Colored glaze and firing method thereof
Through the specific composition of the black color glaze and the shuttle kiln firing method, the problem of low maturity of the black color glaze in the existing technology is solved, and the glaze surface shows a rich and bright colorful effect under light refraction, which is in line with the East. The "mysterious color" expression of artistic thought.
Patent Information
- Application Number
- CN202411068550.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The existing technology is difficult to effectively produce deep, mysterious and colorful black glaze, and its maturity is low, making it difficult to show a clear layered and rich color effect under light refraction.
It uses potassium feldspar, quartz powder, calcium carbonate, black mud, wood ash, yellow sand soil, white soil, soybean pole ash, agate, zirconium silicate, titanium oxide, blue and white materials, five flower soil, rice washing water, and oxidation The glaze composed of zinc, sodium silicate and glass powder is controlled through the shuttle kiln firing method to control the kiln’s mild air pressure to form a glaze surface with unique colors.
It realizes that the glaze surface shows a rich, bright and colorful effect under light refraction, and has the brilliant colors generated by the difference in temperature coefficients at high temperatures. The glaze color is rich in layers and crystal clear, which is in line with the "mysterious color" expression of oriental artistic thought.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pottery making, and in particular to a black-colored glaze and a firing method thereof. Background Art
[0002] Pottery, an ancient handicraft, is derived from human wisdom in using natural materials. It is carefully shaped from clay or pottery, and after being baptized by fire, it turns mud into treasure and becomes an indispensable tool in life. Over time, pottery making skills, like civilization itself, have evolved from simple to sophisticated. Craftsmen have not only mastered more complex molding techniques, but also invented glaze, a magical substance that, when covered on the surface of the pottery and then calcined at high temperature, can form a dense glassy layer, greatly improving the practicality and ornamental value of pottery.
[0003] The application of glaze is not only a technological breakthrough, but also a reflection of aesthetic pursuit. It makes the surface of pottery smooth and delicate, easy to clean, and also provides artists with a new creative medium. Faced with consumers' increasing aesthetic needs and personalized pursuits, the ceramic industry has set off a wave of innovation in recent years. Ceramics masters and scientific researchers work together to develop new glaze formulas, explore unprecedented artistic effects, and strive to make every ceramic work a unique art treasure. They draw inspiration from nature, trying to capture the colorful light and shadow of sunrise and sunset, the rich colors of the changing seasons, and the magnificent textures of mountains, rivers, lakes and seas, and integrate them into the glaze, so that the ceramic surface presents an unpredictable visual feast.
[0004] However, in this journey of pursuing the ultimate beauty, there is a special skill called "Xuancai glaze", which is still like an insurmountable peak, challenging the wisdom and patience of countless potters. Xuancai glaze, as the name suggests, pursues a deep, mysterious and colorful effect. It requires the glaze surface to show a fantasy scene with distinct layers and rich colors under the refraction of light, as if the stars in the universe and the dreamland are solidified on the ceramics. This glaze color not only tests the scientific ratio of the glaze itself, but also requires precise control of the firing temperature and time. Any slight deviation may greatly reduce the effect.
[0005] Although many ceramic artists have invested a lot of time and energy, tried countless glaze combinations, and adjusted firing parameters countless times, the maturity of Xuancai glaze skills is still not high. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a black-colored glaze and a firing method thereof.
[0007] In order to solve the above technical problems, the technical solution of the present invention is:
[0008] A black colored glaze, which is composed of the following components in percentage by weight:
[0009] Potassium feldspar 25.2-30.8%, quartz powder 8.1-9.9%, calcium carbonate 8.1-9.9%, black mud 4.5-5.5%, wood ash 4.5-5.5%, yellow sand soil 5.4-6.6%, white mud 8.1-9.9%, soybean straw ash 2.7-3.3%, agate 2.7-3.3%, zirconium silicate 2.7-3.3%, titanium oxide 2.7-3.3%, blue and white material 0.9-1.1%, five-color soil 5.4-6.6%, rice water 2.7-3.3%, zinc oxide 2.7-3.3%, sodium silicate 0.72-0.88%, glass powder 2.88-3.52%.
[0010] Preferably, it consists of the following components in weight percentage:
[0011] The potassium feldspar comprises 28%, quartz powder 9%, calcium carbonate 9%, black mud 5%, wood ash 5%, yellow sand soil 6%, white mud 9%, soybean stalk ash 3%, agate 3%, zirconium silicate 3%, titanium oxide 3%, blue and white material 1%, five-color soil 6%, rice washing water 3%, zinc oxide 3%, sodium silicate 0.8% and glass powder 3.2%.
