Preparation method of high-barrier PP film

By using a three-dimensional composite system of heat sealing film, barrier film and protective film in high-barrier packaging film, combining random polypropylene copolymer and nano-layered silicate modified polyvinyl alcohol and other materials, the ductility of aluminum foil material is solved. and the problem of insufficient flexibility have achieved improvements in high barrier performance and stability.

CN118977492AActive Publication Date: 2024-11-19ZHEJIANG JINSHENG DEOCRATION MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411040510.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The existing high-barrier packaging film is mainly aluminum foil material, with insufficient ductility and flexibility, and is prone to break when impacted by external forces, resulting in poor packaging stability and risk of food spoilage.

Method used

Using a three-dimensional composite system of heat sealing film, barrier film and protective film to form a layer-by-layer barrier composite sealing structure, and using random polypropylene copolymers, nano-layered silicate modified polyvinyl alcohol and silica sol to improve the film's Barrier performance and flexibility.

Benefits of technology

It realizes the maintenance of high barrier properties and enhances flexibility, enhances the stability and impact resistance of the membrane, and reduces the risk of food spoilage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004972252650000121
    Figure BDA0004972252650000121
Patent Text Reader

Abstract

The invention belongs to the technical field of PP films, and particularly relates to a preparation method of a high-barrier PP film, the high-barrier PP film is sequentially provided with a PP-based protective film, a barrier film and a heat sealing film from outside to inside, the thickness of the PP-based protective film is 0.014-0.018 mm, the thickness of the barrier film is 0.011-0.015 mm, and the thickness of the heat sealing film is 0.065-0.085 mm, and the invention provides the preparation method of the high-barrier PP film. The stability defect of an existing PP film is overcome, a layer-by-layer barrier composite sealing structure is formed through a three-dimensional composite system of the heat sealing film, the barrier film and the protective film, and the overall barrier performance of the PP film is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of PP films, and particularly relates to a method for preparing a high-barrier PP film. Background Art

[0002] At present, the high-barrier packaging film on the market uses aluminum foil as the barrier material, and its product structure is a composite structure of three or more layers. Due to the characteristics of metal materials, this type of packaging film has excellent barrier properties. At the same time, aluminum foil composite packaging film can meet the sterilization requirements of boiling and steaming in the processing technology of food companies, and is also a commonly used packaging form in high-barrier food packaging. However, the packaging of this system uses aluminum foil as the main material, and the aluminum foil production process is formed by aluminum ingot calendering process to form a micron-level film. Its ductility and flexibility are cross-cutting. When subjected to external impact or extrusion, the aluminum foil in the aluminum foil packaging is prone to breakage, resulting in poor packaging stability and the risk of food spoilage.

[0003] Therefore, there is an urgent need in the market for a polypropylene-based film having both good barrier properties and flexibility. Summary of the invention

[0004] In view of the problems in the prior art, the present invention provides a method for preparing a high barrier PP film, which solves the stability defects of the existing PP film and utilizes a three-dimensional composite system of a heat-sealing film, a barrier film and a protective film to form a layer-by-layer barrier composite sealing structure, thereby ensuring the overall barrier performance of the PP film.

[0005] In order to achieve the above technical objectives, the technical solution of the present invention is:

[0006] A method for preparing a high-barrier PP film, wherein the high-barrier PP film is sequentially provided with a PP-based protective film, a barrier film and a heat-sealing film from the outside to the inside, wherein the thickness of the PP-based protective film is 0.014-0.018 mm, the thickness of the barrier film is 0.011-0.015 mm, and the thickness of the heat-sealing film is 0.065-0.085 mm.

[0007] The mass ratio of the heat-sealing film includes: 60-70 parts of polypropylene, 10-15 parts of polyethylene, 1-5 parts of silica sol, and 5-8 parts of vinyl trichlorosilane. The polypropylene adopts random polypropylene copolymer, which contains 3-5% of ethylene molecules by mass, and the ethylene molecules are randomly inserted into the polymer main chain, which reduces the rigidity, improves the impact resistance and improves the transparency by hindering the crystalline arrangement of the polymer molecules; the polyethylene adopts linear low-density polyethylene, which is a basically linear polymer with a large number of short side chains, so the linear low-density polyethylene has a smaller shear sensitivity; the concentration of the silica sol is 45-50%, and the silica sol is a dispersion of nano-scale silica particles in water. In the silica sol, the silica particles are large. The particle size of the silica sol is as small as about 10-20nm, and has a relatively large specific surface area. At the same time, the silica sol has good permeability, forming diffuse penetration in the film, and when the water evaporates, the colloidal particles are firmly attached to form silicon-oxygen bonding, thereby improving the rigidity and hardness of the heat-sealing film; the vinyl trichlorosilane can contain vinyl and chlorine groups, and has good chemical activity. When the vinyl trichlorosilane is mixed with the silica sol, the water molecules in the silica sol react with the chlorine groups on the vinyl trichlorosilane, and are hydrolyzed in situ to form vinyl trihydroxy silane. The vinyl trihydroxy silane will form condensation polymerization under temperature conditions, thereby ensuring the water and oil antifouling properties of the film and improving the adhesion of the heat-sealing film.

