Orange red luminescent material with high thermal stability and preparation method thereof
Through the combination of Sc(NbO4)x(TaO4)1-x:ySm3+ material and commercial yellow phosphor, the problem of poor color rendering of white LEDs in orange-red spectral spectral is solved, and white LEDs with high thermal stability and high color rendering index are achieved , improves luminous performance and cost-effectiveness.
Patent Information
- Application Number
- CN202411050797.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
Existing white LEDs have poor color rendering properties and are costly when achieving orange-red spectral components, and lack high-performance orange-red phosphor materials to improve luminous performance.
Sc(NbO4)x(TaO4)1-x:ySm3+ is used as the orange-red luminescent material, and is prepared by sol-gel method or high-temperature solid phase method, Sm3+ is used as the activation ion, Sc(NbO4)x(TaO4)1-x matrix It has a monoclinic symmetric structure and rich near-UV to blue light absorption band, and obtains the highest luminous efficiency when the doping concentration is 2 at % and improves the color rendering index of white LEDs in combination with commercial yellow phosphors.
It significantly improves the color rendering index of white light LEDs under near-ultraviolet or blue light chip excitation, and has good luminescence thermal stability, and is suitable for the field of white light LEDs.
Smart Images

Figure CN118978916A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rare earth luminescent materials, and in particular relates to an orange-red luminescent material with high thermal stability and a preparation method thereof. Background Art
[0002] White light emitting diodes (WLEDs) are considered to be the best choice to replace traditional solid-state lighting due to their long life, high efficiency, energy saving and environmental protection. At present, there are two main methods to achieve white light LEDs. One is to use InGaN blue chips and yellow phosphor Y3Al5O 12 :Ce 3+ The white light obtained by this scheme is obtained by combining the near-ultraviolet (370-410nm) chip with the three-primary color phosphor. However, the white light obtained by this scheme lacks the orange-red and red spectral components, so the color rendering is relatively poor and the color temperature is high. Another method is usually achieved by combining the near-ultraviolet (370-410nm) chip with the three-primary color phosphor. Compared with the former, the white light obtained by the three-primary color phosphor excited by the near-ultraviolet (NUV) chip has a higher color rendering index (CRI) and luminous efficiency, but the corresponding cost is also higher. Therefore, the development of a new high-performance orange-red phosphor material has important practical application value for improving the luminous performance of white light LEDs with InGaN blue chips and yellow phosphors.
[0003] The ions that can be used to achieve orange-red luminescence are mainly rare earth ions Eu 2+ 、Eu 3+ 、Sm 3+ and transition metal ions Mn 4+ Among them, Sm 3+ It has multiple strong absorption bands in the ultraviolet-visible region. After the electrons in its 4f orbit absorb the energy of the ultraviolet-visible band, 4 G 5 / 2 The energy level radiates to the ground state 6 H J / 2 (J=5,7,9) energy levels can emit visible light with wavelengths of 575, 615 and 660nm, corresponding to orange-red. 3+ The new orange-red phosphor materials doped with Sm have attracted extensive attention and research. 3+ :Li2LaTiTaO 710 (Dalton Trans.2023,52,9068-9076), Sm 3+ :NaBi(MoO4)2(Opt.Laser Technol.2022,147,7), etc.
[0004] The matrix material has an important influence on the luminescent properties of rare earth luminescent ions, especially the luminescent efficiency and thermal stability of luminescence. Tantalate niobate materials are good matrices for doped luminescent materials due to their simple composition. They can provide a suitable coordination environment for transition metal and rare earth ions, and have the advantages of low phonon energy, low structural symmetry, and stable physical and chemical properties. At present, there is no research on Sm 3+ Report on doped scandium tantalate niobate material as a new type of high-performance orange-red luminescent material. Summary of the invention
[0005] The purpose of the present invention is to overcome the above problems existing in the conventional technology, and to provide an orange-red luminescent material with high thermal stability and a preparation method thereof. The orange-red phosphor has a rich absorption band in the near-ultraviolet to blue light band, and can be well matched with the currently commercialized near-ultraviolet and blue light chips. By mixing the orange-red luminescent material with commercial yellow phosphor, the color rendering index of white light LEDs excited by near-ultraviolet or blue light chips can be significantly improved, so it has strong practical application value in the field of white light LEDs.
