Fluorine-containing carbon-based two-dimensional flaky material as well as preparation method and application thereof
By adding fluorine elements to the preparation of graphene materials, the surface potential energy is reduced and the stability is improved, and the problem of poor dispersion and aging in the solvent is solved, and efficient and stable graphene materials are achieved, which is suitable for large-scale production. and high-performance applications.
Patent Information
- Application Number
- CN202410864421.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-30
- Publication Date
- 2024-11-19
AI Technical Summary
Due to the high surface potential energy of graphene materials, it is difficult to disperse in solvents, easily agglomerate, and is not resistant to ultraviolet and infrared light excitation, and has poor aging. The existing improvement methods have defects and are difficult to meet the needs of large-scale production and high-performance.
Using the preparation method of carbon-based two-dimensional sheet-like material with fluorine-containing elements, the preparation is prepared by adding graphene oxide powder, KH-570 and perfluorooctanate to deionized water, stirring, grinding and centrifuging in a three-roller machine, and finally drying in a vacuum. Graphene material with low surface potential energy is produced to improve its solubility and stability in solvents.
This method simplifies the preparation process of graphene materials, reduces production difficulty, and improves production efficiency. The material has high fluorine content and low potential energy, reduces agglomeration, enhances stability and corrosion resistance, and is suitable for large-scale production and It is used in nanocomposite materials and conductive coatings and other fields.
Smart Images

Figure CN118978152A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of material technology, and mainly relates to a carbon-based two-dimensional sheet material containing fluorine elements, and a preparation method and application thereof. Background Art
[0002] Two-dimensional graphene sheet material is an excellent interface material with thermal conductivity, electrical conductivity and wave absorption properties. Adding graphene to many engineering coatings can improve the required performance. At the same time, the large specific surface area and reactivity of graphene give it good modification ability, thereby expanding the scope of graphene application.
[0003] However, there are still many problems with graphene materials. Due to its high surface potential energy, it cannot be well dispersed in the solvent and is prone to agglomeration. In addition, in the environment, graphene materials are easily excited by ultraviolet and infrared light, resulting in electronic transitions, and are therefore not resistant to aging.
[0004] In order to better solve this kind of problem, two methods are currently used to improve it. First, due to the self-aggregation characteristics of graphene, in order to better prepare a complete graphene film, we use the intercalation method to combine with the material to achieve the purpose of heat transfer and conductivity. Secondly, the graphene is modified to reduce the surface potential energy so that it can be better soluble in the solution. However, no matter which of the above two methods is used, there are corresponding defects, so it is very necessary to find a better method for graphene modification and application. Summary of the invention
[0005] Technical problem to be solved: The present invention provides a carbon-based two-dimensional sheet material containing fluorine elements and its preparation method and application, so that it has lower surface potential energy than before modification, is better dissolved in solvents, and reduces graphene agglomeration. The preparation process is safe and pollution-free, which is conducive to large-scale production.
[0006] Technical solution: A method for preparing a carbon-based two-dimensional sheet material containing fluorine elements, the preparation steps are as follows: a. Using deionized water as a solvent, add 0.1-0.6g of graphene oxide powder to 200mL of deionized water, and stir to obtain a black viscous solution; b. Add 0.01-0.5g of KH-570 in step a, and stir to dissolve; c. Add 0.2-1g of ammonium perfluorooctanoate in step b, set the temperature to 60-90°C, and stir to obtain a uniform and stable colloidal solution; d. Pour the solution in step c into a three-roll mill, grind evenly to obtain a homogenate, put it into a centrifuge, and centrifuge and wash; e. Put the washed material in step d into a vacuum drying oven, vacuum dry it, and obtain the final powder product.
[0007] Preferably, the added amount of the above-mentioned graphene oxide powder is 0.1g.
[0008] Preferably, the amount of KH-570 added is 0.2 g.
[0009] Preferably, the amount of ammonium perfluorooctanoate added is 0.5 g.
[0010] The carbon-based two-dimensional sheet material containing fluorine element obtained by the above preparation method.
[0011] The above-mentioned carbon-based two-dimensional sheet material containing fluorine elements is used in the manufacture of wave-absorbing and heat-conducting interface materials.
[0012] The wave-absorbing and heat-conducting interface material is prepared from the above-mentioned carbon-based two-dimensional sheet material containing fluorine elements.
[0013] Beneficial effects: In the process of preparing graphene materials, we found that the process is simple and easy to operate, which not only reduces the technical difficulty of production, but also provides the possibility for large-scale quantitative production. The simplicity of this preparation method significantly improves the production efficiency of graphene, which helps to meet the large-scale demand for this high-performance material in the market. At the same time, the prepared graphene material has a high fluorine content, which brings it excellent performance, such as enhanced material stability and corrosion resistance. In addition, this graphene material also has the characteristics of low potential energy, which means that during storage and use, its intermolecular interactions are weak, so the material is not easy to agglomerate. This advantage is crucial to maintaining the dispersibility and application performance of graphene, especially in occasions where highly dispersed and stable graphene is required, such as nanocomposites, conductive coatings and other fields. In general, this preparation method is not only simple and easy, suitable for large-scale production, but also the resulting graphene material has a high fluorine content, low potential energy, and is not easy to agglomerate, and has extremely high practical value and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 : Infrared image of graphite powder after preparation in Example 2.
