Low-temperature lead-free transmutation glaze and preparation method thereof, and art ceramic and preparation method thereof

By adding borax and calcined zinc oxide to the kiln-changing glaze, the kiln-changing temperature is reduced and combined with oil-based printing and oil-based printing, the problem of high firing temperature of the kiln-changing glaze is solved, and the low-temperature fast firing and economical and durable kiln-changing effect is achieved. It is suitable for building ceramics , and reduce environmental and human hazards.

CN118978338AActive Publication Date: 2024-11-19DONGGUAN CITY WONDERFUL CERAMICS IND PARK +2
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411093608.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-19
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The existing kiln-fired glaze has a high firing temperature, which cannot meet the low-temperature and fast firing requirements of building ceramics, which limits its application in the field of building ceramics.

Method used

By adding borax, calcined zinc oxide and titanium dioxide to the raw materials of the kiln-changing glaze, the kiln-changing temperature is reduced, and a low-temperature lead-free kiln-changing glaze is prepared by ball milling, sieving and drying, and blending it with oily oil and camphor oil to the appropriate dilute consistency , achieve crystallization effect at lower temperatures.

Benefits of technology

It achieves good kiln transformation effect of kiln-changing glaze at lower temperatures (950-1030℃), meets the low-temperature and fast firing requirements of building ceramics, and lead-free formula reduces environmental pollution and human body hazards, providing economical and durable cost advantages and good artistic effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978338A_ABST
    Figure CN118978338A_ABST
Patent Text Reader

Abstract

The invention provides low-temperature lead-free transmutation glaze and a preparation method thereof as well as art ceramic and a preparation method thereof, and the low-temperature lead-free transmutation glaze comprises the following raw materials in percentage by mass: 38-55% of borax, 0-3% of calcite, 5-25% of barium carbonate, 4-12% of titanium dioxide, 6-14% of calcined zinc oxide, 30-50% of strontium carbonate and 1-6% of lithium carbonate. The borax is added into the raw materials of the low-temperature lead-free transmutation glaze, so that the overall temperature of the transmutation glaze is reduced, a crystallization effect can be conveniently generated at a relatively low temperature, and the added calcined zinc oxide and titanium dioxide can generate crystallization effects in different forms, so that the transmutation effect is richer; and the transmutation glaze meets the low-temperature fast firing requirement of architectural ceramics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of ceramic technology, and in particular to a low-temperature lead-free kiln-changed glaze and a preparation method thereof, and artistic ceramics and a preparation method thereof. Background Art

[0002] Kiln-changed glaze is an artistic glaze with great ornamental value and decorative effect. Using it to decorate ceramic products can enhance the ornamental and artistic quality of ceramics. At present, kiln-changed glaze is mainly used in artistic ceramics and daily-use ceramics, but its firing temperature is relatively high, usually around 1300°C, and the firing cycle is relatively long, generally up to several hours. Therefore, kiln-changed glaze cannot meet the requirements of low-temperature fast firing of architectural ceramics, and it is difficult to be widely promoted and applied in the field of architectural ceramics.

[0003] Therefore, the prior art has defects and needs to be improved and developed. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a low-temperature lead-free kiln-changed glaze and a preparation method, artistic ceramics and a preparation method in view of the above-mentioned defects of the prior art, aiming to solve the problem that the kiln-changed glaze in the prior art cannot meet the low-temperature and fast-firing requirements of building ceramics.

[0005] The technical solution adopted by the present invention to solve the technical problem is as follows:

[0006] The first aspect of the present application provides a low-temperature lead-free kiln-changed glaze, wherein the raw materials of the low-temperature lead-free kiln-changed glaze, calculated by mass percentage, include:

[0007] Borax 38-55%, calcite 0-3%, barium carbonate 5-25%, titanium dioxide 4-12%, calcined zinc oxide 6-14%, strontium carbonate 30-50%, lithium carbonate 1-6%.

[0008] In one embodiment of the present application, the chemical components of the low-temperature lead-free kiln-changed glaze, measured by mass percentage, include:

[0009] SiO2 1~6%, SrO 28~44%, Al2O3 0~1%, CaO+MgO 1~4%, K2O+Na2O 6~12%, Fe2O3 0~1%, TiO2 4~13%, ZnO 6~16%, BaO 2~20%, B2O3 7~12%, Li2O 0.5~2.5%.

