High-temperature-resistant flame-retardant storage battery cap piece and production process thereof

Through the blend cross-linking of modified high-temperature resistant additives and ABS resin and the synergistic effect of modified flame retardant, the problem of insufficient smoke emission and flame retardant performance when the battery shell is burned under extreme conditions is solved, and the battery cap is realized High efficiency and high temperature resistance and flame retardant performance are improved.

CN118978786AInactive Publication Date: 2024-11-19ANHUI QIANGXU PLASTIC IND TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411088920.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing battery housing materials generate a large amount of smoke when burned under extreme conditions, and the flame retardant performance is insufficient, making it difficult to simultaneously improve the flame retardant performance and reduce smoke emissions.

Method used

Modified high-temperature resistant additives are blended with ABS resin and cross-linked by gamma ray irradiation. Combined with the use of modified flame retardants, the modified flame retardants are prepared by co-precipitation method and in-situ polymerization method, and the surface is covered with polyphosphorus Nitrile and hydrotalcite enhance flame retardant performance and smoke suppression effect.

Benefits of technology

It significantly improves the high temperature resistance and flame retardant performance of the battery cap plate, reduces smoke emissions during combustion, and enhances the thermal deformation temperature and flame retardant performance of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant flame-retardant storage battery cap piece and a production process thereof, and belongs to the technical field of high polymer materials, and the production process comprises the following steps: S1, adding ABS resin and a modified high-temperature-resistant auxiliary agent into a mixer for uniform mixing, then adding into an extruder for melt extrusion, and placing under gamma rays for irradiation treatment to obtain modified ABS plastic; s2, adding the modified ABS plastic, the curing agent, the modified flame retardant and the plasticizer into a mixer, uniformly mixing, adding into an extruder, carrying out melt extrusion, cooling, pelletizing and drying to obtain battery cap piece master batches; s3, inputting the master batch of the storage battery cover sheet into cover pressing equipment through a hopper for heating and melting, then injecting the master batch into a mold, and carrying out mold closing, compression molding, cooling shaping and slitting to obtain the storage battery cover sheet; the ABS resin is used as a base material, and under the synergistic effect of the modified high-temperature-resistant additive and the modified flame retardant, the flame retardant property of the storage battery cover plate and the smoke suppression property during combustion are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a high temperature resistant and flame retardant battery cover sheet and a production process thereof. Background Art

[0002] With the rapid development of new energy vehicles, energy storage equipment and portable electrical equipment, the requirements for battery safety and reliability are increasing. The battery casing, as the protective shell of the battery, has a direct impact on the safety and service life of the battery. Especially under extreme conditions, the high temperature resistance and flame retardant properties of the battery casing have gradually become the focus of industry attention.

[0003] At present, the material of the battery casing is usually based on ABS resin. The side groups of the ABS resin molecular chain contain a large number of aromatic structures, which are easy to burn and release a large amount of black smoke when burning, causing serious harm to the human body and the environment. Although traditional flame retardants have achieved a certain flame retardant effect, the smoke suppression performance of the material when burning is not obvious. Therefore, how to improve the flame retardant properties of the battery casing while reducing the smoke generated during combustion is a technical problem that needs to be solved at present. Summary of the invention

[0004] The purpose of the present invention is to provide a high temperature resistant and flame retardant battery cover sheet and a production process thereof, so as to solve the problems in the background technology.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A production process of a high temperature resistant flame retardant battery cover sheet, comprising the following steps:

[0007] S1, adding ABS resin and modified high temperature resistant additive into a mixer and uniformly mixing, then adding into an extruder for melt extrusion, and then placing under γ ray for irradiation treatment to obtain modified ABS plastic;

[0008] S2, adding modified ABS plastic, curing agent, modified flame retardant and plasticizer into a mixer and mixing them evenly, then adding them into an extruder for melt extrusion, cooling, pelletizing and drying to obtain a battery cover masterbatch;

[0009] S3, feeding the master batch of the battery cover sheet into the capping equipment through the hopper, heating and melting, and then injecting into the mold, and then closing the mold, pressing, cooling and shaping, and then cutting to obtain the battery cover sheet;

[0010] The weight ratio of the ABS resin to the modified high temperature resistant auxiliary agent is 110-120:3-8; the weight ratio of the modified ABS plastic, the curing agent, the modified flame retardant and the plasticizer is 90-110:0.2-0.8:3-6:0.3-0.6.

