Method for synergistically preparing high-added-value gypsum product through deep iron removal of high-iron gypsum
By pretreating high-iron gypsum in inorganic acid solution and dissolving-recrystallization in salt solution, combined with the use of crystal form regulators, the problem of iron impurities removal in high-iron gypsum was successfully solved, and the preparation and resource utilization of high-value-added gypsum was achieved. use.
Patent Information
- Application Number
- CN202410544881.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-05-06
AI Technical Summary
The prior art is difficult to deeply remove iron impurities in high-iron gypsum, resulting in limited resource utilization of titanium gypsum. The existing methods are complex in technology, high in cost and cannot effectively remove iron impurities inside gypsum inclusions and between particles.
By pretreating high-iron gypsum in an inorganic acid solution, the iron content is reduced, and then heating it in the salt solution system and adding crystal form regulators to carry out the dissolution-recrystallization process to regulate the morphology and particle size of the gypsum to achieve iron impurities Deep removal and preparation of high value added gypsum.
The deep removal of iron impurities in high-iron gypsum was achieved, and a high-value-added gypsum product with an iron content of less than 5 mg/g was obtained. The drying compressive strength exceeded 20MPa and the conversion rate reached more than 99%.
Smart Images

Figure CN118978353A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical solid waste treatment and disposal, and specifically relates to a method for deeply and efficiently removing iron impurities in high-iron gypsum and converting it into high-value alpha-hemihydrate gypsum. Background Art
[0002] High-iron gypsum mainly refers to titanium gypsum, which is an industrial solid waste discharged when titanium dioxide is produced by sulfuric acid method. Its main component is calcium sulfate dihydrate. About 5-6 tons of titanium gypsum are produced for every ton of titanium dioxide. At present, the emission of titanium gypsum in my country is about 18 million tons / a, and the utilization rate is only 10%. The large amount of idle titanium gypsum piled up causes serious pollution to the surrounding soil, water and atmosphere, and ultimately affects human health. In the process of producing titanium dioxide by sulfuric acid method of titanium concentrate, the iron in the raw material will enter the titanium dioxide waste acid with the liquid phase, and the titanium dioxide waste acid will be converted into iron-containing titanium gypsum after lime neutralization. The presence of iron impurities makes titanium gypsum appear dark green or red after iron oxidation, which affects the appearance and performance of titanium gypsum, making it much more difficult to utilize titanium gypsum as a resource. For this reason, the main use of titanium gypsum is still limited to cement retarders, wall materials, composite cementitious materials, etc., with a narrow scope of application and low product added value. Therefore, the deep removal of iron impurities in titanium gypsum can greatly broaden and deepen the scope and level of its resource utilization.
[0003] Patent CN116655270A discloses a method for preparing building gypsum by pre-treating titanium gypsum with acidic wastewater using a sulfuric acid process. This method treats the titanium gypsum with acid washing, and then obtains the building gypsum through calcination, aging and modification with an admixture, which improves the resource utilization rate of the titanium gypsum to a certain extent. However, calcination brings about higher energy consumption, and the main component of the obtained building gypsum is β-hemihydrate gypsum of lower value.
[0004] Patent CN114349039A discloses a method for regulating the crystal morphology and particle size of α-hemihydrate gypsum in a solution system. The method prepares α-hemihydrate gypsum with high purity and high strength by adding crystal seeds for regulation, but the patent does not involve the step-by-step removal of iron and the control of the appropriate range of iron in the removal process. At the same time, there are reports in the prior art (such as patent CN117626398A): titanium gypsum is different from desulfurized gypsum. Desulfurized gypsum contains very few impurities such as iron hydroxide, magnesium hydroxide, metatitanic acid, and aluminum hydroxide, while titanium gypsum contains a large amount of impurities such as iron, silicon, titanium, magnesium, and aluminum. These impurities do not all exist in the form of free ions, but exist in large quantities in the form of hydroxides, oxide solid particles and / or colloids. These impurities will have a strong common inhibitory effect on the preparation of hemihydrate gypsum whiskers from titanium gypsum.
[0005] Patent CN117626398A discloses a method for preparing semi-hydrated gypsum whiskers using titanium gypsum in an ethylene glycol-water system. The patent involves first removing impurities with sulfuric acid until the iron content is 1-5 mg / g, the silicon content is 0.5-2 mg / g, the titanium content is 0.5-1 mg / g, the magnesium content is 0.1-0.5 mg / g, and the aluminum content is 0-0.05 mg / g. Then, a suspension having a content of 1.5wt% to 3wt% of the removed titanium gypsum is prepared in the ethylene glycol-water system. Then, a long-term reaction (such as 5-8 hours as exemplified in the embodiment) is carried out at 90-100°C to obtain the semi-hydrated gypsum whiskers.
[0006] The present invention uses high-iron gypsum (titanium gypsum) as the treatment object. During the research and development process, it was found that when the raw material high-iron gypsum (titanium gypsum) is added to an inorganic acid solution for pretreatment to an iron content of 1.0wt% to 5.0wt%, the formation of hemihydrate gypsum can be accelerated by relying on a salt solution system with a pH of 1.0 to 2.5. Based on this, the present invention was formed.
