Preparation method of photochromic superfine foaming gloves
In the preparation method of photochromic ultrafine foaming gloves, using stirring, maturation and photochromic solutions, the problem of incompatibility of existing photochromic glove materials and nitrile gloves is solved, and uniform color change on the surface of the gloves is achieved and wear-resistant effect, meeting the special needs of labor protection gloves.
Patent Information
- Application Number
- CN202411133911.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-19
AI Technical Summary
When existing photochromic gloves add photochromic materials to the nitrile glove latex system, the materials are incompatible with the aqueous system, resulting in a degradation of the surface performance of the gloves and the inability to form a uniform discolored film, which lacks wear resistance.
A method of preparing photochromic ultrafine foaming gloves is adopted. By stirring the latex after color adjustment, controlling the viscosity, preheating the glove core, immersing the coagulant and ultrafine foaming agent, maturing, and photochromic A uniform film is formed in the solution to improve wear resistance.
The uniform photochromic film formation on the surface of the glove is achieved, which improves the wear resistance, meets the special needs of labor protection gloves, provides concealment and camouflage effects, and fills the gap in photochromic gloves.
Smart Images

Figure CN118978741A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glove preparation, and in particular to a method for preparing photochromic ultrafine foamed gloves. Background Art
[0002] At present, nitrile gloves are widely used in petrochemical, paint printing, agriculture and animal husbandry, automobile machinery maintenance and other industries. They are the most important labor protection tools for protecting hands in people's daily labor. They have the advantages of being light, sensitive, soft, oil-proof, acid-resistant, alkali-resistant, and corrosion-resistant. The products are relatively mature. Existing photochromic gloves usually add photochromic materials directly to the glove latex materials. Most of the existing latex systems are water-based systems. Photochromic materials are not very compatible with water-based systems. If they are directly added to the nitrile latex system, the existing stirring method will destroy the system on the surface of the nitrile latex itself, thereby reducing the overall performance. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing photochromic ultrafine foamed gloves, which forms a uniform film of color-changing material on the surface of the gloves, and the film plays a good role in protecting the gloves and improving the good wear resistance.
[0004] The above technical objectives of the present invention are achieved through the following technical solutions:
[0005] A method for preparing photochromic ultrafine foam gloves, characterized in that it comprises the following steps:
[0006] S1, stirring and preparing the latex after color adjustment;
[0007] S2, stirring the latex evenly and letting it stand to control the viscosity range;
[0008] S3, putting the nylon glove core into a hand mold of corresponding size and putting it into an oven for preheating;
[0009] S4, the preheated glove core is immersed in the coagulant;
[0010] S5, placing the glove core into the prepared latex for uniform gelation;
[0011] S6, immersing the homogenized gloves evenly into the ultrafine foaming agent;
[0012] S7, placing in an oven for primary aging;
[0013] S8, cooling the matured ultrafine foam gloves and immersing them in a photochromic solution;
[0014] S9, placing the gloves in an oven for secondary aging, and obtaining the photochromic ultrafine foamed gloves after cooling.
[0015] Preferably, the latex configured in S1 includes a latex system, a thickener and a color paste. The latex system is mainly composed of nitrile latex, and any combination and proportion of styrene-butadiene latex, chloroprene latex, natural latex or water-based polyurethane are added, wherein the nitrile latex accounts for more than 70%, the thickener is added in an amount of 2%-15% of the latex system, and the color paste is added in an amount of 2%-10% of the latex system. The thickener is selected from one or more of hydroxymethyl cellulose, casein, polyacrylate thickener or polyurethane thickener.
[0016] Preferably, the viscosity range of the latex in S2 is controlled to be 3000 mpa·s-6000 mpa·s.
[0017] Preferably, the oven preheating temperature in S3 is 40°C-60°C, and the preheating time is 30min-40min.