[0012] A method for firing the above-mentioned Xuancai glaze, which uses a shuttle kiln, wherein the left side of the shuttle kiln is provided with fire holes No. 1, No. 2, No. 3, No. 4, No. 5 and No. 6 at intervals, and the right side is provided with fire holes No. 7, No. 8, No. 9, No. 10, No. 11 and No. 12 at intervals; the ceramic body is glazed and then fired, and the glaze used for glazing is prepared by adding water to the Xuancai glaze and ball milling for 36 hours, and the specific firing steps are as follows:
[0013] 1. Start the fire: At room temperature, light the No. 1 and No. 3 fire holes on the left, and the No. 8 and No. 12 fire holes on the right. Open the kiln door, fire for 2 hours, and raise the temperature to 120℃.
[0014] 2. Add No. 4 and No. 9 fire holes, fire for 2 hours, and raise the temperature to 300℃;
[0015] 3. Add fire holes No. 2, No. 5, No. 6, No. 7, No. 10 and No. 11, and fire for 3 hours. Close the kiln door when the temperature reaches 500℃.
[0016] 4. Continue firing for 2 hours and raise the temperature to 800°C, then reduce the pressure and keep warm for 30 minutes;
[0017] 5. Continue firing for 1.5 hours. When the temperature reaches 960℃, reduce all air doors to 1-1.5mm, close the skylight to 10cm, and let the temperature in the kiln return to a reduced state. Fire for 3 hours. When the temperature reaches 1100℃, keep warm for 30 minutes.
[0018] 6. When the temperature rises to 1190℃, increase the air door, pull the skylight to about 15cm, reduce reduction, until the oxidation firing state, the firing time is 3 hours, the temperature is fired to 1220℃, and keep warm for 50 minutes;
[0019] 7. Raise the temperature to 1280℃, reduce the air door, and close the skylight to between 13cm-16cm to form a weak reduction in the kiln. Keep warm for 1.2 hours and turn off the fire. At the same time, close all skylights, seal the fire port and the fire viewing hole.
[0020] Preferably, the water content of the glaze is 46-48% (weight percentage).
[0021] The functions of some components in the present invention are described as follows:
[0022] 1. Rice washing water: Rice washing water is the water after washing rice. Rice washing water is made by soaking rice for more than 30 minutes, filtering out rice and impurities, and letting it stand for 24 hours before use. Rice washing water is acidic, with a pH value of 5.5-6. The water molecules in rice washing water can separate grease very well. In glaze water, it can also make different glazes separate when fired at high temperatures, resulting in different glaze color changes.
[0023] 2. White clay: White clay has good acid solubility, very low cation exchange capacity, good fire resistance and other physical and chemical properties in ceramic glaze water, good plasticity and high adhesion.
[0024] 3. The role of potassium feldspar in glaze is:
[0025] (1) Increasing the calcium carbonate content and lowering the melting temperature, thereby reducing the amount of alkali used, this characteristic makes potassium feldspar one of the key components of glaze formula.
[0026] (2) Potassium feldspar can adjust the viscosity of the glaze, which plays a vital role in controlling the fluidity of the glaze.
[0027] (3) Potassium feldspar can slow down the melting speed of the glaze, making the glaze surface more stable, thereby obtaining a more uniform and smooth glaze surface.
[0028] 4. Soybean straw ash: Soybean ash contains calcium carbonate salt, which can reduce the melting point and viscosity of the glaze in the glaze, thereby making the glaze melt, which helps to lower the melting point of the glaze, increase the vitrification degree of the glaze surface, improve the glaze effect, and adjust the glaze color.
[0029] 5. Agate: Agate is composed of silicon dioxide (SiO2). Silicon dioxide is a common component in many rocks and minerals. As a variant of quartz, agate has a crystalline structure that gives it a special appearance and physical properties. In addition, agate has a variety of colors, including red, blue, green, purple, black, white, etc. Some agates also have color band characteristics, which are all determined by the structural content of silicon dioxide inside. Agate plays a great role in the richness and variation of color.
[0030] The glaze liquid in the present invention can be obtained by using the existing production process. The percentages not specified are all mass percentages.