[0007] The present invention develops a method with simple process, low cost, deep removal of iron impurities and preparation of high value-added gypsum products, which is of great significance for the comprehensive utilization of titanium gypsum. It solves the problems that the current methods for removing iron impurities from high-iron gypsum (titanium gypsum) are generally complicated, costly and unable to effectively remove iron impurities inside gypsum inclusions and between particles, and also overcomes some technical prejudices formed in this field. Summary of the invention
[0008] In view of this, the present invention provides a method for deeply removing iron impurities in high-iron gypsum and preparing high-quality and high-value-added gypsum products.
[0009] As a preferred embodiment, the present invention provides a method for deep iron removal of high-iron gypsum to prepare high-value-added gypsum products, comprising the following steps:
[0010] (1) adding raw material high iron gypsum to an inorganic acid solution for pretreatment, stirring sufficiently for a period of time to separate the solid and liquid, and separating the solid phase to obtain the pretreated high iron gypsum, wherein the iron content of the pretreated high iron gypsum is 1.0 wt% to 5.0 wt%; the iron content of the raw material high iron stone in step (1) is greater than 5 wt%;
[0011] (2) adding the pretreated high-iron gypsum to a salt solution system and mixing to form a gypsum suspension slurry; in the salt solution system, the salt is selected from at least one of soluble sulfate, hydrochloride, and nitrate, preferably sulfate, and the salt concentration in the salt solution system is 10wt%-20wt%; the solid content of the obtained gypsum suspension slurry is 5%-30%; the pH value of the salt solution is 1.0-2.5;
[0012] (3) heating the gypsum suspension slurry to above 90° C., adding a crystal form regulator, and stirring and reacting at this temperature, wherein the crystal form regulator is a short columnar α-hemihydrate gypsum crystal, and the particle size of the crystal form regulator is 12-65 μm;
[0013] (4) After a period of reaction, the suspended slurry is separated into solid and liquid while hot, and the separated solid phase is washed with boiling water and dried to obtain a high-purity and high-value-added gypsum product.
[0014] The separated liquid phase is returned to constitute an important component of the aqueous solution system after treatment.
[0015] As a preferred embodiment, the present invention provides a method for recovering titanium from high-iron gypsum and preparing a high-value-added gypsum product, wherein in step (1), the iron content in the raw material high-iron gypsum is <25wt% and >5wt%, and the content of calcium sulfate dihydrate (CaSO4·2H2O) is >70%.
[0016] As a preferred embodiment, the present invention provides a method for recovering titanium from high-iron gypsum and preparing a high-value-added gypsum product, wherein the raw material high-iron gypsum can be titanium gypsum.
[0017] As a preferred embodiment, the present invention provides a method for recovering titanium from high-iron gypsum and preparing a high-value-added gypsum product, wherein the inorganic acid solution in step (1) is one or more of sulfuric acid, hydrochloric acid or nitric acid, preferably sulfuric acid, and the pH value of the inorganic acid solution is 1.0-5.0, preferably 1.0-4.0, further preferably 1.0-3.0, and further preferably 1.5-2.5.
[0018] As a preferred embodiment, the present invention provides a method for recovering titanium from high-iron gypsum and preparing a high-value-added gypsum product, wherein the pretreatment temperature in step (1) is ≤40°C, preferably 20-40°C, the pretreatment solid-liquid ratio (g / mL) is 1 / 5-1 / 20, preferably 1 / 7-1 / 20, and the pretreatment time is 15-60 min.
[0019] In the present invention, during pretreatment, the temperature cannot be too high, otherwise it is not conducive to controlling the iron content in the pretreated high-iron gypsum. During pretreatment, the hydrogen ion concentration in the inorganic acid solution cannot be too high, otherwise it is not conducive to controlling the iron content in the pretreated high-iron gypsum.
[0020] In step (1) of the present invention, a large amount of inorganic acid with a relatively low concentration is used to controllably pretreat the raw material high-iron gypsum (titanium gypsum), preliminarily remove part of the iron impurities in the high-iron gypsum, and keep the iron content in the high-iron gypsum within a certain range; the advantage of doing so is that if the iron content in the high-iron gypsum is too high, the subsequent phase change reaction will be hindered, making it impossible to transform the dihydrate gypsum into α-hemihydrate gypsum; if the iron content in the high-iron gypsum is too low, the phase change rate will be affected, resulting in a prolonged phase change time, or even the inability to complete the phase change.
[0021] The iron content in the pretreated high-iron gypsum in step (2) is greater than or equal to 1.0wt%, preferably between 1.0wt% and 5.0wt%, the pH value of the salt solution is 1.0-2.5, and the solid content (mass percentage) in the gypsum suspension slurry is 5%-30%, preferably 15-30%, and more preferably 20-25%.
[0022] As a preferred embodiment, the present invention provides a method for recovering titanium from high-iron gypsum and preparing a high-value-added gypsum product, wherein the liquid phase separated in step (1) can be reused.
[0023] The iron content in the pretreated high-iron gypsum obtained in step (1) is 1.0wt% to 3.0wt%.
[0024] In step (2), the solid content (mass percentage) of the gypsum suspension slurry is 5%-30%, preferably 15-30%, and more preferably 20-25%.
[0025] In step (2) of the present invention, the concentration of the salt solution system is controlled to be 10wt%-20wt% and the solid content (mass percentage) in the obtained gypsum suspension slurry is controlled to be 5%-30%, preferably 15-30%, and more preferably 20-25% in order to ensure that the phase change process of dihydrate gypsum to α-hemihydrate gypsum is carried out normally and a high-quality gypsum product with a low iron content can be obtained, while controlling the cost of the processing process. Too low salt concentration will cause the phase change process of dihydrate gypsum to α-hemihydrate gypsum to fail to proceed, and too high salt concentration will cause too many impurity salt ions to enter the final gypsum product, reducing the quality of the gypsum product. Too high solid content will reduce the removal efficiency of iron impurities and make it impossible to achieve deep iron removal. Too low solid content will cause excessive acidic liquid to be produced, and the processing cost is high.
