Sodium-ion battery negative electrode material and preparation method and application thereof

By heat treatment of biomass raw materials, crushing and dispersed spray drying of resin materials, combined with nitrogen and hydrogen reduction and carbonization treatment, high-performance sodium ion battery negative electrode materials are prepared, solving the problem of insufficient performance of existing biomass hard carbon materials, and realizing the High-efficiency and long-life sodium ion battery negative electrode material.

CN118978145APending Publication Date: 2024-11-19三一红象电池有限公司

Patent Information

Application Number
CN202411057020.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The low efficiency and poor cycle performance and rate performance of existing biomass hard carbon materials in sodium ion batteries have hindered their application in industrial industrialization.

Method used

By heat-treating and crushing the biomass raw material, after removal of impurities, dispersing it with the resin material to form a slurry, spray-drying to obtain a carbon-covered material, and then carbonization is performed in a nitrogen-hydrogen mixed atmosphere and in an inactive atmosphere. Prepare high-performance sodium ion battery negative electrode material.

Benefits of technology

The first-time Coulomb efficiency, cycle performance and rate performance of the material have been improved, with the first-time efficiency reaching more than 88%, the capacity retention rate of 500 turns is above 95%, and the first-time charging capacity and 5C rate retention rate have also been significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978145A_ABST
    Figure CN118978145A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of battery materials, and particularly relates to a sodium ion battery negative electrode material and a preparation method and application thereof. According to the preparation method provided by the invention, the biomass raw material is firstly subjected to heat treatment and impurity removal treatment, so that impurities in the biomass raw material can be removed, and the cycle performance of the material is improved; carbon coating and secondary granulation are performed by adopting a resin material, so that the specific surface area of the material can be reduced, and the first effect and dynamic performance of the material are improved; according to the invention, reduction treatment is carried out in a nitrogen-hydrogen mixed atmosphere, then carbonization treatment is carried out in an inactive atmosphere, double-layer structure carbon coating can be realized in cooperation with limitation of treatment time, a bottom coating layer contains more functional groups and can be combined with a hard carbon precursor material more tightly, and a surface coating layer is subjected to reduction treatment, so that the hardness of the hard carbon precursor material is improved. The number of functional groups and defects is reduced; and the material first efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of battery materials, and specifically relates to a sodium ion battery negative electrode material and a preparation method and application thereof. Background Art

[0002] With the growing demand for power and energy storage batteries, the need for low-cost battery technology has become increasingly urgent. Currently, lithium-ion batteries are mainly used, but the scarcity and uneven distribution of lithium resources have gradually become prominent. As an effective supplement to lithium-ion batteries, sodium-ion batteries are increasingly attracting people's attention.

[0003] Due to the low cost and abundance of sodium resources, sodium-ion battery research has made rapid progress in the past decade and has broad prospects in the field of low-cost batteries. One of the main factors hindering the commercialization of sodium-ion batteries is the lack of high-performance negative electrode materials. Hard carbon materials have a high sodium storage capacity because they have more defects and vacancies. At the same time, they have disordered structures and large interlayer spacing, which can achieve rapid insertion and extraction of sodium ions. They are considered to be one of the most promising negative electrode materials for sodium-ion batteries.

[0004] At present, the raw materials used to prepare hard carbon include biomass, asphalt, coal-based, resins, etc. Among them, biomass is an important precursor for preparing hard carbon negative electrode materials due to its wide source, green environmental protection, and low cost. However, the existing hard carbon negative electrode materials using biomass as precursors have high impurity content and high specific surface area, resulting in low first coulomb efficiency and poor cycle performance, and the inherent rate performance advantage is not prominent, which seriously hinders the application of biomass hard carbon negative electrode materials in the industrialization of sodium ion batteries.

[0005] Therefore, how to obtain a hard carbon negative electrode material with high initial efficiency, long cycle life and high rate is an urgent problem to be solved in the field of sodium ion batteries. Summary of the invention

[0006] Therefore, the technical problem to be solved by the present application is to alleviate or overcome the defects of the biomass hard carbon materials in the prior art, such as low first coulombic efficiency, poor cycle performance and rate performance, so as to provide a sodium ion battery negative electrode material and its preparation method and application.

