 22-A, Fig.26A (a) is the electrode before the processing step. Fig.26A (b) is the electrode after the processing step.

[0068] Fig.26B is a photograph showing the appearance of the active material recovered in Example 22-B, Fig.26B (a) is the electrode before the processing step. Fig.26B (b) is the electrode after processing in one direction. Fig.26B(c) is an electrode further processed in the above-mentioned 45-degree direction.

[0069] Fig.26C is a photograph showing the appearance of the active material recovered in Example 22-C, Fig.26C (a) is the electrode before the processing step. Fig.26C (b) is the electrode after processing in one direction. Fig.26C (c) is an electrode that has been further processed in the above 45-degree direction. Fig.26C (d) is an electrode that has been further processed in the above-mentioned 135-degree direction.

[0070] Fig. 27 is a photograph showing the appearance of the active material recovered in Example 23, Fig. 27 (a) is the electrode before the processing step. Fig. 27 (b) is the electrode after the processing step.

[0071] Fig.28A is a photograph showing the appearance of the active material recovered in Example 24-A, Fig.28A (a) is the electrode before the processing step. Fig.28A (b) is the electrode after the processing step.

[0072] Fig.28B is a photograph showing the appearance of the active material recovered in Example 24-B, Fig.28B (a) is the electrode before the processing step. Fig.28B (b) The electrode after a processing step in one direction, Fig.28B (c) is an electrode that has been further processed in the above-mentioned 45-degree direction.

[0073] Fig.28C is a photograph showing the appearance of the active material recovered in Example 24-C, Fig.28C (a) is the electrode before the processing step. Fig.28C (b) is the electrode after processing in one direction. Fig.28C (c) is an electrode that has been further processed in the above 45-degree direction. Fig.28C (d) is an electrode that has been further processed in the above-mentioned 135-degree direction.

[0074] Fig.29 is a photograph showing the appearance of the active material recovered in Example 25, Fig.29 (a) is the electrode before the processing step. Fig.29(b) is an electrode after the processing step and before the peeling step, Fig.29 (c) is the electrode after the peeling step.

[0075] Fig.30 is a photograph showing the appearance of the active material recovered in Example 26, Fig.30 (a) is the electrode before the processing step. Fig.30 (b) is an electrode after the processing step and before the peeling step, Fig.30 (c) is the electrode after the peeling step.

[0076] Fig.31 is a photograph showing the appearance of the active material recovered in Example 27, Fig.31 (a) is the electrode before the processing step. Fig.31 (b) is an electrode after the processing step and before the peeling step, Fig.31 (c) is the electrode after the peeling step.

[0077] Fig.32 is a photograph showing the appearance of the active material recovered in Example 28, Fig.32 (a) is the electrode before the processing step. Fig.32 (b) is an electrode after the processing step and before the peeling step, Fig.32 (c) is the electrode after the peeling step.

[0078] Fig.33 is a photograph showing the appearance of the active material recovered in Example 29, Fig.33 (a) is the electrode before the processing step. Fig.33 (b) is an electrode after the processing step and before the peeling step, Fig.33 (c) is the electrode after the peeling step.

[0079] Fig.34 is a photograph showing the appearance of the active material recovered in Example 30, Fig.34 (a) is the electrode before the processing step. Fig.34 (b) is an electrode after the processing step and before the peeling step, Fig.34 (c) is the electrode after the peeling step.

[0080] Fig.35 is a photograph showing the appearance of the active material recovered in Example 31, Fig.35 (a) is the electrode before the processing step. Fig.35 (b) is an electrode after the processing step and before the peeling step, Fig.35(c) is the electrode after the peeling step.

[0081] Fig.36 is a photograph showing the appearance of the active material recovered in Example 32, Fig.36 (a) is the electrode before the processing step. Fig.36 (b) is an electrode after the processing step and before the peeling step, Fig.36 (c) is the electrode after the peeling step.

[0082] Fig.37 is a photograph showing the appearance of the active material recovered in Example 33, Fig.37 (a) is the electrode before the processing step. Fig.37 (b) is an electrode after the processing step and before the peeling step, Fig.37 (c) is the electrode after the peeling step.

[0083] Fig.38 is a photograph showing the appearance of the active material recovered in Example 34, Fig.38 (a) is the electrode before the processing step. Fig.38 (b) is an electrode after the processing step and before the peeling step, Fig.38 (c) is the electrode after the peeling step.

[0084] Fig.39 is a photograph showing the appearance of the active material recovered in Example 35, Fig.39 (a) is the electrode before the processing step. Fig.39 (b) is an electrode after the processing step and before the peeling step, Fig.39 (c) is the electrode after the peeling step.

[0085] Fig.40 is a photograph showing the appearance of the active material recovered in Example 36, Fig.40 (a) is the electrode before the processing step. Fig.40 (b) is an electrode after the processing step and before the peeling step, Fig.40 (c) is the electrode after the peeling step.

[0086] Fig.41 is a photograph showing the appearance of the active material recovered in Example 37, Fig.41 (a) is the electrode before the processing step. Fig.41 (b) is an electrode after the processing step and before the peeling step, Fig.41 (c) is the electrode after the peeling step.

[0087] Fig.42 is a photograph showing the appearance of the active material recovered in Example 38, Fig.42 (a) is the electrode before the processing step. Fig.42 (b) is an electrode after the processing step and before the peeling step, Fig.42 (c) is the electrode after the peeling step.

[0088] Fig.43 is a photograph showing the appearance of the active material recovered in Example 39, Fig.43 (a) is the electrode before the processing step. Fig.43 (b) is an electrode after the processing step and before the peeling step, Fig.43 (c) is the electrode after the peeling step.

[0089] Fig.44 is a photograph showing the appearance of the active material recovered in Example 40, Fig.44 (a) is the electrode before the processing step. Fig.44 (b) is an electrode after the processing step and before the peeling step, Fig.44 (c) is the electrode after the peeling step.

[0090] Fig.45 is a photograph showing the appearance of the active material recovered in Example 41, Fig.45 (a) is the electrode before the processing step. Fig.45 (b) is an electrode after the processing step and before the peeling step, Fig.45 (c) is the electrode after the peeling step.

[0091] Fig.46 is a photograph showing the appearance of the active material recovered in Example 42, Fig.46 (a) is the electrode before the processing step. Fig.46 (b) is an electrode after the processing step and before the peeling step, Fig.46 (c) is the electrode after the peeling step.

[0092] Fig.47 is a photograph showing the appearance of the active material recovered in Example 43, Fig.47 (a) is the electrode before the processing step. Fig.47 (b) is an electrode after the processing step and before the peeling step, Fig.47 (c) is the electrode after the peeling step.

[0093] Fig.48 is a photograph showing the appearance of the active material recovered in Example 44, Fig.48 (a) is the electrode before the processing step. Fig.48 (b) is an electrode after the processing step and before the peeling step, Fig.48 (c) is the electrode after the peeling step.

[0094] Fig.49 is a photograph showing the appearance of the active material recovered in Example 45, Fig.49 (a) is the electrode before the processing step. Fig.49 (b) is an electrode after the processing step and before the peeling step, Fig.49 (c) is the electrode after the peeling step.

[0095] Fig.50 is a photograph showing the appearance of the active material recovered in Example 46, Fig.50 (a) is the electrode before the processing step. Fig.50 (b) is an electrode after the processing step and before the peeling step, Fig.50 (c) is the electrode after the peeling step.

[0096] Fig.51 is a photograph showing the appearance of the active material recovered in Example 47, Fig.51 (a) is the electrode before the processing step. Fig.51 (b) is an electrode after the processing step and before the peeling step, Fig.51 (c) is the electrode after the peeling step.

[0097] Fig.52 is a photograph showing the appearance of the active material recovered in Example 48, Fig.52 (a) is the electrode before the processing step. Fig.52 (b) is an electrode after the processing step and before the peeling step, Fig.52 (c) is the electrode after the peeling step.

[0098] Fig.53 is a photograph showing the appearance of the active material recovered in Example 49, Fig.53 (a) is the electrode before the processing step. Fig.53 (b) is an electrode after the processing step and before the peeling step, Fig.53 (c) is the electrode after the peeling step.

[0099] Fig.54 is a photograph showing the appearance of the active material recovered in Example 50, Fig.54 (a) is the electrode before the processing step. Fig.54(b) is an electrode after the processing step and before the peeling step, Fig.54 (c) is the electrode after the peeling step.

[0100] Fig.55 is a photograph showing the appearance of the active material recovered in Example 51, Fig.55 (a) is the electrode before the processing step. Fig.55 (b) is an electrode after the processing step and before the peeling step, Fig.55 (c) is the electrode after the peeling step.

[0101] Fig.56 is a photograph showing the appearance of the active material recovered in Example 52, Fig.56 (a) is the electrode before the processing step. Fig.56 (b) is an electrode after the processing step and before the peeling step, Fig.56 (c) is the electrode after the peeling step.

[0102] Fig.57 is a photograph showing the appearance of the active material recovered in Example 53, Fig.57 (a) is the electrode before the processing step. Fig.57 (b) is an electrode after the processing step and before the peeling step, Fig.57 (c) is the electrode after the peeling step.

[0103] Fig.58 is a photograph showing the appearance of the active material recovered in Example 54, Fig.58 (a) is the electrode before the processing step. Fig.58 (b) is an electrode after the processing step and before the peeling step, Fig.58 (c) is the electrode after the peeling step.