[0008] The preparation method of the heat-sealing film comprises the following steps: a1, slowly dropping silica sol into vinyl trichlorosilane and performing low-temperature ultrasound for 0.5-1h to obtain a mixed suspension, wherein the slow dropping speed is 5-8mL / min, the temperature of the low-temperature ultrasound is 5-10°C, and the ultrasound frequency is 60-80kHz; in this step, the silica sol is slowly dropped into vinyl trichlorosilane to convert the chlorine group in the vinyl trichlorosilane into a hydroxyl group to obtain vinyl trihydroxysilane, and the low-temperature ultrasound can completely disperse the vinyl trihydroxysilane and prevent the vinyl trihydroxysilane from being dispersed. a2, grinding and stirring polypropylene and polyethylene, melting to form a mixed solution, and then spraying and granulating the mixed solution to form composite particles, wherein the grinding and stirring adopts wet grinding, and the solvent is ethanol, and the mass ratio of ethanol to polypropylene is 1:20-30; the temperature is 5-10°C, the pressure is 0.3-0.5MPa, and the melting temperature is 180-190°C; the spray drying temperature of the composite particles is 20-30°C, the spray speed is 1-2mL / min, and the area is 100-200cm 2In this step, polypropylene and polyethylene are ground and mixed to completely refine the polypropylene and polyethylene and form a homogenized mixture; during the melting process, polypropylene and polyethylene are homogenously mixed to ensure that polyethylene is doped in polypropylene. When the mixed solution is sprayed and granulated, the droplets are composited into particles at room temperature. The polyethylene in the composite particles is homogeneously dispersed in the polypropylene to obtain homogeneous polypropylene-polyethylene composite particles; a3, the composite particles are placed in the mixed suspension and stirred fully, and a heat-sealing masterbatch is obtained by freeze-drying. The stirring speed of the sufficient stirring is 300-500r / min and the temperature is 5-10°C; the freeze-drying temperature is -20°C; in this step, the mixed suspension is attached to the surface of the composite particles by stirring to form a surface liquid film. The surface liquid film is formed during freeze-drying to deposit the silicon oxide precursor on the surface of the composite particles.

[0009] The barrier film adopts a nano-layered silicate modified polyvinyl alcohol film, and the nano-layered silicate adopts a modified layered nano-montmorillonite. Montmorillonite is a kind of soil-like mineral composed of nano-thick silicate sheets with negative charges on the surface, which are piled together by the electrostatic effect between the layers. The unit cell in its crystal structure is composed of two layers of silicon-oxygen tetrahedrons with a layer of aluminum-oxygen octahedron in the middle. Layered nano-silicate has a high interlayer pore structure, which makes it have a high specific surface area and pore volume, so that it can effectively block the penetration of some molecules. At the same time, the layered montmorillonite has certain chemical stability and thermal stability, and can show good durability and durability while maintaining the barrier effect. Therefore, nano-montmorillonite is added to polyvinyl alcohol as a modifier to form a layered covering effect, thereby achieving a good barrier effect. However, montmorillonite itself is an inorganic material with a large number of gaps, and has a poor stability problem when in contact with polyvinyl alcohol. To address this problem, the layered montmorillonite needs to be surface modified, and surface activity is formed through the adhesion of silicon oxide material precursors, which effectively improves the connection stability between polyvinyl alcohol and layered montmorillonite. The intermittent coverage of silicon oxide materials effectively ensures the surface performance of the layered montmorillonite itself, and still maintains good performance. The preparation method of the modified layered montmorillonite comprises the following steps: b1, adding ethyl cellulose to ether and stirring evenly to form a homogeneous solution, then slowly dropping trichloromethylsilane to form a coating solution, wherein the concentration of the ethyl cellulose in the ether is 300-500 g / L, the stirring speed for uniform stirring is 300-500 r / min, the speed of slow dropping is 2-3 mL / min, the mass ratio of the trichloromethylsilane to the methyl cellulose is 1:0.8-1, and this step utilizes the good solubility of ethyl cellulose and trichloromethylsilane in ether to form a homogeneous dispersion in the ether, and at the same time, the trichloromethylsilane forms a homogeneous dispersion during the slow addition process, thereby reducing the problem of agglomeration; b2, placing the layered nano-montmorillonite in the coating solution and stirring for 20-30 min, filtering and standing for 0.5-1h, drying to obtain prefabricated modified layered nano-montmorillonite, the stirring temperature is 5-10°C, the stirring speed is 200-500r / min, the static atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 12-15:1, the temperature is 10-15°C, and the drying temperature is 5-10°C; this step utilizes the liquid state of the coating liquid and the solid state of the layered nano-montmorillonite to achieve liquid film deposition of the coating liquid on the surface of the layered nano-montmorillonite, based on the viscosity and bonding of ethyl cellulose itself, the liquid is combined The coating solution forms a stable liquid film on the surface of the layered nano-montmorillonite, but does not penetrate between the layers of the layered nano-montmorillonite, thereby realizing surface liquid film deposition. After filtration, the layered nano-montmorillonite containing the liquid film is allowed to stand for treatment. When the layered nano-montmorillonite containing the liquid film encounters water molecules, the ether in the liquid film is insoluble in water. Ethyl cellulose is hydrophobic, and only trichloromethylsilane is hydrolyzed to be converted into trihydroxymethylsilane, and the water molecules will not penetrate into the interlayer gaps of the layered nano-montmorillonite. Low-temperature drying can remove the ether solution while the trihydroxymethylsilane is stable. agent, thereby achieving the effect of drying. It should be noted that ether is a volatile substance and is constantly volatilizing during the standing and drying processes; b3, the prefabricated modified layered nano-montmorillonite is allowed to stand for reaction for 1-2 hours, then placed in ether for ultrasonication for 20-30 minutes, filtered and dried under reduced pressure to obtain modified layered nano-montmorillonite, the atmosphere of the standing reaction is a nitrogen atmosphere, and the temperature is 60-70°C; the mass ratio of the prefabricated modified layered nano-montmorillonite to ether is 1:8-10, the ultrasonic temperature is 5-10°C, and the ultrasonic frequency is 70-90kHz , the pressure of the reduced pressure drying is 80-85% of the atmospheric pressure, and the temperature is 30-35°C; this step uses a constant temperature static reaction to form a surface polycondensation of trihydroxymethylsilane, and the ethyl cellulose at this time is used as a physical barrier, that is, a surface film with a silicon-oxygen structure as a framework is formed on the surface of the layered nano-montmorillonite, and the silicon-oxygen structure forms a stable connection with the layered nano-montmorillonite; the prefabricated modified layered nano-montmorillonite after the static reaction is immersed in ether to form a stable dissolution, and the ethyl cellulose is dissolved in ether to achieve the removal effect, and the silicon-oxygen framework is directly exposed. The layered nano-montmorillonite uses ethyl cellulose to form a barrier and adhesion, and trichloromethylsilane forms a surface deposition, and at the same time cooperates with in-situ hydrolysis and in-situ polycondensation to form a silicon-oxygen framework modified layered nano-montmorillonite. .