[0007] To this end, this application provides the following technical solutions:

[0008] The present application provides a method for preparing a negative electrode material for a sodium ion battery, comprising the following steps:

[0009] S1, heat-treating the biomass raw material, crushing it, and removing impurities to obtain a hard carbon precursor;

[0010] S2, dispersing the resin material and the hard carbon precursor in water to obtain a slurry, and spray drying to obtain a secondary particle carbon coating material;

[0011] S3, subjecting the carbon-coated material to a reduction treatment in a nitrogen-hydrogen mixed atmosphere for 10 min-60 min, and then subjecting it to a carbonization treatment in an inactive atmosphere for 3 h-7 h, to obtain a negative electrode material for a sodium ion battery.

[0012] In some optional embodiments, the time for reduction treatment in a nitrogen-hydrogen mixed atmosphere is 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, or within the range of any of the above values; the time for carbonization treatment in an inactive atmosphere is 3 h, 4 h, 5 h, 6 h, 7 h, or within the range of any of the above values.

[0013] In some optional embodiments, in step S3, the temperature of the reduction treatment is 500° C.-1000° C.;

[0014] And / or, the temperature of the carbonization treatment is 1200°C-1500°C.

[0015] In some optional embodiments, the temperature of the reduction treatment is 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, or within the range of any of the above values; the temperature of the carbonization treatment is 1200°C, 1250°C, 1300°C, 1400°C, 1480°C, 1500°C, or within the range of any of the above values.

[0016] In some optional embodiments, in step S3, the volume proportion of hydrogen in the nitrogen-hydrogen mixed atmosphere is 3%-10%; for example, the volume proportion of hydrogen can be 3%, 4%, 5%, 6%, 7%, or within the range of any of the above values.

[0017] And / or, the inactive atmosphere includes a nitrogen atmosphere or an inert gas atmosphere.

[0018] In some optional embodiments, in step S1, the impurity removal treatment includes at least one of pickling impurity removal or halogen gas impurity removal;

[0019] And / or, the heat treatment temperature is 300℃-600℃, and the heat treatment time is 1h-5h; in some optional embodiments, the heat treatment temperature is 300℃, 380℃, 400℃, 430℃, 470℃, 500℃, 550℃, 600℃, or within the range of any of the above values; the heat treatment time can be 1h, 2h, 2.5h, 3h, 4h, 5h, or within the range of any of the above values.

[0020] And / or, the material is crushed to an average particle size of 400nm-10μm. In some optional embodiments, the material is crushed to an average particle size of 400nm-700nm, or 5μm-10μm.

[0021] In some optional embodiments, in step S1, the material is crushed to an average particle size of 400nm-700nm; the smaller the particle size of the material, the more conducive it is to the removal of impurities in the material. Considering the difficulty of the crushing process, it is preferred to control the average particle size of the material to 400nm-700nm. This is because crushing the material to the nanoscale can reduce the difficulty of impurity removal and the number of pickling times. The impurity elements can be effectively removed by one pickling, thereby improving the impurity removal effect. If the material particle size is large, multiple picklings are required to remove impurities.

[0022] And / or, the pickling and impurity removal treatment includes using a 1M-5M inorganic acid at a concentration of 40°C-80°C for 1h-3h;

[0023] Optionally, the inorganic acid includes at least one of hydrochloric acid, sulfuric acid, and hydrofluoric acid;

[0024] And / or, the treatment temperature of the hydrogen halide gas impurity removal is 600° C.-1000° C., and the treatment time is 1 h-3 h.

[0025] In some optional embodiments, in step S2, the mass ratio of the resin material to the hard carbon precursor is (1:49)-(3:17);

[0026] And / or, the solid content of the slurry is 15-40wt%.

[0027] In the present application, the biomass raw materials are conventional biomass raw materials known in the art, including but not limited to bamboo, straw, coconut shell, cotton, poplar, reed, etc.

[0028] In the present application, the resin material includes at least one of phenolic resin, epoxy resin, polyester resin and the like.

[0029] In the present application, in the pickling and impurity removal step, the solid-liquid ratio of the acid solution used in each impurity removal process is (1:100)-(1:50).