[0010] A second aspect of the present application provides a method for preparing the low-temperature lead-free kiln-changed glaze as described above, comprising:

[0011] The raw materials of low-temperature lead-free kiln-changed glaze are mixed according to 38-55% of borax, 0-3% of calcite, 5-25% of barium carbonate, 4-12% of titanium dioxide, 6-14% of calcined zinc oxide, 30-50% of strontium carbonate and 1-6% of lithium carbonate to obtain a mixed powder;

[0012] After adding a solvent to the mixed powder, the mixed powder is subjected to ball milling, sieving and drying to obtain glaze powder;

[0013] The glaze powder is blended to a predetermined consistency using oily printing ink and camphor oil to obtain a low-temperature lead-free kiln-changed glaze.

[0014] In one embodiment of the present application, the raw materials of the low-temperature lead-free kiln-changed glaze are mixed according to 38-55% borax, 0-3% calcite, 5-25% barium carbonate, 4-12% titanium dioxide, 6-14% calcined zinc oxide, 30-50% strontium carbonate, and 1-6% lithium carbonate to obtain a mixed powder, and further include:

[0015] The raw materials of low-temperature lead-free kiln-changed glaze are mixed according to 38-55% of borax, 0-3% of calcite, 5-25% of barium carbonate, 4-12% of titanium dioxide, 6-14% of calcined zinc oxide, 30-50% of strontium carbonate, and 1-6% of lithium carbonate, and a coloring metal oxide is added to obtain a mixed powder;

[0016] Wherein, the colored metal oxide includes one or more of red iron oxide, green chromium oxide, vanadium pentoxide, cobalt oxide, nickelous oxide, cupric oxide, and manganese oxide.

[0017] In one embodiment of the present application, after adding a solvent to the mixed powder, ball milling, sieving and drying are performed to obtain a glaze powder, comprising:

[0018] Adding water and sodium tripolyphosphate to the mixed powder and then ball milling, the fineness of the glaze slurry after ball milling is less than or equal to 0.2% on a 300-mesh sieve;

[0019] The ball-milled glaze slurry is sieved and then dried to obtain a block glaze;

[0020] The block glaze is ground and passed through a 100-mesh sieve to obtain glaze powder.

[0021] A third aspect of the present application provides a method for preparing artistic ceramics, which includes:

[0022] preparing a ceramic body, and firing the ceramic body in a kiln to obtain a ceramic painting substrate;

[0023] Using the low-temperature lead-free kiln-changed glaze as described above to paint on the surface of the ceramic painting substrate;

[0024] The painted ceramic painting substrate is dried in a drying kiln and then fired in a roller kiln.

[0025] In one embodiment of the present application, the method of preparing a ceramic body and firing the ceramic body in a kiln to obtain a ceramic painting substrate comprises:

[0026] The raw materials for the blank are mixed, water, water glass and sodium tripolyphosphate are added, and the mixture is ball-milled in a ball mill to obtain a slurry with a fineness of 0.5-1.2% of the residue on a 300-mesh sieve;

[0027] After the slurry is aged for 24 hours, spray granulation is performed to obtain a green body powder, and the green body powder is pressed and molded to obtain a molded green body;

[0028] The formed green body is dried in a drying kiln to obtain a ceramic green body, wherein the moisture entering the kiln is less than or equal to 0.8% and the temperature leaving the kiln is 110° C.;

[0029] The ceramic body is put into a kiln for firing to obtain a ceramic painting substrate, wherein the firing temperature of the ceramic body is 1220-1240° C., the firing time is 35-45 minutes, and the water absorption rate of the fired ceramic painting substrate is less than or equal to 0.5%.

[0030] In one embodiment of the present application, the mineral raw materials for the blank include, by mass percentage:

[0031] High temperature aluminum sand 5-8%, aluminum potassium sand 20-35%, washed sand 15-22%, black talc 2-8%, black mud 2-5%, waste porcelain powder 1-5%, bentonite 8-14%, sodium sand 16-35%;

[0032] The chemical components of the ceramic body, measured by mass percentage, include:

[0033] SiO2 60~72%, Al2O3 18~24%, CaO+MgO 0~3%, K2O+Na2O 4~6%, Fe2O3 0~2%, TiO2 0~1%, loss on ignition 6~11%.

