High-strength stone-like brick and preparation method thereof
By using specific raw materials and high-temperature firing technology in imitation stone bricks, combined with the bonding effect of epoxy resin, the problem of poor glaze hardness and bonding effect of imitation stone bricks is solved, and its strength and service life are significantly improved.
Patent Information
- Application Number
- CN202410899904.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The glaze surface of existing imitation stone bricks is not hard and has poor bonding effect, which leads to prone to cracking and falling off after long-term use.
The preparation method of imitation stone bricks including cement, spherical soil, stone powder, coarse and fine aggregates, fiber additives, feldspar, quartz, kaolin, moissanite, oxidation additives, metal additives, calcium carbonate and epoxy resins, etc., is adopted. Through the bonding of high-temperature firing and epoxy resin, the bonding force and strength of the glaze surface and the base brick are enhanced.
It effectively improves the surface strength and adhesion of imitation stone bricks, reduces the problem of glaze falling off, extends service life, and improves the aesthetics and scratch resistance of glaze.
Smart Images

Figure CN118978360A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of imitation stone brick preparation, in particular to a high-strength imitation stone brick and a preparation method thereof. Background Art
[0002] Imitation stone bricks are ceramic tiles that imitate the pattern, color, texture and shape of natural stones. Imitation stone bricks imitate natural stones, so that after the imitation stone bricks are laid, they have a natural stone feeling, but will not cause light refraction to the surrounding residents. They are also hard and corrosion-resistant and can withstand long-term exposure to the sun and rain. Compared with natural stones, imitation stone bricks have the advantages of low price, light weight, easy processing, and various colors. Although imitation stone bricks are designed to be very similar to natural stones, there are still some differences. Imitation stone bricks are man-made materials, while stones are natural materials. The hardness and toughness of imitation stone bricks are usually adjusted according to actual needs, while stones have their fixed natural physical properties. However, the production and processing process of imitation stone bricks is relatively simple, so the price is relatively low. Since imitation stone bricks can simulate the characteristics of various natural stones, compared with stones, imitation stone bricks are lighter in weight, which can reduce the burden on buildings and speed up the progress of construction. They are very suitable for occasions where they are used in large areas.
[0003] The surface of the current imitation stone bricks is all covered with a layer of ceramic glaze, which can provide good aesthetics for the imitation stone bricks and has good anti-slip effect. However, due to its characteristics, the glaze of the imitation stone bricks has the problem of low hardness and poor bonding effect. Therefore, after long-term use of the imitation stone bricks, the glaze of the imitation stone bricks is prone to cracking and falling off, affecting the use of the imitation stone bricks. Summary of the invention
[0004] The object of the present invention is to provide a high-strength imitation stone brick and a preparation method thereof to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solution: a high-strength imitation stone brick and a preparation method thereof, wherein the imitation stone brick comprises a base brick and a glaze, and the base brick of the imitation stone brick comprises the following raw materials by weight:
[0006] 10-20 parts of cement, 20-40 parts of ball clay, 15-20 parts of stone powder, 10-15 parts of coarse aggregate, 8-10 parts of fine aggregate, 5-10 parts of fiber additives and 10-20 parts of water;
[0007] The glaze surface of the imitation stone brick comprises the following raw materials by weight:
[0008] 5-10 parts of feldspar, 5-10 parts of quartz, 10-15 parts of kaolin, 5-8 parts of moissanite, 5-8 parts of oxidizing additives, 3-7 parts of metal additives, 2-4 parts of calcium carbonate, 2-3 parts of epoxy resin and 5-10 parts of water.
[0009] In a further embodiment, the coarse aggregate is composed of 5mm-7mm crushed stone and pebbles, and the fine aggregate is composed of 2mm-3mm gravel or crushed stone. By selecting coarse and fine aggregates, the base bricks can make the raw materials of the base bricks better intertwined and combined with each other, thereby improving the strength of the imitation stone brick base bricks.
[0010] In a further embodiment, the metal additives include one or more of copper, cobalt, iron, manganese and cadmium. The metal elements can change the color and glossiness of the glaze layer, while calcium carbonate can increase the elasticity and scratch resistance of the glaze layer, making the imitation stone bricks not only beautiful but also with better hardness and surface wear resistance.
[0011] In a further embodiment, the oxidizing additive is aluminum oxide, zirconium oxide and calcium oxide, wherein the aluminum oxide content is 40%-50%, the zirconium oxide content is 30%-40%, and the calcium oxide content is 20%-30%. The oxides can increase the transparency, glossiness and color saturation of the glaze layer, and can be used to improve the transparency and brightness of the glaze surface, and enhance the hardness and stability of the glaze surface.