[0026] The reaction temperature in step (3) is 90-105°C, preferably 95-100°C, and the stirring rate is 100-300 rpm.
[0027] In step (3), the amount of the crystal modifier added is 9.5%-30% of the mass of the pretreated high-iron gypsum, preferably 10%-20%, and more preferably 11.5-17%.
[0028] The reaction time in step (4) is 30 min-60 min.
[0029] As a preferred embodiment, the present invention provides a method for preparing high-value-added gypsum products by deep iron removal of high-iron gypsum, wherein the crystal form regulator is a short columnar α-hemihydrate gypsum crystal with regular morphology, and its average aspect ratio is less than or equal to 4.0, and the addition amount is 9.5%-30% of the mass of the pretreated high-iron gypsum, and the particle size of the crystal form regulator is preferably 20-50μm. The main reason for controlling the morphology and particle size of the crystal form regulator in the present invention is that the morphology and size of the crystal form regulator directly affect the morphology and size of the gypsum product. The ideal gypsum product is a large-size short columnar crystal. On the one hand, such a product has a small specific surface area and weak adsorption, which inhibits the surface adsorption of iron impurities by the gypsum product. On the other hand, the standard consistency has low water demand and high mechanical strength, and is a high-value-added high-strength gypsum product. A crystal form regulator with a small aspect ratio can induce a short columnar gypsum product with a small aspect ratio, while a large-grained crystal form regulator can induce a large-grained gypsum product. However, if the crystal form regulator has a large particle size, the amount added is large, which is unreasonable in cost. Therefore, it is necessary to control the morphology and size of the crystal form regulator. In the present invention, if too little crystal form regulator is added, it is difficult to synergize with the reserved iron. If the amount added is too large, the residual iron in the product will increase, thereby affecting the performance of the final product.
[0030] As a preferred embodiment, the present invention provides a method for deep iron removal of high-iron gypsum and synergistic preparation of high-value-added gypsum products. If the gypsum product produced in this process is short columnar α-hemihydrate gypsum crystals with regular morphology, with an average aspect ratio of less than or equal to 4.0 and a particle size of 20-50 μm, then this gypsum product can also be used as a crystal form regulator.
[0031] The iron content in the gypsum product obtained by the present invention is less than 5 mg / g, and the iron content is less than 2 mg / g after optimization.
[0032] The drying compressive strength of the gypsum product obtained by the present invention is greater than 20MPa, and after optimization, the drying compressive strength can be greater than 40MPa.
[0033] The present invention first removes part of the iron impurities in the high-iron gypsum by acid leaching pretreatment, and then fully releases the iron impurities in the gypsum inclusions and the lattice through the dissolution process regulated by the gypsum phase, and at the same time regulates the existence form of iron in the solution to prevent it from entering the gypsum lattice again during the recrystallization process, and reduces the adsorption of iron on the surface of the gypsum product by adding a crystal form regulator to regulate the morphology and particle size of the recrystallized product, and finally achieves efficient separation of iron impurities and gypsum products by releasing iron impurities and weakening the eutectic and adsorption effect of iron, and simultaneously forms high-purity and high-strength α-hemihydrate gypsum. The present invention realizes the synergy of deep iron removal of high-iron gypsum and preparation of high-value-added gypsum products.
[0034] Rationale
[0035] The present invention creatively combines sulfuric acid leaching and phase reconstruction. The high-iron gypsum is first pretreated with sulfuric acid leaching to reduce the iron content to a certain range. The iron impurities inside the gypsum inclusions are then removed through phase reconstruction, ultimately achieving rapid and deep removal of iron impurities in the high-iron gypsum.
[0036] In the sulfuric acid leaching pretreatment process, in addition to reducing the iron content in the high-iron gypsum to ensure the normal phase transformation of dihydrate gypsum to α-hemihydrate gypsum, it is also necessary to ensure that the iron impurities in the high-iron gypsum have a certain content (such as 1.0wt% to 5.0wt%), and the iron content cannot be too low, because the presence of iron impurities can provide nodule sites to a certain extent, which is beneficial to the formation of hemihydrate gypsum crystal nuclei, promote the phase change reaction, increase the phase change rate, and shorten the phase change time.
[0037] Under normal pressure, dihydrate gypsum can be transformed into α-hemihydrate gypsum in a salt solution at a certain temperature (above 90°C). This process is a dissolution-recrystallization process. The dissolution process will release the iron impurities in the dihydrate gypsum inclusions into the liquid phase. During the recrystallization process, the particle size and morphology of the gypsum crystal product are regulated by adding a crystal form regulator to form a large-grained crystalline product with a regular morphology, thereby effectively weakening the adsorption of iron in the liquid phase on the surface of the recrystallized gypsum product. At the same time, the addition of acid can effectively dissolve iron impurities on the one hand, and on the other hand, it can regulate the existence form of iron in the solution. Iron in the solution is mainly in the form of FeSO4 + and Fe(SO4)2 - The iron impurities exist in the form of α-hemihydrate gypsum, making it difficult for them to enter the crystal lattice during the recrystallization process of α-hemihydrate gypsum, thereby promoting the migration of iron impurities into the solution and further improving the iron removal rate. Ultimately, based on the complete release of iron impurities by phase transformation, the weakening of iron surface adsorption by crystal form regulation, and the inhibition of iron entering the crystal lattice by iron form regulation, the deep removal of iron impurities in high-iron gypsum is achieved, and high-value-added α-hemihydrate gypsum products are produced.