[0010] The mass ratio of the barrier film is: 35-45 parts of polyvinyl alcohol, 15-18 parts of modified nano-layered silicate, 5-10 parts of silica sol, and 0.3-0.5 parts of trichloromethylsilane; the concentration of the silica sol is 45-50%, and the silica sol is a dispersion of nano-scale silicon dioxide particles in water. The modified nano-layered silicate adopts silica-oxygen modified layered nano-montmorillonite. The silica-oxygen framework of the silica-oxygen modified layered nano-montmorillonite not only contains a porous structure, but also has hydroxyl groups, which promote the penetration of polyvinyl alcohol into the porous framework. At the same time, the alcohol hydroxyl groups on the polyvinyl alcohol react with the hydroxyl groups of trichloromethylsilane, silica sol and modified nano-layered silicate, thereby not only ensuring the firmness and mechanical strength of the barrier film, but also greatly improving the barrier effect of the barrier film due to the internal silica-oxygen structure. The preparation method of the barrier film comprises the following steps: c1, adding trichloromethylsilane to silica sol and dispersing it under low temperature ultrasonic dispersion for 20-30 minutes to obtain a homogeneous dispersion liquid, wherein the low temperature of the low temperature ultrasonic dispersion is 5-10°C and the ultrasonic frequency is 70-90kHz, and in this step, trichloromethylsilane forms a hydrolysis reaction with water molecules in the silica sol to produce trihydroxymethylsilane, and the trihydroxymethylsilane is dispersed under the action of low temperature ultrasound, that is, the trihydroxymethylsilane is homogeneously dispersed in water; c2, adding polyvinyl alcohol to water and stirring evenly to form a viscous liquid, and then adding modified nano-layered silicate and performing low temperature ultrasonic treatment for 20-30 minutes to obtain a preliminary mixed liquid, wherein the mass ratio of polyvinyl alcohol to water is 10:11-14, the stirring speed for uniform stirring is 300-500r / min, and the temperature of the low temperature ultrasonic treatment is 5-10°C, the ultrasonic frequency is 90-100kHz. This step utilizes the solubility of polyvinyl alcohol in water to form a viscous polyvinyl alcohol aqueous solution, and adds the modified nano-layered silicate. After low-temperature ultrasonic dispersion, the modified nano-layered silicate is uniformly dispersed in the polyvinyl alcohol. At the same time, low-temperature ultrasound can ensure that the silanol group on the surface of the modified nano-layered silicate remains stable and will not undergo condensation prematurely; c3, the homogeneous dispersion is added dropwise to the preliminary mixed solution and rapidly stirred for 20-30 minutes, and freeze-dried to obtain a barrier masterbatch. The dropping speed is 3-5mL / min, the rapid stirring speed is 1000-2000r / min, and the temperature is not higher than 20°C; this step utilizes rapid stirring to homogeneously disperse the silica sol containing trihydroxymethylsilane in polyvinyl alcohol, and removes water molecules during freeze-drying to obtain a barrier masterbatch.This process uses silica sol as a hydrolyzing agent to ensure that trichloromethylsilane forms a hydroxyl hydrolysis product, and both are added to polyvinyl alcohol as additives to form a silicon-oxygen system connection structure on the outside of the layered nanosilicate, effectively improving the gap treatment between adjacent layered nanosilicates and improving the barrier effect of the barrier film. At the same time, the silicon-oxygen modified layered nano-montmorillonite, which is a modified layered nanosilicate, contains a silicon hydroxyl structure on its surface, and the silicon hydroxyl is produced by the hydrolysis of trichloromethylsilane, which is the same as the hydrolysis product of trichloromethylsilane-silica sol, and can form a stable silicon hydroxyl reaction structure under temperature conditions, ensuring the connectivity of adjacent layered silicates to improve the overall barrier effect of the barrier film.