[0015] Figure 2 : The change of fluorine content in the graphite powder after washing after the preparation in Example 2 is completed.
[0016] Figure 3 : Physical display of graphene powder prepared in Example 2;
[0017] Figure 4 : A microscopic schematic diagram of the graphene powder prepared in Example 2. DETAILED DESCRIPTION
[0018] The present invention will be further described below in conjunction with specific embodiments.It should be noted that each of the following embodiments is exemplary, and is not intended to limit the scope of the present invention.After reading content of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the claims of the present application equally.
[0019] Test conditions:
[0020] 1. Test the structural changes of samples by Fourier infrared spectroscopy;
[0021] 2. Use spectrophotometry to test the fluorine content in the solvent.
[0022] Embodiment 1:
[0023] With deionized water as solvent, 0.01 graphene oxide powder is added to 200 mL of deionized water, the stirring temperature is 40° C., and the mixture is stirred for 30 minutes to obtain a black viscous solution; then 0.2 g of KH-570 is added and the mixture is stirred for 30 minutes to dissolve the mixture; in step c, 0.2 g of ammonium perfluorooctanoate particles is added to the above solution, the temperature is set to 70° C., and the mixture is stirred for 30 minutes to obtain a uniform and stable colloidal solution; the solution is poured into a three-roll mill, uniformly ground to obtain a homogenate, and the mixture is put into a centrifuge for centrifugal washing at a centrifugal speed of 10000 r / min; finally, the washed material is put into a vacuum drying oven for vacuum drying to obtain a final powder product.
[0024] Embodiment 2:
[0025] With deionized water as solvent, 0.1 g of graphene oxide powder is added to 200 mL of deionized water, the stirring temperature is 40° C., and the mixture is stirred for 30 min to obtain a black viscous solution; then 0.2 g of KH-570 is added and the mixture is stirred for 30 min to dissolve the mixture; in step c, 0.2 g of ammonium perfluorooctanoate particles is added to the above solution, the temperature is set to 70° C., and the mixture is stirred for 30 min to obtain a uniform and stable colloidal solution; the solution is poured into a three-roll mill, uniformly ground to obtain a homogenate, and the mixture is put into a centrifuge for centrifugal washing at a centrifugal speed of 7500 r / min; finally, the washed material is put into a vacuum drying oven for vacuum drying to obtain a final powder product.
[0026] Embodiment 3:
[0027] With deionized water as solvent, 0.6 g of graphene oxide powder is added to 200 mL of deionized water, the stirring temperature is 40° C., and the mixture is stirred for 30 min to obtain a black viscous solution; then 0.2 g of KH-570 is added and the mixture is stirred for 30 min to dissolve the mixture; in step c, 0.2 g of ammonium perfluorooctanoate particles is added to the above solution, the temperature is set to 70° C., and the mixture is stirred for 30 min to obtain a uniform and stable colloidal solution; the solution is poured into a three-roll mill, uniformly ground to obtain a homogenate, and the mixture is put into a centrifuge for centrifugal washing at a centrifugal speed of 10,000 r / min; finally, the washed material is put into a vacuum drying oven for vacuum drying to obtain a final powder product.
[0028] In Examples 1 to 3, we used the mass of graphene oxide powder as a variable to prepare a carbon-based two-dimensional sheet material containing fluorine element to obtain the mass of graphene oxide powder for preparing graphite micropowder. A carbon-based two-dimensional sheet material containing fluorine element was prepared according to the above preparation method using graphene powders with masses of 0.01g, 0.1g and 0.5g.
[0029] The experimental results are summarized as follows:
[0030]
[0031] Embodiment 4:
[0032] With deionized water as solvent, 0.1 g of graphene oxide powder is added to 200 mL of deionized water, the stirring temperature is 40° C., and the mixture is stirred for 30 min to obtain a black viscous solution; then 0.005 g of KH-570 is added and stirred for 30 min to dissolve it; in step c, 0.2 g of ammonium perfluorooctanoate particles is added to the above solution, the temperature is set to 70° C., and the mixture is stirred for 30 min to obtain a uniform and stable colloidal solution; the solution is poured into a three-roll mill, uniformly ground to obtain a homogenate, and the slurry is placed in a centrifuge for centrifugal washing at a centrifugal speed of 10,000 r / min; finally, the washed material is placed in a vacuum drying oven for vacuum drying to obtain a final powder product.
[0033] Embodiment 5:
[0034] With deionized water as solvent, 0.1 g of graphene oxide powder is added to 200 mL of deionized water, the stirring temperature is 40° C., and the mixture is stirred for 30 min to obtain a black viscous solution; then 0.7 g of KH-570 is added and the mixture is stirred for 30 min to dissolve the mixture; in step c, 0.2 g of ammonium perfluorooctanoate particles is added to the above solution, the temperature is set to 70° C., and the mixture is stirred for 30 min to obtain a uniform and stable colloidal solution; the solution is poured into a three-roll mill, uniformly ground to obtain a homogenate, and the mixture is put into a centrifuge for centrifugal washing at a centrifugal speed of 10,000 r / min; finally, the washed material is put into a vacuum drying oven for vacuum drying to obtain a final powder product.