[0038] Advantages of the Invention
[0039] The present invention can achieve deep removal of iron in high-iron gypsum, and the iron content in the obtained gypsum product is less than 5 mg / g, and the iron content is less than 2 mg / g after optimization.
[0040] The product obtained by the present invention is a high-value-added gypsum product with a drying compressive strength of >20MPa, and after optimization, the drying compressive strength can be >40MPa.
[0041] The invention realizes the unification of deep iron removal of high-iron gypsum and preparation of high value-added gypsum products, and the conversion rate of alpha-hemihydrate gypsum is greater than or equal to 99%. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] The accompanying drawings are only suitable for further understanding of the patent application scheme and constitute a part of the specification. Together with the application implementation cases, they are used to explain the technical method of the patent application and do not constitute a limitation on the application technical scheme.
[0043] Figure 1 It is a technical flow chart of the present invention;
[0044] Figure 2 The microscopic morphology of the crystal form regulator used in Examples 1, 2 and Comparative Examples 1, 4, and 5;
[0045] Figure 3 This is a microscopic morphology of the gypsum product obtained in Example 1;
[0046] Figure 4 This is a microscopic morphology of the gypsum product obtained in Example 2;
[0047] Figure 5 This is the microscopic morphology of the gypsum product obtained in Comparative Example 1;
[0048] Figure 6 This is the microscopic morphology of the gypsum product obtained in Comparative Example 2;
[0049] Figure 7 This is a microscopic morphology of the gypsum product obtained in Comparative Example 3;
[0050] Figure 8 This is a microscopic morphology of the gypsum product obtained in Comparative Example 4;
[0051] Fig. 9 This is a microscopic morphology of the gypsum product obtained in Comparative Example 5;
[0052] Fig.10 The microscopic morphology of the crystal form regulator used in Examples 3, 4 and Comparative Examples 6, 7, and 8;
[0053] Fig.11 This is a microscopic morphology of the gypsum product obtained in Example 3;
[0054] Fig.12 This is a microscopic morphology of the gypsum product obtained in Comparative Example 6;
[0055] Fig.13 This is a microscopic morphology of the gypsum product obtained in Example 4;
[0056] Fig.14 This is a microscopic morphology of the gypsum product obtained in Comparative Example 7;
[0057] Fig.15 This is the microscopic morphology of the gypsum product obtained in Comparative Example 8.
[0058] from Figure 1 The basic process of the present invention can be seen.
[0059] from Figure 2 The microscopic morphology of the crystal form regulator can be seen in the figure. Specifically, the crystal form regulator is a short columnar α-hemihydrate gypsum crystal with regular morphology, an average aspect ratio of 0.6, and a particle size of 35 μm.
[0060] from Figure 3 It can be seen that the gypsum product obtained in Example 1 is evenly distributed short columnar crystals.
[0061] from Figure 4 It can be seen that the gypsum product obtained in Example 2 is evenly distributed short columnar crystals.
[0062] from Figure 5 It can be seen that the gypsum product obtained in Comparative Example 1 is finely broken plate-like or block-like crystals.
[0063] from Figure 6 It can be seen that the gypsum product obtained in Comparative Example 2 is long rod-shaped crystals.
[0064] from Figure 7 It can be seen that the gypsum product obtained in Comparative Example 3 is long rod-shaped crystals.
[0065] from Figure 8 It can be seen that the gypsum product obtained in Comparative Example 4 is mainly plate-like crystals with occasional columnar crystals, indicating that most of the crystals have not undergone phase changes.
[0066] from Fig. 9 It can be seen that the gypsum product obtained in Comparative Example 5 is long rod-shaped crystals.
[0067] from Fig.10 The microscopic morphology of the crystal form regulator can be seen in the figure. Specifically, the crystal form regulator is a short columnar α-hemihydrate gypsum crystal with regular morphology, an average aspect ratio of 1.1, and a particle size of 30 μm.
[0068] from Fig.11 It can be seen that the gypsum product obtained in Example 3 is evenly distributed short columnar crystals.
[0069] from Fig.12 It can be seen that the gypsum product obtained in Comparative Example 6 is extremely unevenly distributed long rod-shaped and short columnar crystals.
[0070] from Fig.13 It can be seen that the gypsum product obtained in Example 4 is evenly distributed short columnar crystals.
[0071] from Fig.14 It can be seen that the gypsum product obtained in Comparative Example 7 is mainly plate-like crystals with occasional columnar crystals, indicating that most of the crystals have not undergone phase changes.
[0072] from Fig.15 It can be seen that the gypsum product obtained in Comparative Example 8 is a mixture of short columnar and finely divided needle-shaped crystals. DETAILED DESCRIPTION
[0073] The technical solution of the present application is further described below in conjunction with specific implementation cases, but the protection scope of the present invention is not limited thereto.