[0034] In one embodiment of the present application, the painted ceramic painting substrate is dried in a drying kiln and then fired in a roller kiln, comprising:

[0035] The painted ceramic painting substrate is dried in a drying kiln and then placed in a roller kiln for firing in an oxidizing atmosphere at a firing temperature of 950 to 1030° C. and a firing cycle of 60 to 90 minutes.

[0036] A fourth aspect of the present application provides an artistic ceramic, wherein the artistic ceramic is prepared based on the preparation method of the artistic ceramic as described above.

[0037] The present invention discloses a low-temperature lead-free kiln-changed glaze and a preparation method, and an artistic ceramic and a preparation method. The raw materials of the low-temperature lead-free kiln-changed glaze include, by mass percentage, 38-55% borax, 0-3% calcite, 5-25% barium carbonate, 4-12% titanium dioxide, 6-14% calcined zinc oxide, 30-50% strontium carbonate, and 1-6% lithium carbonate. The present invention reduces the overall temperature of the kiln-changed glaze by adding borax to the raw materials of the low-temperature lead-free kiln-changed glaze, and facilitates the crystallization effect at a relatively low temperature. The added calcined zinc oxide and titanium dioxide can produce crystallization effects of different forms, making the kiln-changed effect richer, and making the kiln-changed glaze meet the low-temperature fast-firing requirements of architectural ceramics. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 The present invention is a flowchart of a preferred embodiment of a method for preparing a low-temperature lead-free kiln-changed glaze.

[0039] Figure 2 It is a kiln-change effect diagram of Example 1 in the present invention.

[0040] Figure 3 This is a kiln-change effect diagram of Example 2 of the present invention. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solution and advantages of the present invention clearer and more specific, the present invention is further described in detail below with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0042] The first aspect of the present application provides a low-temperature lead-free kiln-changed glaze, wherein the raw materials of the low-temperature lead-free kiln-changed glaze, calculated by mass percentage, include:

[0043] Borax 38-55%, calcite 0-3%, barium carbonate 5-25%, titanium dioxide 4-12%, calcined zinc oxide 6-14%, strontium carbonate 30-50%, lithium carbonate 1-6%.

[0044] Specifically, the embodiment of the present application adds borax to the raw materials. Borax has a low single melting temperature, which reduces the liquidus temperature of the batching system, that is, reduces the overall temperature of the kiln-changed glaze, and accelerates and strengthens the melting process, which is convenient for producing crystallization effect at a lower temperature; strontium carbonate and barium carbonate decomposed strontium oxide and barium oxide are both good fluxing agents. Unlike calcium oxide and magnesium oxide, strontium oxide and barium oxide have a wider fluxing range. The formula also contains more sodium oxide, which reduces the melt viscosity and is also conducive to crystallization in the low temperature section; the addition of lithium carbonate can also greatly reduce the melt viscosity of the glaze melt, which is conducive to crystal precipitation.

[0045] In the embodiment of the present application, calcined zinc oxide and rutile titanium dioxide are added to the raw materials. The two will produce different forms of crystallization effects, making the kiln-fired effect richer. Rutile titanium dioxide is titanium oxide, and the titanium oxide content mainly affects the formation of crystals. When the titanium oxide content increases from 0% to 14%, the crystals appear from nothing, gradually increase to cover the glaze surface, and a better white crystallization effect appears.

[0046] Therefore, the embodiment of the present application reduces the overall temperature of the kiln-changed glaze by adding borax to the kiln-changed glaze raw materials, thereby facilitating the crystallization effect at a lower temperature. The added calcined zinc oxide and titanium dioxide can produce crystallization effects in different forms, making the kiln-changed effect richer, and making the kiln-changed glaze meet the low-temperature and fast-firing requirements of building ceramics.