[0011] Furthermore, the modified high temperature resistant additive is prepared by the following steps:

[0012] Add N-(4-fluorophenyl) maleimide and triallyl isocyanurate to xylene, stir and mix, add benzoyl peroxide, heat to 100-110°C in a nitrogen atmosphere, stir and react for 4-5 hours, cool, place in methanol for suction filtration, wash and dry to obtain a modified high temperature resistant additive. Using benzoyl peroxide as an initiator and N-(4-fluorophenyl) maleimide as a heat-resistant monomer, a free radical precipitation polymerization method is used to free radical polymerize N-(4-fluorophenyl) maleimide and triallyl isocyanurate to obtain a modified high temperature resistant additive containing a triallyl isocyanurate copolymer.

[0013] Furthermore, the usage ratio of xylene, N-(4-fluorophenyl)maleimide, triallyl isocyanurate and benzoyl peroxide is 60 mL: 1-3 g: 0.5-6 g: 0.2 g.

[0014] Furthermore, the modified flame retardant is prepared by the following steps:

[0015] A1. Add carbon microspheres to deionized water, stir and mix, adjust the pH value to 10-11 with a 20wt% sodium hydroxide solution, and then simultaneously drip an alkali solution and a salt solution, control the dripping time to 30min, and maintain the pH value at 10-11. After the dripping is completed, crystallize at 70-80°C for 6-7h, cool, filter, wash, dry, and grind into powder to obtain modified carbon microspheres; use carbon microspheres as capsule cores, adopt a coprecipitation method, and cover a layer of layered dihydroxy composite metal oxide on the surface of the carbon microspheres by electrostatic adsorption to obtain modified carbon microspheres coated with hydrotalcite;

[0016] A2. Add modified carbon microspheres to acetonitrile, disperse by ultrasonic for 20 minutes, add 4,4'-diaminodiphenyl ether and triethylamine, stir and mix, then add hexachlorocyclotriphosphazene solution dropwise at 30-40°C, control the dropping time to be 50 minutes, continue to stir and react for 5-6 hours after the dropping is completed, cool, filter, wash, dry and grind to obtain a modified flame retardant; use acetonitrile as solvent and triethylamine as catalyst, adopt in-situ polymerization method, and polycondense the chlorine atoms in the hexachlorocyclotriphosphazene molecule with 4,4'-diaminodiphenyl ether on the surface of the modified carbon microspheres to obtain a double-shell modified flame retardant coated with polyphosphazene.

[0017] Furthermore, the usage ratio of the deionized water, carbon microspheres, alkaline solution and salt solution is 100mL:2-4g:60mL:70mL; the alkaline solution is prepared by dissolving sodium hydroxide and sodium carbonate in 100mL of deionized water in a mass ratio of 1:1-3; the salt solution is prepared by dissolving magnesium nitrate hexahydrate and aluminum nitrate nonahydrate in 100mL of deionized water in a mass ratio of 1.5-3:1.

[0018] Furthermore, the dosage ratio of the acetonitrile, modified carbon microspheres, 4,4'-diaminodiphenyl ether, triethylamine, and hexachlorocyclotriphosphazene solution is 80mL: 0.5-3g: 0.2-0.5g: 18mL: 40-60mL; the hexachlorocyclotriphosphazene solution is composed of hexachlorocyclotriphosphazene and acetonitrile in a dosage ratio of 0.2-1g: 100mL.

[0019] A high temperature resistant and flame retardant battery cover sheet is produced by the above production process.

[0020] Beneficial effects of the present invention:

[0021] The modified high temperature resistant additive of the present invention contains triallyl isocyanurate groups, which can be chemically cross-linked with butadiene in the ABS resin molecular chain under irradiation conditions, and the modified high temperature resistant additive is wound around the ABS resin molecular chain to form a stable three-dimensional cross-linked network structure, thereby improving the compatibility of the modified high temperature resistant additive with the ABS resin. At the same time, N-(4-fluorophenyl) maleimide containing a five-membered ring and a benzene ring structure is introduced into the modified high temperature resistant additive. When the material is heated, the five-membered ring and the benzene ring can limit the degree of freedom of the ABS resin molecular chain, making it difficult for the ABS resin molecular chain to rotate, thereby increasing the thermal deformation temperature of the battery cover sheet and enhancing the high temperature resistance of the battery cover sheet.