[0104] Fig.59 is a photograph showing the appearance of the active material recovered in Example 55, Fig.59 (a) is the electrode before the processing step. Fig.59 (b) is an electrode after the processing step and before the peeling step, Fig.59 (c) is the electrode after the peeling step.

[0105] Fig.60 is a photograph showing the appearance of the active material recovered in Example 56, Fig.60 (a) is the electrode before the processing step. Fig.60 (b) is an electrode after the processing step and before the peeling step, Fig.60(c) is the electrode after the peeling step.

[0106] Fig.61 is a photograph showing the appearance of the active material recovered in Example 57, Fig.61 (a) is the electrode before the processing step. Fig.61 (b) is an electrode after the processing step and before the peeling step, Fig.61 (c) is the electrode after the peeling step.

[0107] Fig.62 is a photograph showing the appearance of the active material recovered in Example 58, Fig.62 (a) is the electrode before the processing step. Fig.62 (b) is an electrode after the processing step and before the peeling step, Fig.62 (c) is the electrode after the peeling step.

[0108] Fig.63 is a photograph showing the appearance of the active material recovered in Example 59, Fig.63 (a) is the electrode before the processing step. Fig.63 (b) is an electrode after the processing step and before the peeling step, Fig.63 (c) is the electrode after the peeling step.

[0109] Fig.64 is a photograph showing the appearance of the active material recovered in Example 60, Fig.64 (a) is the electrode before the processing step. Fig.64 (b) is an electrode after the processing step and before the peeling step, Fig.64 (c) is the electrode after the peeling step.

[0110] Fig.65 is a photograph showing the appearance of the active material recovered in Example 61, Fig.65 (a) is the electrode before the processing step. Fig.65 (b) is an electrode after the processing step and before the peeling step, Fig.65 (c) is the electrode after the peeling step.

[0111] Fig.66 is a photograph showing the appearance of the active material recovered in Example 62, Fig.66 (a) is the electrode before the processing step. Fig.66 (b) is an electrode after the processing step and before the peeling step, Fig.66 (c) is the electrode after the peeling step.

[0112] Fig.67 is a photograph showing the appearance of the active material recovered in Example 63, Fig.67 (a) is the electrode before the processing step. Fig.67 (b) is an electrode after the processing step and before the peeling step, Fig.67 (c) is the electrode after the peeling step.

[0113] Fig.68 is a photograph showing the appearance of the active material recovered in Example 64, Fig.68 (a) is the electrode before the processing step. Fig.68 (b) is an electrode after the processing step and before the peeling step, Fig.68 (c) is the electrode after the peeling step.

[0114] Fig.69 is a photograph showing the appearance of the active material recovered in Example 65, Fig.69 (a) is the electrode before the processing step. Fig.69 (b) is an electrode after the processing step and before the peeling step, Fig.69 (c) is the electrode after the peeling step.

[0115] Fig.70 is a photograph showing the appearance of the active material recovered in Example 66, Fig.70 (a) is the electrode before the processing step. Fig.70 (b) is an electrode after the processing step and before the peeling step, Fig.70 (c) is the electrode after the peeling step.

[0116] Fig.71 is a photograph showing the appearance of the active material recovered in Example 67, Fig.71 (a) is the electrode before the processing step. Fig.71 (b) is an electrode after the processing step and before the peeling step, Fig.71 (c) is the electrode after the peeling step.

[0117] Fig.72 is a photograph showing the appearance of the active material recovered in Example 68, Fig.72 (a) is the electrode before the processing step. Fig.72 (b) is an electrode after the processing step and before the peeling step, Fig.72 (c) is the electrode after the peeling step.

[0118] Fig.73 is a photograph showing the appearance of the active material recovered in Example 69, Fig.73 (a) is the electrode before the processing step. Fig.73 (b) is an electrode after the processing step and before the peeling step, Fig.73 (c) is the electrode after the peeling step.

[0119] Fig.74 is a photograph showing the appearance of the active material recovered in Example 70, Fig.74 (a) is the electrode before the processing step. Fig.74 (b) is an electrode after the processing step and before the peeling step, Fig.74 (c) is the electrode after the peeling step.

[0120] Fig.75 is a photograph showing the appearance of the active material recovered in Example 71, Fig.75 (a) is the electrode before the processing step. Fig.75 (b) is an electrode after the processing step and before the peeling step, Fig.75 (c) is the electrode after the peeling step.

[0121] Fig.76 is a photograph showing the appearance of the active material recovered in Example 72, Fig.76 (a) is the electrode before the processing step. Fig.76 (b) is an electrode after the processing step and before the peeling step, Fig.76 (c) is the electrode after the peeling step.

[0122] Fig.77 is a photograph showing the appearance of the active material recovered in Comparative Example 1. Fig.77 (a) is the electrode that has not been processed. Fig.77 (b) is an electrode that has not been subjected to a processing step but has been subjected to a peeling step.

[0123] Fig.78 is a photograph showing the appearance of the active material recovered in Comparative Example 2. Fig.78 (a) is the electrode that has not been processed. Fig.78 (b) is an electrode that has not been subjected to a processing step but has been subjected to a peeling step.

[0124] Fig.79 is a photograph showing the appearance of the active material recovered in Comparative Example 3. Fig.79 (a) is the electrode that has not been processed. Fig.79 (b) is an electrode that has not been subjected to a processing step but has been subjected to a peeling step.

[0125] Fig.80is a photograph showing the appearance of the active material recovered in Comparative Example 4. Fig.80 (a) is the electrode that has not been processed. Fig.80 (b) is an electrode that has not been subjected to a processing step but has been subjected to a peeling step.

[0126] Fig.81 is a photograph showing the appearance of the active material recovered in Comparative Example 5. Fig.81 (a) is the electrode that has not been processed. Fig.81 (b) is an electrode that has not been subjected to a processing step but has been subjected to a peeling step.

[0127] Fig.82 is a photograph showing the appearance of the active material recovered in Comparative Example 6, Fig.82 (a) is the electrode that has not been processed. Fig.82 (b) is an electrode that has not been subjected to a processing step but has been subjected to a peeling step. DETAILED DESCRIPTION

[0128] (Method for recovering active material in power storage device)

[0129] The method for recovering active material in a power storage device of the present invention includes a processing step, preferably a peeling step and a drying step, and may further include other steps as necessary.

[0130] Furthermore, the valuable material recovery method of the present invention is based on the following knowledge of the present inventors: In the prior art, in the gas flow treatment of electrodes, the electrodes are deformed every time they collide, and the active material cannot be recovered efficiently.

[0131] Therefore, the inventors have found that by applying external stimulation to an electrode processed into a shape that does not deform (e.g., a wavy shape), the active material attached to the center of the electrode can be peeled off because the electrode does not deform (does not curl), and the recovery rate of the active material becomes higher. In addition, since the miniaturization of the electrode can be suppressed, the mixing of impurities into the recovered active material can be reduced (high-purity active material can be recovered).

[0132] The method for recovering active material from an electricity storage device of the present invention is a method for recovering active material from an electricity storage device, and comprises a processing step, preferably a peeling step, and further comprises other steps as necessary.

[0133] The method for recovering active materials from an electric storage device of the present invention has the following advantages: since it is a non-baking process for discharging and decomposing the electric storage device to be recovered, fuel and electricity for baking are not required, and carbon dioxide generated by thermal decomposition of organic electrolytes, plastics, etc. is not generated, so the impact on the environment is small. In addition, compared with a melting process for melting the electric storage device to be recovered and a baking process for baking and pulverizing, the present invention can suppress the oxidation or thermal degradation of the raw materials constituting the electric storage battery, and thus has the advantages of a wide variety of recycled raw materials and excellent quality and purity.

[0134] In the conventional non-calcining recovery method, the recovery rate of the active material is reduced because the electrode collides with the wall of the container and deforms during the stripping process of stripping the active material from the electrode of the power storage device contained in the container by airflow. In addition, aluminum and copper as the current collector peeled off by the collision are mixed into the recovered active material, resulting in a reduction in the purity of the active material.

[0135] The present invention includes a processing step of processing the electrode of the power storage device into a wavy shape before the stripping step, so that in the subsequent stripping step, even if an external stimulus is applied to the electrode, the electrode is difficult to deform, thereby achieving a high recovery rate and high purity of the active material.

[0136] <Processing steps>

[0137] The processing step is a step of processing at least a portion of the electrode in the power storage device including the electrode with the active material attached thereto into a wavy shape. By performing the processing step, even if an external stimulus is applied to the electrode in the stripping step described later, the impulse applied to the electrode will not be locally concentrated but will be dispersed as a whole, so that the electrode will not be deformed, and the active material can be efficiently stripped from the electrode. In addition, since the end of the electrode is difficult to be scraped, the mixing of the fragments of the electrode can be suppressed, and the high-purity active material can be recovered.

[0138] Furthermore, the above-mentioned processing steps may be performed a plurality of times.

[0139] By performing the above processing steps, even in a power storage device in which the metal foil and the positive electrode material are in close contact with each other, the metal foil and the positive electrode material can be easily separated, and the active material can be efficiently separated from the electrode and recovered.