[0035] In Examples 2, 4, and 5, we used the mass of KH-570 as a variable to prepare a carbon-based two-dimensional sheet material containing fluorine elements to obtain the optimal mass of KH-570 for preparing graphite micropowder. A carbon-based two-dimensional sheet material containing fluorine elements was prepared according to the above preparation method using KH-570 with masses of 0.01 g, 0.2 g, and 0.5 g.
[0036] The experimental results are summarized as follows:
[0037]
[0038] Embodiment 6:
[0039] With deionized water as solvent, 0.1 g of graphene oxide powder is added to 200 mL of deionized water, the stirring temperature is 40° C., and the mixture is stirred for 30 min to obtain a black viscous solution; then 0.1 g of KH-570 is added and stirred for 30 min to dissolve it; in step c, 0.02 g of ammonium perfluorooctanoate particles are added to the above solution, the temperature is set to 70° C., and the mixture is stirred for 30 min to obtain a uniform and stable colloidal solution; the solution is poured into a three-roll mill, uniformly ground to obtain a homogenate, and the slurry is placed in a centrifuge for centrifugal washing at a centrifugal speed of 10,000 r / min. Finally, the washed material is placed in a vacuum drying oven for vacuum drying to obtain a final powder product.
[0040] Embodiment 7:
[0041] With deionized water as solvent, 0.1 g of graphene oxide powder is added to 200 mL of deionized water, the stirring temperature is 40° C., and the mixture is stirred for 30 min to obtain a black viscous solution; then 0.2 g of KH-57 is added and the mixture is stirred for 30 min to dissolve the mixture; in step c, 1.1 g of ammonium perfluorooctanoate particles is added to the above solution, the temperature is set to 70° C., and the mixture is stirred for 30 min to obtain a uniform and stable colloidal solution; the solution is poured into a three-roll mill, uniformly ground to obtain a homogenate, and the mixture is put into a centrifuge for centrifugal washing at a centrifugal speed of 7500 r / min; finally, the washed material is put into a vacuum drying oven for vacuum drying to obtain a final powder product.
[0042] In Examples 2, 6, and 7, we used the mass of ammonium perfluorooctanoate as a variable to prepare a carbon-based two-dimensional sheet material containing fluorine elements to obtain the mass of the optimal ammonium perfluorooctanoate powder for preparing fluorine-containing graphene. A carbon-based two-dimensional sheet material containing fluorine elements was prepared according to the above preparation method using KH-570 with masses of 0.08g, 0.5g, and 2g.
[0043] The experimental results are summarized as follows:
[0044]
Claims
1. A method for preparing a carbon-based two-dimensional sheet material containing fluorine, characterized in that: The preparation steps are as follows: a. using deionized water as solvent, adding 0.1-0.6 g of graphene oxide powder to 200 mL of deionized water, and stirring to obtain a black viscous solution; b. adding 0.01-0.5 g of KH-570 to step a, and stirring to dissolve; c. Add 0.2-1 g of ammonium perfluorooctanoate in step b, set the temperature to 60-90°C, and stir to obtain a uniform and stable colloidal solution; d. Pour the solution in step c into a three-roll mill, grind evenly to obtain a homogenate, put it into a centrifuge, and centrifuge and wash; e. Place the washed material in step d into a vacuum drying oven and vacuum dry to obtain a final powder product.
2. The method for preparing a fluorine-based carbon-based two-dimensional sheet material according to claim 1, characterized in that: The added amount of the graphene oxide powder is 0.1 g.
3. The method for preparing a fluorine-based carbon-based two-dimensional sheet material according to claim 1, characterized in that: The added amount of KH-570 is 0.2 g.
4. The method for preparing a fluorine-based carbon-based two-dimensional sheet material according to claim 1, characterized in that: The amount of ammonium perfluorooctanoate added is 0.5 g.
5. A carbon-based two-dimensional sheet material containing fluorine element obtained by the preparation method according to any one of claims 1 to 4.
6. Use of the fluorine-containing carbon-based two-dimensional sheet material according to claim 5 in the manufacture of wave-absorbing and heat-conducting interface materials.
7. Wave absorbing and thermally conductive interface material, characterized in that: It is made from the carbon-based two-dimensional sheet material containing fluorine element as described in claim 5.
Citation Information
Patent Citations
Fluorine-containing surfactant modified graphene preparation method for electrode of electric double-layer capacitor
CN102693843A
Preparation method of dodecafluoroheptyl-propyl-POSS modified graphene oxide
CN104477904A
Preparation method of graphene modified polymer composite material
CN112852076A
Preparation method for perfluorotriethylamine group-based highly thermally conductive and lubricating nanofluid
WO2020052293A1
Preparation method for graphene-based modifier, heavily-shielded network cable material containing graphene-based modifier