[0018] Preferably, the coagulant in S4 includes a solvent and a core material accounting for 1%-7% by mass, the solvent is selected from one of methanol or ethanol, and the core material is selected from one or more of glacial acetic acid, calcium chloride, calcium nitrate or hydrochloric acid. The preheated gloves are first immersed in the coagulant for 5 seconds and then taken out, and then immersed vertically downward for 1min-3min.
[0019] Preferably, the specific step of S5 is: putting the glove core into the prepared latex, slowly and evenly moving it downward, slowly and evenly taking it out after the palm is immersed in the position, and slowly and evenly rotating the hand model immersed in the gel for 3-10 circles to make it evenly gelled.
[0020] Preferably, the ultrafine foaming agent in S6 includes a solvent and a core material accounting for 1%-7% by mass, the solvent is selected from one of methanol or ethanol, the core material is selected from one or more of glacial acetic acid, hydrochloric acid or perchloric acid, and the impregnation time of the ultrafine foaming agent is 5s-10s.
[0021] Preferably, the one-time aging in S7 is: first aging at a temperature of 70° C.-80° C. for 30 min-60 min, and then aging at a temperature of 90° C.-110° C. for 60 min-90 min.
[0022] Preferably, the photochromic solution in S8 comprises a solvent methanol and a core material accounting for 10%-25% by mass, wherein the core material is selected from a copolymer prepared by copolymerizing an unsaturated monomer containing an o-hydroxybenzyl imine structure with styrene or methyl methacrylate, a copolymer prepared by copolymerizing a p-(methacrylic acid amide) phenylmercuric disulfide complex with styrene, methyl methacrylate, butyl acrylate or acrylamide monomer, a polymer containing an azobenzene structure or a polymer containing an indanedione structural unit, or a mixture of the above, and the ultrafine foamed gloves are cooled for 30 minutes and then immersed in the photochromic solution for 30 minutes to 60 minutes.
[0023] Preferably, the secondary aging temperature in S9 is 90° C.-110° C., the aging time is 60 min-90 min, and the cooling time is 30 min.
[0024] In summary, the present invention has the following beneficial effects:
[0025] 1. The photochromic material used in the present invention can change the structure of its material polymer under light conditions, resulting in a change in its maximum absorption wavelength of light. Therefore, the color of the material changes with the change of light conditions, and can return to its original color after the light stops.
[0026] 2. The advantage of the present invention is that it fills the blank of photochromic gloves in the field of labor protection gloves, meets the special needs of customers, and achieves appearance effects such as colorful black, colorful gray, etc. At the same time, it can utilize the color change of the material to achieve concealment and camouflage effects.
[0027] 3. The present invention uses the matured ultrafine foamed gloves to enter the uniform photochromic solution, and forms a uniform photochromic film on the surface of the gloves through the whole gloves in the photochromic solution. The film plays a role in protecting the gloves and has good wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The present invention is a flow chart of a method for preparing photochromic ultrafine foamed gloves. DETAILED DESCRIPTION
[0029] The specific implementation manner of the present invention is further described below in conjunction with the accompanying drawings, and this embodiment does not constitute a limitation of the present invention.
[0030] Example 1
[0031] like Figure 1 The method for preparing a photochromic ultrafine foamed glove shown comprises the following steps:
[0032] S1, stirring and configuring the latex after the coloring is completed, specifically, pouring 2000g of nitrile latex, 300g of styrene butadiene latex, and 100g of waterborne polyurethane into a plastic bucket, turning on the mixer to start stirring, adding 250g of thickener hydroxymethyl cellulose and 75g of black pulp, stirring for 3 hours and then standing for 1 hour;
[0033] S2, stirring the latex evenly and letting it stand to control the viscosity to 3500mpa.s;
[0034] S3, put the nylon glove core into the hand mold of corresponding size, and put it into the oven for preheating at 60℃ for 30min;
[0035] S4, the preheated gloves are immersed in the coagulant for 5 seconds, then taken out and immersed vertically downward for 3 minutes. The coagulant includes 2.5% glacial acetic acid and 97.5% methanol by mass.