[0030] The present application also provides a sodium ion battery negative electrode material, which is prepared by the above-mentioned preparation method.

[0031] The present application also provides a negative electrode sheet, comprising:

[0032] a negative electrode current collector, and

[0033] A negative electrode active material layer is disposed on at least one side of the negative electrode current collector, and the negative electrode active material layer includes the above-mentioned sodium ion battery negative electrode material.

[0034] The present application also provides a sodium ion battery, comprising the above-mentioned negative electrode plate.

[0035] The present application also provides an electrical device, comprising the above-mentioned sodium ion battery.

[0036] In the present application, the composition and preparation method of the above-mentioned negative electrode sheet and sodium ion battery are conventional in the field. Generally, a sodium ion battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the battery charging and discharging process, active ions are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, which mainly plays the role of preventing the positive and negative electrodes from short-circuiting, and at the same time allows ions to pass through.

[0037] In some embodiments, the above-mentioned electrical equipment may also include a battery module or battery pack assembled from the above-mentioned sodium ion battery. The sodium ion battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.

[0038] As the electrical device, a sodium ion battery, a battery module or a battery pack can be selected according to its use requirements. As an example of an electrical device, a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc., in order to meet the electrical device's requirements for high power and high energy density of sodium ion batteries, a battery pack or a battery module can be used.

[0039] Another example device may be a mobile phone, a tablet computer, a laptop computer, etc. Such a device is usually required to be thin and light, and a sodium ion battery may be used as a power source.

[0040] The technical solution of this application has the following advantages:

[0041] The preparation method of the negative electrode material of a sodium ion battery provided in the present application comprises the following steps: S1, heat-treating a biomass raw material, crushing it, and removing impurities to obtain a hard carbon precursor; S2, dispersing a resin material and a hard carbon precursor in water to obtain a slurry, and spray-drying it to obtain a carbon-coated material; S3, reducing the carbon-coated material in a nitrogen-hydrogen mixed atmosphere for 10 min-60 min, and then carbonizing it in an inactive atmosphere for 3 h-7 h to obtain a negative electrode material for a sodium ion battery. In the present application, the biomass raw materials are first subjected to heat treatment and impurity removal treatment, which can remove impurities in the biomass raw materials and improve the recycling performance of the material; resin materials are used for carbon coating and secondary granulation, which can reduce the specific surface area of ​​the material and improve the initial efficiency and kinetic performance of the material; by first performing a reduction treatment in a nitrogen-hydrogen mixed atmosphere and then performing a carbonization treatment in an inactive atmosphere, a double-layer carbon coating can be achieved by limiting the treatment time. The bottom coating layer contains more functional groups and can be more closely combined with the hard carbon precursor material. The surface coating layer is reduced to reduce the number of functional groups and defects, thereby improving the initial efficiency of the material.

[0042] The preparation method of the negative electrode material for a sodium ion battery provided in the present application crushes the material to the nanometer level before removing impurities, which can reduce the difficulty of impurity removal, reduce the number of acid washing times, improve the impurity removal effect, and further improve the material cycle performance.

[0043] The sodium ion battery provided in the present application adopts the sodium ion battery negative electrode material prepared by the above method as the negative electrode active material, so that the sodium ion battery exhibits good kinetic performance and cycle performance and high first efficiency. The assembled CR2032 button-type sodium ion battery is tested, and the first efficiency can reach more than 88%, and the 500-cycle capacity retention rate is more than 95%. At the same time, the first charge capacity and 5C rate retention rate are also much better than those of the comparative example. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0045] Figure 1 It is a process flow chart of the preparation process of the negative electrode material of the sodium ion battery in the embodiment of the present application. DETAILED DESCRIPTION

[0046] The following examples are provided for a better understanding of the present application, but are not limited to the best implementation mode described, and do not limit the content and protection scope of the present application. Any product identical or similar to the present application obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the protection scope of the present application.