[0012] In a further embodiment, the moissanite is a moissanite powdered solid material, and the particle size of the moissanite powder is 20-50 μm. The moissanite is an artificially synthesized powder raw material. The hardness of moissanite is close to that of diamond and has a good refractive index. Therefore, the hardness of moissanite is used to enhance the strength and hardness of the glaze on the surface of the imitation stone brick, and can provide a better light refraction effect for the glaze, making the glaze more transparent and harder, thereby improving the strength and surface beauty of the imitation stone brick.
[0013] A method for preparing a high-strength imitation stone brick, the imitation stone brick preparation comprising the following steps:
[0014] S1. Add the coarse aggregate and fine aggregate of the base brick into the mixing equipment for screening, and select the aggregate with qualified particle diameter;
[0015] S2. After the coarse aggregate and fine aggregate are selected, cement, ball clay, stone powder, coarse aggregate, fine aggregate, fiber additive and water are added to the mixing equipment, and the mixing equipment is started to mix the raw materials;
[0016] S3. The mixed base brick raw materials are placed into a brick mold, and then the mold is closed to extrude the raw materials into a blank;
[0017] S4. Select feldspar, quartz, kaolin and moissanite and add them to the stirring device, then start the stirring device to stir the solid raw materials first, and then add the oxidizing additive, the metal additive, calcium carbonate and water to mix the raw materials;
[0018] S5. Spread the epoxy resin onto the blank in the mold, then add the mixed raw materials in S4 to the brick mold of S3, spread it on the blank, and then close the mold again to form a finished blank of imitation stone brick;
[0019] S6. The finished blank is removed from the mold and then placed in a natural environment for curing;
[0020] S7. Put the cured finished blank into a high-temperature firing kiln, and then perform high-temperature firing to form the finished blank. After the fired finished blank is naturally cooled, the finished imitation stone brick is obtained.
[0021] In a further embodiment, the sintering temperature of the blank is 1100° C.-1600° C., and the sintering time is 45 min-1.5 h.
[0022] In a further embodiment, the finished blank is dried by natural curing, and the finished blank is dried to 5wt%-8wt% to form a dry blank. The finished blank is naturally cured and dried to reduce the water content therein, which can greatly improve the efficiency of the subsequent sintering process, prevent long-term high-temperature sintering from causing damage to the finished blank, and improve the yield rate of the production process.
[0023] In a further embodiment, the natural curing time of the finished blank is 2h-3h, the epoxy resin is made of polyacid-modified epoxy acrylate and bisphenol A, which are mixed with water, and a curing agent is added during use to enhance the bonding effect between the epoxy resin and the glaze and base brick. Because the epoxy resin has strong bonding strength, it can provide a more stable bonding effect for the base brick and surface glaze of the imitation stone brick.
[0024] In a further embodiment, a colorant is added during the raw material mixing process in S4 to change the glaze color of the finished product. This is because current imitation stone bricks have colorants added to them in order to meet the architectural needs of different users. The colorant is a raw material additive that can change the color, thereby changing the surface color of the imitation stone bricks. In addition, during the mold compression molding process, different styles of mold types are selected to produce imitation stone bricks in different shapes and with different surface patterns, making the use of imitation stone bricks more flexible and varied.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1. The glaze surface of the imitation stone brick can effectively improve the strength of the glaze body on the surface of the imitation stone brick through metal additives and oxidizing additives, so that the surface strength of the imitation stone brick is improved, thereby reducing the problem of imitation stone bricks being broken due to long-term use or external force, and improving the strength and service life of the imitation stone brick;
[0027] 2. In the present invention, the glaze of the imitation stone brick is added with metal additives, oxidizing additives and calcium carbonate, which can not only improve the strength and hardness of the glaze of the imitation stone brick, but also the metal elements in the metal additives can change the color and glossiness of the glaze layer, and the oxides can increase the transparency, glossiness and color saturation of the glaze layer, and can increase the elasticity and scratch resistance of the glaze layer, which can effectively improve the aesthetics of the glaze surface, and at the same time improve the scratch resistance of the glaze surface, thereby ensuring the aesthetics and durability of the imitation stone brick;