[0011] The mass ratio of the PP-based protective film is: 100 parts of polypropylene, 0.5-0.8 parts of nano titanium dioxide, 0.5-0.8 parts of antioxidant, 0.5-0.8 parts of trichloromethylsilane, 0.5-0.8 parts of white carbon black, 0.1-0.3 parts of bis(sebacate) ester, and 0.1-0.3 parts of lubricant; the antioxidant is trihydroxynitrile, and the lubricant is zinc stearate. The preparation method of the PP-based protective film comprises the following steps: d1, adding nano titanium dioxide to trichloromethylsilane, stirring, spraying into a reaction kettle, standing at low temperature for 20-30 minutes, and purging to obtain a primary mixture, the stirring speed is 100-300r / min, the spraying speed is 10-30mL, the low-temperature standing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor in the mixed atmosphere is 10-14:1, and the temperature is 5-10°C; the purging uses nitrogen at 20°C, and the purging speed is

[0012] 10-20mL / min; this step utilizes liquid trichloromethylsilane and solid nano titanium dioxide, which are mixed and sprayed to form in-situ hydrolysis under the atmosphere system; d2, dicaprate, antioxidant and lubricant are added to polypropylene for melt mixing to obtain a prefabricated mixed liquid, the melt mixing temperature is 200-220°C, d3, the prefabricated mixed liquid is granulated to form prefabricated particles, and mixed with the primary mixture to obtain a protective film masterbatch; the granulation temperature is 20-30°C.

[0013] The method for preparing the high barrier PP film comprises the following steps:

[0014] Step 1, placing the heat sealing masterbatch, the barrier masterbatch and the protective film masterbatch into three extruders respectively for melt extrusion and compounding to obtain a composite film, wherein the temperature of the melt extrusion is 220-250° C.;

[0015] Step 2, stretching the composite film to obtain a high barrier PP film, wherein the stretching temperature of the stretching treatment is 140-160° C., and the transverse stretching multiple is 6-8.

[0016] It can be seen from the above description that the present invention has the following advantages:

[0017] 1. The present invention solves the stability defect of the existing PP film, and utilizes a three-dimensional composite system of a heat-sealing film, a barrier film and a protective film to form a layer-by-layer barrier composite sealing structure, thereby ensuring the overall barrier performance of the PP film.

[0018] 2. The present invention utilizes trichloromethylsilane hydrolyzate in heat-sealing film, barrier film and protective film as a proppant and connectivity, thereby improving the connection stability between film layers. At the same time, the supporting effect of the hydrolyzate itself not only ensures the flexibility of the PP film, but also has good stiffness.

[0019] 3. The present invention utilizes the encapsulation characteristics of trichloromethylsilane to effectively prevent the excitation problem of nano-titanium dioxide, reduce the generation of free radicals in the protective film, and form an excellent anti-aging system in conjunction with the use of antioxidants. At the same time, the transparency of trichloromethylsilane itself does not affect the ultraviolet reflection characteristics of nano-titanium dioxide. DETAILED DESCRIPTION

[0020] The present invention is described in detail with reference to the embodiments, but no limitation is imposed on the claims of the present invention.

[0021] Example 1

[0022] A method for preparing a high-barrier PP film, wherein the high-barrier PP film is sequentially provided with a PP-based protective film, a barrier film and a heat-sealing film from the outside to the inside, the thickness of the PP-based protective film is 0.014 mm, the thickness of the barrier film is 0.011 mm, and the thickness of the heat-sealing film is 0.065 mm.

[0023] The mass ratio of the heat-sealing film includes: 60 parts of polypropylene, 10 parts of polyethylene, 1 part of silica sol, and 5 parts of vinyl trichlorosilane. The polypropylene adopts a random polypropylene copolymer, which contains 3% by mass of ethylene molecules, and the ethylene molecules are randomly inserted into the polymer main chain; the concentration of the silica sol is 45%, and the silica sol is a dispersion of nano-scale silica particles in water. In the silica sol, the size of the silica particles is about 10-20nm. The preparation method of the heat-sealing film comprises the following steps: a1, slowly dropping silica sol into vinyl trichlorosilane and performing low-temperature ultrasound for 0.5 h to obtain a mixed suspension, wherein the slow dropping speed is 5 mL / min, the low-temperature ultrasound temperature is 5°C, and the ultrasound frequency is 60 kHz; a2, grinding and stirring polypropylene and polyethylene to melt to form a mixed liquid, and then spraying and granulating the mixed liquid to form composite particles, wherein the grinding and stirring adopts wet grinding, and the solvent is ethanol, and the mass ratio of ethanol to polypropylene is 1:20; the temperature is 5°C, the pressure is 0.3 MPa, and the melting temperature is 180°C; the spray drying temperature of the composite particles is 20°C, the spray speed is 1 mL / min, and the area is 100 cm 2 a3, putting the composite particles into the mixed suspension and stirring them fully, and freeze-drying them to obtain a heat-sealing masterbatch, wherein the stirring speed of the stirring is 300 r / min and the temperature is 5°C; the freeze-drying temperature is -20°C.