[0047] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0048] Example 1

[0049] This embodiment provides a sodium ion battery negative electrode material, and its preparation process flow chart is as follows Figure 1 The specific steps and operation parameters are as follows:

[0050] (1) The bamboo was heat treated at 500°C for 3 h, and then crushed in a jet mill to an average particle size of 550 nm. The nano-scale biomass particles were treated with 3M hydrochloric acid at 60°C for 3 h with a solid-liquid ratio of 1:70 to remove impurities in the material and obtain a hard carbon precursor;

[0051] (2) 10 parts of epoxy resin (manufacturer Wengjiang reagent, model hyperbranched epoxy resin) and 90 parts of hard carbon precursor were mixed and water was added to form a slurry with a solid content of 30 wt%, which was then spray-dried to obtain carbon-coated secondary particles with an average particle size of 10 μm;

[0052] (3) The carbon-coated secondary particles were reduced at 800°C for 30 min in a nitrogen-hydrogen mixed gas atmosphere (hydrogen volume percentage is 5%), and then heated to 1400°C for carbonization treatment for 5 h in a pure nitrogen atmosphere to obtain the final sodium ion battery negative electrode material.

[0053] Example 2

[0054] This embodiment provides a sodium ion battery negative electrode material, and its preparation process flow chart is as follows Figure 1 The specific steps and operation parameters are as follows:

[0055] (1) The bamboo was heat treated at 300°C for 1 h, and then crushed in a jet mill to an average particle size of 400 nm. The nano-scale biomass particles were treated with 1M hydrochloric acid at 40°C for 1 h with a solid-liquid ratio of 1:100 to remove impurities in the material and obtain a hard carbon precursor;

[0056] (2) 5 parts of resin (manufacturer Wengjiang reagent, model hyperbranched epoxy resin) and 95 parts of hard carbon precursor were mixed and water was added to form a slurry with a solid content of 15 wt%, which was then spray-dried to obtain carbon-coated secondary particles with an average particle size of 5 μm;

[0057] (3) The carbon-coated secondary particles were reduced at 500°C for 10 min in a nitrogen-hydrogen mixed gas atmosphere (hydrogen volume percentage is 3%), and then heated to 1200°C for carbonization treatment for 3 h in a pure nitrogen atmosphere to obtain the final sodium ion battery negative electrode material.

[0058] Example 3

[0059] This embodiment provides a sodium ion battery negative electrode material, and its preparation process flow chart is as follows Figure 1 The specific steps and operation parameters are as follows:

[0060] (1) The bamboo was heat treated at 600°C for 5 h, and then crushed in a jet mill to an average particle size of 700 nm. The nano-scale biomass particles were treated with 5M hydrochloric acid at 80°C for 3 h with a solid-liquid ratio of 1:50 to remove impurities in the material and obtain a hard carbon precursor;

[0061] (2) 15 parts of resin (manufacturer Wengjiang reagent, model hyperbranched epoxy resin) and 85 parts of hard carbon precursor were mixed and water was added to form a slurry with a solid content of 40 wt%, which was then spray-dried to obtain carbon-coated secondary particles with an average particle size of 15 μm;

[0062] (3) The carbon-coated secondary particles were reduced at 1000°C for 60 min in a nitrogen-hydrogen mixed gas atmosphere (hydrogen volume ratio is 10%), and then heated to 1500°C for carbonization treatment for 7 h in a pure nitrogen atmosphere to obtain the final sodium ion battery negative electrode material.

[0063] Example 4

[0064] This embodiment provides a sodium ion battery negative electrode material, and its preparation process flow chart is as follows Figure 1 The specific steps and operation parameters are as follows:

[0065] (1) The corn stalks were heat treated at 500°C for 3 h, and then crushed in a jet mill to an average particle size of 550 nm. The nano-scale biomass particles were treated with 3M hydrochloric acid at 60°C for 3 h with a solid-liquid ratio of 1:70 to remove impurities in the material and obtain a hard carbon precursor;

[0066] (2) 10 parts of phenolic resin (manufacturer Wengjiang reagent, model PC80091) and 90 parts of hard carbon precursor were mixed and water was added to form a slurry with a solid content of 30 wt%, which was then spray-dried to obtain carbon-coated secondary particles with an average particle size of 10 μm;

[0067] (3) The carbon-coated secondary particles were reduced at 800°C for 30 min in a nitrogen-hydrogen mixed gas atmosphere (hydrogen volume percentage is 5%), and then heated to 1400°C for carbonization treatment for 5 h in a pure nitrogen atmosphere to obtain the final sodium ion battery negative electrode material.