[0006] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:
[0007] The present invention provides an orange-red luminescent material with high thermal stability. The molecular formula of the orange-red luminescent material is Sc(NbO4): x (TaO4) 1-x :ySm 3+ , where x=0.1~0.9, y=0.005~0.1.
[0008] Furthermore, the orange-red luminescent material is Sc(NbO4) x (TaO4) 1-x The complex is based on Sm 3+ as active ions.
[0009] Furthermore, the orange-red luminescent material contains Sc(NbO4) x (TaO4) 1-x The structure of the matrix is monoclinic symmetric and the space group is P12 / a1.
[0010] Furthermore, the activation ions Sm doped into the orange-red luminescent material 3+ The concentration is generally 0.5 at% to 10 at%, where at% represents atomic percentage, that is, y=0.005 to 0.1 in the molecular formula.
[0011] Furthermore, the activated ions Sm in the orange-red luminescent material 3+ The highest luminous efficiency can be obtained when the doping concentration is 2at%. When the doping concentration is higher than 2at%, Sm3+ The concentration quenching effect of luminescence is caused by dipole-dipole interaction.
[0012] Furthermore, the orange-red luminescent material has rich absorption bands in the near-ultraviolet to blue light band, and can be well matched with currently commercialized near-ultraviolet and blue light chips, thereby being effectively excited; mixing the orange-red luminescent material with commercial yellow phosphor can improve the color rendering index of white light LEDs in which near-ultraviolet or blue light chips excite yellow phosphors.
[0013] Furthermore, the luminescence mechanism of the orange-red luminescent material is: the activation ion Sm 3+ Under near-ultraviolet or blue light excitation, the electrons on its 4f energy level jump from the ground state to the high-energy excited state, and then non-radiatively to the first excited state. 4 G 5 / 2 , then from 4 G 5 / 2 The energy level radiates to the ground state 6 H J / 2 (J=5,7,9) energy levels can emit visible light with central wavelengths of approximately 575, 615 and 660nm, and the corresponding luminescent color is orange-red.
[0014] Furthermore, the orange-red luminescent material has good luminescence thermal stability, and the activation energy E related to the luminescence thermal stability is a Greater than 0.1eV.
[0015] The present invention also provides a method for preparing the above-mentioned orange-red luminescent material with high thermal stability, and the preparation method adopts a sol-gel method or a high-temperature solid phase method.
[0016] When the preparation method adopts the sol-gel method, the method specifically comprises the following steps:
[0017] 1) Calculate and weigh the corresponding reagents according to the stoichiometric ratio, add Nb2O5 and Ta2O5 to HF, and dissolve them in a water bath at 80°C for 6 to 12 hours to obtain a clear and transparent solution;
[0018] 2) Precipitating mixed tantalum-niobium hydroxide from the resulting mixture by adding aqueous ammonia. The precipitate was washed three times with deionized water to remove fluoride ions, with a solid-liquid volume ratio of 1:3, and dried at 100°C;
[0019] 3) Add appropriate amounts of Sc(NO3)3 and Sm(NO3)3 solutions to the precipitate, stir, and then adjust the pH value of the resulting suspension to 8-9 using 25% ammonia solution;
[0020] 4) filtering off the residue, washing with deionized water, and then drying at 110-120° C. to obtain a dry gel;
[0021] 5) calcining at 950-1050° C. for 2-4 hours to obtain a powder solid, and then finely grinding the powder solid to obtain a luminescent powder material.
[0022] The beneficial effects of the present invention are:
[0023] The present invention provides an orange-red luminescent material with high thermal stability and a preparation method thereof. The orange-red phosphor has rich absorption bands in the near-ultraviolet to blue light band, and can be well matched with currently commercialized near-ultraviolet and blue light chips. By mixing the orange-red luminescent material with commercial yellow phosphor, the color rendering index of white light LEDs excited by near-ultraviolet or blue light chips can be significantly improved; in addition, the orange-red luminescent material also has good luminescent thermal stability, and therefore has strong practical application value in the field of white light LEDs.
