Antibacterial degradable PBSA / PLA non-woven fabric and preparation method thereof
Through the preparation of PBSA/PLA nonwoven fabrics, combined with specific components in antibacterial masterbatches and spunbond technology, the problems of rough touch and poor antibacterial properties of biodegradable nonwoven fabrics are solved, and soft and efficient antibacterial nonwoven products are realized , suitable for infants and young children's diapers and feminine hygiene products.
Patent Information
- Application Number
- CN202411045106.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
The existing biodegradable non-woven fabrics are limited in the fields of infant diapers and feminine hygiene products, due to their rough touch and poor antibacterial properties.
By using the preparation method of PBSA/PLA nonwoven fabric, by adjusting the blending ratio of PBSA and PLA, combining tea tree essential oil, chitosan, ammonium dihydrogen phosphate and nanotitanium dioxide in the antibacterial masterbatch, it is modified through blending and Spunbond technology produces soft non-woven fabrics with excellent antibacterial properties.
It has achieved a significant improvement in the softening of the touch and antibacterial properties of non-woven fabrics. It is suitable for medical and health fields, especially in infant diapers and feminine hygiene products.
Smart Images

Figure CN118979343A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and particularly relates to an antibacterial and degradable PBSA / PLA non-woven fabric and a preparation method thereof. Background Art
[0002] Non-woven fabrics are also called non-woven fabrics. According to different preparation methods, there are needle-punched non-woven fabrics, melt-blown non-woven fabrics, spunbond non-woven fabrics, spunlace non-woven fabrics, wet-laid non-woven fabrics, etc. Non-woven fabrics are soft, moisture-proof, breathable, thin, non-toxic and tasteless, low-priced and recyclable. At the same time, they do not produce fiber scraps, are flexible and durable, so they have been widely used in the medical and health fields. In recent years, the growth rate of the world's demand for non-woven fabrics has been higher than the growth of the global economy. Traditional non-woven fabric materials are mostly petroleum-based materials such as PP and PET, which are difficult to degrade in the natural environment. If they are discarded at will, they are easy to cause environmental pollution. Therefore, the development of biodegradable non-woven fabric materials has received more and more attention. Polylactic acid (abbreviated as PLA) is a new type of biodegradable material made from starch raw materials from renewable plant resources (such as corn, cassava, etc.). It is mainly to obtain glucose from starch raw materials through saccharification, and then ferment glucose and certain strains to produce high-purity lactic acid, and then synthesize polylactic acid of a certain molecular weight through chemical synthesis. It has good biodegradability and can be completely degraded by microorganisms in nature after use, eventually generating carbon dioxide and water without polluting the environment. This is very beneficial to environmental protection and is a recognized environmentally friendly material. Since the source of polylactic acid raw materials is sufficient and renewable, and it has excellent biocompatibility, skin-friendly, and anti-allergic, it is an ideal raw material for disposable sanitary products. However, due to its processing characteristics being different from the petroleum-based chemical fibers used in the prior art, it cannot directly replace the above-mentioned petroleum-based chemical fibers and adopts the existing structure and processing technology.
[0003] CN108823977A discloses a method for preparing an antibacterial PLA nonwoven fabric, which comprises pre-treating the PLA nonwoven fabric to obtain a first PLA nonwoven fabric; performing medium treatment on the first PLA nonwoven fabric to obtain a second PLA nonwoven fabric; preparing a cationic nanosilver solution; placing the second PLA nonwoven fabric in the cationic nanosilver solution for treatment to obtain a third PLA nonwoven fabric; and obtaining a PLA nanosilver nonwoven fabric based on the third PLA nonwoven fabric. Since PLA has poor toughness and high strength, the prepared PLA nonwoven fabric has a rough surface and a hard feel, and is not suitable for use in the field of infant diapers and female hygiene products.