[0068] Example 5

[0069] This embodiment provides a sodium ion battery negative electrode material, and its preparation process flow chart is as follows Figure 1 The specific steps and operation parameters are as follows:

[0070] (1) The bamboo was heat treated at 500°C for 3 h, and then crushed in a jet mill to an average particle size of 900 nm. The nano-scale carbon particles were treated with 3M hydrochloric acid at 60°C for 3 h with a solid-liquid ratio of 1:70. The acid washing step was repeated 3 times to remove impurities in the material to obtain a hard carbon precursor.

[0071] (2) 10 parts of epoxy resin (manufacturer Wengjiang reagent, model hyperbranched epoxy resin) and 90 parts of hard carbon precursor were mixed and water was added to form a slurry with a solid content of 30 wt%, which was then spray-dried to obtain carbon-coated secondary particles with an average particle size of 10 μm;

[0072] (3) The carbon-coated secondary particles were reduced at 800°C for 30 min in a nitrogen-hydrogen mixed gas atmosphere (hydrogen volume percentage is 5%), and then heated to 1400°C for carbonization treatment for 5 h in a pure nitrogen atmosphere to obtain the final sodium ion battery negative electrode material.

[0073] Comparative Example 1

[0074] This comparative example provides a sodium ion battery negative electrode material, and the specific steps and operating parameters are as follows:

[0075] (1) The bamboo was heat treated at 300°C for 1 h, and then crushed in a jet mill to an average particle size of 400 nm. The nano-scale biomass particles were treated with 1M hydrochloric acid at 40°C for 1 h with a solid-liquid ratio of 1:100 to remove impurities in the material and obtain a hard carbon precursor;

[0076] (2) 5 parts of resin (manufacturer Wengjiang reagent, model hyperbranched epoxy resin) and 95 parts of hard carbon precursor were mixed and water was added to form a slurry with a solid content of 15 wt%, which was then spray-dried to obtain carbon-coated secondary particles with an average particle size of 5 μm;

[0077] (3) The carbon-coated secondary particles were reduced at 500°C for 120 min in a nitrogen-hydrogen mixed gas atmosphere (hydrogen accounting for 3% by volume), and then heated to 1200°C for carbonization treatment for 9 h in a pure nitrogen atmosphere to obtain the final sodium ion battery negative electrode material.

[0078] Comparative Example 2

[0079] This comparative example provides a sodium ion battery negative electrode material, and the specific steps and operating parameters are as follows:

[0080] (1) The bamboo was heat treated at 300°C for 1 h, and then crushed in a jet mill to an average particle size of 400 nm. The nano-scale biomass particles were treated with 1M hydrochloric acid at 40°C for 1 h with a solid-liquid ratio of 1:100 to remove impurities in the material and obtain a hard carbon precursor;

[0081] (2) 5 parts of resin (manufacturer Wengjiang reagent, model hyperbranched epoxy resin) and 95 parts of hard carbon precursor were mixed and water was added to form a slurry with a solid content of 15 wt%, which was then spray-dried to obtain carbon-coated secondary particles with an average particle size of 5 μm;

[0082] (3) The carbon-coated secondary particles were reduced at 500°C for 5 min in a nitrogen-hydrogen mixed gas atmosphere (hydrogen volume percentage is 3%), and then heated to 1200°C for carbonization treatment for 1 h in a pure nitrogen atmosphere to obtain the final sodium ion battery negative electrode material.

[0083] Comparative Example 3

[0084] This comparative example provides a sodium ion battery negative electrode material, and the specific steps and operating parameters are as follows:

[0085] (1) The bamboo was heat treated at 300°C for 1 h, and then crushed in a jet mill to an average particle size of 400 nm. The nano-scale biomass particles were treated with 1M hydrochloric acid at 40°C for 1 h with a solid-liquid ratio of 1:100 to remove impurities in the material and obtain a hard carbon precursor;

[0086] (2) 5 parts of resin (manufacturer Wengjiang reagent, model hyperbranched epoxy resin) and 95 parts of hard carbon precursor were mixed and water was added to form a slurry with a solid content of 15 wt%, which was then spray-dried to obtain carbon-coated secondary particles with an average particle size of 5 μm;

[0087] (3) The carbon-coated secondary particles were heat treated at 500°C for 10 min in a pure nitrogen atmosphere, and then heated to 1200°C for carbonization treatment for 3 h in a pure nitrogen atmosphere to obtain the final sodium ion battery negative electrode material.