[0024] Of course, any product implementing the present invention does not necessarily need to achieve all of the above advantages at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0026] Figure 1 To prepare Sc(NbO4) by sol-gel method 0.5 (TaO4) 0.5 :ySm 3+ XRD pattern of orange-red luminescent material;
[0027] Figure 2 Sc(NbO4) 0.5 (TaO4) 0.5 :ySm 3+ Emission spectrum of orange-red luminescent material;
[0028] Figure 3 Sc(NbO4) 0.5 (TaO4) 0.5 :ySm 3+ CIE chromaticity coordinate diagram of orange-red luminescent materials;
[0029] Figure 4 2at%Sm 3+ Doped Sc(NbO4) 0.5 (TaO4) 0.5 Excitation spectrum of orange-red luminescent material, monitoring wavelength is 605nm;
[0030] Figure 5 2at%Sm 3+ Doped Sc(NbO4) 0.5 (TaO4) 0.5 Temperature-dependent emission spectra of orange-red luminescent materials;
[0031] Figure 6 2at%Sm 3+ Doped Sc(NbO4) 0.5 (TaO4) 0.5 Schematic diagram of temperature-dependent fluorescence lifetime of orange-red luminescent materials;
[0032] Figure 7 2at%Sm 3+ Doped Sc(NbO4) 0.5 (TaO4) 0.5 The normalized temperature-dependent emission intensity of orange-red luminescent materials varies with temperature;
[0033] Figure 8 2at%Sm 3+ Doped Sc(NbO4) 0.5 (TaO4) 0.5 The relationship between the fitted fluorescence lifetime value of the orange-red luminescent material and the temperature;
[0034] Fig. 9 To use the Arrhenius formula for 2at% Sm 3+ Doped Sc(NbO4) 0.5 (TaO4) 0.5 Fitting diagram of variable temperature emission spectrum of orange-red luminescent material;
[0035] Fig.10 2at% Sm is packaged for 405nm blue light chip 3+ Doped Sc(NbO4) 0.5 (TaO4) 0.5 Orange-red phosphor and commercial GaYAG:Ce 3+ Yellow phosphor and individually packaged commercial GaYAG:Ce 3+ LED spectrum of yellow phosphor;
[0036] Fig.11 To prepare 2at% Sm by sol-gel method 3+ Doped Sc(NbO4) 0.1 (TaO4) 0.9 Excitation spectrum of orange-red luminescent material, monitoring wavelength 605nm;
[0037] Fig.12 To prepare 2at% Sm by sol-gel method 3+Doped Sc(NbO4) 0.1 (TaO4) 0.9 Temperature-dependent emission spectrum of orange-red luminescent materials;
[0038] Fig.13 To prepare 2at% Sm by sol-gel method 3+ Doped Sc(NbO4) 0.1 (TaO4) 0.9 Cloud diagram of the temperature-dependent emission spectrum of orange-red luminescent materials;
[0039] Fig.14 2at%Sm 3+ Doped Sc(NbO4) 0.1 (TaO4) 0.9 Arrhenius formula fitting results of orange-red luminescent materials;
[0040] Fig.15 To prepare 2at% Sm by sol-gel method 3+ Doped Sc(NbO4) 0.9 (TaO4) 0.1 Excitation spectrum of orange-red luminescent material, monitoring wavelength 605nm;
[0041] Fig.16 To prepare 2at% Sm by sol-gel method 3+ Doped Sc(NbO4) 0.9 (TaO4) 0.1 Temperature-dependent emission spectrum of orange-red luminescent materials;
[0042] Fig.17 To prepare 2at% Sm by sol-gel method 3+ Doped Sc(NbO4) 0.9 (TaO4) 0.1 Cloud diagram of the temperature-dependent emission spectrum of orange-red luminescent materials;
[0043] Fig.18 2at%Sm 3+ Doped Sc(NbO4) 0.9 (TaO4) 0.1 Arrhenius formula fitting results for orange-red luminescent materials. DETAILED DESCRIPTION
[0044] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0045] Example 1
[0046] Preparation of Sc(NbO4) by sol-gel method 0.5 (TaO4) 0.5 :ySm 3+ Orange-red luminescent material, wherein y=0.005-0.1.