[0031] The above technical solution has the following advantages:
[0032] The Xuancai glaze of the present invention is made of high-quality mountain materials, agate, quartz sand, white mud and Wuhua soil in Huaning Xiangyang coal seam, and other materials. It is mixed with overnight rice washing water, soybean stalks burned into ash, pure wood ash, etc. in proportion, and it takes 36 hours to ball-mill into glaze slurry, and then it is fired at a high temperature of 1280°C and re-reduced. The ratio of the present invention is complicated and has undergone tens of thousands of tests. Only then can the temperature coefficient of the bottom glaze be high, the temperature coefficient of the surface glaze be low, and the temperature coefficients are different at high temperatures to produce various gorgeous colors. The glaze color is not only rich and bright in color, but also colorful and crystal clear. The Xuancai glaze of the present invention is born from the oriental art thought system. The content expressed is the reflection of the bright state of mind of "mysterious color", the manifestation of consciousness from Lingshan, and the perception and description of the natural state and the truth of the universe. DETAILED DESCRIPTION
[0033] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0034] Example 1
[0035] A black colored glaze, which is composed of the following components in percentage by weight:
[0036] Potassium feldspar 28%, quartz powder 9%, calcium carbonate 9%, black mud (local) 5%, wood ash 5%, yellow sand soil 6%, white mud 9%, soybean stalk ash 3%, agate (local Dongshan material) 3%, zirconium silicate 3%, titanium oxide 3%, blue and white material (cobalt material) 1%, five-color soil (local material) 6%, rice washing water 3%, zinc oxide 3%, sodium silicate 0.8%, glass powder 3.2%.
[0037] The firing adopts a shuttle kiln, wherein the left side of the shuttle kiln is provided with fire holes No. 1, No. 2, No. 3, No. 4, No. 5 and No. 6 at intervals, and the right side is provided with fire holes No. 7, No. 8, No. 9, No. 10, No. 11 and No. 12 at intervals; the ceramic body is glazed and then fired, and the glaze liquid used for glazing is prepared by adding water to the black color glaze and ball milling for 36 hours, and the water content of the glaze liquid is 46% (weight percentage), and the specific firing steps are as follows:
[0038] 1. Start the fire: At room temperature, light the No. 1 and No. 3 fire holes on the left, and the No. 8 and No. 12 fire holes on the right. Open the kiln door, fire for 2 hours, and raise the temperature to 120℃.
[0039] 2. Add No. 4 and No. 9 fire holes, fire for 2 hours, and raise the temperature to 300℃;
[0040] 3. Add fire holes No. 2, No. 5, No. 6, No. 7, No. 10 and No. 11, and fire for 3 hours. Close the kiln door when the temperature reaches 500℃.
[0041] 4. Continue firing for 2 hours and raise the temperature to 800°C, then reduce the pressure and keep warm for 30 minutes;
[0042] 5. Continue firing for 1.5 hours. When the temperature reaches 960℃, reduce all air doors to 1-1.5mm, close the skylight to 10cm, and let the temperature in the kiln return to a reduced state. Fire for 3 hours. When the temperature reaches 1100℃, keep warm for 30 minutes.
[0043] 6. When the temperature rises to 1190℃, increase the air door, pull the skylight to about 15cm, reduce reduction, until the oxidation firing state, the firing time is 3 hours, the temperature is fired to 1220℃, and keep warm for 50 minutes;
[0044] 7. Raise the temperature to 1280℃, reduce the air door, and close the skylight to between 13cm-16cm to form a weak reduction in the kiln. Keep warm for 1.2 hours and turn off the fire. At the same time, close all skylights, seal the fire port and the fire viewing hole.
[0045] Example 2
[0046] A black colored glaze, which is composed of the following components in percentage by weight:
[0047] Potassium feldspar 26.4%, quartz powder 8.1%, calcium carbonate 8.1%, black mud 4.5%, wood ash 4.5%, yellow sand soil 6.6%, white mud 9.9%, soybean straw ash 3.3%, agate 3.3%, zirconium silicate 3.3%, titanium oxide 3.3%, blue and white material 1.1%, five-color soil 6.6%, rice washing water 3.3%, zinc oxide 3.3%, sodium silicate 0.88%, glass powder 3.52%.
[0048] During the firing process, the water content of the glaze liquid is 48% (weight percentage) and the rest is the same as in Example 1.
[0049] Example 3
[0050] A black colored glaze, which is composed of the following components in percentage by weight:
[0051] Potassium feldspar 29.8%, quartz powder 9.9%, calcium carbonate 9.9%, black mud 5.5%, wood ash 5.5%, yellow sand soil 5.2%, white mud 8.1%, soybean straw ash 2.7%, agate 2.7%, zirconium silicate 2.7%, titanium oxide 2.7%, blue and white material 0.9%, five-color soil 5.4%, rice washing water 2.7%, zinc oxide 2.7%, sodium silicate 0.72%, glass powder 2.88%.
[0052] During the glaze making process, the water content of the glaze liquid is 47% (weight percentage) and the rest is the same as in Example 1.