[0140] As at least a part of the above-mentioned electrode, there is no particular limitation, and it can be appropriately selected according to the purpose, for example, the whole of the above-mentioned electrode, only the end of the above-mentioned electrode, etc. can be cited. Among these, from the viewpoint of being able to suppress the deformation of the above-mentioned electrode in the stripping process, the whole of the above-mentioned electrode is particularly preferred. As the whole of the above-mentioned electrode, for example, only one direction, one direction and a direction different from the above-mentioned one direction, etc. can be cited. Among these, one direction of the whole and a direction different from the above-mentioned one direction are particularly preferred.

[0141] When one direction of the electrode as a whole and a direction different from the above-mentioned direction are wavy in shape, the angle of the above-mentioned direction different from the above-mentioned direction is not particularly limited and can be appropriately selected according to the purpose, but is preferably greater than 30 degrees, and more preferably 90 degrees (orthogonal direction).

[0142] When the above processing steps are performed multiple times, the processing can be performed at an angle of 45 degrees with respect to one direction in the first processing step in the second and subsequent processing steps, and can be performed at an angle of 135 degrees in the third and subsequent processing steps.

[0143] As the radius of curvature of the above-mentioned wavy shape, there is no particular limitation, and it can be appropriately selected according to the purpose, but it is preferably more than 0mm and less than 5mm, more preferably more than 0.1mm and less than 2mm, and particularly preferably more than 0.1mm and less than 0.5mm. When the above-mentioned radius of curvature is more than 0.1mm, it is possible to prevent the bending and breaking of the electrode, and when the above-mentioned radius of curvature is less than 2mm, it is possible to suppress the deformation of the electrode caused by external stimulation, and it is possible to prevent the miniaturization of the electrode. In addition, when the above-mentioned radius of curvature is less than 1mm, by locally producing the peeling of the electrode and the active material constituting the electrode, the peeling efficiency can be improved, and the time of applying external stimulation can be shortened, so high energy efficiency can be obtained.

[0144] The smaller the radius of curvature is, the more the surface of the electrode and the active material (microparticle layer) are slightly peeled off by the processing of the wavy shape, so the peeling recovery efficiency of the active material is higher. In addition, the smaller the radius of curvature is, the higher the purity of the recovered active material is.

[0145] In particular, when the radius of curvature is 0.1 mm or more and 0.5 mm or less, the active material can be efficiently peeled off from the electrode even without performing the peeling step.

[0146] Furthermore, when the processing steps are performed a plurality of times, the radius of curvature may not be changed or may be changed, thereby further peeling off the active material.

[0147] The radius of curvature of the wavy shape can be measured, for example, by a non-contact measurement method, a stylus measurement method, etc. As equipment used for the non-contact measurement method, for example, NH-3Ps (Mitaka Optical Instruments Co., Ltd.) can be cited. In addition, as methods other than the above, a method of taking a close-up shot of the cross-sectional view of the electrode and approximately calculating the curvature based on the image of the recorded cross-sectional shape can be cited.

[0148] The processing method in the processing step is not particularly limited as long as the electrode can be processed into a wavy shape, and can be appropriately selected according to the purpose, for example, a method of processing using a dedicated tool, a method of clamping and pressing the electrode with a wavy plate, etc. Among these, from the viewpoint of being able to process a part of the electrode and the viewpoint of easy operation, a method of processing using an equipment that processes a flat substrate into a wavy shape is particularly preferred.

[0149] The dedicated tool is not particularly limited and can be appropriately selected according to the purpose. For example, a gear-shaped tool (eg, GSWD18, GREEN STUFF WORLD corrugated plate linear maker micro tool) or a rack-shaped tool can be used.

[0150] As the dedicated tool, a commercial product or a tool produced by a 3D printer may be used. The 3D printer is not particularly limited and can be appropriately selected according to the purpose. For example, Photon Mono SE (manufactured by ANYCUBIC) or the like can be used.

[0151] <<Active substances>>

[0152] The active material is a material that can be traded instead of being discarded, and examples thereof include carbon (C), cobalt, nickel, manganese, lithium, titanium, iron, phosphorus, sulfur, and fluorine.

[0153] - Power storage device -

[0154] The power storage device is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include lithium ion secondary batteries, lithium ion capacitors, all-solid batteries, and all-resin batteries.

[0155] The above-mentioned power storage device is, for example, a secondary battery that is charged and discharged by the movement of lithium ions between the positive electrode and the negative electrode, and for example, a power storage device having a positive electrode, a negative electrode, a separator, an electrolyte containing an electrolyte and an organic solvent, and a battery case, i.e., an outer container (one side is made of aluminum or iron) for accommodating the positive electrode, the negative electrode, the separator, and the electrolyte. In addition, the lithium ion secondary battery that is the object of the present invention may also be in a state where the positive electrode, the negative electrode, etc. are detached.

[0156] The electricity storage device may be a stacked type in which the positive electrode, the negative electrode, and the separator are stacked, or a wound type in which the stacked type electricity storage device is wound.

[0157] Furthermore, the positive electrode, the negative electrode, and the separator may be alternately stacked.

[0158] The shape, structure, size, etc. of the power storage device to be used for active material recovery in the present invention are not particularly limited. Examples of the shape of the power storage device include stacked, cylindrical, button, coin, square, and flat.

[0159] In addition, there is no particular limitation on the form of the power storage device, and it can be appropriately selected according to the purpose, and examples thereof include a battery unit, a battery module, a battery pack, etc. Here, a battery module refers to a structure in which a plurality of battery units as unit batteries are connected and concentrated in one frame, and a battery pack refers to a structure in which a plurality of battery modules are concentrated in one frame. In addition, the battery pack may also include a control controller and a cooling device.

[0160] --positive electrode--

[0161] The positive electrode has a structure including a positive electrode material and an active material layer on a positive electrode current collector, and its shape may be, for example, a flat plate.

[0162] The thickness of the positive electrode current collector is not particularly limited and can be appropriately selected depending on the intended purpose. For example, the thickness may be 50 μm or more and 100 μm or less.

[0163] The thickness of the active material layer is not particularly limited and can be appropriately selected depending on the intended purpose. For example, the thickness may be 100 μm or more and 150 μm or less.

[0164] Furthermore, the method for recovering active materials from an electricity storage device of the present invention can efficiently recover active materials even in a battery having a thickness other than the thickness of the positive electrode current collector and the thickness of the active material layer.

[0165] As the positive electrode current collector, there is no particular restriction on its shape, structure, size, etc. As the structure of the positive electrode current collector, for example, a multilayer structure (laminate) can be mentioned. As the shape of the positive electrode current collector, for example, a foil can be mentioned. As the material of the positive electrode current collector, for example, stainless steel, nickel, aluminum, copper, titanium, tantalum, etc. can be mentioned. Among these, aluminum is particularly preferred. From the viewpoints of non-doped lithium ions, cost and conductivity, aluminum is widely used. In addition, in order to impart desired characteristics, aluminum alloys to which other metals (silicon, manganese, etc.) are added are also used. The lithium ion secondary battery that becomes the object of recovery of valuables in the present invention contains aluminum as a positive electrode collector as described above.

[0166] The positive electrode material, for example, at least includes a positive electrode active material containing a rare valuable object, and includes a conductive agent and a binding resin as required. There is no particular limitation on the rare valuable object, but as the recycling object of the valuable object recycling method of the present invention, it is preferably at least one of cobalt and nickel because it is expensive.

[0167] Examples of the positive electrode active material include lithium manganese oxide (LiMn2O4) known as an LMO system, lithium cobalt oxide (LiCoO2) known as an LCO system, and LiNi3O4 known as a ternary system or NCM system. x Co y Mn z O2 (x+y+z=1), LiNi called NCA system x Co y Al z (x+y+z=1), lithium iron phosphate (LiFePO4), lithium cobalt nickel oxide (LiCo 1 / 2 Ni 1 / 2 O2), lithium titanate (Li2TiO3), etc. In addition, these materials may be used in combination as the positive electrode active material.

[0168] Examples of the conductive agent include carbon black, graphite, carbon fiber, and metal carbide.

[0169] Examples of the binder resin include homopolymers or copolymers such as vinylidene fluoride, tetrafluoroethylene, acrylonitrile, and ethylene oxide, and styrene-butadiene rubber.

[0170] --negative electrode--

[0171] The negative electrode has a structure including a negative electrode material and an active material layer on a negative electrode current collector. Examples of the shape of the negative electrode include a flat plate shape.

[0172] The thickness of the negative electrode current collector is not particularly limited and can be appropriately selected depending on the intended purpose. For example, the thickness may be 50 μm or more and 100 μm or less.

[0173] The thickness of the active material layer is not particularly limited and can be appropriately selected depending on the intended purpose. For example, the thickness may be 100 μm or more and 150 μm or less.

[0174] Furthermore, the method for recovering active materials from an electricity storage device of the present invention can efficiently recover active materials even in a battery having a thickness other than the above-mentioned thickness of the negative electrode current collector and the above-mentioned thickness of the active material layer.

[0175] As the negative electrode collector, there are no particular restrictions on its structure, size, etc. As the material of the negative electrode collector, copper is widely used from the viewpoints of non-doping with lithium ions, cost and conductivity. In addition, in order to impart the desired characteristics, copper alloys in which other metals are added to copper are also used. In addition, foil is widely used in the shape of the negative electrode collector. The lithium ion secondary battery that becomes the recycling object of valuables in the present invention includes copper foil as a negative electrode collector, for example. In addition, in the case where the copper foil is composed of a copper alloy, the copper alloy is obtained as a light product through the subsequent wet screening process, but sometimes it is necessary to further separate the alloy into copper and other metal components. Therefore, a lithium ion secondary battery containing a copper foil composed of copper as a negative electrode collector is suitable as a recycling object of valuables in the present invention. Here, the "copper foil" used in this specification also includes a foil of a copper alloy (Cu≥70%). The thickness of the foil is preferably 1μm to 100μm.