[0028] 3. The present invention adds a layer of epoxy resin between the base brick and the glaze of the imitation stone brick. The epoxy resin is an excellent adhesive with strong adhesion. The polar hydroxyl group and ether bond contained in its molecular chain give it high adhesion to a variety of substances. The epoxy resin is spread flat on the base brick blank, and then the glaze mixed raw materials are spread on the epoxy resin. Then, through the pressing of a high-pressure mold, the epoxy resin repeatedly enters the glaze and the base brick to form a high-strength bonding layer, so that a strong bonding force is formed between the glaze of the imitation stone brick and the base brick, thereby ensuring that the connection between the glaze of the imitation stone brick and the base brick is stronger and more stable, reducing the problem of glaze falling off of the imitation stone brick, and ensuring the stability of use and the life of the imitation stone brick. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of the framework of the preparation process of the imitation stone brick of the present invention. DETAILED DESCRIPTION
[0030] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The following is combined with Figure 1 The application is further described with examples;
[0032] Embodiment 1
[0033] This embodiment provides an imitation stone brick, and the preparation method thereof comprises the following steps:
[0034] 1) Raw materials for base bricks: 10kg cement, 20kg ball soil, 15kg stone powder, 10kg coarse aggregate, 8kg fine aggregate, 5kg fiber additive and 10kg water;
[0035] 2) Glaze raw materials: 5kg of feldspar, 5kg of quartz, 10kg of kaolin, 5kg of moissanite, 5kg of oxidizing additive, 3kg of metal additive, 2kg of calcium carbonate, 2kg of epoxy resin and 5kg of water;
[0036] 3) Add the coarse aggregate and fine aggregate of the base brick into the mixing equipment respectively for screening, and select the aggregate with qualified particle diameter;
[0037] 4) After the coarse aggregate and fine aggregate are selected, cement, ball clay, stone powder, coarse aggregate, fine aggregate, fiber additive and water are added to the mixing equipment, and the mixing equipment is started to mix the raw materials;
[0038] 5) Put the mixed base brick raw materials into the brick mold, and then close the mold to extrude the raw materials into blanks;
[0039] 6) feldspar, quartz, kaolin and moissanite are selected and added to a stirring device, and then the stirring device is started to stir the solid raw materials first, and then an oxidizing additive, a metal additive, calcium carbonate and water are added to mix the raw materials;
[0040] 7) Spread the epoxy resin on the blank in the mold, then add the mixed raw materials into the brick mold, spread it on the blank, and then close the mold again to form the finished blank of the imitation stone brick;
[0041] 8) Take the finished blank out of the mold and place it in a natural environment for curing;
[0042] 9) The cured finished blank is placed in a high-temperature firing kiln, and then fired and formed at high temperature. The fired finished blank is naturally cooled to obtain a finished imitation stone brick.
[0043] The Mohs hardness of the imitation stone brick surface is level 5, and the bonding strength between the glaze and the base brick is 0.7MPa.
[0044] Embodiment 2
[0045] This embodiment provides an imitation stone brick, and the preparation method thereof comprises the following steps:
[0046] 1) Raw materials for base bricks: 10kg cement, 20kg ball soil, 15kg stone powder, 10kg coarse aggregate, 8kg fine aggregate, 5kg fiber additive and 10kg water;
[0047] 2) Glaze raw materials: 5kg of feldspar, 5kg of quartz, 10kg of kaolin, 4kg of moissanite, 4kg of oxidizing additive, 2kg of metal additive, 2kg of calcium carbonate, 2kg of epoxy resin and 5kg of water;
[0048] 3) Add the coarse aggregate and fine aggregate of the base brick into the mixing equipment respectively for screening, and select the aggregate with qualified particle diameter;
[0049] 4) After the coarse aggregate and fine aggregate are selected, cement, ball clay, stone powder, coarse aggregate, fine aggregate, fiber additive and water are added to the mixing equipment, and the mixing equipment is started to mix the raw materials;
[0050] 5) Put the mixed base brick raw materials into the brick mold, and then close the mold to extrude the raw materials into blanks;
[0051] 6) feldspar, quartz, kaolin and moissanite are selected and added to a stirring device, and then the stirring device is started to stir the solid raw materials first, and then an oxidizing additive, a metal additive, calcium carbonate and water are added to mix the raw materials;
[0052] 7) Spread the epoxy resin on the blank in the mold, then add the mixed raw materials into the brick mold, spread it on the blank, and then close the mold again to form the finished blank of the imitation stone brick;
[0053] 8) Take the finished blank out of the mold and place it in a natural environment for curing;
[0054] 9) The cured finished blank is placed in a high-temperature firing kiln, and then fired and formed at high temperature. The fired finished blank is naturally cooled to obtain a finished imitation stone brick.