[0004] CN101824708B discloses a fully degradable polylactic acid fiber melt-blown nonwoven fabric and a preparation method thereof. The nonwoven fabric is made by spinning polylactic acid slices at a melting temperature of 180-185°C, and the fiber filaments stretched by hot air are self-bonded and hot-rolled; the average fineness of the fiber filaments of the nonwoven fabric is 0.52-5 μm, and the surface density is 5-50 g / m 2 , thickness of 0.1 to 0.9 mm, longitudinal strength to transverse strength ratio of 0.9 to 1.2, and bacterial filtration efficiency of more than 95%; wherein the weight average molecular weight of the polylactic acid slice is 80,000 to 150,000, the melt index is 75 to 85 g / 10 min; the hot rolling bonding point density ranges from 2.5×10 4 ~15×10 4 Point / m 2 The bonding area accounts for 8-20% of the total area of the fiber web. However, the defects of the polylactic acid melt-blown nonwoven fabric are poor antibacterial properties, hard surface touch, poor comfort, and are not suitable for use in infant diapers and female hygiene products.
[0005] CN113584725A discloses a preparation process of a PHBV and PLA biodegradable antibacterial and deodorizing spunbonded nonwoven fabric, comprising 1% to 20% PHBV material and 80% to 99% PLA material in a weight ratio, wherein the spunbonded nonwoven fabric is obtained from PHBV bio-based fully degradable antibacterial masterbatch and PLA bio-based fully degradable masterbatch through the following spunbonding process: S1, feeding the bio-based green and environmentally friendly antibacterial masterbatch into a screw extruder, heating and melting, and extruding the spinning melt; and adding a certain amount of The proportion of bio-based PLA masterbatch is fully stirred and mixed in a mixing hopper to obtain a molten material; S2, the molten material is filtered through a filter screen, metered and distributed, and extruded from the small holes of the spinneret of the spinning device by a metering pump to form many filament streams; S3, after being cooled by side blowing in the quenching chamber, the melt stream is cooled into filaments, and then stretched by high-speed airflow in the drafting area and laid on the mesh curtain, and the fibers are laid into a net on the web laying machine; S4, the mesh curtain is transported to the hot rolling mill through self-bonding or hot rolling to obtain a non-woven fabric. This technology achieves antibacterial and antiviral effects by adding bio-based degradable masterbatch to the fiber and controlling the process, but how to control the process to achieve the antibacterial effect is not specifically explained.
[0006] CN106048894B discloses a nonwoven fabric, comprising the following materials in parts by weight: PET 70-80 parts, PLA15-20 parts, antibacterial agent 5-10 parts, acrylic adhesive 10-15 parts, diatomaceous earth 1-2 parts, wherein the antibacterial agent is a nano silver chitosan antibacterial agent, which is prepared by reacting dialdehyde chitosan with silver nitrate, and the mass ratio of the sum of the mass of nano silver and dialdehyde chitosan in the nano silver chitosan antibacterial agent to the mass of the solvent is 1:1. The production process of the non-woven fabric comprises the following steps: step 1, opening, mixing, finely opening, filtering and combing PET fiber and PLA fiber to obtain mixed fiber; step 2, uniformly mixing the antibacterial agent and acrylic acid to obtain an impregnation solution, and impregnating the mixed fiber to obtain a non-woven fabric to be treated; step 3, soaking the non-woven fabric to be treated obtained in step 2 in a 500 mg / L diatomaceous earth suspension under continuous flow conditions for 30-50 hours; step 4, drying, baking, cooling and reeling the non-woven fabric obtained in step 3 to obtain a finished non-woven fabric. However, the antibacterial effect obtained by impregnating mixed fibers with antibacterial agents is unstable. In addition, this technology uses PET resin as the main component, and non-woven fabrics made from PET cannot be completely degraded.
[0007] Therefore, the current biodegradable non-woven products are limited in their application in the fields of infant diapers and women's products due to the limitations of their formula and process. How to carry out technological innovation to address the defects of biodegradable non-woven fabrics such as rough touch and poor antibacterial properties is an urgent problem that needs to be solved. Summary of the invention
[0008] In order to solve the above problems, the purpose of the present invention is to provide an antibacterial and degradable PBSA (polybutylene succinate-adipate) / PLA (polylactic acid) non-woven fabric and a preparation method thereof. The present invention prepares a non-woven fabric product with a soft and smooth touch and excellent antibacterial properties through raw material selection, formula design, blending modification, and spunbond process, and its comprehensive performance can meet the use requirements of infant diapers and female hygiene products.