[0176] The negative electrode material, for example, at least includes a negative electrode active material, and includes a conductive agent and a binding resin as required. As the above-mentioned negative electrode active material, from the viewpoints of capacity, cost, etc., carbon materials such as graphite and hard carbon, titanates, silicon, and respective composites are widely used. Among these, the lithium ion secondary battery as the recycling object of the present invention is particularly preferably composed of carbon as a negative electrode active material.

[0177] In addition, the positive electrode current collector and the negative electrode current collector generally have a laminated structure.

[0178] --Electrolytes--

[0179] The electrolyte is not particularly limited and can be appropriately selected depending on the intended purpose. Examples of the electrolyte include nonaqueous electrolyte solutions and solid electrolytes.

[0180] ---Non-aqueous electrolyte---

[0181] Examples of the non-aqueous electrolyte include a non-aqueous electrolyte containing a lithium salt and an organic solvent.

[0182] The lithium salt is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(pentafluoroethanesulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, etc. These can be used alone or in combination of two or more.

[0183] The organic solvent is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include ethylene carbonate, dimethyl carbonate, propylene carbonate, diethyl carbonate, ethyl methyl carbonate, etc. These may be used alone or in combination of two or more.

[0184] Among these, a mixed solvent of ethylene carbonate and dimethyl carbonate is particularly preferred because the solubility of the lithium salt is high.

[0185] ---Solid electrolyte---

[0186] The solid electrolyte is not particularly limited as long as it is a solid electrolyte having conductivity for lithium ions as carriers for battery reactions, and can be appropriately selected depending on the purpose. Examples thereof include oxide-based solid electrolytes and sulfide-based solid electrolytes.

[0187] Examples of the oxide-based solid electrolyte include perovskite-type oxides, NASICON-type oxides, LISICON-type oxides, and garnet-type oxides.

[0188] Examples of the sulfide-based solid electrolyte include Li2S-P2S5, Li2S-SiS2, Li7P3S 11 , Li2S-SiS2-Li3PO4, etc.

[0189] The material of the outer container (frame) of the lithium ion secondary battery is not particularly limited, and examples thereof include aluminum, iron, stainless steel, and resin (plastic).

[0190] <Peeling process>

[0191] The peeling step may include applying an external stimulus to the electrode to peel the active material from the electrode. The peeling step may be performed after the processing step.

[0192] <<External Stimuli>>

[0193] The external stimulus is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include air flow, water flow, shock waves, etc. Among these, air flow is particularly preferred because water is not used in the peeling step.

[0194] As the wind speed of the above-mentioned airflow, there is no particular restriction, and it can be appropriately selected according to the purpose, but it is preferably more than 5m / s and less than 100m / s. When the above-mentioned wind speed is more than 5m / s, the above-mentioned active material can be efficiently stripped, and when the above-mentioned wind speed is less than 100m / s, the scraping of the end of the above-mentioned electrode can be prevented, the mixing of the fragments of the above-mentioned electrode can be suppressed, and the high-purity active material can be recovered. In addition, the so-called above-mentioned wind speed refers to the average wind speed.

[0195] The time of the stripping process using the airflow is not particularly limited and can be appropriately selected according to the purpose, but is preferably 0.5 minutes or more and 2.0 minutes or less. When the time is 0.5 minutes or more, the active material can be efficiently stripped, and when it is 2.0 minutes or less, the end of the electrode can be prevented from being scraped, the mixing of the fragments of the electrode can be suppressed, and the high-purity active material can be recovered.

[0196] Figure 2 This is a schematic diagram showing an example of a method of recovering active materials from a power storage device according to the present invention when airflow is used as an external stimulus.

[0197] In the method for recovering active materials from an electrical storage device of the present invention using airflow, an electrode 4 is placed in a container 2 having a mesh 3 on the upper portion, and an airflow as an external stimulus is applied to the electrode 4. The airflow is generated in the direction of the arrow from an airflow nozzle 1. By scanning the airflow nozzle 1, the direction of the airflow 5 can be changed.

[0198] The direction of the airflow 5 is not particularly limited as long as it can apply external stimulation to the electrode 4, and can be appropriately selected according to the purpose.

[0199] The flow rate of the water flow is not particularly limited and can be appropriately selected according to the purpose, but is preferably 0.05 m / s or more and 10 m / s or less, more preferably 1 m / s or more and 5 m / s or less. When the wind speed is 5 cm / s or more, the active material can be efficiently stripped, and when the wind speed is 100 cm / s or less, the end of the electrode can be prevented from being scraped, the mixing of the fragments of the electrode can be suppressed, and the high-purity active material can be recovered. In addition, the so-called flow rate refers to the average flow rate.

[0200] The time of the stripping process using the water flow is not particularly limited and can be appropriately selected according to the purpose, but is preferably 0.1 minutes or more and 5.0 minutes or less. When the time is 0.1 minutes or more, the active material can be efficiently stripped, and when it is 5.0 minutes or less, the end of the electrode can be prevented from being scraped, the mixing of the fragments of the electrode can be suppressed, and the high-purity active material can be recovered.

[0201] Figure 3 This is a schematic diagram showing an example of the method of recovering active materials from a power storage device according to the present invention when water flow is used as an external stimulus.

[0202] In the method for recovering active materials from an electrical storage device of the present invention using a water flow, an electrode 4 is placed in water 7 in a container 2, and a water flow as an external stimulus is applied to the electrode 4. The water flow is generated by a stirrer 6 having a stirring portion placed in the water 4. The water flow 7 can be generated by rotating the stirring portion of the stirrer 6.

[0203] The direction of the water flow 7 is not particularly limited as long as it can apply external stimulation to the electrode 4, and can be appropriately selected according to the purpose.

[0204] The voltage for applying the shock wave is not particularly limited and can be appropriately selected depending on the intended purpose, but is preferably 10 kV or more and 200 kV or less.

[0205] The distance from the counter electrode of the electric pulse device when applying the shock wave is not particularly limited and can be appropriately selected depending on the purpose, but is preferably, for example, 0.5 cm to 30 cm.

[0206] The number of pulses when applying the shock wave is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 or more and 100 or less, for example.

[0207] Figure 4 This is a schematic diagram showing an example of a method of recovering active material from a power storage device according to the present invention when a shock wave is used as an external stimulus.

[0208] In the method for recovering active materials from an electrical storage device of the present invention using shock waves, an electrode 4 is placed in water 7 in a container 2, and a shock wave as an external stimulus is applied to the electrode 4. The shock wave 12 is generated from the insulation breakdown generating counter electrode 10 of a high voltage electric pulse generating device 9 connected to a power supply device 11 by placing the counter electrode 10 for insulation breakdown generating into the water 4.

[0209] The temperature of the peeling step is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0° C. to 200° C. In a dry state of the electrode, the active material is easily peeled off.

[0210] <Drying process>

[0211] The drying step is a step of applying heat to the electrode to dry the electrode. The drying step is preferably performed before the peeling step.

[0212] By performing the drying step, scattering of the organic solvent contained in the power storage device can be reduced, and the active material can be further separated from the electrode.

[0213] The drying conditions in the drying step are not particularly limited and can be appropriately selected depending on the intended purpose. Examples of the drying conditions include drying at 50° C. or higher for 15 minutes or longer.

[0214] <Other Process>

[0215] The other steps are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other steps include an electric discharge step and a cutting step.

[0216] The discharge step is not particularly limited and can be appropriately selected according to the purpose. For example, by discharging at a fixed resistance of 2Ω for 6 hours or more, the voltage of 0.1 V or less can be maintained for 2 hours or more to complete the discharge.

[0217] In the power storage device for material recycling, there is often residual electric energy. The more electric energy that remains, the more likely it is that the battery will heat up or ignite during operation. Therefore, by performing the discharge process, the risk of heating up or ignition of the battery during operation can be reduced. For example, in the case of a single battery cell of a 3.7V power storage device, it can be safely disassembled when it is 0.3V or less, and it can be disassembled more safely when it is 0.1V or less.

[0218] In a battery pack composed of a plurality of battery cells, the discharge state of each battery cell may be non-uniform. Therefore, it is preferable to measure the voltage of each battery cell constituting the battery pack or to discharge the battery cell to a voltage having a set safety factor.

[0219] [Example]

[0220] Hereinafter, examples of the present invention will be described, but the present invention is not limited to these examples.

[0221] (Example 1)

[0222] <Discharge process>

[0223] The vehicle-mounted lithium-ion battery A (Prius PHV, 21.5Ah: 3 hour rate, thickness of the positive electrode collector: 100μm, thickness of the positive electrode active material layer: 100μm, thickness of the negative electrode collector: 100μm, thickness of the negative electrode active material layer: 100μm) used as a power storage device was discharged at a fixed resistance of 2Ω for 6 hours, and the voltage below 0.1V was maintained for more than 2 hours.

[0224] <Cutting process>

[0225] The inner shell of the lithium ion battery A was removed using an upper circular saw (K-210, Hozan), and then the current collecting portion of the inner shell was cut using a cutter to obtain an electrode of 4 cm×4 cm.