[0088] Comparative Example 4

[0089] This comparative example provides a sodium ion battery negative electrode material, and the specific steps and operating parameters are as follows:

[0090] (1) The bamboo was heat treated at 300°C for 1 h, and then crushed in a jet mill to an average particle size of 400 nm. The nano-scale biomass particles were treated with 1M hydrochloric acid at 40°C for 1 h with a solid-liquid ratio of 1:100 to remove impurities in the material and obtain a hard carbon precursor;

[0091] (2) 5 parts of resin (manufacturer Wengjiang reagent, model hyperbranched epoxy resin) and 95 parts of hard carbon precursor were mixed and water was added to form a slurry with a solid content of 15 wt%, which was then spray-dried to obtain carbon-coated secondary particles with an average particle size of 5 μm;

[0092] (3) The carbon-coated secondary particles were reduced at 500°C for 10 min in a nitrogen-hydrogen mixture (3% by volume) atmosphere, and then heated to 1200°C for reduction for 3 h in a nitrogen-hydrogen mixture (3% by volume) atmosphere to obtain the final sodium ion battery negative electrode material.

[0093] Test Case

[0094] The sodium ion battery negative electrode materials provided in each embodiment and comparative example were assembled into button batteries, and the electrical performance test was performed. The assembly method of the button batteries is as follows:

[0095] The sodium ion battery negative electrode material prepared in the embodiment or comparative example, the conductive agent Ketjen black, the binder sodium carboxymethyl cellulose, styrene butadiene rubber, and water were mixed in a mass ratio of 94:1.5:1.5:3:100 to obtain a slurry, and then the slurry was coated on an aluminum foil, and after drying and rolling, a surface density of 6 mg / cm 2 , compacted density is 1mg / cm 3 The sodium ion battery hard carbon negative electrode uses a sodium sheet as the counter electrode, glass fiber as the diaphragm, and the electrolyte solute is 1moL / L NaPF 6 The solvent was composed of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1, and CR2032 button-type sodium-ion batteries were assembled in an argon-filled glove box.

[0096] Performance Test:

[0097] (1) First effect and gram capacity

[0098] The test temperature is 25℃, discharge to 0.001V at 0.1C constant current, let stand for 5 minutes, charge to 1.5V at 0.1C constant current, first effect = charging capacity of this cycle / discharging capacity of this cycle × 100%, gram capacity is the gram capacity of this cycle, 1C = 350mAh.

[0099] (2) Cycle test

[0100] The test temperature is 25℃, discharge at 0.5C constant current to 0.001V, let stand for 5min, charge at 0.5C constant current to 1.5V, let stand for 5min, and perform discharge-charge cycle, capacity retention rate = nth cycle charging capacity / first cycle charging capacity × 100%, 1C = 350mAh.

[0101] (3) Ratio test

[0102] Test temperature 25℃, discharge to 0.001V at 0.1C constant current, stand for 5min, charge to 1.5V at 0.1C constant current, stand for 5min, discharge to 0.001V at 0.2C constant current, stand for 5min, charge to 1.5V at 0.2C constant current, stand for 5min, discharge to 0.001V at 0.5C constant current, stand for 5min, charge to 1.5V at 0.5C constant current, stand for 5min, discharge to 0.001V, let stand for 5min, charge to 1.5V with 1C constant current, let stand for 5min, discharge to 0.001V with 2C constant current, let stand for 5min, charge to 1.5V with 2C constant current, let stand for 5min, discharge to 0.001V with 5C constant current, let stand for 5min, charge to 1.5V with 5C constant current, let stand for 5min, rate retention rate = nC charging capacity / 0.1C charging capacity × 100%, 1C = 350mAh.

[0103] The test results are shown in the table below.