[0009] The technical solution of the present invention is as follows:
[0010] The present invention provides an antibacterial and degradable PBSA / PLA non-woven fabric, which comprises the following components in parts by weight:
[0011] PBSA: 9-90 parts by weight;
[0012] PLA: 5-20 parts by weight;
[0013] Antibacterial masterbatch: 0.5-10 parts by weight;
[0014] Chain extender: 0.1-1 parts by weight:
[0015] Lubricant: 1-8 parts by weight;
[0016] Anti-hydrolysis agent: 0.1-2 parts by weight;
[0017] Nucleating agent: 0.1-1 parts by weight;
[0018] Antioxidant: 0.2-1.0 parts by weight;
[0019] The fiber diameter of the PBSA / PLA nonwoven fabric is 12-18 μm.
[0020] Furthermore, the melt index of the PBSA at 190° C. and 2.16 kg is 10-50 g / 10 min.
[0021] Furthermore, the melt index of the PLA at 190° C. and 2.16 kg is 15-50 g / 10 min.
[0022] Furthermore, the antibacterial masterbatch comprises the following components: 40-90 parts by weight of PBSA, 1-3 parts by weight of tea tree essential oil, 2-5 parts by weight of chitosan, 3-8 parts by weight of ammonium dihydrogen phosphate, 5-10 parts by weight of nano titanium dioxide, 0.5-2 parts by weight of dispersant and 0.2-0.5 parts by weight of antioxidant.
[0023] Among them, tea tree essential oil has a broad-spectrum antibacterial activity and has a good killing or inhibitory effect on many bacteria and fungi; its main component terpene can destroy the bacterial cell wall, thereby achieving an antibacterial effect. Chitosan is a natural high-molecular polymer extracted from animal shells, which has a broad-spectrum antibacterial property. Its mechanism includes destroying the permeability of bacterial cell membranes and affecting the synthesis of bacterial cell phospholipids and proteins. When ammonium dihydrogen phosphate is usually used as an antibacterial agent, it can inhibit the growth and reproduction of bacteria by changing the internal environment of bacteria. Nano-titanium dioxide decomposes bacteria under the action of photocatalysis to achieve an antibacterial effect. When the electron energy reaches or exceeds its band gap energy, the electron is excited from the valence band to the conduction band, and corresponding holes are generated in the valence band. These free radicals and active oxygen ions can effectively destroy the structure of bacteria.
[0024] Furthermore, the preparation method of the antibacterial masterbatch is as follows: first, tea tree essential oil, chitosan, ammonium dihydrogen phosphate, nano titanium dioxide, dispersant and antioxidant are weighed according to respective weight portions and added into a high-speed mixer, and mixed at a temperature of 50-70° C. for 5-10 minutes to obtain an antibacterial auxiliary agent mixture; then, the obtained antibacterial auxiliary agent mixture is evenly mixed with PBSA, and extruded and granulated by a twin-screw extruder to obtain an antibacterial masterbatch.
[0025] In the preparation process of the antibacterial masterbatch, the dispersant is ethylene-acrylic acid copolymer, and the dispersant is added to promote the dispersion effect of PBSA and four antibacterial agents, which helps to disperse the antibacterial agent powder into the PBSA resin, ensures that each component is evenly distributed during the mixing process, avoids the formation of agglomeration, and thus improves the performance and stability of the antibacterial masterbatch. The addition of the antioxidant can be used to avoid the degradation of the material during high-temperature processing, extend the service life of the product and maintain its stable performance.
[0026] Furthermore, in the preparation process of the antibacterial masterbatch, the equipment used for mixing is a high-speed mixer, and the rotation speed is set to 300-800rpm.