[0047] Nb2O5 and Ta2O5 were added to hydrofluoric acid (HF) in a stoichiometric ratio of 1:1, and dissolved in a water bath at 80°C for 8 hours to obtain a clear and transparent solution; mixed tantalum and niobium hydroxides were precipitated from the obtained mixture by adding ammonia water. The precipitate was washed three times with deionized water to remove fluoride ions, with a solid-liquid volume ratio of 1:3, and dried at 100°C; appropriate amounts of scandium nitrate (Sc(NO3)3) and samarium nitrate (Sm(NO3)3) solutions were added to the precipitate in ratios of 0.995:0.005, 0.99:0.01, 0.98:0.02, 0.97:0.03, 0.95:0.05, 0.92:0.08, and 0.9:0.1, respectively, to prepare seven samples, and after stirring, the pH value of the resulting suspension was adjusted to about 8 to 9 using a 25% ammonia solution; the residue was filtered out, washed with deionized water, and then dried at 115°C to obtain a dry gel; it was then calcined at 1000°C for 3 hours to obtain a powder solid; the synthesized powder was finely ground in an agate mortar to obtain Sc(NbO4) 0.5 (TaO4) 0.5 :ySm 3+ Orange-red luminescent material, y=0.005, 0.01, 0.02, 0.03, 0.05, 0.08, 0.1.
[0048] The XRD characterization results of the 7 samples prepared are as follows: Figure 1 As shown in the figure, the prepared samples are consistent with pure ScNbO4 and ScTaO4, belong to the monoclinic system, the space group is P12 / a1, no impurity phase appears, and the doped Sm 3+ All successfully entered the lattice.
[0049] The emission spectra of 7 samples excited by 407nm blue light are as follows Figure 2 As shown, there are three emission bands in the 540-690nm visible light band, with central wavelengths at 567, 617 and 659nm, corresponding to Sm 3+ of 4 G 5 / 2 → 6 H 5 / 2 , 4 G 5 / 2 → 6 H 7 / 2 and4 G 5 / 2 → 6 H 9 / 2 In particular, when y = 0.02, that is, Sm 3+ When the doping concentration is 2at%, the emission intensity of the sample is the strongest, indicating that Sm 3+ In Sc(NbO4) 0.5 (TaO4) 0.5 The optimum doping concentration in the matrix is 2 at%.
[0050] According to the emission spectrum of the sample, the CIE chromaticity coordinate diagram of the sample is drawn, as shown in Figure 3 It is obvious that the luminescent colors of the seven samples are all located in the orange-red position in the CIE chromaticity coordinate diagram, and the corresponding chromaticity coordinate range is x=0.548~0.569, y=0.422~0.440.
[0051] 2at%Sm 3+ The excitation spectrum of the doped sample (monitoring wavelength is 605nm) is as follows Figure 4 As shown, the sample has a large number of excitation bands in the near-ultraviolet and blue light bands, among which the excitation intensity at 407nm is the strongest, indicating that the sample can be well matched with the current near-ultraviolet and blue light excited LEDs for use in high-performance white light LEDs.
[0052] For 2at%Sm 3+ Doped Sc(NbO4) 0.5 (TaO4) 0.5 The thermal stability of luminescence of orange-red phosphor was analyzed. Figure 5 and Figure 6 They are the temperature-dependent emission spectrum and temperature-dependent fluorescence lifetime of the sample between 330K and 510K. From the relationship between the normalized temperature-dependent emission intensity of the sample and the temperature, it can be seen that ( Figure 7 ), with the increase of temperature, the emission intensity of the sample gradually decreases, and the sample still has more than 80% of the room temperature emission intensity at 420K. In addition, the fluorescence lifetime of the sample does not change with the change of temperature ( Figure 8 ), indicating that the sample has good thermal stability of luminescence. The activation energy E of the sample was obtained by fitting the variable temperature emission spectrum of the sample using the Arrhenius formula. a is 0.272eV, such as Fig. 9 As shown, it indicates that the sample has excellent luminescence thermal stability.
[0053] In order to further verify that Sc(NbO4) 0.5 (TaO4) 0.5 :ySm 3+ The application of orange-red luminescent materials in the field of white light LEDs will 3+Doped Sc(NbO4) 0.5 (TaO4) 0.5 Orange-red phosphor and commercial GaYAG:Ce 3+ Yellow phosphor is co-packaged with 405nm blue light chip, in which GaYAG:Ce 3+ Yellow phosphor with 2at% Sm 3+ Doped Sc(NbO4) 0.5 (TaO4) 0.5 The weight ratio of the orange-red phosphor is 3:1.
[0054] In order to better compare the experimental results, the spectra of the co-packaged white LED and the white LED packaged with yellow phosphor were compared. Fig.10 Obviously, the spectrum of the co-packaged white LED is wider than that of the white LED with yellow phosphor packaged alone, which effectively compensates for the spectrum components of the white LED with yellow phosphor packaged alone in the orange-red region and has a better color rendering effect.