[0024] The barrier film adopts a polyvinyl alcohol film modified by nano-layered silicate, and the mass ratio of the barrier film is: 35 parts of polyvinyl alcohol, 15 parts of modified nano-layered silicate, 5 parts of silica sol, and 0.3 parts of trichloromethylsilane; the concentration of the silica sol is 45%, and the silica sol is a dispersion of nano-scale silicon dioxide particles in water. The modified nano-layered silicate adopts silica-modified layered nano-montmorillonite, and the preparation method of the modified layered montmorillonite comprises the following steps: b1, adding ethyl cellulose to ether and stirring evenly to form a homogeneous liquid, and then slowly dripping trichloromethylsilane to form a coating liquid, the concentration of the ethyl cellulose in the ether is 300g / L, the stirring speed for uniform stirring is 300r / min, the speed of slow dripping is 2mL / min, and the mass ratio of the trichloromethylsilane to the methyl cellulose is 1:0.8; b2, place the layered nano-montmorillonite in the coating solution and stir for 20 minutes, filter and let it stand for 0.5 hours, and dry to obtain the prefabricated modified layered nano-montmorillonite, the stirring temperature is 5°C, the stirring speed is 200r / min, the standing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 12:1, the temperature is 10°C, and the drying temperature is 5°C; b3, let the prefabricated modified layered nano-montmorillonite stand for reaction for 1 hour, then put it into ether for ultrasonication for 20 minutes, filter and dry under reduced pressure to obtain modified layered nano-montmorillonite, the standing reaction atmosphere is a nitrogen atmosphere, the temperature is 60°C; the mass ratio of the prefabricated modified layered nano-montmorillonite to ether is 1:8, the ultrasonic temperature is 5°C, the ultrasonic frequency is 70kHz, the pressure of the reduced pressure drying is 80% of the atmospheric pressure, and the temperature is 30°C.

[0025] The preparation method of the barrier film comprises the following steps: c1, adding trichloromethylsilane to silica sol and performing low-temperature ultrasonic dispersion for 20 minutes to obtain a homogeneous dispersion liquid, wherein the low-temperature temperature of the low-temperature ultrasonic dispersion is 5°C and the ultrasonic frequency is 70kHz; c2, adding polyvinyl alcohol to water and stirring evenly to form a viscous liquid, then adding modified nano-layered silicate and performing low-temperature ultrasonic treatment for 20 minutes to obtain a preliminary mixed liquid, wherein the mass ratio of polyvinyl alcohol to water is 10:11, the stirring speed for uniform stirring is 300r / min, the temperature of the low-temperature ultrasonic treatment is 5°C, and the ultrasonic frequency is 90kHz; c3, dropping the homogeneous dispersion liquid into the preliminary mixed liquid and stirring rapidly for 20 minutes, and freeze-drying to obtain a barrier masterbatch, wherein the dropping speed is 3mL / min, the stirring speed for rapid stirring is 1000r / min, and the temperature is 20°C.

[0026] The mass ratio of the PP-based protective film is: 100 parts of polypropylene, 0.5 parts of nano titanium dioxide, 0.5 parts of antioxidant, 0.5 parts of trichloromethylsilane, 0.5 parts of white carbon black, 0.1 parts of bissebacate, and 0.1 parts of lubricant; the antioxidant is trihydroxynitrile, and the lubricant is zinc stearate. The preparation method of the PP-based protective film comprises the following steps: d1, adding nano titanium dioxide to trichloromethylsilane, stirring, spraying into a reactor, standing at low temperature for 20 minutes, and purging to obtain a primary mixture, the stirring speed is 100r / min, the spraying speed is 10mL, the low-temperature standing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor in the mixed atmosphere is 10:1, and the temperature is 5°C; the purging uses 20°C nitrogen, and the purging speed is 10mL / min; d2, adding dicaprate, an antioxidant and a lubricant to polypropylene for melt mixing to obtain a prefabricated mixed liquid, the melt mixing temperature is 200°C, d3, granulating the prefabricated mixed liquid to form prefabricated particles, and mixing with the primary mixture to obtain a protective film masterbatch; the granulation temperature is 20°C.

[0027] The method for preparing the high barrier PP film comprises the following steps:

[0028] Step 1, placing the heat sealing masterbatch, the barrier masterbatch and the protective film masterbatch into three extruders respectively for melt extrusion and compounding to obtain a composite film, wherein the temperature of the melt extrusion is 220° C.;

[0029] Step 2, stretching the composite film to obtain a high barrier PP film, wherein the stretching temperature of the stretching treatment is 140° C. and the transverse stretching multiple is 6.

[0030] Example 2

[0031] A method for preparing a high-barrier PP film, wherein the high-barrier PP film is sequentially provided with a PP-based protective film, a barrier film and a heat-sealing film from the outside to the inside, wherein the thickness of the PP-based protective film is 0.018 mm, the thickness of the barrier film is 0.015 mm, and the thickness of the heat-sealing film is 0.085 mm.

[0032] The mass ratio of the heat-sealing film includes: 70 parts of polypropylene, 15 parts of polyethylene, 5 parts of silica sol, and 8 parts of vinyl trichlorosilane. The polypropylene adopts a random polypropylene copolymer, which contains 5% by mass of ethylene molecules, and the ethylene molecules are randomly inserted into the polymer main chain; the concentration of the silica sol is 50%, and the silica sol is a dispersion of nano-scale silica particles in water. In the silica sol, the size of the silica particles is about 10-20nm. The preparation method of the heat-sealing film comprises the following steps: a1, slowly dropping silica sol into vinyl trichlorosilane and performing low-temperature ultrasound for 1 hour to obtain a mixed suspension, wherein the slow dropping speed is 8 mL / min, the low-temperature ultrasound temperature is 10°C, and the ultrasound frequency is 80 kHz; a2, grinding and stirring polypropylene and polyethylene to melt to form a mixed liquid, and then spraying and granulating the mixed liquid to form composite particles, wherein the grinding and stirring adopts wet grinding, and the solvent is ethanol, and the mass ratio of ethanol to polypropylene is 1:30; the temperature is 10°C, the pressure is 0.5 MPa, and the melting temperature is 190°C; the spray drying temperature of the composite particles is 30°C, the spray speed is 2 mL / min, and the area is 200 cm 2 a3, putting the composite particles into the mixed suspension and stirring them fully, and freeze-drying them to obtain a heat-sealing masterbatch, wherein the stirring speed of the stirring is 500 r / min and the temperature is 10°C; the freeze-drying temperature is -20°C.