[0226] <Processing steps>

[0227] The positive electrode (4 cm×4 cm) of the obtained electrode was processed using a processing jig so that the entire electrode had a wavy shape with a curvature radius of 2 mm. Then, the active material in the container after the processing step was recovered. Figure 5 A photograph showing the appearance of the recovered active material is shown in FIG. Figure 5 (a) is the electrode before the processing step. Figure 5 (b) is the electrode after the processing step.

[0228] (Example 2-A)

[0229] The active material was recovered in the same manner as in Example 1 except that the processing was changed to one direction and an orthogonal direction. Fig. 6A A photograph showing the appearance of the recovered active material is shown in FIG. Fig. 6A (a) is the electrode before the processing step. Fig. 6A (b) is the electrode after the processing step.

[0230] (Example 2-B)

[0231] The active material was recovered in the same manner as in Example 1 except that the processing was changed to one direction and a direction at 45 degrees relative to the one direction. Figure 6B A photograph showing the appearance of the recovered active material is shown in FIG. Figure 6B (a) is the electrode before the processing step. Figure 6B (b) is an electrode after a processing step along one direction mentioned above, Figure 6B (c) is an electrode that has been further processed in the above-mentioned 45-degree direction.

[0232] (Example 2-C)

[0233] The active material was recovered in the same manner as in Example 1 except that the processing was changed to one direction, a direction at 45 degrees relative to the one direction, and a direction at 135 degrees corresponding to the one direction. Figure 6C A photograph showing the appearance of the recovered active material is shown in FIG. Figure 6C (a) is the electrode before the processing step. Figure 6C (b) is an electrode after a processing step along one direction mentioned above, Figure 6C (c) is an electrode that has been further processed in the above 45-degree direction. Figure 6C (d) is an electrode that has been further processed in the above-mentioned 135-degree direction.

[0234] (Example 3)

[0235] The active material was recovered in the same manner as in Example 1 except that the curvature radius of the processed shape was changed to 1 mm. Figure 7 A photograph showing the appearance of the recovered active material is shown in FIG. Figure 7 (a) is the electrode before the processing step. Figure 7 (b) is the electrode after the processing step.

[0236] (Example 4-A)

[0237] The active material was recovered in the same manner as in Example 3 except that the processing was changed to one direction and an orthogonal direction. Fig. 8A A photograph showing the appearance of the recovered active material is shown in FIG. Fig. 8A (a) is the electrode before the processing step. Fig. 8A (b) is the electrode after the processing step.

[0238] (Example 4-B)

[0239] The active material was recovered in the same manner as in Example 3 except that the processing was changed to one direction and a direction at 45 degrees relative to the one direction. Figure 8B A photograph showing the appearance of the recovered active material is shown in FIG. Figure 8B (a) is the electrode before the processing step. Figure 8B (b) is an electrode after a processing step along one direction mentioned above, Figure 8B (c) is an electrode that has been further processed in the above-mentioned 45-degree direction.

[0240] (Example 4-C)

[0241] The active material was recovered in the same manner as in Example 3 except that the processing was changed to one direction, a direction at 45 degrees relative to the one direction, and a direction at 135 degrees relative to the one direction. Figure 8C A photograph showing the appearance of the recovered active material is shown in FIG. Figure 8C (a) is the electrode before the processing step. Figure 8C (b) is an electrode after a processing step along one direction mentioned above, Figure 8C (c) is an electrode that has been further processed in the above 45-degree direction. Figure 8C (d) is an electrode that has been further processed in the above-mentioned 135-degree direction.

[0242] (Example 5)

[0243] The active material was recovered in the same manner as in Example 1 except that the curvature radius of the processed shape was changed to 0.5 mm. Fig. 9 A photograph showing the appearance of the recovered active material is shown in FIG. Fig. 9 (a) is the electrode before the processing step. Fig. 9 (b) is the electrode after the processing step.

[0244] (Example 6-A)

[0245] The active material was recovered in the same manner as in Example 5 except that the processing was changed to one direction and an orthogonal direction. Fig. 10A A photograph showing the appearance of the recovered active material is shown in FIG. Fig. 10A (a) is the electrode before the processing step. Fig. 10A (b) is the electrode after the processing step.

[0246] (Example 6-B)

[0247] The active material was recovered in the same manner as in Example 5, except that the processing was changed to one direction and a direction at 45 degrees relative to the one direction. Fig. 10B A photograph showing the appearance of the recovered active material is shown in FIG. Fig. 10B (a) is the electrode before the processing step. Fig. 10B (b) is an electrode after a processing step along one direction mentioned above, Fig. 10B (c) is an electrode that has been further processed in the above-mentioned 45-degree direction.

[0248] (Example 6-C)

[0249] The active material was recovered in the same manner as in Example 5 except that the processing was changed to one direction, a direction at 45 degrees relative to the one direction, and a direction at 135 degrees relative to the one direction. Fig. 10C A photograph showing the appearance of the recovered active material is shown in FIG. Fig. 10C (a) is the electrode before the processing step. Fig. 10C (b) is an electrode after a processing step along one direction mentioned above, Fig. 10C (c) is an electrode that has been further processed in the above 45-degree direction. Fig. 10C (d) is an electrode that has been further processed in the above-mentioned 135-degree direction.

[0250] (Example 7)

[0251] The active material was recovered in the same manner as in Example 1 except that the object to be processed was changed to the negative electrode. Fig.11 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.11 (a) is the electrode before the processing step. Fig.11 (b) is the electrode after the processing step.

[0252] (Example 8)

[0253] The active material was recovered in the same manner as in Example 2 except that the object to be processed was changed to the negative electrode. Fig.12 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.12 (a) is the electrode before the processing step. Fig.12 (b) is the electrode after the processing step.

[0254] (Example 9)

[0255] The active material was recovered in the same manner as in Example 3 except that the object to be processed was changed to the negative electrode. Fig.13 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.13 (a) is the electrode before the processing step. Fig.13 (b) is the electrode after the processing step.

[0256] (Example 10)

[0257] The active material was recovered in the same manner as in Example 4 except that the object to be processed was changed to the negative electrode. Fig.14 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.14 (a) is the electrode before the processing step. Fig.14 (b) is the electrode after the processing step.

[0258] (Example 11)

[0259] The active material was recovered in the same manner as in Example 5, except that the object to be processed was changed to the negative electrode. Fig.15 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.15 (a) is the electrode before the processing step. Fig.15 (b) is the electrode after the processing step.

[0260] (Example 12)

[0261] The active material was recovered in the same manner as in Example 6 except that the object to be processed was changed to the negative electrode. Fig.16A photograph showing the appearance of the recovered active material is shown in FIG. Fig.16 (a) is the electrode before the processing step. Fig.16 (b) is the electrode after the processing step.

[0262] (Example 13)

[0263] The active material was recovered in the same manner as in Example 1 except that the processing object was changed to a stack of positive and negative electrodes. Fig.17 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.17 (a) is the electrode before the processing step. Fig.17 (b) is the electrode after the processing step.

[0264] (Example 14)

[0265] The active material was recovered in the same manner as in Example 2 except that the object to be processed was changed to a stack of positive and negative electrodes. Fig.18 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.18 (a) is the electrode before the processing step. Fig.18 (b) is the electrode after the processing step.

[0266] (Example 15)

[0267] The active material was recovered in the same manner as in Example 3 except that the object to be processed was changed to a stack of positive and negative electrodes. Fig.19 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.19 (a) is the electrode before the processing step. Fig.19 (b) is the electrode after the processing step.

[0268] (Example 16)

[0269] The active material was recovered in the same manner as in Example 4 except that the object to be processed was changed to a stack of positive and negative electrodes. Fig. 20 A photograph showing the appearance of the recovered active material is shown in FIG. Fig. 20 (a) is the electrode before the processing step. Fig. 20 (b) is the electrode after the processing step.

[0270] (Example 17)

[0271] The active material was recovered in the same manner as in Example 5, except that the processing object was changed to a stack of positive electrodes and negative electrodes. Fig.21A photograph showing the appearance of the recovered active material is shown in FIG. Fig.21 (a) is the electrode before the processing step. Fig.21 (b) is the electrode after the processing step.

[0272] (Example 18)

[0273] The active material was recovered in the same manner as in Example 6 except that the object to be processed was changed to a stack of positive and negative electrodes. Fig. 22 A photograph showing the appearance of the recovered active material is shown in FIG. Fig. 22 (a) is the electrode before the processing step. Fig. 22 (b) is the electrode after the processing step.

[0274] (Example 19)

[0275] The active material was recovered in the same manner as in Example 1, except that the battery was changed to a lithium-ion battery B for vehicle use (RAV4, 51Ah: 3 hour rate, thickness of the positive electrode collector: 50 μm, thickness of the positive electrode active material layer: 150 μm, thickness of the negative electrode collector: 50 μm, thickness of the negative electrode active material layer: 150 μm). Fig.23 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.23 (a) is the electrode before the processing step. Fig.23 (b) is an electrode after the processing step. In addition, the lithium ion battery B is a power storage device in which the metal foil and the positive electrode material are more closely connected than the lithium ion battery A.

[0276] (Example 20-A)

[0277] The active material was recovered in the same manner as in Example 2 except that the battery was changed to a lithium ion battery B for vehicle use. Fig.24A A photograph showing the appearance of the recovered active material is shown in FIG. Fig.24A (a) is the electrode before the processing step. Fig.24A (b) is the electrode after the processing step.