[0055] The Mohs hardness of the imitation stone brick surface is 4-5, and the bonding strength between the glaze and the base brick is 0.5MPa.
[0056] Embodiment 3
[0057] This embodiment provides an imitation stone brick, and the preparation method thereof comprises the following steps:
[0058] 1) Raw materials for base bricks: 10kg cement, 20kg ball soil, 15kg stone powder, 10kg coarse aggregate, 8kg fine aggregate, 5kg fiber additive and 10kg water;
[0059] 2) Glaze raw materials: 5kg of feldspar, 5kg of quartz, 10kg of kaolin, 3kg of moissanite, 3kg of oxidizing additive, 1kg of metal additive, 1kg of calcium carbonate, 1kg of epoxy resin and 5kg of water;
[0060] 3) Add the coarse aggregate and fine aggregate of the base brick into the mixing equipment respectively for screening, and select the aggregate with qualified particle diameter;
[0061] 4) After the coarse aggregate and fine aggregate are selected, cement, ball clay, stone powder, coarse aggregate, fine aggregate, fiber additive and water are added to the mixing equipment, and the mixing equipment is started to mix the raw materials;
[0062] 5) Put the mixed base brick raw materials into the brick mold, and then close the mold to extrude the raw materials into blanks;
[0063] 6) feldspar, quartz, kaolin and moissanite are selected and added to a stirring device, and then the stirring device is started to stir the solid raw materials first, and then an oxidizing additive, a metal additive, calcium carbonate and water are added to mix the raw materials;
[0064] 7) Spread the epoxy resin on the blank in the mold, then add the mixed raw materials into the brick mold, spread it on the blank, and then close the mold again to form the finished blank of the imitation stone brick;
[0065] 8) Take the finished blank out of the mold and place it in a natural environment for curing;
[0066] 9) The cured finished blank is placed in a high-temperature firing kiln, and then fired and formed at high temperature. The fired finished blank is naturally cooled to obtain a finished imitation stone brick.
[0067] The Mohs hardness of the imitation stone brick surface is 4, and the bonding strength between the glaze and the base brick is 0.4MPa.
[0068] According to the comparison between Example 2 and Example 3 and Example 1, when the glaze is produced, when the moissanite, oxidizing additives, metal additives and calcium carbonate are reduced, the surface hardness of the imitation stone brick is reduced, and the reduction in the amount of epoxy resin added also reduces the bonding strength between the glaze of the imitation stone brick and the base brick, and the surface strength and bonding strength of the imitation stone brick are reduced. Therefore, the imitation stone brick is prone to surface breakage and falling off during use. Therefore, adding the above-mentioned raw materials can effectively improve the strength, hardness and bonding effect of the imitation stone brick, thereby ensuring the stability and service life of the imitation stone brick.
[0069] Embodiment 4
[0070] This embodiment provides an imitation stone brick, and the preparation method thereof comprises the following steps:
[0071] 1) Raw materials for base bricks: 10kg cement, 20kg ball soil, 15kg stone powder, 10kg coarse aggregate, 8kg fine aggregate, 5kg fiber additive and 10kg water;
[0072] 2) Glaze raw materials: 5kg of feldspar, 5kg of quartz, 10kg of kaolin, 6kg of moissanite, 6kg of oxidizing additives, 4kg of metal additives, 3kg of calcium carbonate, 3kg of epoxy resin and 5kg of water;
[0073] 3) Add the coarse aggregate and fine aggregate of the base brick into the mixing equipment respectively for screening, and select the aggregate with qualified particle diameter;
[0074] 4) After the coarse aggregate and fine aggregate are selected, cement, ball clay, stone powder, coarse aggregate, fine aggregate, fiber additive and water are added to the mixing equipment, and the mixing equipment is started to mix the raw materials;
[0075] 5) Put the mixed base brick raw materials into the brick mold, and then close the mold to extrude the raw materials into blanks;
[0076] 6) feldspar, quartz, kaolin and moissanite are selected and added to a stirring device, and then the stirring device is started to stir the solid raw materials first, and then an oxidizing additive, a metal additive, calcium carbonate and water are added to mix the raw materials;
[0077] 7) Spread the epoxy resin on the blank in the mold, then add the mixed raw materials into the brick mold, spread it on the blank, and then close the mold again to form the finished blank of the imitation stone brick;
[0078] 8) Take the finished blank out of the mold and place it in a natural environment for curing;
[0079] 9) The cured finished blank is placed in a high-temperature firing kiln, and then fired and formed at high temperature. The fired finished blank is naturally cooled to obtain a finished imitation stone brick.