[0033] The barrier film adopts a polyvinyl alcohol film modified by nano-layered silicate, and the mass ratio of the barrier film is: 45 parts of polyvinyl alcohol, 18 parts of modified nano-layered silicate, 10 parts of silica sol, and 0.5 parts of trichloromethylsilane; the concentration of the silica sol is 50%, and the silica sol is a dispersion of nano-scale silicon dioxide particles in water. The modified nano-layered silicate adopts silica-modified layered nano-montmorillonite, and the preparation method of the modified layered montmorillonite includes the following steps: b1, adding ethyl cellulose to ether and stirring evenly to form a homogeneous liquid, and then slowly dripping trichloromethylsilane to form a coating liquid, the concentration of the ethyl cellulose in the ether is 500g / L, the stirring speed for uniform stirring is 500r / min, the speed of slow dripping is 3mL / min, and the mass ratio of the trichloromethylsilane to the methyl cellulose is 1:1; b2, adding ethyl cellulose to ether and stirring evenly to form a homogeneous liquid, and then slowly dripping trichloromethylsilane to form a coating liquid, the concentration of the ethyl cellulose in the ether is 500g / L, the stirring speed for uniform stirring is 500r / min, the speed of slow dripping is 3mL / min, and the mass ratio of the trichloromethylsilane to the methyl cellulose is 1:1; 2. Place the layered nano-montmorillonite in the coating solution and stir for 30 minutes. After filtering, let it stand for 1 hour and dry it to obtain the prefabricated modified layered nano-montmorillonite. The stirring temperature is 10°C, the stirring speed is 500r / min, the standing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 15:1, the temperature is 15°C, and the drying temperature is 10°C; b3. Let the prefabricated modified layered nano-montmorillonite stand for reaction for 2 hours, then put it in ether for ultrasonication for 30 minutes, filter it and dry it under reduced pressure to obtain modified layered nano-montmorillonite. The standing reaction atmosphere is a nitrogen atmosphere and the temperature is 70°C; the mass ratio of the prefabricated modified layered nano-montmorillonite to ether is 1:10, the ultrasonic temperature is 10°C, the ultrasonic frequency is 90kHz, the pressure of the reduced pressure drying is 85% of the atmospheric pressure, and the temperature is 35°C.

[0034] The preparation method of the barrier film comprises the following steps: c1, adding trichloromethylsilane to silica sol and performing low-temperature ultrasonic dispersion for 30 minutes to obtain a homogeneous dispersion liquid, wherein the low-temperature temperature of the low-temperature ultrasonic dispersion is 10°C and the ultrasonic frequency is 90kHz; c2, adding polyvinyl alcohol to water and stirring evenly to form a viscous liquid, then adding modified nano-layered silicate and performing low-temperature ultrasonic treatment for 30 minutes to obtain a preliminary mixed liquid, wherein the mass ratio of polyvinyl alcohol to water is 10:14, the stirring speed for uniform stirring is 300-500r / min, the temperature of the low-temperature ultrasonic treatment is 10°C, and the ultrasonic frequency is 100kHz; c3, dropping the homogeneous dispersion liquid into the preliminary mixed liquid and stirring rapidly for 30 minutes, and freeze-drying to obtain a barrier masterbatch, wherein the dropping speed is 5mL / min, the stirring speed of rapid stirring is 2000r / min, and the temperature is 10°C.

[0035] The mass ratio of the PP-based protective film is: 100 parts of polypropylene, 0.8 parts of nano titanium dioxide, 0.8 parts of antioxidant, 0.8 parts of trichloromethylsilane, 0.8 parts of white carbon black, 0.3 parts of bissebacate, and 0.3 parts of lubricant; the antioxidant is trihydroxynitrile, and the lubricant is zinc stearate. The preparation method of the PP-based protective film comprises the following steps: d1, adding nano titanium dioxide to trichloromethylsilane, stirring, spraying into a reactor, standing at low temperature for 30 minutes, purging to obtain a primary mixture, the stirring speed is 300r / min, the spraying speed is 30mL, the low-temperature standing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor in the mixed atmosphere is 14:1, and the temperature is 10°C; the purging uses 20°C nitrogen, and the purging speed is 20mL / min; d2, adding dicaprate, an antioxidant and a lubricant to polypropylene for melt mixing to obtain a prefabricated mixed liquid, the melt mixing temperature is 220°C, d3, granulating the prefabricated mixed liquid to form prefabricated particles, and mixing with the primary mixture to obtain a protective film masterbatch; the granulation temperature is 30°C.