[0278] (Example 20-B)

[0279] The active material was recovered in the same manner as in Example 19 except that the processing was changed to one direction and a direction at 45 degrees relative to the one direction. Fig. 24B A photograph showing the appearance of the recovered active material is shown in FIG. Fig. 24B (a) is the electrode before the processing step. Fig. 24B(b) is an electrode after a processing step along one direction mentioned above, Fig. 24B (c) is an electrode that has been further processed in the above-mentioned 45-degree direction.

[0280] (Example 20-C)

[0281] The active material was recovered in the same manner as in Example 19 except that the processing was changed to one direction, a direction at 45 degrees relative to the one direction, and a direction at 135 degrees relative to the one direction. FIG84 shows a photograph showing the appearance of the recovered active material. Fig.24C (a) is the electrode before the processing step. Fig.24C (b) is an electrode after a processing step along one direction mentioned above, Fig.24C (c) is an electrode that has been further processed in the above 45-degree direction. Fig.24C (d) is an electrode that has been further processed in the above-mentioned 135-degree direction.

[0282] (Example 21)

[0283] The active material was recovered in the same manner as in Example 3 except that the battery was changed to a lithium ion battery B for vehicle use. Fig.25 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.25 (a) is the electrode before the processing step. Fig.25 (b) is the electrode after the processing step.

[0284] (Example 22-A)

[0285] The active material was recovered in the same manner as in Example 4 except that the battery was changed to a lithium ion battery B for vehicle use. Fig.26A A photograph showing the appearance of the recovered active material is shown in FIG. Fig.26A (a) is the electrode before the processing step. Fig.26A (b) is the electrode after the processing step.

[0286] (Example 22-B)

[0287] The active material was recovered in the same manner as in Example 21 except that the processing was changed to one direction and a direction at 45 degrees relative to the one direction. Fig.26B A photograph showing the appearance of the recovered active material is shown in FIG. Fig.26B (a) is the electrode before the processing step. Fig.26B (b) is an electrode after a processing step along one direction mentioned above, Fig.26B(c) is an electrode that has been further processed in the above-mentioned 45-degree direction.

[0288] (Example 22-C)

[0289] The active material was recovered in the same manner as in Example 21 except that the processing was changed to one direction, a direction at 45 degrees relative to the one direction, and a direction at 135 degrees relative to the one direction. Fig.26C A photograph showing the appearance of the recovered active material is shown in FIG. Fig.26C (a) is the electrode before the processing step. Fig.26C (b) is an electrode after a processing step along one direction mentioned above, Fig.26C (c) is an electrode that has been further processed in the above-mentioned 45-degree direction. Fig.26C (d) is an electrode that has been further processed in the above-mentioned 135-degree direction.

[0290] (Example 23)

[0291] The active material was recovered in the same manner as in Example 5 except that the battery was changed to a lithium ion battery B for vehicle use. Fig. 27 A photograph showing the appearance of the recovered active material is shown in FIG. Fig. 27 (a) is the electrode before the processing step. Fig. 27 (b) is the electrode after the processing step.

[0292] (Example 24-A)

[0293] The active material was recovered in the same manner as in Example 6 except that the battery was changed to a lithium ion battery B for vehicle use. Fig.28A A photograph showing the appearance of the recovered active material is shown in FIG. Fig.28A (a) is the electrode before the processing step. Fig.28A (b) is the electrode after the processing step.

[0294] (Example 24-B)

[0295] The active material was recovered in the same manner as in Example 23 except that the processing was changed to one direction and a direction at 45 degrees relative to the one direction. Fig.28B A photograph showing the appearance of the recovered active material is shown in FIG. Fig.28B (a) is the electrode before the processing step. Fig.28B (b) is an electrode after a processing step along one direction mentioned above, Fig.28B(c) is an electrode that has been further processed in the above-mentioned 45-degree direction.

[0296] (Example 24-C)

[0297] The active material was recovered in the same manner as in Example 23 except that the processing was changed to one direction, a direction at 45 degrees relative to the one direction, and a direction at 135 degrees relative to the one direction. Fig.28C A photograph showing the appearance of the recovered active material is shown in FIG. Fig.28C (a) is the electrode before the processing step. Fig.28C (b) is an electrode after a processing step along one direction mentioned above, Fig.28C (c) is an electrode that has been further processed in the above 45-degree direction. Fig.28C (d) is an electrode that has been further processed in the above-mentioned 135-degree direction.

[0298] (Example 25)

[0299] <Peeling process>

[0300] In Example 1, after the processing step, the positive electrode of the processed battery A was placed in a container (material: stainless steel, 18L), and a metal mesh was set on the top of the container. A blower (GBL800E blower BOSCH) was used from the top of the container to send airflow as an external stimulus to make the electrode float and collide in the container. Afterwards, the active material in the container after the stripping step was recovered. Fig.29 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.29 (a) is the electrode before the processing step. Fig.29 (b) is an electrode after the processing step and before the peeling step, Fig.29 (c) is the electrode after the peeling step.

[0301] The setting conditions of the above-mentioned GBL800E blower BOSCH are as follows.

[0302] [Setting conditions]

[0303] Speed: 0~16,000min -1 (Rpm)

[0304] Maximum air volume: 4.5m 3 / min

[0305] Maximum wind pressure: 7.2kPa

[0306] Average wind speed: 43m / s

[0307] Duration: 0.5 minutes

[0308] (Example 26)

[0309] The active material was recovered in the same manner as in Example 25, except that the processing was changed to one direction and an orthogonal direction. Fig.30 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.30 (a) is the electrode before the processing step. Fig.30 (b) is an electrode after the processing step and before the peeling step, Fig.30 (c) is the electrode after the peeling step.

[0310] (Example 27)

[0311] The active material was recovered in the same manner as in Example 25, except that the curvature radius of the processed shape was changed to 1 mm. Fig.31 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.31 (a) is the electrode before the processing step. Fig.31 (b) is an electrode after the processing step and before the peeling step, Fig.31 (c) is the electrode after the peeling step.

[0312] (Example 28)

[0313] The active material was recovered in the same manner as in Example 27 except that the processing was changed to one direction and an orthogonal direction. Fig.32 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.32 (a) is the electrode before the processing step. Fig.32 (b) is an electrode after the processing step and before the peeling step, Fig.32 (c) is the electrode after the peeling step.

[0314] (Example 29)

[0315] The active material was recovered in the same manner as in Example 25, except that the curvature radius of the processed shape was changed to 0.5 mm. Fig.33 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.33 (a) is the electrode before the processing step. Fig.33 (b) is an electrode after the processing step and before the peeling step, Fig.33 (c) is the electrode after the peeling step.

[0316] (Example 30)

[0317] The active material was recovered in the same manner as in Example 29, except that the processing was changed to one direction and an orthogonal direction. Fig.34 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.34 (a) is the electrode before the processing step. Fig.34 (b) is an electrode after the processing step and before the peeling step, Fig.34 (c) is the electrode after the peeling step.

[0318] (Example 31)

[0319] The active material was recovered in the same manner as in Example 25 except that the electrode was changed to a negative electrode. Fig.35 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.35 (a) is the electrode before the processing step. Fig.35 (b) is an electrode after the processing step and before the peeling step, Fig.35 (c) is the electrode after the peeling step.

[0320] (Example 32)

[0321] The active material was recovered in the same manner as in Example 26 except that the electrode was changed to a negative electrode. Fig.36 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.36 (a) is the electrode before the processing step. Fig.36 (b) is an electrode after the processing step and before the peeling step, Fig.36 (c) is the electrode after the peeling step.

[0322] (Example 33)

[0323] The active material was recovered in the same manner as in Example 27 except that the electrode was changed to a negative electrode. Fig.37 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.37 (a) is the electrode before the processing step. Fig.37 (b) is an electrode after the processing step and before the peeling step, Fig.37 (c) is the electrode after the peeling step.

[0324] (Example 34)

[0325] The active material was recovered in the same manner as in Example 28 except that the electrode was changed to a negative electrode. Fig.38 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.38 (a) is the electrode before the processing step. Fig.38 (b) is an electrode after the processing step and before the peeling step, Fig.38 (c) is the electrode after the peeling step.

[0326] (Example 35)

[0327] The active material was recovered in the same manner as in Example 29 except that the electrode was changed to a negative electrode. Fig.39 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.39 (a) is the electrode before the processing step. Fig.39 (b) is an electrode after the processing step and before the peeling step, Fig.39 (c) is the electrode after the peeling step.

[0328] (Example 36)

[0329] The active material was recovered in the same manner as in Example 30 except that the electrode was changed to a negative electrode. Fig.40 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.40 (a) is the electrode before the processing step. Fig.40 (b) is an electrode after the processing step and before the peeling step, Fig.40 (c) is the electrode after the peeling step.

[0330] (Example 37)

[0331] The active material was recovered in the same manner as in Example 25 except that the electrodes were changed to positive electrodes and negative electrodes. Fig.41 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.41 (a) is the electrode before the processing step. Fig.41 (b) is an electrode after the processing step and before the peeling step, Fig.41 (c) is the electrode after the peeling step.

[0332] (Example 38)

[0333] The active material was recovered in the same manner as in Example 26 except that the electrodes were changed to positive electrodes and negative electrodes. Fig.42 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.42 (a) is the electrode before the processing step. Fig.42 (b) is an electrode after the processing step and before the peeling step, Fig.42 (c) is the electrode after the peeling step.