[0074] Example 1
[0075] Table 1 Main element composition and proportion in raw material high iron gypsum (titanium gypsum)
[0076]
[0077] according to Figure 1 According to the process flow shown, 600 mL of sulfuric acid solution with a pH of 2 is prepared and added to the pretreatment tank, 60 g of high-iron gypsum (element composition is shown in Table 1) is added thereto, and leaching is stirred for 30 minutes at room temperature. After solid-liquid separation, pretreated high-iron gypsum (iron content is 1.30 wt%) is obtained. A 12 wt% sodium sulfate solution is prepared, and its pH is adjusted to 1 with sulfuric acid. 50 g of pretreated high-iron gypsum is added to the sodium sulfate solution and mixed to form a suspension slurry with a solid mass fraction of 20%. The suspension slurry is added to a three-necked round-bottom flask, the reaction temperature is set to 95°C, the stirring rate is 120 rpm, and when the temperature of the suspension slurry reaches the set temperature, 8 g of a crystal form regulator (such as Figure 2 The crystal modifier is a regular α-hemihydrate gypsum crystal with an average aspect ratio of 0.6 and a particle size of 35 μm. After reacting for 45 minutes, the solid-liquid separation is immediately carried out while hot. The separated solid phase is washed with boiling water and transferred to a 60°C oven to be dried to constant weight. The microscopic morphology of the gypsum product is as follows: Figure 3 As shown, the iron content is 1.73 mg / g, the drying compressive strength is 40.36 MPa, and the conversion rate of α-hemihydrate gypsum is as high as 99.11%.
[0078] Conversion rate calculation method:
[0079]
[0080] Among them, m a is the theoretical mass of raw materials completely converted into α-hemihydrate gypsum, m 原 is the weight of raw materials, M g is the relative molecular mass of dihydrate gypsum, M b is the relative molecular mass of α-hemihydrate gypsum.
[0081]
[0082] Among them, x is the conversion rate, m a is the theoretical mass of raw materials completely converted into α-hemihydrate gypsum, m b is the mass of α-hemihydrate gypsum in the final product.
[0083] M 原 =60g, M g =172 g / mol, M b =145 g / mol, m b =58.06g Substituting into the above formula, the conversion rate x is 99.11%.
[0084] Example 2
[0085] according to Figure 1 According to the process flow shown, 600 mL of sulfuric acid solution with a pH of 3 is prepared and added to the pretreatment tank, 100 g of high-iron gypsum (element composition is shown in Table 1) is added thereto, and leaching is carried out under stirring for 30 minutes at room temperature. After solid-liquid separation, pretreated high-iron gypsum (iron content is 1.56 wt%) is obtained. A 16 wt% potassium sulfate solution is prepared, and its pH is adjusted to 2 with sulfuric acid. 50 g of pretreated high-iron gypsum is added to the potassium sulfate solution and mixed to form a suspension slurry with a solid mass fraction of 25%. The suspension slurry is added to a three-necked round-bottom flask, the reaction temperature is set to 97°C, the stirring rate is 100 rpm, and when the temperature of the suspension slurry reaches the set temperature, 6 g of a crystal form regulator (such as Figure 2 The crystal modifier is a regular α-hemihydrate gypsum crystal with an average aspect ratio of 0.6 and a particle size of 35 μm. After reacting for 50 minutes, the solid-liquid separation is immediately carried out while hot. The separated solid phase is washed with boiling water and transferred to a 60°C oven to be dried to constant weight. The microscopic morphology of the gypsum product is as follows: Figure 4 As shown, its iron content is 3.46 mg / g and its drying compressive strength is 37.83 MPa.
[0086] Comparative Example 1
[0087] according to Figure 1 According to the process flow shown, 600 mL of deionized water is added to the pretreatment tank, 60 g of high-iron gypsum (element composition is shown in Table 1) is added thereto, and the mixture is stirred and leached for 30 minutes at room temperature. After solid-liquid separation, pretreated high-iron gypsum (iron content is 6.67 wt%) is obtained. A 12 wt% sodium sulfate solution is prepared, and its pH is adjusted to 1 with sulfuric acid. 50 g of pretreated high-iron gypsum is added to the sodium sulfate solution and mixed to form a suspension slurry with a solid mass fraction of 20%. The suspension slurry is added to a three-necked round-bottom flask, the reaction temperature is set to 95 ° C, the stirring rate is 120 rpm, and when the temperature of the suspension slurry reaches the set temperature, 8 g of a crystal form regulator (such as Figure 2 The crystal modifier is a regular α-hemihydrate gypsum crystal with an average aspect ratio of 0.6 and a particle size of 35 μm. After reacting for 45 minutes, the solid-liquid separation is immediately carried out while hot. The separated solid phase is washed with boiling water and transferred to a 60°C oven to be dried to constant weight. The microscopic morphology of the gypsum product is as follows: Figure 5 As shown, its iron content is 36.37 mg / g, and its main component is dihydrate gypsum, which has no gelling properties and no compressive strength.
[0088] Comparative Example 2
[0089] according to Figure 1 According to the process flow shown, 600 mL of sulfuric acid solution with a pH of 2 is prepared and added to the pretreatment tank. 60 g of high-iron gypsum (element composition is shown in Table 1) is added thereto. Stirring and leaching are carried out at room temperature for 30 minutes. After solid-liquid separation, pretreated high-iron gypsum (iron content is 1.30 wt%) is obtained. A 12 wt% sodium sulfate solution is prepared, and its pH is adjusted to 1 with sulfuric acid. 50 g of pretreated high-iron gypsum is added to the sodium sulfate solution and mixed to form a suspension slurry with a solid mass fraction of 20%. The suspension slurry is added to a three-necked round-bottom flask, the reaction temperature is set to 95°C, the stirring rate is 120 rpm, and no crystal modifier is added. After reacting for 45 minutes, solid-liquid separation is immediately carried out while hot. The separated solid phase is washed with boiling water and transferred to a 60°C oven to be dried to constant weight to obtain the microscopic morphology of the gypsum product as shown below. Figure 6 As shown, its iron content is 8.66 mg / g and its drying compressive strength is 8.62 MPa.