[0036] The method for preparing the high barrier PP film comprises the following steps:

[0037] Step 1, placing the heat sealing masterbatch, the barrier masterbatch and the protective film masterbatch into three extruders respectively for melt extrusion and compounding to obtain a composite film, wherein the temperature of the melt extrusion is 250° C.;

[0038] Step 2, stretching the composite film to obtain a high barrier PP film, wherein the stretching temperature of the stretching treatment is 160° C. and the transverse stretching multiple is 8.

[0039] Example 3

[0040] A method for preparing a high-barrier PP film, wherein the high-barrier PP film is sequentially provided with a PP-based protective film, a barrier film and a heat-sealing film from the outside to the inside, the thickness of the PP-based protective film is 0.016 mm, the thickness of the barrier film is 0.013 mm, and the thickness of the heat-sealing film is 0.075 mm.

[0041] The mass ratio of the heat-sealing film includes: 65 parts of polypropylene, 12 parts of polyethylene, 3 parts of silica sol, and 7 parts of vinyl trichlorosilane. The polypropylene adopts a random polypropylene copolymer, which contains 4% by mass of ethylene molecules, and the ethylene molecules are randomly inserted into the polymer main chain; the concentration of the silica sol is 50%, and the silica sol is a dispersion of nano-scale silica particles in water. In the silica sol, the size of the silica particles is about 10-20nm. The preparation method of the heat-sealing film comprises the following steps: a1, slowly dropping silica sol into vinyl trichlorosilane and performing low-temperature ultrasound for 0.5 h to obtain a mixed suspension, wherein the slow dropping speed is 7 mL / min, the low-temperature ultrasound temperature is 8°C, and the ultrasound frequency is 70 kHz; a2, grinding and stirring polypropylene and polyethylene to melt to form a mixed liquid, and then spraying and granulating the mixed liquid to form composite particles, wherein the grinding and stirring adopts wet grinding, and the solvent is ethanol, and the mass ratio of ethanol to polypropylene is 1:25; the temperature is 8°C, the pressure is 0.4 MPa, and the melting temperature is 185°C; the spray drying temperature of the composite particles is 25°C, the spray speed is 2 mL / min, and the area is 150 cm 2 a3, putting the composite particles into the mixed suspension and stirring them fully, and freeze-drying them to obtain a heat-sealing masterbatch, wherein the stirring speed of the stirring is 400 r / min and the temperature is 8°C; the freeze-drying temperature is -20°C.

[0042] The barrier film adopts a polyvinyl alcohol film modified by nano-layered silicate, and the mass ratio of the barrier film is: 40 parts of polyvinyl alcohol, 17 parts of modified nano-layered silicate, 8 parts of silica sol, and 0.4 parts of trichloromethylsilane; the concentration of the silica sol is 50%, and the silica sol is a dispersion of nano-scale silicon dioxide particles in water. The modified nano-layered silicate adopts silicon-oxygen modified layered nano-montmorillonite, and the preparation method of the modified layered montmorillonite includes the following steps: b1, ethyl cellulose is added to ether and stirred evenly to form a homogeneous liquid, and then trichloromethylsilane is slowly added to form a coating liquid, the concentration of the ethyl cellulose in the ether is 400g / L, the stirring speed for stirring evenly is 400r / min, the speed of slowly adding is 3mL / min, and the mass ratio of the trichloromethylsilane to the methyl cellulose is 1:0.9 b2, the layered nano-montmorillonite is placed in the coating solution and stirred for 25 minutes, filtered and then allowed to stand for 1 hour, and dried to obtain a prefabricated modified layered nano-montmorillonite, the stirring temperature is 8°C, the stirring speed is 400r / min, the standing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 13:1, the temperature is 12°C, and the drying temperature is 8°C; b3, the prefabricated modified layered nano-montmorillonite is allowed to stand for reaction for 2 hours, then placed in ether for ultrasonication for 25 minutes, filtered and dried under reduced pressure to obtain modified layered nano-montmorillonite, the standing reaction atmosphere is a nitrogen atmosphere, the temperature is 65°C; the mass ratio of the prefabricated modified layered nano-montmorillonite to ether is 1:9, the ultrasonic temperature is 8°C, the ultrasonic frequency is 80kHz, the pressure of the reduced pressure drying is 83% of the atmospheric pressure, and the temperature is 30°C.

[0043] The preparation method of the barrier film comprises the following steps: c1, adding trichloromethylsilane to silica sol and performing low-temperature ultrasonic dispersion for 25 minutes to obtain a homogeneous dispersion liquid, wherein the low-temperature temperature of the low-temperature ultrasonic dispersion is 8°C and the ultrasonic frequency is 80kHz; c2, adding polyvinyl alcohol to water and stirring evenly to form a viscous liquid, then adding modified nano-layered silicate and performing low-temperature ultrasonic treatment for 25 minutes to obtain a preliminary mixed liquid, wherein the mass ratio of polyvinyl alcohol to water is 10:13, the stirring speed for uniform stirring is 400r / min, the temperature of the low-temperature ultrasonic treatment is 8°C, and the ultrasonic frequency is 95kHz; c3, dropping the homogeneous dispersion liquid into the preliminary mixed liquid and stirring rapidly for 25 minutes, and freeze-drying to obtain a barrier masterbatch, wherein the dropping speed is 4mL / min, the stirring speed of rapid stirring is 1500r / min, and the temperature is 15°C.