[0047] In a specific embodiment of the present application, the chemical components of the low-temperature lead-free kiln-changed glaze, measured by mass percentage, include:

[0048] SiO2 1~6%, SrO 28~44%, Al2O3 0~1%, CaO+MgO 1~4%, K2O+Na2O 6~12%, Fe2O3 0~1%, TiO2 4~13%, ZnO 6~16%, BaO 2~20%, B2O3 7~12%, Li2O 0.5~2.5%.

[0049] The second aspect of the present application also provides a method for preparing a low-temperature lead-free kiln-changed glaze, such as Figure 1 As shown, the preparation method of the low-temperature lead-free kiln-changed glaze comprises:

[0050] Step S100, mixing the raw materials of low-temperature lead-free kiln-changed glaze according to 38-55% borax, 0-3% calcite, 5-25% barium carbonate, 4-12% titanium dioxide, 6-14% calcined zinc oxide, 30-50% strontium carbonate, and 1-6% lithium carbonate to obtain a mixed powder.

[0051] In the embodiment of the present application, in the step S100, the raw materials of the low-temperature lead-free kiln-changed glaze are mixed according to 38-55% borax, 0-3% calcite, 5-25% barium carbonate, 4-12% titanium dioxide, 6-14% calcined zinc oxide, 30-50% strontium carbonate, and 1-6% lithium carbonate, and a color metal oxide is added to obtain a mixed powder. The color metal oxide includes one or more of red iron oxide, green chromium oxide, vanadium pentoxide, cobalt oxide, nickelous oxide, copper oxide, and manganese oxide.

[0052] Specifically, the kiln-changed glaze components are mainly borax, calcite, barium carbonate, strontium carbonate, lithium carbonate, titanium dioxide, and calcined zinc oxide. The ratio of the basic glaze is fixed, and the proportion of the added color metal oxides is: 0.3-4% red iron oxide, 0.3-3% chromium oxide green, 0.2-3% cobalt oxide, 0.6-3% nickelous oxide, 0.2-3% copper oxide, and 1-4% manganese oxide. The embodiment of the present application can use a certain color metal oxide alone, or can mix color metal oxides to achieve the effect of other colors.

[0053] The kiln-changing formula components of the embodiments of the present application all use lead-free raw materials, which not only achieves better kiln-changing effects but also reduces pollution to the environment.

[0054] like Figure 1 As shown, the method for preparing the low-temperature lead-free kiln-changed glaze also includes:

[0055] Step S200: After adding a solvent to the mixed powder, the mixed powder is subjected to ball milling, sieving and drying to obtain glaze powder.

[0056] In an embodiment of the present application, step S200 specifically includes: adding water and sodium tripolyphosphate to the mixed powder and then ball milling, wherein the fineness of the glaze slurry after ball milling is less than or equal to 0.2% of the residue on a 300-mesh sieve; sieving the glaze slurry after ball milling, and drying it to obtain a block glaze; grinding the block glaze, and passing it through a 100-mesh sieve to obtain glaze powder.

[0057] Specifically, 45-55% of water and 1.5-3.0% of sodium tripolyphosphate are added according to the ratio of kiln-changed glaze for ball milling. Since borax has good water absorption, more sodium tripolyphosphate needs to be added for degumming, otherwise the glaze slurry will have greater thixotropy and will be more difficult to produce balls. The colored oxides can be ground together, and the color will be brighter and more uniform after grinding. The fineness of the glaze slurry after ball milling is 300 mesh residue ≤0.2%.

[0058] The fineness of the calcined zinc oxide in the basic raw material is 80 mesh sieve residue. In order to ensure the kiln-changing effect, the calcined zinc oxide is added last during ball milling. After a short period of ball milling and mixing, the slurry can be released. The fineness of the overall glaze slurry is 100 mesh sieve to prevent the zinc oxide particles from being too small and melting in the glaze melt, which is not conducive to the growth of crystals. After the ball-milled glaze slurry is sieved, it is dried into blocks, ground and sieved through a 100 mesh sieve into powder.

[0059] In the embodiment of the present application, by grinding the block glaze and then passing it through a 100-mesh sieve, a glaze powder with uniform particle size and moderate fineness can be obtained, which makes it easier to form a uniform and smooth glaze layer during the glazing process.