[0090] Comparative Example 3
[0091] according to Figure 1 According to the process flow shown, 600 mL of sulfuric acid solution with a pH of 2 is prepared and added to the pretreatment tank. 60 g of high-iron gypsum (element composition is shown in Table 1) is added thereto. Stirring and leaching are carried out at room temperature for 30 minutes. After solid-liquid separation, pretreated high-iron gypsum (iron content is 1.30 wt%) is obtained. A 12 wt% sodium sulfate solution is prepared, and its pH is adjusted to 3 with sulfuric acid. 50 g of pretreated high-iron gypsum is added to the sodium sulfate solution and mixed to form a suspension slurry with a solid mass fraction of 20%. The suspension slurry is added to a three-necked round-bottom flask, the reaction temperature is set to 95°C, the stirring rate is 120 rpm, and no crystal modifier is added. After reacting for 45 minutes, solid-liquid separation is immediately carried out while hot. The separated solid phase is washed with boiling water and transferred to a 60°C oven to dry to constant weight to obtain a gypsum product with a microscopic morphology as shown below. Figure 7 As shown, its iron content is 10.39 mg / g and its drying compressive strength is 5.50 MPa.
[0092] Comparative Example 4
[0093] according to Figure 1According to the process flow shown, 600 mL of sulfuric acid solution with a hydrogen ion concentration of 0.4 mol / L is prepared and added to the pretreatment tank, 60 g of high-iron gypsum (element composition is shown in Table 1) is added thereto, and leaching is stirred for 30 minutes at room temperature. After solid-liquid separation, pretreated high-iron gypsum (iron content is 0.52 wt%) is obtained. A 12 wt% sodium sulfate solution is prepared, and its pH is adjusted to 1 with sulfuric acid. 50 g of pretreated high-iron gypsum is added to the sodium sulfate solution and mixed to form a suspension slurry with a solid mass fraction of 20%. The suspension slurry is added to a three-necked round-bottom flask, the reaction temperature is set to 95°C, the stirring rate is 120 rpm, and when the temperature of the suspension slurry reaches the set temperature, 8 g of a crystal form regulator (such as Figure 2 The crystal modifier is a regular α-hemihydrate gypsum crystal with an average aspect ratio of 0.6 and a particle size of 35 μm. After reacting for 45 minutes, the solid-liquid separation is immediately carried out while hot. The separated solid phase is washed with boiling water and transferred to a 60°C oven to be dried to constant weight. The microscopic morphology of the gypsum product is as follows: Figure 8 As shown, its iron content is 4.76 mg / g, and its main component is dihydrate gypsum, which has no gelling properties and no compressive strength.
[0094] Comparative Example 5
[0095] according to Figure 1 According to the process flow shown, 600 mL of sulfuric acid solution with a pH of 2 is prepared and added to the pretreatment tank, 60 g of high-iron gypsum (element composition is shown in Table 1) is added thereto, and leaching is stirred for 30 minutes at room temperature. After solid-liquid separation, pretreated high-iron gypsum (iron content is 1.30 wt%) is obtained. A 12 wt% sodium sulfate solution is prepared, and its hydrogen ion concentration is adjusted to 0.4 mol / L with sulfuric acid. 50 g of pretreated high-iron gypsum is added to the sodium sulfate solution and mixed to form a suspension slurry with a solid mass fraction of 20%. The suspension slurry is added to a three-necked round-bottom flask, the reaction temperature is set to 95°C, the stirring rate is 120 rpm, and when the temperature of the suspension slurry reaches the set temperature, 8 g of a crystal form regulator (such as Figure 2 The crystal modifier is a regular α-hemihydrate gypsum crystal with an average aspect ratio of 0.6 and a particle size of 35 μm. After reacting for 45 minutes, the solid-liquid separation is immediately carried out while hot. The separated solid phase is washed with boiling water and transferred to a 60°C oven to be dried to constant weight. The microscopic morphology of the gypsum product is as follows: Fig. 9 As shown, its iron content is 7.79 mg / g and its drying compressive strength is 9.13 MPa.
[0096] Example 3
[0097] according to Figure 1 According to the process flow shown in the figure, 600 mL of hydrochloric acid solution with a pH of 5 was prepared and added to the pretreatment tank, and 60 g of high-iron gypsum (element composition is shown in Table 2) was added thereto.