[0044] The mass ratio of the PP-based protective film is: 100 parts of polypropylene, 0.7 parts of nano titanium dioxide, 0.7 parts of antioxidant, 0.7 parts of trichloromethylsilane, 0.6 parts of white carbon black, 0.2 parts of bissebacate, and 0.2 parts of lubricant; the antioxidant is trihydroxynitrile, and the lubricant is zinc stearate. The preparation method of the PP-based protective film comprises the following steps: d1, adding nano titanium dioxide to trichloromethylsilane, stirring, spraying into a reactor, standing at low temperature for 25 minutes, purging to obtain a primary mixture, the stirring speed is 200r / min, the spraying speed is 20mL, the low-temperature standing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor in the mixed atmosphere is 12:1, and the temperature is 8°C; the purging uses nitrogen at 20°C, and the purging speed is 15mL / min; d2, adding dicaprate, an antioxidant and a lubricant to polypropylene for melt mixing to obtain a prefabricated mixed liquid, the melt mixing temperature is 210°C, d3, granulating the prefabricated mixed liquid to form prefabricated particles, and mixing with the primary mixture to obtain a protective film masterbatch; the granulation temperature is 25°C.

[0045] The method for preparing the high barrier PP film comprises the following steps:

[0046] Step 1, placing the heat sealing masterbatch, the barrier masterbatch and the protective film masterbatch into three extruders respectively for melt extrusion and compounding to obtain a composite film, wherein the temperature of the melt extrusion is 240° C.;

[0047] Step 2, stretching the composite film to obtain a high barrier PP film, wherein the stretching temperature of the stretching treatment is 150° C. and the transverse stretching multiple is 7.

[0048] Comparative Example 1

[0049] The comparative example uses a commercially available high-barrier PP film and Huayao Packaging's cast polypropylene food-grade high-barrier packaging roll film.

[0050] Performance Testing

[0051] The products prepared in Examples 1-3 and the samples of Comparative Example 1 were tested for performance, and the results are as follows:

[0052]

[0053] The above data show that the high barrier PP film prepared in the present invention has good oxygen and water vapor barrier properties, which are higher than the commercially available high barrier PP films. At the same time, the high barrier PP film prepared in the present application has good anti-aging properties and meets daily use.

[0054] It is understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.

Claims

1. A method for preparing a high barrier PP film, characterized in that: The high barrier PP film is provided with a PP-based protective film, a barrier film and a heat-sealing film in sequence from the outside to the inside. The thickness of the PP-based protective film is 0.014-0.018 mm, the thickness of the barrier film is 0.011-0.015 mm, and the thickness of the heat-sealing film is 0.065-0.085 mm.

2. The method for preparing a high barrier PP film according to claim 1, characterized in that: The mass ratio of the heat-sealing film includes: 60-70 parts of polypropylene, 10-15 parts of polyethylene, 1-5 parts of silica sol, and 5-8 parts of vinyl trichlorosilane.

3. The method for preparing a high barrier PP film according to claim 2, characterized in that: The polypropylene adopts a random polypropylene copolymer, which contains 3-5% by mass of ethylene molecules, and the ethylene molecules are randomly inserted into the polymer main chain.

4. The method for preparing a high barrier PP film according to claim 2, characterized in that: The concentration of the silica sol is 45-50%. The silica sol is a dispersion of nanometer-sized silicon dioxide particles in water. In the silica sol, the size of the silicon dioxide particles is about 10-20 nm.

5. The method for preparing a high barrier PP film according to claim 1, characterized in that: The barrier film is a nano-layered silicate-modified polyvinyl alcohol film.

6. The method for preparing a high barrier PP film according to claim 5, characterized in that: The mass ratio of the barrier film is: 35-45 parts of polyvinyl alcohol, 15-18 parts of modified nano-layered silicate, 5-10 parts of silica sol, and 0.3-0.5 parts of trichloromethylsilane.

7. The method for preparing a high barrier PP film according to claim 6, characterized in that: The concentration of the silica sol is 45-50%, and the silica sol is a dispersion of nanometer-level silicon dioxide particles in water.

8. The method for preparing a high barrier PP film according to claim 6, characterized in that: The modified nano-layered silicate adopts silicon-oxygen modified layered nano-montmorillonite.

9. The method for preparing a high barrier PP film according to claim 1, characterized in that: The mass ratio of the PP-based protective film is: 100 parts of polypropylene, 0.5-0.8 parts of nano titanium dioxide, 0.5-0.8 parts of antioxidant, 0.5-0.8 parts of trichloromethylsilane, 0.5-0.8 parts of white carbon black, 0.1-0.3 parts of bis(sebacate) ester, and 0.1-0.3 parts of lubricant; the antioxidant is trihydroxynitrile, and the lubricant is zinc stearate.

10. The method for preparing a high barrier PP film according to claim 1, characterized in that: The method for preparing the high barrier PP film comprises the following steps: Step 1, placing the heat sealing masterbatch, the barrier masterbatch and the protective film masterbatch into three extruders respectively for melt extrusion and compounding to obtain a composite film, wherein the temperature of the melt extrusion is 220-250° C.; Step 2, stretching the composite film to obtain a high barrier PP film, wherein the stretching temperature of the stretching treatment is 140-160° C., and the transverse stretching multiple is 6-8.

Citation Information

Patent Citations

  • High-barrier composite film

    CN106883565A

  • Barrier POF thermal shrinkage printing packaging film and preparation method thereof

    CN112590344A

  • Modified polyolefin composite membrane composition, modified polyolefin composite membrane and preparation method and application thereof

    CN112721372A

  • Recyclable polypropylene composite film

    CN212147845U