[0080] The Mohs hardness of the imitation stone brick surface is level 5, and the bonding strength between the glaze and the base brick is 0.8MPa.
[0081] Embodiment 5
[0082] This embodiment provides an imitation stone brick, and the preparation method thereof comprises the following steps:
[0083] 1) Raw materials for base bricks: 10kg cement, 20kg ball soil, 15kg stone powder, 10kg coarse aggregate, 8kg fine aggregate, 5kg fiber additive and 10kg water;
[0084] 2) Glaze raw materials: 5kg of feldspar, 5kg of quartz, 10kg of kaolin, 7kg of moissanite, 7kg of oxidizing additive, 5kg of metal additive, 4kg of calcium carbonate, 4kg of epoxy resin and 5kg of water;
[0085] 3) Add the coarse aggregate and fine aggregate of the base brick into the mixing equipment respectively for screening, and select the aggregate with qualified particle diameter;
[0086] 4) After the coarse aggregate and fine aggregate are selected, cement, ball clay, stone powder, coarse aggregate, fine aggregate, fiber additive and water are added to the mixing equipment, and the mixing equipment is started to mix the raw materials;
[0087] 5) Put the mixed base brick raw materials into the brick mold, and then close the mold to extrude the raw materials into blanks;
[0088] 6) feldspar, quartz, kaolin and moissanite are selected and added to a stirring device, and then the stirring device is started to stir the solid raw materials first, and then an oxidizing additive, a metal additive, calcium carbonate and water are added to mix the raw materials;
[0089] 7) Spread the epoxy resin on the blank in the mold, then add the mixed raw materials into the brick mold, spread it on the blank, and then close the mold again to form the finished blank of the imitation stone brick;
[0090] 8) Take the finished blank out of the mold and place it in a natural environment for curing;
[0091] 9) The cured finished blank is placed in a high-temperature firing kiln, and then fired and formed at high temperature. The fired finished blank is naturally cooled to obtain a finished imitation stone brick.
[0092] The Mohs hardness of the imitation stone brick surface is 6, and the bonding strength between the glaze and the base brick is 1MPa.
[0093] According to the comparison between Example 4 and Example 5 and Example 1, when the glaze is produced, when moissanite, oxidizing additives, metal additives and calcium carbonate are added, the surface strength of the imitation stone brick can be effectively increased, and increasing the amount of epoxy resin added can effectively improve the bonding strength between the glaze and the base brick of the imitation stone brick, and by increasing the surface strength and bonding strength of the imitation stone brick, the hardness, anti-cracking and anti-falling effects of the imitation stone brick are improved.
[0094] Embodiment 6
[0095] This embodiment provides an imitation stone brick, and the preparation method thereof comprises the following steps:
[0096] 1) Raw materials for base bricks: 10kg cement, 20kg ball soil, 15kg stone powder, 10kg coarse aggregate, 8kg fine aggregate, 5kg fiber additive and 10kg water;
[0097] 2) Glaze raw materials: 5kg feldspar, 5kg quartz, 10kg kaolin and 5kg water;
[0098] 3) Add the coarse aggregate and fine aggregate of the base brick into the mixing equipment respectively for screening, and select the aggregate with qualified particle diameter;
[0099] 4) After the coarse aggregate and fine aggregate are selected, cement, ball clay, stone powder, coarse aggregate, fine aggregate, fiber additive and water are added to the mixing equipment, and the mixing equipment is started to mix the raw materials;
[0100] 5) Put the mixed base brick raw materials into the brick mold, and then close the mold to extrude the raw materials into blanks;
[0101] 6) feldspar, quartz, kaolin and moissanite are selected and added to a stirring device, and then the stirring device is started to stir the solid raw materials first, and then an oxidizing additive, a metal additive, calcium carbonate and water are added to mix the raw materials;
[0102] 7) Spread the epoxy resin on the blank in the mold, then add the mixed raw materials into the brick mold, spread it on the blank, and then close the mold again to form the finished blank of the imitation stone brick;
[0103] 8) Take the finished blank out of the mold and place it in a natural environment for curing;
[0104] 9) The cured finished blank is placed in a high-temperature firing kiln, and then fired and formed at high temperature. The fired finished blank is naturally cooled to obtain a finished imitation stone brick.