[0098] Table 2 Main element composition and proportion in raw material high iron gypsum (titanium gypsum)
[0099]
[0100] Stir and leach for 20 minutes at room temperature, and obtain pretreated high-iron gypsum (iron content is 2.96wt%) after solid-liquid separation. Prepare a 12wt% sodium chloride solution, and adjust its pH to 2 with hydrochloric acid. Add 50g of pretreated high-iron gypsum to the sodium chloride solution and mix well to form a suspension slurry with a solid mass fraction of 15%. Add the suspension slurry to a three-necked round-bottom flask, set the reaction temperature to 97°C, and the stirring rate to 150rpm. When the temperature of the suspension slurry reaches the set temperature, add 10g of a crystal modifier (such as Fig.10 The crystal modifier is a regular α-hemihydrate gypsum crystal with an average aspect ratio of 1.1 and a particle size of 30 μm. After 60 minutes of reaction, solid-liquid separation is immediately performed while hot. The separated solid phase is washed with boiling water and transferred to a 60°C oven to be dried to constant weight. The microscopic morphology of the gypsum product is as follows: Fig.11 As shown, its iron content is 6.58 mg / g and its drying compressive strength is 31.44 MPa.
[0101] Comparative Example 6
[0102] according to Figure 1 According to the process flow shown, 600 mL of hydrochloric acid solution with a pH of 5 is prepared and added to the pretreatment tank. 60 g of high-iron gypsum (element composition is shown in Table 2) is added thereto. Stir and leach for 20 minutes at room temperature. After solid-liquid separation, pretreated high-iron gypsum (iron content is 2.96 wt%) is obtained. A 12 wt% sodium chloride solution is prepared, and its pH is adjusted to 2 with hydrochloric acid. 50 g of pretreated high-iron gypsum is added to the sodium chloride solution and mixed to form a suspension slurry with a solid mass fraction of 15%. The suspension slurry is added to a three-necked round-bottom flask, the reaction temperature is set to 97°C, the stirring rate is 150 rpm, and when the temperature of the suspension slurry reaches the set temperature, 4.5 g of a crystal form regulator (such as Fig.10 The crystal modifier is a regular α-hemihydrate gypsum crystal with an average aspect ratio of 1.1 and a particle size of 30 μm. After 60 minutes of reaction, solid-liquid separation is immediately performed while hot. The separated solid phase is washed with boiling water and transferred to a 60°C oven to be dried to constant weight. The microscopic morphology of the gypsum product is as follows: Fig.12 As shown, its iron content is 12.06 mg / g and its drying compressive strength is 11.86 MPa.
[0103] Example 4
[0104] according to Figure 1According to the process flow shown, 600 mL of hydrochloric acid solution with a pH of 4 is prepared and added to the pretreatment tank, 80 g of high-iron gypsum (element composition is shown in Table 2) is added thereto, and leaching is stirred for 20 minutes at room temperature. After solid-liquid separation, pretreated high-iron gypsum (iron content is 2.52 wt%) is obtained. A 15% sodium nitrate solution is prepared, and its pH is adjusted to 3 with nitric acid. 50 g of pretreated high-iron gypsum is added to the sodium nitrate solution and mixed to form a suspension slurry with a solid mass fraction of 20%. The suspension slurry is added to a three-necked round-bottom flask, the reaction temperature is set to 95°C, the stirring rate is 120 rpm, and when the temperature of the suspension slurry reaches the set temperature, 7 g of a crystal form regulator (such as Fig.10 The crystal modifier is a regular α-hemihydrate gypsum crystal with an average aspect ratio of 1.1 and a particle size of 30 μm. After 60 minutes of reaction, solid-liquid separation is immediately performed while hot. The separated solid phase is washed with boiling water and transferred to a 60°C oven to be dried to constant weight. The microscopic morphology of the gypsum product is as follows: Fig.13 As shown, its iron content is 3.51 mg / g and its drying compressive strength is 35.69 MPa.
[0105] Comparative Example 7
[0106] according to Figure 1 According to the process flow shown, 600 mL of hydrochloric acid solution with a pH of 1 is prepared and added to the pretreatment tank, 60 g of high-iron gypsum (element composition is shown in Table 2) is added thereto, and leaching is stirred for 30 minutes at room temperature. After solid-liquid separation, pretreated high-iron gypsum (iron content is 0.66 wt%) is obtained. A 15% sodium nitrate solution is prepared, and its pH is adjusted to 3 with nitric acid. 50 g of pretreated high-iron gypsum is added to the sodium nitrate solution and mixed to form a suspension slurry with a solid mass fraction of 20%. The suspension slurry is added to a three-necked round-bottom flask, the reaction temperature is set to 95°C, the stirring rate is 120 rpm, and when the temperature of the suspension slurry reaches the set temperature, 7 g of a crystal form regulator (such as Fig.10 The crystal modifier is a regular morphology of α-hemihydrate gypsum crystals, with an average aspect ratio of 1.1 and a particle size of 30 μm). After 90 minutes of reaction, solid-liquid separation is immediately carried out while hot. The separated solid phase is washed with boiling water and transferred to a 60°C oven to be dried to constant weight. The microscopic morphology of the gypsum product is as follows: Fig.14 As shown, its iron content is 5.70 mg / g, and its main component is dihydrate gypsum, which has no gelling property and no compressive strength.