[0022] The surface of the modified flame retardant of the present invention contains polyphosphazene with strong hydrophobicity. When blended with ABS resin, the dispersibility and compatibility of the modified flame retardant in the ABS resin matrix can be improved. When the material encounters high-temperature combustion, the polyphosphazene on the surface of the modified flame retardant can decompose to generate phosphorus-containing groups, capture active free radicals generated by the ABS resin in the flame zone, thereby inhibiting the chain combustion reaction of the flame. At the same time, the hydrotalcite coating layer in the modified flame retardant will generate alkaline porous metal oxides with a large specific surface area at high temperature, so as to adsorb the generated harmful gases, particles and other smoke, thereby improving the smoke suppression effect of the modified flame retardant when it acts, and reducing the smoke generated when the battery cover is burned. In addition, the carbon microspheres as the capsule core of the modified flame retardant will decompose in the gas phase to generate inert free radicals, capture free radicals that promote chain growth, and delay the combustion chain reaction. The coke generated in the solid phase can hinder the transfer of oxygen and heat, further improving the flame retardant performance of the prepared battery cover.

[0023] The present invention uses ABS resin as a base material, and improves the heat deformation temperature of the battery cover sheet by blending a modified high-temperature resistant auxiliary agent with the ABS resin for irradiation cross-linking modification, thereby enhancing the high-temperature resistance of the battery cover sheet. At the same time, the introduction of the modified flame retardant can not only improve the flame retardancy of the battery cover sheet, but also exert the smoke suppression effect of the modified flame retardant. Under the synergistic effect of the two, the flame retardancy of the battery cover sheet is further improved. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Example 1

[0026] This embodiment provides a modified high temperature resistant additive, which is prepared by the following steps:

[0027] Add 1 g of N-(4-fluorophenyl)maleimide and 0.5 g of triallyl isocyanurate to 60 mL of xylene, stir and mix, add 0.2 g of benzoyl peroxide, heat to 100 ° C in a nitrogen atmosphere, stir and react for 4 hours, cool, place in methanol for suction filtration, and then wash and dry to obtain a modified high temperature resistant additive.

[0028] Example 2

[0029] This embodiment provides a modified high temperature resistant additive, which is prepared by the following steps:

[0030] Add 2 g of N-(4-fluorophenyl)maleimide and 3 g of triallyl isocyanurate to 60 mL of xylene, stir and mix, add 0.2 g of benzoyl peroxide, heat to 105 ° C in a nitrogen atmosphere, stir and react for 4.5 hours, cool, place in methanol for suction filtration, and then wash and dry to obtain a modified high temperature resistant additive.

[0031] Example 3

[0032] This embodiment provides a modified high temperature resistant additive, which is prepared by the following steps:

[0033] Add 3 g of N-(4-fluorophenyl)maleimide and 6 g of triallyl isocyanurate to 60 mL of xylene, stir and mix, add 0.2 g of benzoyl peroxide, heat to 110 ° C in a nitrogen atmosphere, stir and react for 5 hours, cool, place in methanol for suction filtration, and then wash and dry to obtain a modified high temperature resistant additive.

[0034] Example 4

[0035] This embodiment provides a modified flame retardant, which is prepared by the following steps:

[0036] A1. Add 2 g of sodium hydroxide and 2 g of sodium carbonate to 100 mL of deionized water, stir and dissolve to obtain an alkaline solution; add 3 g of magnesium nitrate hexahydrate and 2 g of aluminum nitrate nonahydrate to 100 mL of deionized water, stir and dissolve to obtain a salt solution;

[0037] A2. Add 2 g of carbon microspheres to 100 mL of deionized water, stir and mix, adjust the pH value to 10 with a 20 wt% sodium hydroxide solution, and then simultaneously add 60 mL of alkaline solution and 70 mL of salt solution, control the addition time to 30 min, and keep the pH value at 10. After the addition is completed, crystallize at 70 ° C for 6 h, cool, filter, wash, dry, and grind into powder to obtain modified carbon microspheres;