[0060] like Figure 1 As shown, the method for preparing the low-temperature lead-free kiln-changed glaze also includes:

[0061] Step S300: Use oily printing ink and camphor oil to blend the glaze powder to a predetermined consistency to obtain a low-temperature lead-free kiln-changed glaze.

[0062] Specifically, a certain amount of oily printing ink and camphor oil are added, and the glaze powder is blended to a suitable consistency before artistic painting. That is, in the embodiment of the present application, different oxides, frits, and pigments are mixed in a certain proportion, and after adding a suitable amount of solvent and ball-milling to a certain fineness, the mixture is sieved, dried, and prepared into powder, and printing ink is added to blend to a suitable consistency for painting creation.

[0063] The embodiments of the present application use oily printing ink and camphor oil as solvents, which helps to better mix the components in the glaze powder, reduce the agglomeration phenomenon between particles, and improve the overall uniformity of the glaze; moreover, the addition of solvents can stabilize the performance of the glaze, prevent stratification or precipitation in subsequent processing, and ensure the stable quality of the glaze.

[0064] The low-temperature lead-free kiln-changed glaze prepared in the embodiment of the present application meets the requirements of low-temperature and fast firing of architectural ceramics, thereby achieving better cultural and artistic effects and enriching the categories of architectural ceramic decorations.

[0065] The third aspect of the present application also provides a method for preparing artistic ceramics, comprising: preparing a ceramic body, firing the ceramic body in a kiln to obtain a ceramic painting substrate; painting on the surface of the ceramic painting substrate using the low-temperature lead-free kiln-changed glaze as described above; and drying the painted ceramic painting substrate in a drying kiln and firing it in a roller kiln.

[0066] Specifically, artistic paintings can be divided into single-layer and multi-layer paintings according to the artistic effects, ensuring that the glaze layer thickness is above 0.6mm to have a good kiln-changing effect.

[0067] In the embodiment of the present application, the ceramic body is fired to achieve high-temperature vitrification; after the painting is completed, the painted ceramic painting substrate is fired again to achieve low-temperature glazing. Therefore, the embodiment of the present application adopts a secondary firing process, i.e., high-temperature vitrification and low-temperature glazing, to ensure the splicing alignment effect of large murals, and has a better effect on large-scale products, especially rock slabs.

[0068] In an embodiment of the present application, the preparation of a ceramic body, firing the ceramic body in a kiln to obtain a ceramic painting substrate, includes: mixing a mineral raw material for the body, adding water, water glass and sodium tripolyphosphate, and ball-milling in a ball mill to obtain a slurry with a fineness of 300 mesh residue of 0.5-1.2%; aging the slurry for 24 hours, spray granulating to obtain a body powder, and pressing the body powder to obtain a molded body; drying the molded body in a drying kiln to obtain a ceramic body, wherein the moisture entering the kiln is less than or equal to 0.8%, and the kiln outlet temperature is 110°C; firing the ceramic body in a kiln to obtain a ceramic painting substrate, wherein the firing temperature of the molded body is 1220-1240°C, the firing time is 35-45 minutes, and the water absorption rate of the ceramic painting substrate after firing is less than or equal to 0.5%.

[0069] The different blank mineral raw materials of the embodiments of the present application are ball-milled, powdered, aged, pressed, dried, and fired at high temperature to form porcelain unglazed bricks as ceramic painting substrates. The ceramic painting substrates of the embodiments of the present application use but are not limited to porcelain unglazed bricks fired with this formula. The surface tests of porcelain unglazed bricks with a water absorption rate of 0 to 0.5% all have good kiln-changing effects, but the kiln-changing colors are slightly different. Artistic creation is performed on the surface of the prepared painting substrate, and it is fired in a roller kiln after being dried in a drying kiln.

[0070] Specifically, after the blank is prepared according to the blank formula, an appropriate amount of water is added, 0.3-0.5% water glass and sodium tripolyphosphate are added as debonding agents, and the blank is input into a ball mill to be ball-milled into a slurry with a fineness of 0.5-1.2% of the residue on a 300-mesh sieve, and spray granulation is performed after aging for 24 hours to obtain a blank powder. After the blank powder is aged, it is formed by a large-tonnage press and dried in a drying kiln. The temperature out of the drying kiln is 110°C, and the water content in the kiln is ≤0.8%. The maximum firing temperature of the ceramic blank is 1220-1240°C, the firing time is 35-45 minutes, and the water absorption rate of the fired porcelain unglazed brick is ≤0.5%.