[0055] Example 2
[0056] Preparation of 2at% Sm by sol-gel method 3+ Doped Sc(NbO4) 0.1 (TaO4) 0.9 Orange-red luminescent material.
[0057] Nb2O5 and Ta2O5 were added to hydrofluoric acid (HF) in a stoichiometric ratio of 1:9, and dissolved in a water bath at 80°C for 8 hours to obtain a clear and transparent solution; mixed tantalum-niobium hydroxide was precipitated from the resulting mixture by adding ammonia water. The precipitate was washed three times with deionized water to remove fluoride ions, with a solid-liquid volume ratio of 1:3, and dried at 100°C; scandium nitrate (Sc(NO3)3) and samarium nitrate (Sm(NO3)3) solutions in a ratio of 0.98:0.02 were added to the precipitate, and after stirring, the pH value of the resulting suspension was adjusted to about 8 to 9 using a 25% ammonia solution; the residue was filtered off, washed with deionized water, and then dried at 115°C to obtain a dry gel; it was then calcined at 1000°C for 3 hours to obtain a powder solid; the synthesized powder was finely ground in an agate mortar to obtain 2at% Sm 3+ Doped Sc(NbO4) 0.1 (TaO4) 0.9 Orange-red luminescent material.
[0058] The excitation spectrum (monitoring wavelength 605nm) and temperature-dependent emission spectrum of the sample are as follows: Fig.11 , Fig.12 and Fig.13 As shown. 2at% Sm 3+ Doped Sc(NbO4)0.1 (TaO4) 0.9 Excitation spectra of orange-red luminescent materials and 2at% Sm 3+ Doped Sc(NbO4) 0.5 (TaO4) 0.5 There is no obvious difference in the samples. However, by fitting the 2at% Sm 3+ Doped Sc(NbO4) 0.1 (TaO4) 0.9 The temperature-dependent emission spectrum of the orange-red luminescent material is used to obtain the activation energy E of the sample. a 0.137eV( Fig.14 ), less than 2at% Sm 3+ Doped Sc(NbO4) 0.5 (TaO4) 0.5 The sample has a luminescence thermal stability of 0.272 eV, indicating that its luminescence thermal stability may be slightly worse than that of 2 at% Sm 3+ Doped Sc(NbO4) 0.5 (TaO4) 0.5 sample.
[0059] Example 3
[0060] Preparation of 2at% Sm by sol-gel method 3+ Doped Sc(NbO4) 0.9 (TaO4) 0.1 Orange-red luminescent material.
[0061] Nb2O5 and Ta2O5 were added to hydrofluoric acid (HF) in a stoichiometric ratio of 9:1, and dissolved in a water bath at 80°C for 8 hours to obtain a clear and transparent solution; mixed tantalum-niobium hydroxide was precipitated from the resulting mixture by adding ammonia water. The precipitate was washed three times with deionized water to remove fluoride ions, with a solid-liquid volume ratio of 1:3, and dried at 100°C; scandium nitrate (Sc(NO3)3) and samarium nitrate (Sm(NO3)3) solutions in a ratio of 0.98:0.02 were added to the precipitate, and after stirring, the pH value of the resulting suspension was adjusted to about 8 to 9 using a 25% ammonia solution; the residue was filtered off, washed with deionized water, and then dried at 115°C to obtain a dry gel; it was then calcined at 1000°C for 3 hours to obtain a powder solid; the synthesized powder was finely ground in an agate mortar to obtain 2at% Sm 3+ Doped Sc(NbO4) 0.9 (TaO4) 0.1 Orange-red luminescent material.
[0062] The excitation spectrum (monitoring wavelength 605nm) and temperature-dependent emission spectrum of the sample are as follows: Fig.15 , Fig.16 and Fig.17As shown. It can be seen that 2at% Sm 3+ Doped Sc(NbO4) 0.9 (TaO4) 0.1 Excitation spectra of orange-red luminescent materials and 2at% Sm 3+ Doped Sc(NbO4) 0.5 (TaO4) 0.5 and Sc(NbO4) 0.1 (TaO4) 0.9 There is no obvious difference in the samples. However, through fitting, we get 2at% Sm 3+ Doped Sc(NbO4) 0.9 (TaO4) 0.1 The temperature-dependent emission spectrum of the orange-red luminescent material is used to obtain the activation energy E of the sample. a 0.113eV( Fig.18 ), less than 2at% Sm 3+ Doped Sc(NbO4) 0.5 (TaO4) 0.5 The sample has a 0.272eV and Sc(NbO4) 0.1 (TaO4) 0.9 The sample has a luminescence thermal stability of 0.137 eV, indicating that its luminescence thermal stability may be slightly worse than that of 2 at% Sm 3+ Doped Sc(NbO4) 0.5 (TaO4) 0.5 and Sc(NbO4) 0.1 (TaO4) 0.9 sample.