[0038] A3. Add 0.5 g of modified carbon microspheres to 80 mL of acetonitrile, ultrasonically disperse for 20 min, add 0.2 g of 4,4'-diaminodiphenyl ether and 18 mL of triethylamine, stir and mix, then add 40 mL of hexachlorocyclotriphosphazene solution dropwise at 30 °C, control the dropping time to 50 min, continue stirring and reacting for 5 h after the dropping is completed, cool, filter, wash, dry and grind to obtain a modified flame retardant.

[0039] Example 5

[0040] This embodiment provides a modified flame retardant, which is prepared by the following steps:

[0041] A1. Add 2 g of sodium hydroxide and 4 g of sodium carbonate to 100 mL of deionized water, stir and dissolve to obtain an alkaline solution; add 5 g of magnesium nitrate hexahydrate and 2 g of aluminum nitrate nonahydrate to 100 mL of deionized water, stir and dissolve to obtain a salt solution;

[0042] A2. Add 3 g of carbon microspheres to 100 mL of deionized water, stir and mix, adjust the pH value to 10.5 with a 20 wt% sodium hydroxide solution, and then simultaneously add 60 mL of alkaline solution and 70 mL of salt solution, control the addition time to 30 min, and keep the pH value at 10.5. After the addition is completed, crystallize at 75 ° C for 6.5 h, cool, filter, wash, dry, and grind into powder to obtain modified carbon microspheres;

[0043] A3. Add 2 g of modified carbon microspheres to 80 mL of acetonitrile, ultrasonically disperse for 20 min, add 0.3 g of 4,4'-diaminodiphenyl ether and 18 mL of triethylamine, stir and mix, and then add 50 mL of hexachlorocyclotriphosphazene solution dropwise at 35 °C, control the addition time to 50 min, and after the addition is completed, continue stirring the reaction for 5.5 h. After cooling, filter, wash, dry and grind to obtain a modified flame retardant.

[0044] Example 6

[0045] This embodiment provides a modified flame retardant, which is prepared by the following steps:

[0046] A1. Add 2 g of sodium hydroxide and 6 g of sodium carbonate to 100 mL of deionized water, stir and dissolve to obtain an alkaline solution; add 6 g of magnesium nitrate hexahydrate and 2 g of aluminum nitrate nonahydrate to 100 mL of deionized water, stir and dissolve to obtain a salt solution;

[0047] A2. Add 4 g of carbon microspheres to 100 mL of deionized water, stir and mix, adjust the pH value to 11 with a 20 wt% sodium hydroxide solution, and then simultaneously add 60 mL of alkaline solution and 70 mL of salt solution, control the addition time to 30 min, and keep the pH value at 11. After the addition is completed, crystallize at 80 ° C for 7 h, cool, filter, wash, dry, and grind into powder to obtain modified carbon microspheres;

[0048] A3. Add 3 g of modified carbon microspheres to 80 mL of acetonitrile, ultrasonically disperse for 20 min, add 0.5 g of 4,4'-diaminodiphenyl ether and 18 mL of triethylamine, stir and mix, and then add 60 mL of hexachlorocyclotriphosphazene solution dropwise at 40 °C, control the dropping time to 50 min, and continue stirring the reaction for 6 h after the addition is completed. After cooling, filter, wash, dry and grind to obtain a modified flame retardant.

[0049] Example 7

[0050] This embodiment provides a production process for a high temperature resistant and flame retardant battery cover sheet, comprising the following steps:

[0051] S1, adding 110 parts by weight of ABS resin and 3 parts by weight of modified high temperature resistant additive into a mixer and uniformly mixing, then adding into an extruder for melt extrusion, and then placing under γ rays for irradiation treatment to obtain modified ABS plastic;

[0052] S2, adding 90 parts by weight of modified ABS plastic, 0.2 parts by weight of curing agent, 3 parts by weight of modified flame retardant, and 0.3 parts by weight of plasticizer into a mixer and mixing them evenly, then adding them into an extruder for melt extrusion, cooling, pelletizing, and drying to obtain a battery cover masterbatch;

[0053] S3, the master batch of the battery cover piece is input into the capping equipment through the hopper to be heated and melted, and then injected into the mold, and after the mold is closed, compression molding, cooling and shaping, and then cutting, the battery cover piece is obtained.