[0334] (Example 39)

[0335] The active material was recovered in the same manner as in Example 27 except that the electrodes were changed to positive electrodes and negative electrodes. Fig.43 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.43 (a) is the electrode before the processing step. Fig.43 (b) is an electrode after the processing step and before the peeling step, Fig.43 (c) is the electrode after the peeling step.

[0336] (Example 40)

[0337] The active material was recovered in the same manner as in Example 28 except that the electrodes were changed to positive electrodes and negative electrodes. Fig.44 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.44 (a) is the electrode before the processing step. Fig.44 (b) is an electrode after the processing step and before the peeling step, Fig.44 (c) is the electrode after the peeling step.

[0338] (Example 41)

[0339] The active material was recovered in the same manner as in Example 29 except that the electrodes were changed to positive electrodes and negative electrodes. Fig.45 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.45 (a) is the electrode before the processing step. Fig.45 (b) is an electrode after the processing step and before the peeling step, Fig.45 (c) is the electrode after the peeling step.

[0340] (Example 42)

[0341] The active material was recovered in the same manner as in Example 30 except that the electrodes were changed to positive electrodes and negative electrodes. Fig.46 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.46 (a) is the electrode before the processing step. Fig.46 (b) is an electrode after the processing step and before the peeling step, Fig.46 (c) is the electrode after the peeling step.

[0342] (Example 43)

[0343] The active material was recovered in the same manner as in Example 25, except that the battery was changed to Battery B. Fig.47 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.47 (a) is the electrode before the processing step. Fig.47 (b) is an electrode after the processing step and before the peeling step, Fig.47 (c) is the electrode after the peeling step.

[0344] (Example 44)

[0345] The active material was recovered in the same manner as in Example 26, except that the battery was changed to Battery B. Fig.48 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.48 (a) is the electrode before the processing step. Fig.48 (b) is an electrode after the processing step and before the peeling step, Fig.48 (c) is the electrode after the peeling step.

[0346] (Example 45)

[0347] The active material was recovered in the same manner as in Example 27 except that the battery was changed to Battery B. Fig.49 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.49 (a) is the electrode before the processing step. Fig.49 (b) is an electrode after the processing step and before the peeling step, Fig.49 (c) is the electrode after the peeling step.

[0348] (Example 46)

[0349] The active material was recovered in the same manner as in Example 28, except that the battery was changed to Battery B. Fig.50 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.50 (a) is the electrode before the processing step. Fig.50 (b) is an electrode after the processing step and before the peeling step, Fig.50 (c) is the electrode after the peeling step.

[0350] (Example 47)

[0351] The active material was recovered in the same manner as in Example 29, except that the battery was changed to Battery B. Fig.51 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.51 (a) is the electrode before the processing step. Fig.51 (b) is an electrode after the processing step and before the peeling step, Fig.51 (c) is the electrode after the peeling step.

[0352] (Example 48)

[0353] The active material was recovered in the same manner as in Example 30, except that the battery was changed to Battery B. Fig.52 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.52 (a) is the electrode before the processing step. Fig.52 (b) is an electrode after the processing step and before the peeling step, Fig.52 (c) is the electrode after the peeling step.

[0354] (Example 49)

[0355] <Peeling process>

[0356] In Example 1, after the processing step, the positive electrode of the processed battery A was placed in a container (material: plastic, 5L of water), and a stirrer (device name: Mazera ZZ-2321, manufactured by Tokyo Rikakigi Co., Ltd.) was used to apply water flow from the top of the container as an external stimulus to make the electrode float and collide in the container. After that, the active material in the container after the stripping step was recovered. Fig.53 A photograph showing the appearance of the recovered active material is shown in FIG.

[0357] The setting conditions of the above-mentioned mixer are as follows. Fig.53 (a) is the electrode before the processing step. Fig.53 (b) is an electrode after the processing step and before the peeling step, Fig.53 (c) is the electrode after the peeling step.

[0358] [Setting conditions]

[0359] Speed: 500rpm

[0360] Average flow rate: 300m / min (5m / sec)

[0361] Duration: 1 minute

[0362] (Example 50)

[0363] The active material was recovered in the same manner as in Example 49, except that the processing was changed to one direction and an orthogonal direction. Fig.54 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.54 (a) is the electrode before the processing step. Fig.54 (b) is an electrode after the processing step and before the peeling step, Fig.54 (c) is the electrode after the peeling step.

[0364] (Example 51)

[0365] The active material was recovered in the same manner as in Example 49, except that the curvature radius of the processed shape was changed to 1 mm. Fig.55 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.55 (a) is the electrode before the processing step. Fig.55 (b) is an electrode after the processing step and before the peeling step, Fig.55 (c) is the electrode after the peeling step.

[0366] (Example 52)

[0367] The active material was recovered in the same manner as in Example 51, except that the processing was changed to one direction and an orthogonal direction. Fig.56 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.56 (a) is the electrode before the processing step. Fig.56 (b) is an electrode after the processing step and before the peeling step, Fig.56 (c) is the electrode after the peeling step.

[0368] (Example 53)

[0369] The active material was recovered in the same manner as in Example 49, except that the curvature radius of the processed shape was changed to 0.5 mm. Fig.57 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.57 (a) is the electrode before the processing step. Fig.57 (b) is an electrode after the processing step and before the peeling step, Fig.57 (c) is the electrode after the peeling step.

[0370] (Example 54)

[0371] The active material was recovered in the same manner as in Example 53, except that the processing was changed to one direction and an orthogonal direction. Fig.58 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.58 (a) is the electrode before the processing step. Fig.58 (b) is an electrode after the processing step and before the peeling step, Fig.58 (c) is the electrode after the peeling step.

[0372] (Example 55)

[0373] The active material was recovered in the same manner as in Example 49, except that the battery was changed to Battery B. Fig.59 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.59 (a) is the electrode before the processing step. Fig.59 (b) is an electrode after the processing step and before the peeling step, Fig.59 (c) is the electrode after the peeling step.

[0374] (Example 56)

[0375] The active material was recovered in the same manner as in Example 50, except that the battery was changed to Battery B. Fig.60 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.60 (a) is the electrode before the processing step. Fig.60 (b) is an electrode after the processing step and before the peeling step, Fig.60 (c) is the electrode after the peeling step.

[0376] (Example 57)

[0377] The active material was recovered in the same manner as in Example 51, except that the battery was changed to Battery B. Fig.61 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.61 (a) is the electrode before the processing step. Fig.61 (b) is an electrode after the processing step and before the peeling step, Fig.61 (c) is the electrode after the peeling step.

[0378] (Example 58)

[0379] The active material was recovered in the same manner as in Example 52, except that the battery was changed to Battery B. Fig.62 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.62 (a) is the electrode before the processing step. Fig.62 (b) is an electrode after the processing step and before the peeling step, Fig.62 (c) is the electrode after the peeling step.

[0380] (Example 59)

[0381] The active material was recovered in the same manner as in Example 53, except that the battery was changed to Battery B. Fig.63 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.63 (a) is the electrode before the processing step. Fig.63 (b) is an electrode after the processing step and before the peeling step, Fig.63 (c) is the electrode after the peeling step.

[0382] (Example 48)

[0383] In Example 60, except that the battery was changed to Battery B, the active material was recovered in the same manner as in Example 54. Fig.64 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.64 (a) is the electrode before the processing step. Fig.64 (b) is an electrode after the processing step and before the peeling step, Fig.64 (c) is the electrode after the peeling step.

[0384] (Example 61)

[0385] <Peeling process>

[0386] In Example 1, after the processing step, the positive electrode of the processed battery A was placed in a container (material: stainless steel, 5L of water), and a shock wave was generated from the upper part of the container using an electric pulse generator (manufactured by Shibata Science Co., Ltd.) and applied to the electrode. After that, the active material in the container after the stripping step was recovered. Fig.65 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.65 (a) is the electrode before the processing step. Fig.65 (b) is an electrode after the processing step and before the peeling step, Fig.65 (c) is the electrode after the peeling step.

[0387] The setting conditions of the above-mentioned electric pulse generating device are as follows.

[0388] [Setting conditions]

[0389] Applied voltage: 60kV

[0390] Pulse number: 30 times

[0391] ·Distance from the counter electrode of the electric pulse device: 5 cm

[0392] (Example 62)

[0393] The active material was recovered in the same manner as in Example 61, except that the processing was changed to one direction and an orthogonal direction. Fig.66 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.66 (a) is the electrode before the processing step. Fig.66 (b) is an electrode after the processing step and before the peeling step, Fig.66 (c) is the electrode after the peeling step.

[0394] (Example 63)

[0395] The active material was recovered in the same manner as in Example 61, except that the curvature radius of the processed shape was changed to 1 mm. Fig.67 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.67 (a) is the electrode before the processing step. Fig.67 (b) is an electrode after the processing step and before the peeling step, Fig.67 (c) is the electrode after the peeling step.

[0396] (Example 64)

[0397] The active material was recovered in the same manner as in Example 63, except that the processing was changed to one direction and an orthogonal direction. Fig.68 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.68 (a) is the electrode before the processing step. Fig.68 (b) is an electrode after the processing step and before the peeling step, Fig.68 (c) is the electrode after the peeling step.

[0398] (Example 65)

[0399] The active material was recovered in the same manner as in Example 61, except that the curvature radius of the processed shape was changed to 0.5 mm. Fig.69 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.69 (a) is the electrode before the processing step. Fig.69(b) is an electrode after the processing step and before the peeling step, Fig.69 (c) is the electrode after the peeling step.