[0036] S5, put the glove core into the prepared latex, slowly and evenly move it down, slowly and evenly take it out after the palm is immersed in the position, and slowly and evenly rotate the hand model that has been immersed in the latex for 5 circles to make it gel evenly;
[0037] S6, immersing the homogenized gloves evenly in a superfine foaming agent for 5 seconds, wherein the superfine foaming agent includes 3.5% by mass acetic acid and 96.5% by mass methanol;
[0038] S7, placing in an oven for aging once, specifically, first aging at 70° C. for 30 min, and then aging at 90° C. for 60 min;
[0039] S8, cooling the matured ultrafine foam gloves for 30 minutes and then immersing them in a photochromic solution for 30 minutes, wherein the photochromic solution includes 15% by mass of o-hydroxybenzylamine-styrene copolymer and 85% by mass of methanol;
[0040] S9, and then placing in an oven for secondary aging, specifically at a temperature of 90° C., an aging time of 90 min, and a cooling time of 30 min. After cooling, a black photochromic ultrafine foaming glove is obtained. After being exposed to sunlight for 20 minutes, the surface of the glove becomes slightly powdery.
[0041] Example 2
[0042] like Figure 1 The method for preparing a photochromic ultrafine foamed glove shown comprises the following steps:
[0043] S1, stirring the latex after the color matching is completed, specifically pouring 2000g of nitrile latex, 300g of styrene butadiene latex, and 200g of waterborne polyurethane into a plastic bucket, turning on the mixer to start stirring, adding 250g of casein and 75g of black slurry, stirring for 4 hours and then standing for 1 hour;
[0044] S2, stirring the latex evenly and letting it stand to control the viscosity to 4500 mpa·s;
[0045] S3, put the nylon glove core into the hand mold of corresponding size, and put it into the oven for preheating at 50℃ for 40min;
[0046] S4, the preheated gloves are immersed in the coagulant for 5 seconds, then taken out and immersed vertically downward for 3 minutes. The coagulant includes 2.5% glacial acetic acid, 1% hydrochloric acid and 96.5% methanol by mass;
[0047] S5, put the glove core into the prepared latex, slowly and evenly move it down, slowly and evenly take it out after the palm is immersed in the position, and slowly and evenly rotate the hand model that has been immersed in the latex for 5 circles to make it gel evenly;
[0048] S6, immersing the homogenized gloves evenly in a superfine foaming agent for 6 seconds, wherein the superfine foaming agent includes 3.5% by mass acetic acid and 96.5% by mass methanol;
[0049] S7, placing in an oven for aging once, specifically, first aging at 80° C. for 30 min, and then aging at 90° C. for 60 min;
[0050] S8, cooling the matured ultrafine foam gloves for 30 minutes and then immersing them in a photochromic solution for 30 minutes, wherein the photochromic solution comprises 25% by mass of a copolymer of o-hydroxybenzylamine methyl benzoate and 75% by mass of methanol;
[0051] S9, placing the gloves in an oven for secondary aging, specifically at a temperature of 100° C., an aging time of 70 min, and a cooling time of 30 min. After cooling, a black photochromic ultrafine foamed glove is obtained. After being exposed to sunlight for 10 minutes, the surface of the glove begins to change color.