[0054] Example 8

[0055] This embodiment provides a production process for a high temperature resistant and flame retardant battery cover sheet, comprising the following steps:

[0056] S1, adding 115 parts by weight of ABS resin and 5 parts by weight of modified high temperature resistant additive into a mixer and uniformly mixing, then adding into an extruder for melt extrusion, and then placing under γ rays for irradiation treatment to obtain modified ABS plastic;

[0057] S2, adding 100 parts by weight of modified ABS plastic, 0.5 parts by weight of curing agent, 4 parts by weight of modified flame retardant, and 0.4 parts by weight of plasticizer into a mixer and mixing them evenly, then adding them into an extruder for melt extrusion, cooling, pelletizing, and drying to obtain a battery cover masterbatch;

[0058] S3, the master batch of the battery cover piece is input into the capping equipment through the hopper to be heated and melted, and then injected into the mold, and after the mold is closed, compression molding, cooling and shaping, and then cutting, the battery cover piece is obtained.

[0059] Example 9

[0060] This embodiment provides a production process for a high temperature resistant and flame retardant battery cover sheet, comprising the following steps:

[0061] S1, adding 120 parts by weight of ABS resin and 8 parts by weight of modified high temperature resistant additive into a mixer and uniformly mixing, then adding into an extruder for melt extrusion, and then placing under γ rays for irradiation treatment to obtain modified ABS plastic;

[0062] S2, adding 110 parts by weight of modified ABS plastic, 0.8 parts by weight of curing agent, 6 parts by weight of modified flame retardant, and 0.6 parts by weight of plasticizer into a mixer and mixing them evenly, then adding them into an extruder for melt extrusion, cooling, pelletizing, and drying to obtain a battery cover masterbatch;

[0063] S3, the master batch of the battery cover piece is input into the capping equipment through the hopper to be heated and melted, and then injected into the mold, and after the mold is closed, compression molding, cooling and shaping, and then cutting, the battery cover piece is obtained.

[0064] Comparative Example 1: The modified high temperature resistant additive is replaced by an equal amount of N-(4-fluorophenyl)maleimide, and the rest are the same.

[0065] Comparative Example 2: No modified flame retardant was added, and the rest was the same.

[0066] Comparative Example 3: The modified flame retardant was replaced with an equal amount of commercially available flame retardant, and the rest was the same.

[0067] The performance of Examples 7 to 9 and Comparative Examples 1 to 3 was tested. Flame retardant properties: The obtained materials were prepared into 25 mm 2 ×25mm 2 ×6mm 2 For the specimens, refer to GB / T 2406.2-2009 to test the limiting oxygen index of the specimens. The higher the limiting oxygen index, the better the flame retardant performance; smoke suppression performance: refer to GB / T8627-2007, ignite the sample for 4 minutes, and test the smoke density; high temperature resistance performance: refer to GB / T 1634.1-2004, place the sample in a heat deformation tester, set the heating rate to 120℃ / h, the load to 0.45MPa, and test the heat deformation temperature. The results are shown in Table 1:

[0068] Table 1

[0069] project Example 7 Example 8 Example 9 Comparative Example 1 Comparative Example 2 Comparative Example 3 Limiting oxygen index / % 26.1 28.8 33.7 19.2 17.4 23.5 Smoke density / % 68.5 61.3 58.3 79.3 88.5 80.6 Thermal deformation temperature / ℃ 109.5 116.3 121.4 87.4 79.3 94.5

[0070] It can be seen from Table 1 that the battery cover sheets of Examples 7-9 prepared by modified high temperature resistant additives and modified flame retardants have significantly higher limiting oxygen index and heat deformation temperature than those of Comparative Examples 1-3, and have good flame retardant properties. At the same time, the smoke density can be as low as 58.3%, and has good smoke suppression performance. Compared with Comparative Examples 1 and 3, Example 7 has higher flame retardant properties, indicating that under the synergistic effect of the modified cross-linking agent and the modified flame retardant, the prepared battery cover sheets have higher flame retardant properties and high temperature resistance.