[0071] The embodiment of the present application ball-mills the raw materials to a 300-mesh sieve with a residue of 0.5-1.2%, so that the raw material particles are refined, which helps to increase the density and strength of the green body; water glass, as a deflocculating agent, can reduce the viscosity of the mud, improve the fluidity of the mud, and make the spray granulation process smoother. In addition, water glass has a certain adhesiveness, which helps to increase the strength of the green body; sodium tripolyphosphate, as a debonding agent, can further reduce the viscosity of the mud and improve the fluidity of the mud. The embodiment of the present application also controls the moisture entering the kiln to ≤0.8%, and the kiln outlet temperature to 110°C, to ensure that the green body reaches a suitable dry state before firing, and to reduce defects such as cracking during the firing process; the maximum firing temperature of the ceramic green body of the embodiment of the present application is 1220-1240°C, and the firing time is 35-45 minutes, achieving high-temperature vitrification.

[0072] In the embodiment of the present application, the mineral raw materials for the blank include, by mass percentage:

[0073] High-temperature aluminum sand 5-8%, aluminum potassium sand 20-35%, washed sand 15-22%, black talc 2-8%, black mud 2-5%, waste porcelain powder 1-5%, bentonite 8-14%, sodium sand 16-35%.

[0074] The chemical components of the ceramic body, measured by mass percentage, include:

[0075] SiO2 60~72%, Al2O3 18~24%, CaO+MgO 0~3%, K2O+Na2O 4~6%, Fe2O3 0~2%, TiO2 0~1%, loss on ignition 6~11%.

[0076] In one embodiment of the present application, the painted ceramic painting substrate is dried in a drying kiln and then placed in a roller kiln for firing, comprising: after the painted ceramic painting substrate is dried in a drying kiln, placed in a roller kiln and fired in an oxidizing atmosphere with a firing temperature of 950-1030°C and a firing cycle of 60-90 minutes.

[0077] The firing range of the kiln-changed glaze of the embodiment of the present application is between 950 and 1030°C, the firing temperature range is wide, the surface has a good kiln-changed effect after firing, the effect is stable, and the price is low. In addition, the lead-free kiln-changed glaze of the embodiment of the present application has the following differences compared with the lead-containing kiln-changed glaze: (1) Metallic lead is a heavy metal. Even if it is made into a frit, a high-doped lead frit will produce steam after high-temperature firing, which will cause great harm to the human body after inhalation. The lead-free kiln-changed glaze can avoid the above problems and greatly reduce the harm to the human body. (2) When the high-lead frit encounters acid or alkali in the environment, heavy metal ions are easily dissolved, causing strong pollution to the environment, especially groundwater, which is not conducive to human health. (3) Lead-containing kiln-changed glaze is suitable for the painting of abstract art works, because lead oxide has good fluidity, and the contact of different colors can produce a good "mixing" effect, making the art work more abstract; lead-free kiln-changed glaze is more suitable for the creation of figurative art works, the boundaries of the contact parts of different colors are clear, what is painted is what is seen, and the effect is stable.

[0078] The present invention achieves the following effects:

[0079] First, the embodiment of the present application prepares a low-temperature lead-free kiln-changed glaze by adjusting the formula, the firing temperature is between 950-1030°C, and it has a good kiln-changed effect.

[0080] Second, the kiln-changed glaze prepared in the embodiment of the present application is suitable for low-temperature secondary firing process, and has a better cost advantage than high-temperature kiln-changed glaze, is low in price, and is economical and durable.

[0081] Third, the kiln-changed glaze prepared in the embodiment of the present application adopts a secondary firing process, which has a better splicing effect and will not produce obvious dislocation, thereby ensuring the artistic effect of large-scale art paintings.

[0082] Fourth, the kiln-changed glaze prepared in the embodiment of the present application is blended with oily printing oil, which can better adjust the consistency and facilitate the depiction of artistic details.