[0400] (Example 66)

[0401] The active material was recovered in the same manner as in Example 65, except that the processing was changed to one direction and an orthogonal direction. Fig.70 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.70 (a) is the electrode before the processing step. Fig.70 (b) is an electrode after the processing step and before the peeling step, Fig.70 (c) is the electrode after the peeling step.

[0402] (Example 67)

[0403] The active material was recovered in the same manner as in Example 61, except that the battery was changed to Battery B. Fig.71 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.71 (a) is the electrode before the processing step. Fig.71 (b) is an electrode after the processing step and before the peeling step, Fig.71 (c) is the electrode after the peeling step.

[0404] (Example 68)

[0405] The active material was recovered in the same manner as in Example 62, except that the battery was changed to Battery B. Fig.72 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.72 (a) is the electrode before the processing step. Fig.72 (b) is an electrode after the processing step and before the peeling step, Fig.72 (c) is the electrode after the peeling step.

[0406] (Example 69)

[0407] The active material was recovered in the same manner as in Example 63, except that the battery was changed to Battery B. Fig.73 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.73 (a) is the electrode before the processing step. Fig.73 (b) is an electrode after the processing step and before the peeling step, Fig.73 (c) is the electrode after the peeling step.

[0408] (Example 70)

[0409] The active material was recovered in the same manner as in Example 64, except that the battery was changed to Battery B. Fig.74 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.74 (a) is the electrode before the processing step. Fig.74 (b) is an electrode after the processing step and before the peeling step, Fig.74 (c) is the electrode after the peeling step.

[0410] (Example 71)

[0411] The active material was recovered in the same manner as in Example 65, except that the battery was changed to Battery B. Fig.75 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.75 (a) is the electrode before the processing step. Fig.75 (b) is an electrode after the processing step and before the peeling step, Fig.75 (c) is the electrode after the peeling step.

[0412] (Example 72)

[0413] The active material was recovered in the same manner as in Example 66, except that the battery was changed to Battery B. Fig.76 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.76 (a) is the electrode before the processing step. Fig.76 (b) is an electrode after the processing step and before the peeling step, Fig.76 (c) is the electrode after the peeling step.

[0414] (Comparative Example 1)

[0415] The active material was recovered in the same manner as in Example 25, except that the processing step was not performed. Fig.77 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.77 (a) is the electrode that has not been processed. Fig.77 (b) is an electrode that has not been subjected to a processing step but has been subjected to a peeling step.

[0416] (Comparative Example 2)

[0417] The active material was recovered in the same manner as in Example 31 except that the processing step was not performed. Fig.78 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.78 (a) is the electrode that has not been processed. Fig.78 (b) is an electrode that has not been subjected to a processing step but has been subjected to a peeling step.

[0418] (Comparative Example 3)

[0419] The active material was recovered in the same manner as in Example 37 except that the processing step was not performed. Fig.79 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.79 (a) is the electrode that has not been processed. Fig.79 (b) is an electrode that has not been subjected to a processing step but has been subjected to a peeling step.

[0420] (Comparative Example 4)

[0421] The active material was recovered in the same manner as in Example 43, except that the processing step was not performed. Fig.80 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.80 (a) is the electrode that has not been processed. Fig.80 (b) is an electrode that has not been subjected to a processing step but has been subjected to a peeling step.

[0422] (Comparative Example 5)

[0423] The active material was recovered in the same manner as in Example 55, except that the processing step was not performed. Fig.81 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.81 (a) is the electrode that has not been processed. Fig.81 (b) is an electrode that has not been subjected to a processing step but has been subjected to a peeling step.

[0424] (Comparative Example 6)

[0425] The active material was recovered in the same manner as in Example 67, except that the processing step was not performed. Fig.82 A photograph showing the appearance of the recovered active material is shown in FIG. Fig.82 (a) is the electrode that has not been processed. Fig.82 (b) is an electrode that has not been subjected to a processing step but has been subjected to a peeling step.

[0426]

Table 1

[0427]

[0428]

Table 2

[0429]

[0430]

Table 3

[0431]

[0432]

Table 4

[0433]

[0434] <Evaluation>

[0435] The recovery efficiency (%) and purity of the active material in Examples 1 to 72 and Comparative Examples 1 to 6 were evaluated as follows. The results are shown in Tables 5 to 8.

[0436] <Active material recovery efficiency (1) (%)>

[0437] In Examples 1 to 72 and Comparative Examples 1 to 6, the recovery efficiency (%) of the active material was calculated based on the following formula from the recovery amount (g) of the active material recovered in the processing step and the weight (g) of the electrode before the peeling step.

[0438] [Mode]

[0439] Recovery efficiency of active material (%) = recovery amount of active material in the processing step (g) / mass of active material attached to the electrode (g) × 100

[0440] <Active material recovery efficiency (2) (%)>

[0441] In Examples 1 to 72 and Comparative Examples 1 to 6, the recovery efficiency (%) of the active material recovered in the stripping step was calculated based on the following formula from the recovery amount (g) of the active material recovered in the stripping step and the weight (g) of the electrode before the stripping step.

[0442] [Mode]

[0443] Recovery efficiency of active material (%) = recovery amount of active material in the stripping process (g) / mass of active material attached to the electrode (g) × 100

[0444] <Purity of active substances>

[0445] The contents of aluminum and copper contained in the active materials recovered in Examples 1 to 72 and Comparative Examples 1 to 6 were measured by inductively coupled plasma emission spectroscopy, and the impurity content of the active materials was evaluated by weight percentage based on the following formula. (Measured by dissolving the metals contained in the active materials by microwave + acid thermal decomposition)

[0446] [Mode]

[0447] 100 - (Aluminum content of active material (%) + Copper content of active material (%))

[0448] In addition, aluminum content of active material (%) = aluminum content of active material (g) / weight of active material (g) × 100

[0449] Copper content of active material (%) = Copper content of active material (g) / Weight of active material (g) × 100

[0450] <Electrode miniaturization>

[0451] The active materials recovered in Examples 1 to 72 and Comparative Examples 1 to 6 were visually observed, and the miniaturization of the electrodes was evaluated according to the following table or evaluation criteria. In the following evaluation criteria, "○" and "△" indicate acceptable.

[0452] [Evaluation criteria]

[0453] ○: No visible micronized current collector is present

[0454] △: Visibly fine current collectors are present, but can be easily separated using a sieve

[0455] ×: Visibly fine current collectors are present, but difficult to separate using a sieve

[0456]

Table 5

[0457]

[0458]

Table 6

[0459]

[0460]

Table 7

[0461]

[0462]

Table 8

[0463]

[0464] This international application claims the benefit of priority based on Japanese Patent Application No. 2022-060609 filed on March 31, 2022, the entire contents of which are incorporated herein by reference.

[0465] Explanation of symbols

[0466] 1: Air flow nozzle

[0467] 2: Container

[0468] 3: Mesh

[0469] 4: Electrode

[0470] 5: Airflow

[0471] 6: Blender

[0472] 7: Water

[0473] 8: Water Flow

[0474] 9: High voltage electric pulse generator

[0475] 10: Counter electrode for insulation breakdown

[0476] 11: Power supply unit

[0477] 12: Shock wave.

Claims

1. A method for recovering active material from an electrical storage device, characterized in that: have: The processing step is to process the electrode in the power storage device including the electrode to which the active material is attached so that at least a portion of the electrode has a corrugated shape.

2. The method for recovering active material from an electrical storage device according to claim 1, wherein: The recovery method includes a peeling step of applying an external stimulus to the electrode after the processing step to peel the active material from the electrode.

3. The method for recovering active material from an electrical storage device according to claim 2, wherein: The wavy shape is at least any one of a wavy shape as a whole, a wavy shape only at the end, and a wavy shape in one direction as a whole and in a direction different from the one direction.

4. The method for recovering active material from an electrical storage device according to claim 1 or 2, wherein: The curvature radius of the wavy shape is greater than or equal to 0 mm and less than or equal to 5 mm.

5. The method for recovering active material from an electrical storage device according to claim 1 or 2, wherein: The curvature radius of the wavy shape is greater than or equal to 0 mm and less than or equal to 0.5 mm.

6. The method for recovering active material from an electrical storage device according to claim 2 or 3, wherein: The peeling step is performed at a temperature of 0° C. or higher and 200° C. or lower.

7. The method for recovering active material from an electrical storage device according to claim 2 or 3, wherein: The external stimulus is airflow.

8. The method for recovering active material from an electrical storage device according to claim 7, wherein: The airflow is applied to the electrode under the conditions of a wind speed of 5 m / s to 100 m / s and a time of 0.5 minutes to 2.0 minutes.

9. The method for recovering active material from an electrical storage device according to claim 2 or 3, wherein: The external stimulus is water flow.

10. The method for recovering active material from an electrical storage device according to claim 9, wherein: The water flow is applied to the electrode under the conditions of a flow rate of 0.05 m / s or more and 10 m / s and a time of 0.1 minute or more and 5.0 minutes or less.

11. The method for recovering active material from an electrical storage device according to claim 2 or 3, wherein: The external stimulus is a shock wave.

12. The method for recovering active material from an electrical storage device according to claim 11, wherein: The shock wave is applied to the electrode under the conditions that the applied voltage is 10 kV to 200 kV, the distance from the counter electrode of the electric pulse device is 0.5 cm to 30 cm, and the number of pulses is 1 to 100.