[0052] Example 3
[0053] like Figure 1 The method for preparing a photochromic ultrafine foamed glove shown comprises the following steps:
[0054] S1, stirring the latex after the coloring is completed, specifically pouring 2500g of nitrile latex into a plastic bucket, turning on the mixer to start stirring, adding 150g of thickener casein and 100g of black slurry, stirring for 4 hours and then standing for 1 hour;
[0055] S2, stirring the latex evenly and letting it stand to control the viscosity to 3100 mpa·s;
[0056] S3, put the nylon glove core into the hand mold of corresponding size, and put it into the oven for preheating at 60℃ for 30min;
[0057] S4, the preheated gloves are immersed in the coagulant for 5 seconds, then taken out and immersed vertically downward for 2 minutes. The coagulant includes 3% glacial acetic acid and 97% ethanol;
[0058] S5, put the glove core into the prepared latex, slowly and evenly move it down, slowly and evenly take it out after the palm is immersed in the position, and slowly and evenly rotate the hand model that has been immersed in the latex for 3 circles to make it gel evenly;
[0059] S6, immersing the homogenized gloves evenly in an ultrafine foaming agent for 7 seconds, wherein the ultrafine foaming agent comprises 3.5% by mass hydrochloric acid and 96.5% by mass methanol;
[0060] S7, placing in an oven for aging, specifically, first aging at 75° C. for 30 min, and then aging at 95° C. for 60 min;
[0061] S8, cooling the matured ultrafine foam gloves for 30 minutes and then immersing them in a photochromic solution for 30 minutes, wherein the photochromic solution comprises 15% by mass of o-hydroxybenzene amine-styrene copolymer, 5% by mass of 1,3,4-oxadiazole-16-alkoxyazobenzene copolymer and 80% by mass of methanol;
[0062] S9, placing the gloves in an oven for secondary aging, specifically at a temperature of 100° C., an aging time of 70 min, and a cooling time of 30 min. After cooling, a black photochromic ultrafine foamed glove is obtained. After being exposed to sunlight for 20 minutes, the surface of the glove begins to change color.
[0063] Example 4
[0064] like Figure 1 The method for preparing a photochromic ultrafine foamed glove shown comprises the following steps:
[0065] S1, stirring the latex after the color matching is completed, specifically pouring 1800g of nitrile latex, 500g of styrene butadiene latex, 100g of natural latex, and 100g of waterborne polyurethane into a plastic bucket, turning on the mixer to start stirring, adding 300g of casein and 85g of black slurry, stirring for 5 hours and then standing for 1 hour;
[0066] S2, stirring the latex evenly and letting it stand to control the viscosity to 3500 mpa·s;
[0067] S3, put the nylon glove core into the hand mold of corresponding size, and put it into the oven for preheating at 50℃ for 40min;
[0068] S4, the preheated gloves are immersed in the coagulant for 5 seconds and then taken out, and then immersed vertically downward for 1min-3min. The coagulant includes 2.5% glacial acetic acid and 97.5% methanol by mass;
[0069] S5, put the glove core into the prepared latex, slowly and evenly move it down, slowly and evenly take it out after the palm is immersed in the position, and slowly and evenly rotate the hand model that has been immersed in the latex for 3-10 circles to make it gel evenly;
[0070] S6, immersing the homogenized gloves evenly in a superfine foaming agent for 5 seconds, wherein the superfine foaming agent includes 3.5% by mass acetic acid and 96.5% by mass methanol;
[0071] S7, placing in an oven for aging once, specifically, first aging at 80° C. for 30 min, and then aging at 90° C. for 60 min;
[0072] S8, cooling the matured ultrafine foam gloves for 30 minutes and then immersing them in a photochromic solution for 40 minutes, wherein the photochromic solution includes 25% by mass of 1,3,4-oxadiazole-16-alkoxyazobenzene copolymer and 75% by mass of methanol;
[0073] S9, placing the gloves in an oven for secondary aging, specifically at a temperature of 100° C., an aging time of 70 min, and a cooling time of 30 min. After cooling, a black photochromic ultrafine foamed glove is obtained. After being exposed to sunlight for 20 minutes, the surface of the glove begins to change color.