[0027] Furthermore, in the preparation process of the antibacterial masterbatch, the aspect ratio of the twin-screw extruder is 48:1, the PBSA resin enters the twin-screw extruder through the main feeding system connected to the first zone of the twin-screw extruder, and the antibacterial adjuvant mixture enters the twin-screw extruder through the side feeding system connected to the fourth zone of the twin-screw extruder. The PBSA resin and the antibacterial adjuvant mixture enter the twin-screw extruder from different feeding systems respectively, which can ensure better dispersion of the materials.
[0028] Furthermore, in the preparation process of the antibacterial masterbatch, the temperature of each zone of the twin-screw extruder is set to 90-110°C in zone 1, 100-120°C in zone 2, 130-150°C in zone 3, 140-160°C in zone 4, 140-160°C in zone 5, 160-170°C in zone 6, 160-170°C in zone 7, 160-170°C in zone 8, 160-170°C in zone 9, 160-170°C in zone 10, 160-170°C in zone 11, and 160-170°C in zone 12, the screw speed is 200-400r / min, and the feeding rate is 10-50Hz.
[0029] Furthermore, the chain extender includes any one or both of benzoyl peroxide and hexamethylene diisocyanate.
[0030] Furthermore, the lubricant is a combination of at least three of octadecanoic acid, polydimethylsiloxane, polymethylphenylsiloxane, erucamide, oleamide and stearamide.
[0031] Furthermore, the anti-hydrolysis agent includes any one or two of isophorone diisocyanate and polycarbodiimide.
[0032] Furthermore, the nucleating agent includes one of a dibenzylidene sorbitol derivative and N,N′,N″-tricyclohexyl-1,3,5-benzenetricarboxamide.
[0033] Furthermore, the antioxidant is a mixture of N-N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide) and pentaerythritol tetrakis(3-laurylthiopropionate) in a mass ratio of 2:(1-3).
[0034] The present invention also provides a method for preparing the aforementioned PBSA / PLA non-woven fabric, the preparation method comprising the following steps:
[0035] Step S1: Preparation of premix:
[0036] PBSA, PLA, antibacterial masterbatch, chain extender, lubricant, anti-hydrolysis agent, nucleating agent, and antioxidant are weighed according to weight, and mixed in a high-speed mixer for 3-5 minutes to obtain a premix;
[0037] Step S2: preparing modified non-woven fabric:
[0038] The premix prepared in step S1 is melt-extruded through a twin-screw extruder, granulated, and dried to obtain a non-woven fabric modified material;
[0039] Step S3: Preparation of non-woven fabric:
[0040] The modified non-woven fabric prepared in step S2 is used to prepare PBSA / PLA non-woven fabric in a spunbond device.
[0041] Furthermore, in step S1, the temperature of the high-speed mixer is set to 45-70°C, and the rotation speed is set to 300-800rpm.
[0042] Further, in step S2, the aspect ratio of the twin screw extruder is 48:1, and the premix enters the twin screw extruder through a main feeding system connected to a zone of the twin screw extruder. The temperatures of each zone of the twin screw extruder are set to 90-120°C for zone one, 100-130°C for zone two, 140-160°C for zone three, 150-170°C for zone four, 150-180°C for zone five, 160-190°C for zone six, 170-200°C for zone seven, 170-200°C for zone eight, 170-200°C for zone nine, 180-200°C for zone ten, 180-200°C for zone eleven, and 180-200°C for zone twelve, the screw speed is 200-600r / min, and the feeding rate is 20-50Hz.
[0043] Furthermore, the step S3 includes subjecting the modified non-woven fabric to melting, spinning, cooling and blowing, airflow stretching, and filament laying. The spinning is to extrude the molten modified non-woven fabric from the small holes of the spinneret by a feed metering pump to form a melt stream; the cooling and blowing is to rapidly cool and solidify the extruded melt stream under the action of cooling and blowing to form nascent fibers; the airflow stretching is to stretch the nascent fibers using a high-speed airflow to improve the strength and fineness of the fibers; and the filament laying is to lay the stretched fibers into a net on a laying machine.