[0071] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0072] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A production process for high temperature resistant and flame retardant battery cover sheets, It is characterized in that The following steps are involved: S1, adding ABS resin and modified high temperature resistant additive into a mixer and uniformly mixing, then adding into an extruder for melt extrusion, and then placing under γ ray for irradiation treatment to obtain modified ABS plastic; S2, adding modified ABS plastic, curing agent, modified flame retardant and plasticizer into a mixer and mixing them evenly, then adding them into an extruder for melt extrusion, cooling, pelletizing and drying to obtain a battery cover masterbatch; S3, feeding the master batch of the battery cover sheet into the capping equipment through the hopper, heating and melting, and then injecting into the mold, and then closing the mold, pressing, cooling and shaping, and then cutting to obtain the battery cover sheet; The weight ratio of the ABS resin to the modified high temperature resistant auxiliary agent is 110-120:3-8; the weight ratio of the modified ABS plastic, the curing agent, the modified flame retardant and the plasticizer is 90-110:0.2-0.8:3-6:0.3-0.

6.

2. The production process of a high temperature resistant and flame retardant battery cover sheet according to claim 1, It is characterized in that The modified high temperature resistant additive is prepared by the following steps: Add N-(4-fluorophenyl)maleimide and triallyl isocyanurate to xylene, stir and mix, add benzoyl peroxide, heat to 100-110°C in a nitrogen atmosphere, stir and react for 4-5 hours, cool, place in methanol for suction filtration, wash and dry to obtain a modified high temperature resistant additive.

3. The production process of a high temperature resistant and flame retardant battery cover sheet according to claim 2, It is characterized in that The usage ratio of the xylene, N-(4-fluorophenyl)maleimide, triallyl isocyanurate and benzoyl peroxide is 60 mL: 1-3 g: 0.5-6 g: 0.2 g.

4. The production process of a high temperature resistant and flame retardant battery cover sheet according to claim 1, It is characterized in that The modified flame retardant is prepared by the following steps: A1. Add carbon microspheres to deionized water, stir and mix, adjust the pH value to 10-11 with a 20wt% sodium hydroxide solution, and then simultaneously add an alkali solution and a salt solution, control the dropping time to 30min, and keep the pH value at 10-11. After the dropwise addition is completed, crystallize at 70-80°C for 6-7h, cool, filter, wash, dry, and grind into powder to obtain modified carbon microspheres; A2. Add modified carbon microspheres to acetonitrile, ultrasonically disperse for 20 minutes, add 4,4'-diaminodiphenyl ether and triethylamine, stir and mix, and then drop hexachlorocyclotriphosphazene solution at 30-40°C, control the dropping time to 50 minutes, and continue stirring the reaction for 5-6 hours after the dropwise addition is completed. After cooling, filter, wash, dry and grind to obtain a modified flame retardant.

5. The production process of a high temperature resistant and flame retardant battery cover sheet according to claim 4, It is characterized in that The dosage ratio of the deionized water, carbon microspheres, alkaline solution and salt solution is 100mL:2-4g:60mL:70mL; the alkaline solution is prepared by dissolving sodium hydroxide and sodium carbonate in 100mL deionized water in a mass ratio of 1:1-3; the salt solution is prepared by dissolving magnesium nitrate hexahydrate and aluminum nitrate nonahydrate in 100mL deionized water in a mass ratio of 1.5-3:

1.

6. The production process of a high temperature resistant and flame retardant battery cover sheet according to claim 4, It is characterized in that The dosage ratio of acetonitrile, modified carbon microspheres, 4,4'-diaminodiphenyl ether, triethylamine and hexachlorocyclotriphosphazene solution is 80mL: 0.5-3g: 0.2-0.5g: 18mL: 40-60mL; the hexachlorocyclotriphosphazene solution is composed of hexachlorocyclotriphosphazene and acetonitrile in a dosage ratio of 0.2-1g: 100mL.

7. A high temperature resistant and flame retardant battery cover sheet, It is characterized in that Prepared according to the production process according to any one of claims 1 to 6.