[0074] Example 5
[0075] like Figure 1 The method for preparing a photochromic ultrafine foamed glove shown comprises the following steps:
[0076] S1, stirring and configuring the latex after coloring, specifically, pouring 2300g of nitrile latex and 200g of natural latex into a rubber bucket, turning on the mixer to start stirring, adding 300g of thickener hydroxymethyl cellulose and 85g of black pulp, stirring for 5 hours and then standing for 1 hour;
[0077] S2, stirring the latex evenly and letting it stand to control the viscosity to 5500 mpa·s;
[0078] S3, put the nylon glove core into the hand mold of corresponding size, and put it into the oven for preheating at 50℃ for 40min;
[0079] S4, the preheated gloves are immersed in the coagulant for 5 seconds, then taken out and immersed vertically downward for 3 minutes. The coagulant includes 2.5% glacial acetic acid and 97.5% methanol by mass.
[0080] S5, put the glove core into the prepared latex, slowly and evenly move it down, slowly and evenly take it out after the palm is immersed in the position, and slowly and evenly rotate the hand model that has been immersed in the latex for 5 circles to make it gel evenly;
[0081] S6, immersing the homogenized gloves evenly in a superfine foaming agent for 10 seconds, wherein the superfine foaming agent includes 3.5% by mass acetic acid and 96.5% by mass ethanol;
[0082] S7, placing in an oven for aging once, specifically, first aging at 80° C. for 30 min, and then aging at 90° C. for 60 min;
[0083] S8, cooling the matured ultrafine foam gloves for 30 minutes and then immersing them in a photochromic solution for 60 minutes, wherein the photochromic solution includes 25% by mass of 1,3,4-oxadiazole-16-alkoxyazobenzene copolymer and 75% by mass of methanol;
[0084] S9, placing the gloves in an oven for secondary aging, specifically at a temperature of 100° C., an aging time of 70 min, and a cooling time of 30 min. After cooling, a black photochromic ultrafine foamed glove is obtained. After being exposed to sunlight for 20 minutes, the surface of the glove begins to change color.
[0085] Example 6
[0086] like Figure 1 The method for preparing a photochromic ultrafine foamed glove shown comprises the following steps:
[0087] S1, stirring the latex after the coloring is completed, specifically pouring 2000g of nitrile latex, 300g of chloroprene latex, and 200g of waterborne polyurethane into a plastic bucket, turning on the mixer to start stirring, adding 300g of casein and 75g of black slurry, stirring for 4 hours and then standing for 1 hour;
[0088] S2, stirring the latex evenly and letting it stand to control the viscosity to 3500 mpa·s;
[0089] S3, put the nylon glove core into the hand mold of corresponding size, and put it into the oven for preheating at 60℃ for 35min;
[0090] S4, the preheated gloves are immersed in the coagulant for 5 seconds, then taken out and immersed vertically downward for 3 minutes. The coagulant includes 2.5% glacial acetic acid, 1% hydrochloric acid and 96.5% methanol by mass;
[0091] S5, put the glove core into the prepared latex, slowly and evenly move it down, slowly and evenly take it out after the palm is immersed in the position, and slowly and evenly rotate the hand model that has been immersed in the latex for 5 circles to make it gel evenly;
[0092] S6, immersing the homogenized gloves evenly in an ultrafine foaming agent for 10 seconds, wherein the ultrafine foaming agent includes 5.5% by mass acetic acid and 94.5% by mass methanol;
[0093] S7, placing in an oven for aging once, specifically, first aging at 80° C. for 30 min, and then aging at 90° C. for 60 min;
[0094] S8, cooling the matured ultrafine foam gloves for 30 minutes and then immersing them in a photochromic solution for 30 minutes, wherein the photochromic solution comprises 25% by mass of p-(methacrylic acid amide) phenylmercuric disulfide styrene copolymer and 85% by mass of methanol;
[0095] S9, placing the gloves in an oven for secondary aging, specifically at a temperature of 100° C., an aging time of 70 min, and a cooling time of 30 min. After cooling, a black photochromic ultrafine foamed glove is obtained. After being exposed to sunlight for 25 minutes, the surface of the glove begins to change color.