[0083] The fourth aspect of the present application further provides an artistic ceramic, which is prepared based on the preparation method of the artistic ceramic as described above.

[0084] Specific embodiments are listed below for illustration.

[0085] Embodiment 1

[0086] Take 55g of borax, 35g of strontium carbonate, 3g of calcite, 6g of titanium dioxide, 8g of calcined zinc oxide, and 1g of cobalt oxide, add appropriate amounts of sodium tripolyphosphate and CMC, and mix them to a suitable consistency through ball milling, drying, and printing oil. Apply them to the surface of porcelain unglazed tiles, and sinter them in a roller kiln at 1000℃. The surface will have a good kiln-changing effect. The kiln-changing effect is as follows: Figure 2 shown.

[0087] Embodiment 2

[0088] Take 45g of borax, 15g of barium carbonate, 30g of strontium carbonate, 3g of lithium carbonate, 6g of titanium dioxide, 10g of calcined zinc oxide, and 1.0g of cobalt oxide, add appropriate amount of grinding aid, mix them into appropriate thin and thick state after ball milling, drying, and printing oil, apply them to the surface of porcelain unglazed tiles, and burn them in a roller kiln at 990℃. The surface will have a good kiln-changing effect; the kiln-changing effect is as follows: Figure 3 shown.

[0089] The present invention provides a low-temperature lead-free kiln-changed glaze and a preparation method, and an artistic ceramic and a preparation method. The raw materials of the low-temperature lead-free kiln-changed glaze include, by mass percentage, 38-55% borax, 0-3% calcite, 5-25% barium carbonate, 4-12% titanium dioxide, 6-14% calcined zinc oxide, 30-50% strontium carbonate, and 1-6% lithium carbonate. The present invention reduces the overall temperature of the kiln-changed glaze by adding borax to the raw materials of the low-temperature lead-free kiln-changed glaze, and facilitates the crystallization effect at a relatively low temperature. The added calcined zinc oxide and titanium dioxide can produce crystallization effects of different forms, making the kiln-changed effect richer, so that the kiln-changed glaze meets the low-temperature fast firing requirements of architectural ceramics.

[0090] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A low-temperature lead-free kiln-changed glaze, It is characterized in that The raw materials of the low-temperature lead-free kiln-changed glaze include, by mass percentage: Borax 38-55%, calcite 0-3%, barium carbonate 5-25%, titanium dioxide 4-12%, calcined zinc oxide 6-14%, strontium carbonate 30-50%, lithium carbonate 1-6%.

2. The low-temperature lead-free kiln-changed glaze according to claim 1, It is characterized in that The chemical components of the low-temperature lead-free kiln-changed glaze, measured by mass percentage, include: SiO 2 1~6%、SrO 28~44%、Al 2 O 3 0~1%、CaO+MgO 1~4%、K 2 O+Na 2 Of 6~12%、Fe 2 O 3 0~1%、TiO 2 4~13%、ZnO 6~16%、BaO 2~20%、B 2 O 3 7~12%、Li 2 It is 0.5~2.5%.

3. A method for preparing a low-temperature lead-free kiln-changed glaze as claimed in claim 1 or 2, It is characterized in that include: The raw materials of low-temperature lead-free kiln-changed glaze are mixed according to 38-55% of borax, 0-3% of calcite, 5-25% of barium carbonate, 4-12% of titanium dioxide, 6-14% of calcined zinc oxide, 30-50% of strontium carbonate and 1-6% of lithium carbonate to obtain a mixed powder; After adding a solvent to the mixed powder, the mixed powder is subjected to ball milling, sieving and drying to obtain glaze powder; The glaze powder is blended to a predetermined consistency using oily printing ink and camphor oil to obtain a low-temperature lead-free kiln-changed glaze.