[0053] The glazed pottery fired by the present invention forms a natural and colorful effect on the surface of the glazed pottery. Under the refraction of light, the glaze surface can show a fantasy scene with distinct layers and rich colors, as if the stars in the universe and the dreamland are solidified on the ceramics.
[0054] The color of the Xuancai glaze of the present invention is like using the Great Perfection Mind Method to create mental images, depicting the natural scenes, images and illusions of the real world and the realm of emptiness, and constructing a psychological image projection path that gradually progresses in three dimensions, namely, from "image" to "non-image" to "formlessness", forming an independent artistic thought and a clear artistic context, and embarking on a self-contained ceramic art path. The "mental image art" of the Xuancai glaze has been pushed to a higher dimension and level, which is also the profoundness of the color of the Xuancai glaze.
[0055] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.
Claims
1. A kind of black glaze, It is characterized in that It is composed of the following components in weight percentage: Potassium feldspar 25.2-30.8%, quartz powder 8.1-9.9%, calcium carbonate 8.1-9.9%, black mud 4.5-5.5%, wood ash 4.5-5.5%, yellow sand soil 5.4-6.6%, white mud 8.1-9.9%, soybean straw ash 2.7-3.3%, agate 2.7-3.3%, zirconium silicate 2.7-3.3%, titanium oxide 2.7-3.3%, blue and white material 0.9-1.1%, five-color soil 5.4-6.6%, rice water 2.7-3.3%, zinc oxide 2.7-3.3%, sodium silicate 0.72-0.88%, glass powder 2.88-3.52%.
2. The black colored glaze according to claim 1, It is characterized in that It is composed of the following components in weight percentage: The potassium feldspar comprises 28%, quartz powder 9%, calcium carbonate 9%, black mud 5%, wood ash 5%, yellow sand soil 6%, white mud 9%, soybean stalk ash 3%, agate 3%, zirconium silicate 3%, titanium oxide 3%, blue and white material 1%, five-color soil 6%, rice washing water 3%, zinc oxide 3%, sodium silicate 0.8% and glass powder 3.2%.
3. A method for firing the black colored glaze according to claim 1 or 2, Features A shuttle kiln is used, wherein the left side of the shuttle kiln is provided with fire holes No. 1, No. 2, No. 3, No. 4, No. 5 and No. 6 at intervals, and the right side is provided with fire holes No. 7, No. 8, No. 9, No. 10, No. 11 and No. 12 at intervals; the ceramic body is glazed and then fired, and the glaze used for glazing is prepared by adding water to the black color glaze and ball milling for 36 hours, and the specific firing steps are as follows:
1. Start the fire: At room temperature, light the No. 1 and No. 3 fire holes on the left, and the No. 8 and No. 12 fire holes on the right. Open the kiln door, fire for 2 hours, and raise the temperature to 120℃.
2. Add No. 4 and No. 9 fire holes, fire for 2 hours, and raise the temperature to 300℃; 3. Add fire holes No. 2, No. 5, No. 6, No. 7, No. 10 and No. 11, and fire for 3 hours. Close the kiln door when the temperature reaches 500℃.
4. Continue firing for 2 hours and raise the temperature to 800°C, then reduce the pressure and keep warm for 30 minutes; 5. Continue firing for 1.5 hours. When the temperature reaches 960℃, reduce all air doors to 1-1.5mm, close the skylight to 10cm, and let the temperature in the kiln return to a reduced state. Fire for 3 hours. When the temperature reaches 1100℃, keep warm for 30 minutes.
6. When the temperature rises to 1190℃, increase the air door, pull the skylight to about 15cm, reduce reduction, until the oxidation firing state, the firing time is 3 hours, the temperature is fired to 1220℃, and keep warm for 50 minutes; 7. Raise the temperature to 1280℃, reduce the air door, and close the skylight to between 13cm-16cm to form a weak reduction in the kiln. Keep warm for 1.2 hours and turn off the fire. At the same time, close all skylights, seal the fire port and the fire viewing hole.
4. The firing method of the black colored glaze according to claim 3, Features: The water content of the glaze is 46-48% (weight percentage).
Citation Information
Patent Citations
Preparation method of glaze slip for flow-color glazed pottery and firing method of flow-color glazed pottery
CN107500534A
Black-bottomed Zijin oil droplet ceramic product and preparation process thereof
CN108129129A
Secret color glaze and preparation method thereof
CN112279513A
Firewood-fired porcelain yellow glaze
CN113277733A
Snowflake crystal particles, preparation method thereof and preparation method of positioned crystal pattern glazed brick
CN114507014A