[0104] Table 1

[0105]

[0106]

[0107] From the comparison between the embodiments and the comparative examples in the above table, it can be seen that good kinetic performance, cycle performance and higher first efficiency can be achieved through a specific double-layer carbon coating process; from the data comparison between Example 5 and Example 1, it can be seen that by adjusting the particle size of the material after crushing, better impurity removal effect, gram capacity and kinetic performance can be achieved; in Comparative Examples 1 and 4 relative to Example 2, the oxygen-containing functional groups in the carbon coating layer are basically completely reduced by hydrogen, and the next coating layer is loosely combined with the carbon substrate, resulting in poor gram capacity, cycle performance and rate performance; in Comparative Examples 2 and 3 relative to Example 2, the surface layer also has more oxygen-containing functional groups, and more active sodium is consumed during the first charge and discharge process, reducing the first efficiency and cycle performance.

[0108] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A method for preparing a negative electrode material for a sodium ion battery, characterized in that: The steps include: S1, heat-treating the biomass raw material, crushing it, and removing impurities to obtain a hard carbon precursor; S2, dispersing the resin material and the hard carbon precursor into water to obtain a slurry, and spray drying to obtain a carbon-coated material; S3, subjecting the carbon-coated material to a reduction treatment in a nitrogen-hydrogen mixed atmosphere for 10 min-60 min, and then subjecting it to a carbonization treatment in an inactive atmosphere for 3 h-7 h, to obtain a negative electrode material for a sodium ion battery.

2. The method for preparing a negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step S3, the temperature of the reduction treatment is 500°C-1000°C; And / or, the temperature of the carbonization treatment is 1200°C-1500°C.

3. The method for preparing a negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step S3, the volume proportion of hydrogen in the nitrogen-hydrogen mixed atmosphere is 3%-10%; And / or, the inactive atmosphere includes a nitrogen atmosphere or an inert gas atmosphere.

4. The method for preparing a negative electrode material for a sodium ion battery according to any one of claims 1 to 3, characterized in that: In step S1, the impurity removal treatment includes at least one of pickling impurity removal or halogen gas impurity removal; And / or, the heat treatment temperature is 300°C-600°C, and the heat treatment time is 1h-5h; And / or, the material is crushed to have an average particle size of 400 nm-10 μm.

5. The method for preparing a negative electrode material for a sodium ion battery according to claim 4, characterized in that: In step S1, the material is crushed to an average particle size of 400nm-700nm; And / or, the pickling and impurity removal treatment includes using a 1M-5M inorganic acid at a concentration of 40°C-80°C for 1h-3h; Optionally, the inorganic acid includes at least one of hydrochloric acid, sulfuric acid, and hydrofluoric acid; And / or, the treatment temperature of the hydrogen halide gas impurity removal is 600-1000° C., and the treatment time is 1-3 hours.

6. The method for preparing a negative electrode material for a sodium ion battery according to any one of claims 1 to 5, characterized in that: In step S2, the mass ratio of the resin material to the hard carbon precursor is (1:49)-(3:17); And / or, the solid content of the slurry is 15wt%-40wt%.

7. A sodium ion battery negative electrode material, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 6.

8. A negative electrode plate, characterized in that: include: a negative electrode current collector, and A negative electrode active material layer is disposed on at least one side of the negative electrode current collector, and the negative electrode active material layer comprises the sodium ion battery negative electrode material according to claim 7.

9. A sodium ion battery, characterized in that: Including the negative electrode sheet as described in claim 8.

10. An electrical device, characterized in that: Including the sodium ion battery as described in claim 9.

Citation Information

Patent Citations

  • Hard carbon material for power and energy-storage battery and preparation method thereof

    CN101916845A

  • Sodium-ion battery core-shell structure bagasse hard carbon-based negative electrode material and preparation method thereof

    CN116332152A

  • Preparation method of high-capacity hard carbon negative electrode material for sodium ion battery

    CN117374276A

  • Preparation method of hard carbon negative electrode material of sodium ion battery

    CN117466276A

  • Environment-friendly high-cycling-stability biomass hard carbon negative electrode material for sodium-ion battery and preparation method of green environment-friendly high-cycling-stability biomass hard carbon negative electrode material

    CN117509609A

Cited By

  • Composite graphite material, preparation method thereof, negative electrode and battery