[0105] The Mohs hardness of the imitation stone brick surface is 3-4, and the bonding strength between the glaze and the base brick is 0.5MPa.
[0106] According to Example 6 and Example 1, when the glaze is made, if moissanite, oxidizing additives, metal additives, calcium carbonate and epoxy resin are not added, the strength of the imitation stone brick and the bonding strength between the glaze and the base brick are reduced. Therefore, the imitation stone brick glaze made by adding moissanite, oxidizing additives, metal additives, calcium carbonate and epoxy resin has good strength and hardness, and the base brick and glaze of the imitation stone brick will also have better bonding strength, thereby ensuring that the imitation stone brick is more stable to use and has a longer service life.
[0107] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high-strength imitation stone brick, characterized in that: The imitation stone brick comprises a base brick and a glaze, and the base brick of the imitation stone brick comprises the following raw materials by weight: 10-20 parts of cement, 20-40 parts of ball clay, 15-20 parts of stone powder, 10-15 parts of coarse aggregate, 8-10 parts of fine aggregate, 5-10 parts of fiber additives and 10-20 parts of water; The glaze surface of the imitation stone brick comprises the following raw materials by weight: 5-10 parts of feldspar, 5-10 parts of quartz, 10-15 parts of kaolin, 5-8 parts of moissanite, 5-8 parts of oxidizing additives, 3-7 parts of metal additives, 2-4 parts of calcium carbonate, 2-3 parts of epoxy resin and 5-10 parts of water.
2. The high-strength imitation stone brick according to claim 1, characterized in that: The coarse aggregate is composed of crushed stone and pebbles with a size of 5mm-7mm, and the fine aggregate is composed of sand, gravel or crushed stone with a size of 2mm-3mm.
3. The high-strength imitation stone brick according to claim 1, characterized in that: The metal additives include one or more of copper, cobalt, iron, manganese and cadmium.
4. The high-strength imitation stone brick and the preparation method thereof according to claim 1, characterized in that: The oxidizing additives are aluminum oxide, zirconium oxide and calcium oxide, wherein the content of aluminum oxide is 40%-50%, the content of zirconium oxide is 30%-40%, and the content of calcium oxide is 20%-30%.
5. The high-strength imitation stone brick and the preparation method thereof according to claim 1, characterized in that: The moissanite is a moissanite powder solid material, and the particle size of the moissanite powder is 20-50 μm.
6. A method for preparing a high-strength imitation stone brick according to any one of claims 1 to 5, characterized in that: The preparation of the imitation stone brick comprises the following steps: S1. Add the coarse aggregate and fine aggregate of the base brick into the mixing equipment for screening, and select the aggregate with qualified particle diameter; S2. After the coarse aggregate and fine aggregate are selected, cement, ball clay, stone powder, coarse aggregate, fine aggregate, fiber additive and water are added to the mixing equipment, and the mixing equipment is started to mix the raw materials; S3. The mixed base brick raw materials are placed into a brick mold, and then the mold is closed to extrude the raw materials into a blank; S4. Select feldspar, quartz, kaolin and moissanite and add them to the stirring device, then start the stirring device to stir the solid raw materials first, and then add the oxidizing additive, the metal additive, calcium carbonate and water to mix the raw materials; S5. Spread the epoxy resin onto the blank in the mold, then add the mixed raw materials in S4 to the brick mold of S3, spread it on the blank, and then close the mold again to form a finished blank of imitation stone brick; S6. The finished blank is removed from the mold and then placed in a natural environment for curing; S7. Put the cured finished blank into a high-temperature firing kiln, and then perform high-temperature firing to form the finished blank. After the fired finished blank is naturally cooled, the finished imitation stone brick is obtained.
7. The method for preparing a high-strength imitation stone brick according to claim 6, characterized in that: The sintering temperature of the blank is 1100° C.-1600° C., and the sintering time is 45 min-1.5 h.
8. The method for preparing a high-strength imitation stone brick according to claim 6, characterized in that: The finished blank is dried by natural curing, and the finished blank is dried to 5wt%-8wt% to form a dry blank.
9. The method for preparing a high-strength imitation stone brick according to claim 6, characterized in that: The natural curing time of the finished blank is 2h-3h, and the epoxy resin is prepared by mixing polyacid-modified epoxy acrylate and bisphenol A with water.
10. The method for preparing a high-strength imitation stone brick according to claim 6, characterized in that: In the S4, coloring agents are added during the raw material mixing process to change the glaze color of the finished product.