[0063] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A high thermal stability orange-red luminescent material, characterized in that: The molecular formula of the orange-red luminescent material is Sc(NbO4) x (TaO4) 1-x :ySm 3+ , where x=0.1~0.9, y=0.005~0.
1.
2. The high thermal stability orange-red luminescent material according to claim 1, characterized in that: The orange-red luminescent material is Sc(NbO4) x (TaO4) 1-x The complex is based on Sm 3+ as an active ion.
3. The high thermal stability orange-red luminescent material according to claim 2, characterized in that: The orange-red luminescent material contains Sc(NbO4) x (TaO4) 1-x The structure of the matrix is monoclinic symmetric and the space group is P12 / a1.
4. The high thermal stability orange-red luminescent material according to claim 3, characterized in that: The activated ion Sm doped in the orange-red luminescent material 3+ The concentration is generally 0.5 at% to 10 at%, where at% represents atomic percentage, that is, y=0.005 to 0.1 in the molecular formula.
5. The high thermal stability orange-red luminescent material according to claim 4, characterized in that: The activated ion Sm in the orange-red luminescent material 3+ The highest luminous efficiency can be obtained when the doping concentration is 2at%. When the doping concentration is higher than 2at%, Sm 3+ The concentration quenching effect of luminescence is caused by dipole-dipole interaction.
6. The high thermal stability orange-red luminescent material according to claim 1, characterized in that: The orange-red luminescent material has rich absorption bands in the near-ultraviolet to blue light band, and can be well matched with currently commercialized near-ultraviolet and blue light chips, thereby being effectively excited; mixing the orange-red luminescent material with commercial yellow phosphor can improve the color rendering index of white light LEDs in which near-ultraviolet or blue light chips excite yellow phosphors.
7. The orange-red luminescent material with high thermal stability according to claim 1, characterized in that: The luminescence mechanism of the orange-red luminescent material is: the activation ion Sm 3+ Under near-ultraviolet or blue light excitation, the electrons on its 4f energy level jump from the ground state to the high-energy excited state, and then non-radiatively to the first excited state. 4 G 5 / 2 , then from 4 G 5 / 2 The energy level radiates to the ground state 6 H J / 2 (J=5,7,9) energy levels can emit visible light with central wavelengths of approximately 575, 615 and 660nm, and the corresponding luminescent color is orange-red.
8. The orange-red luminescent material with high thermal stability according to claim 1, characterized in that: The orange-red luminescent material has good luminescence thermal stability, and the activation energy E related to the luminescence thermal stability a Greater than 0.1eV.
9. The method for preparing an orange-red luminescent material with high thermal stability according to any one of claims 1 to 8, characterized in that: The preparation method adopts a sol-gel method or a high-temperature solid phase method.
10. The orange-red luminescent material with high thermal stability according to claim 9, characterized in that: When the preparation method adopts the sol-gel method, the method specifically comprises the following steps: 1) Calculate and weigh the corresponding reagents according to the stoichiometric ratio, add Nb2O5 and Ta2O5 to HF, and dissolve them in a water bath at 80°C for 6 to 12 hours to obtain a clear and transparent solution; 2) precipitating mixed tantalum-niobium hydroxide from the resulting mixture by adding ammonia water; the precipitate was washed three times with deionized water to remove fluoride ions, with a solid-liquid volume ratio of 1:3, and dried at 100°C; 3) Add appropriate amounts of Sc(NO3)3 and Sm(NO3)3 solutions to the precipitate, stir, and then adjust the pH value of the resulting suspension to 8-9 using 25% ammonia solution; 4) filtering off the residue, washing with deionized water, and then drying at 110-120° C. to obtain a dry gel; 5) calcining at 950-1050° C. for 2-4 hours to obtain a powder solid, and then finely grinding the powder solid to obtain a luminescent powder material.