4. The method for preparing the low-temperature lead-free kiln-changed glaze according to claim 3, It is characterized in that The raw materials of low-temperature lead-free kiln-changed glaze are mixed according to 38-55% borax, 0-3% calcite, 5-25% barium carbonate, 4-12% titanium dioxide, 6-14% calcined zinc oxide, 30-50% strontium carbonate, and 1-6% lithium carbonate to obtain a mixed powder, and further include: The raw materials of low-temperature lead-free kiln-changed glaze are mixed according to 38-55% of borax, 0-3% of calcite, 5-25% of barium carbonate, 4-12% of titanium dioxide, 6-14% of calcined zinc oxide, 30-50% of strontium carbonate, and 1-6% of lithium carbonate, and a coloring metal oxide is added to obtain a mixed powder; Wherein, the colored metal oxide includes one or more of red iron oxide, green chromium oxide, vanadium pentoxide, cobalt oxide, nickelous oxide, cupric oxide, and manganese oxide.

5. The method for preparing low-temperature lead-free kiln-changed glaze according to claim 3, It is characterized in that After adding a solvent to the mixed powder, ball milling, sieving and drying are performed to obtain glaze powder, including: Adding water and sodium tripolyphosphate to the mixed powder and then ball milling, the fineness of the glaze slurry after ball milling is less than or equal to 0.2% on a 300-mesh sieve; The ball-milled glaze slurry is sieved and then dried to obtain a block glaze; The block glaze is ground and passed through a 100-mesh sieve to obtain glaze powder.

6. A method for preparing artistic ceramics, It is characterized in that include: preparing a ceramic body, and firing the ceramic body in a kiln to obtain a ceramic painting substrate; Using the low-temperature lead-free kiln-changed glaze as claimed in claim 1 or 2 to paint on the surface of the ceramic painting substrate; The painted ceramic painting substrate is dried in a drying kiln and then fired in a roller kiln.

7. The method for preparing artistic ceramics according to claim 6, It is characterized in that The method of preparing a ceramic body and firing the ceramic body in a kiln to obtain a ceramic painting substrate comprises: The raw materials for the blank are mixed, water, water glass and sodium tripolyphosphate are added, and the mixture is ball-milled in a ball mill to obtain a slurry with a fineness of 0.5-1.2% of the residue on a 300-mesh sieve; After the slurry is aged for 24 hours, spray granulation is performed to obtain a green body powder, and the green body powder is pressed and molded to obtain a molded green body; The formed green body is dried in a drying kiln to obtain a ceramic green body, wherein the moisture entering the kiln is less than or equal to 0.8% and the temperature leaving the kiln is 110° C.; The ceramic body is put into a kiln for firing to obtain a ceramic painting substrate, wherein the firing temperature of the ceramic body is 1220-1240° C., the firing time is 35-45 minutes, and the water absorption rate of the fired ceramic painting substrate is less than or equal to 0.5%.

8. The method for preparing artistic ceramics according to claim 7, It is characterized in that The mineral raw materials for the blank include, by mass percentage: High temperature aluminum sand 5-8%, aluminum potassium sand 20-35%, washed sand 15-22%, black talc 2-8%, black mud 2-5%, waste porcelain powder 1-5%, bentonite 8-14%, sodium sand 16-35%; The chemical components of the ceramic body, measured by mass percentage, include: SiO 2 60~72%、Al 2 O 3 18~24%, CaO+MgO 0~3%, K 2 O+Na 2 O 4~6%、Fe 2 O 3 0~2%、TiO 2 0~1%, loss on ignition 6~11%.

9. The method for preparing artistic ceramics according to claim 6, It is characterized in that The painted ceramic painting substrate is dried in a drying kiln and then placed in a roller kiln for firing, comprising: The painted ceramic painting substrate is dried in a drying kiln and then placed in a roller kiln for firing in an oxidizing atmosphere at a firing temperature of 950 to 1030° C. and a firing cycle of 60 to 90 minutes.

10. An artistic ceramic, It is characterized in that The artistic ceramic is prepared based on the preparation method of the artistic ceramic according to any one of claims 6 to 9.

Citation Information

Patent Citations

  • Powdered frit decorative porcelain

    CN101244952A

  • Preparation method of B2O3-TiO2 series fambe ceramic crystalline glaze

    CN102173875A

  • Leadless environmentally-friendly glass glaze, preparation method thereof, and glazed surface preparation method

    CN103466948A

  • Preparation method for ultralow temperature glaze

    CN103910537A

  • Environment-friendly acid-pollution-free etching glaze as well as preparation method and application thereof

    CN112897882A