[0096] Example 7
[0097] like Figure 1 The method for preparing a photochromic ultrafine foamed glove shown comprises the following steps:
[0098] S1, stirring and configuring the latex after color matching, specifically, pouring 2200g of nitrile latex, 150g of chloroprene latex, and 150g of waterborne polyurethane into a plastic bucket, turning on the mixer to start stirring, adding 250g of polyacrylate thickener and 75g of black slurry, stirring for 4 hours and then standing for 1 hour;
[0099] S2, stirring the latex evenly and letting it stand to control the viscosity to 4500 mpa·s;
[0100] S3, put the nylon glove core into the hand mold of corresponding size, and put it into the oven for preheating at 60℃ for 30min;
[0101] S4, the preheated gloves are immersed in the coagulant for 5 seconds, then taken out and immersed vertically downward for 3 minutes. The coagulant includes 2.5% glacial acetic acid, 1% hydrochloric acid and 96.5% methanol by mass;
[0102] S5, put the glove core into the prepared latex, slowly and evenly move it down, slowly and evenly take it out after the palm is immersed in the position, and slowly and evenly rotate the hand model that has been immersed in the latex for 3-10 circles to make it gel evenly;
[0103] S6, immersing the homogenized gloves evenly in a superfine foaming agent for 5s-10s, wherein the superfine foaming agent comprises 5.5% by mass acetic acid and 94.5% by mass ethanol;
[0104] S7, placing in an oven for aging once, specifically, first aging at 70° C. for 30 min, and then aging at 90° C. for 60 min;
[0105] S8, cooling the matured ultrafine foam gloves for 30 minutes and then immersing them in a photochromic solution for 45 minutes, wherein the photochromic solution includes 25% by mass of 1,3-indanedione methyl methacrylate copolymer and 75% by mass of methanol;
[0106] S9, placing the gloves in an oven for secondary aging, specifically at a temperature of 100° C., an aging time of 70 min, and a cooling time of 30 min. After cooling, a black photochromic ultrafine foamed glove is obtained. After being exposed to sunlight for 25 minutes, the surface of the glove begins to change color.
[0107] The wear resistance of the ultrafine foam gloves not soaked in the photochromic solution and the finally obtained photochromic ultrafine foam gloves in the above embodiment was tested according to the American standard wear resistance standard (ASTM D3389-16). The test results are shown in Table 1 below.
[0108] Table 1 Wear resistance test of gloves in various embodiments
[0109]
[0110]
[0111] From the data in Table 1, it can be seen that the ultra-fine foam gloves with the surface immersed in the photochromic solution can effectively improve the wear resistance.
[0112] The photochromic material used in the present invention can change the structure of its material polymer under light conditions, resulting in a change in its maximum absorption wavelength of light. Therefore, the color of the material changes with the change of light conditions, and can return to the original color after the light stops.
[0113] The advantages of the present invention are that it fills the blank of photochromic gloves in the field of labor protection gloves, meets the special needs of customers, and achieves appearance effects such as colorful black, colorful gray, etc. At the same time, it can utilize the color change of the material to achieve concealment and camouflage effects.
[0114] The present invention uses the matured ultrafine foamed gloves to enter the uniform photochromic solution, and forms a uniform photochromic film on the surface of the gloves through the whole gloves in the photochromic solution. The film plays a role in protecting the gloves and has good wear resistance.
[0115] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Those skilled in the art may make various modifications or equivalent substitutions to the present invention within the essence and protection scope of the present invention, and such modifications or equivalent substitutions should also be deemed to fall within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing photochromic ultrafine foam gloves, characterized in that: The steps include: S1, stirring and preparing the latex after color adjustment; S2, stirring the latex evenly and letting it stand to control the viscosity range; S3, putting the nylon glove core into a hand mold of corresponding size and putting it into an oven for preheating; S4, the preheated glove core is immersed in the coagulant; S5, placing the glove core into the prepared latex for uniform gelation; S6, immersing the homogenized gloves evenly into the ultrafine foaming agent; S7, placing in an oven for primary aging; S8, cooling the matured ultrafine foam gloves and immersing them in a photochromic solution; S9, placing the gloves in an oven for secondary aging, and obtaining the photochromic ultrafine foamed gloves after cooling.