[0107] Comparative Example 8
[0108] according to Figure 1According to the process flow shown, 600 mL of hydrochloric acid solution with a pH of 4 is prepared and added to the pretreatment tank, 80 g of high-iron gypsum (element composition is shown in Table 2) is added thereto, and leaching is stirred for 20 minutes at room temperature. After solid-liquid separation, pretreated high-iron gypsum (iron content is 2.52 wt%) is obtained. A 15% sodium nitrate solution is prepared, and its pH is adjusted to 3 with nitric acid. 50 g of pretreated high-iron gypsum is added to the sodium nitrate solution and mixed to form a suspension slurry with a solid mass fraction of 20%. The suspension slurry is added to a three-necked round-bottom flask, the reaction temperature is set to 95°C, the stirring rate is 120 rpm, and when the temperature of the suspension slurry reaches the set temperature, 7 g of a crystal form regulator (such as Fig.10 The crystal modifier is a regular α-hemihydrate gypsum crystal with an average aspect ratio of 1.1 and a particle size of 30 μm. After 80 minutes of reaction, solid-liquid separation is immediately performed while hot. The separated solid phase is washed with boiling water and transferred to a 60°C oven to dry to constant weight. The microscopic morphology of the gypsum product is as follows: Fig.15 As shown, after the phase transition time is extended, the crystals will continue to develop into fine needle-shaped crystals with an iron content of 10.09 mg / g and a drying compressive strength of 14.85 MPa.
Claims
1. A method for deep iron removal of high-iron gypsum and synergistic preparation of high value-added gypsum products, It is characterized in that The following steps are involved: (1) adding raw material high iron gypsum to an inorganic acid solution for pretreatment, stirring sufficiently for a period of time, and then separating the solid and the liquid. The separated solid phase is the pretreated high iron gypsum, and the iron content of the pretreated high iron gypsum is 1.0 wt%~5.0 wt%; the iron content of the raw material high iron stone in step (1) is >5wt%; (2) adding the pretreated high-iron gypsum to a salt solution system and mixing them to form a gypsum suspension slurry; in the salt solution system, the salt is selected from at least one of soluble sulfate, hydrochloride, and nitrate, preferably sulfate, and the salt concentration in the salt solution system is 10wt%-20wt%; the solid content of the obtained gypsum suspension slurry is 5%-30%; the pH value of the salt solution is 1.0-2.5; (3) heating the gypsum suspension slurry to above 90° C., adding a crystal form regulator, and stirring and reacting at this temperature, wherein the crystal form regulator is a short columnar α-hemihydrate gypsum crystal, and the particle size of the crystal form regulator is 12-65 μm; (4) After a period of reaction, the suspended slurry is separated into solid and liquid while hot, and the separated solid phase is washed with boiling water and dried to obtain a high-purity and high-value-added gypsum product.
2. A method for recovering titanium from high-iron gypsum and preparing high-value-added gypsum products according to claim 1, Features: In the step (1), the iron content of the raw material high iron stone is <25wt% and >5wt%, and the content of calcium sulfate dihydrate is >70%.
3. A method for recovering titanium from high-iron gypsum and preparing high-value-added gypsum products according to claim 1, Features: The raw material high iron gypsum includes titanium gypsum.
4. A method for recovering titanium from high-iron gypsum and preparing high-value-added gypsum products according to claim 1, Features: The inorganic acid solution in step (1) is one or more of sulfuric acid, hydrochloric acid or nitric acid, preferably sulfuric acid, and the pH value of the inorganic acid solution is 1.0-5.0, preferably 1.0-4.0, more preferably 1.0-3.0, and even more preferably 1.5-2.
5.
5. A method for recovering titanium from high-iron gypsum and preparing high-value-added gypsum products according to claim 1, Features: In the step (1), the pretreatment temperature is ≤40°C, preferably 20-40°C, the pretreatment solid-liquid ratio (g / mL) is 1 / 5-1 / 20, preferably 1 / 7-1 / 20, and the pretreatment time is 15-60 min.
6. A method for recovering titanium from high-iron gypsum and preparing high-value-added gypsum products according to claim 1, Features: In step (2), the pH value of the salt solution is 1.0-2.5, and the solid content of the gypsum suspension slurry is 5%-30%, preferably 15-30%, and more preferably 20-25%.
7. A method for recovering titanium from high-iron gypsum and preparing high-value-added gypsum products according to claim 1, Features: The reaction temperature in step (3) is 90-105°C, preferably 95-100°C, and the stirring rate is 100-300 rpm.
8. A method for recovering titanium from high-iron gypsum and preparing high-value-added gypsum products according to claim 1, Features: In step (3), the amount of the crystal modifier added is 9.5%-30% of the mass of the pretreated high-iron gypsum, preferably 10%-20%.
9. A method for recovering titanium from high-iron gypsum and preparing high-value-added gypsum products according to claim 1, Features: The reaction time in step (4) is 30 min-60 min.
10. A method for recovering titanium from high-iron gypsum and preparing high-value-added gypsum products according to claim 1, Features: If the produced gypsum product is a short columnar α-hemihydrate gypsum crystal with regular morphology, an average aspect ratio of which is less than or equal to 4.0 and a particle size of 20-50 μm, then this gypsum product can also be used as a crystal form regulator.
11. A method for recovering titanium from high-iron gypsum and preparing high-value-added gypsum products according to claim 1, Features: The iron content of the obtained gypsum product is <5mg / g, and after optimization, the iron content is <2mg / g; The drying compressive strength of the obtained gypsum product is >20MPa, and after optimization, the drying compressive strength can be >40MPa.
Citation Information
Patent Citations
Method for preparing alpha-semi-hydrated gypsum from titanium gypsum
CN103086624A
Method for preparing high-strengthalpha-semihydratetitanium gypsum with industrial wastedihydratetitanium gypsum
CN103964716A
Method for removing iron and preparing green vanadium and iron-based pigment by using titanium white waste acid
CN113526886A
Method for deeply removing arsenic from arsenic gypsum
CN116812960A
Method for manufacturing high purity gypsum
JP2002029740A