2. The method for preparing a photochromic ultrafine foamed glove according to claim 1, characterized in that: The latex configured in S1 includes a latex system, a thickener and a color paste. The latex system is mainly composed of nitrile latex, and any combination and proportion of styrene-butadiene latex, chloroprene latex, natural latex or water-based polyurethane are added, wherein the nitrile latex accounts for more than 70%, the thickener is added in an amount of 2%-15% of the latex system, and the color paste is added in an amount of 2%-10% of the latex system. The thickener is selected from one or more of hydroxymethyl cellulose, casein, polyacrylate thickener or polyurethane thickener.
3. The method for preparing a photochromic ultrafine foamed glove according to claim 1, characterized in that: The viscosity range of the latex in S2 is controlled to be 3000mpa.s-6000mpa.s.
4. The method for preparing a photochromic ultrafine foamed glove according to claim 1, characterized in that: In S3, the oven preheating temperature is 40°C-60°C, and the preheating time is 30min-40min.
5. The method for preparing a photochromic ultrafine foamed glove according to claim 1, characterized in that: The coagulant in S4 includes a solvent and a core material accounting for 1%-7% by mass, the solvent is selected from one of methanol or ethanol, and the core material is selected from one or more of glacial acetic acid, calcium chloride, calcium nitrate or hydrochloric acid. The preheated gloves are immersed in the coagulant for 5 seconds and then taken out, and then immersed vertically downward for 1min-3min.
6. The method for preparing a photochromic ultrafine foamed glove according to claim 1, characterized in that: The specific steps of S5 are: putting the glove core into the prepared latex, slowly and evenly moving it downward, slowly and evenly taking it out after the palm is immersed in the position, and slowly and evenly rotating the hand model immersed in the latex for 3-10 circles to make it gel evenly.
7. The method for preparing a photochromic ultrafine foamed glove according to claim 1, characterized in that: The ultrafine foaming agent in S6 includes a solvent and a core material accounting for 1%-7% by mass, the solvent is selected from one of methanol or ethanol, the core material is selected from one or more of glacial acetic acid, hydrochloric acid or perchloric acid, and the impregnation time of the ultrafine foaming agent is 5s-10s.
8. The method for preparing a photochromic ultrafine foamed glove according to claim 1, characterized in that: The one-time aging in S7 is specifically: first aging at a temperature of 70° C.-80° C. for 30 min-60 min, and then aging at a temperature of 90° C.-110° C. for 60 min-90 min.
9. The method for preparing a photochromic ultrafine foamed glove according to claim 1, characterized in that: The photochromic solution in S8 includes a solvent of methanol and a core material accounting for 10%-25% by mass, wherein the core material is selected from a copolymer prepared by copolymerizing an unsaturated monomer containing an o-hydroxybenzyl imine structure with styrene or methyl methacrylate, a copolymer prepared by copolymerizing a p-(methacrylic acid amide) phenylmercuric disulfide complex with styrene, methyl methacrylate, butyl acrylate or acrylamide monomer, a polymer containing an azobenzene structure or a polymer containing an indanedione structural unit, or a mixture of the above. After cooling the ultrafine foaming gloves for 30 minutes, the gloves are immersed in the photochromic solution for 30 minutes to 60 minutes.
10. The method for preparing photochromic ultrafine foam gloves according to claim 1, characterized in that: In the S9, the secondary aging temperature is 90° C.-110° C., the aging time is 60 min-90 min, and the cooling time is 30 min.