[0044] Further, in step S3, the parameters of the spunbond equipment are set as follows: the temperatures of the melting zones are set to 180-210°C for zone 1, 180-210°C for zone 2, 190-220°C for zone 3, 190-220°C for zone 4, 190-220°C for zone 5, and 190-220°C for zone 6, the die head temperature is 190-220°C, the operating frequency of the feeding metering pump is 10-30Hz, the blowing frequency of the airflow stretching is 30-55Hz, and the setting frequency of the filament laying is 30-60Hz.
[0045] The present invention has the following beneficial technical effects:
[0046] (1) The present invention uses PBSA and PLA with a special melt index range, combining the advantages of both to solve their respective deficiencies in mechanical properties, softness and fluidity. PLA has good mechanical properties, such as elongation, breaking strength and elasticity, however, the surface of PLA is relatively rough and not soft; although PBSA has good softness, its mechanical properties are poor. The invention can further optimize the mechanical properties and softness of the PBSA / PLA blend system by adjusting the blending ratio of PLA and PBSA.
[0047] (2) The present invention first obtains an antibacterial masterbatch by blending and melt-extruding PBSA and four antibacterial agents, and then adds the antibacterial masterbatch into the resin of PBSA and PLA, thereby improving the compatibility of the antibacterial masterbatch and the resin.
[0048] (3) The present invention can improve the compatibility between PBSA and PLA by adding a chain extender, thereby increasing the melt strength and making it less likely for the monofilament to break during the spinning and drawing process. In addition, in order to further improve the crystallization speed and cooling efficiency of the fiber, the present invention also adds a nucleating agent and a lubricant, which helps to accelerate the crystallization and cooling of the fiber after it is ejected from the spinneret, making it less likely for the monofilament to stick together during the high-speed drawing process.
[0049] (4) When the formulation system of the present invention is used for spunbonding to prepare nonwoven fabrics, the spunbonding stability is significantly improved due to its good compatibility and melt strength. At the same time, the blending and modification of PLA with PBSA, four antibacterial agents and other additives finally produces a nonwoven fabric that is not only soft to the touch, but also has excellent antibacterial properties. It is widely used in the medical and health fields, can effectively inhibit the growth of common bacteria, and significantly improves the production quality and application performance of nonwoven fabrics. Therefore, it has broad market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 This is a scanning electron microscope photograph of the nonwoven fabric prepared in Example 1.
[0051] Figure 2 This is a scanning electron microscope photograph of the nonwoven fabric prepared in Comparative Example 1. DETAILED DESCRIPTION
[0052] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.
[0053] Example 1
[0054] Provided is an antibacterial and degradable PBSA / PLA non-woven fabric, comprising the following components in parts by weight:
[0055] PBSA: 85.8 parts by weight;
[0056] PLA: 8 parts by weight;
[0057] Antibacterial masterbatch: 3 parts by weight;
[0058] Chain extender: 0.3 parts by weight:
[0059] Lubricant: 1.2 parts by weight;
[0060] Anti-hydrolysis agent: 0.8 parts by weight;
[0061] Nucleating agent: 0.5 parts by weight;
[0062] Antioxidant: 0.4 parts by weight;
[0063] Among them, the melt index of PBSA at 190°C and 2.16kg is 22g / 10min;
[0064] The melt index of PLA at 190°C and 2.16 kg is 16 g / 10 min.
[0065] The preparation method is as follows:
[0066] Step M: Preparation of antibacterial masterbatch:
[0067] First, a mixture of 1 part by weight of tea tree essential oil, 2 parts by weight of chitosan, 3 parts by weight of ammonium dihydrogen phosphate, 5 parts by weight of nano titanium dioxide, 0.5 parts by weight of ethylene-acrylic acid copolymer, 0.1 parts by weight of N-N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide) and 0.1 parts by weight of pentaerythritol tetrakis(3-laurylthiopropionate) was added into a high-speed mixer, and mixed at a temperature of 60° C. for 5 minutes, with the rotation speed of the high-speed mixer set to 300 rpm, to obtain an antibacterial adjuvant mixture;
[0068] Then, the obtained antibacterial auxiliary agent mixture is fed into a twin-screw extruder from a side feeding system, and 88.3 parts by weight of PBSA is fed into the twin-screw extruder from a main feeding system, and the antibacterial masterbatch is obtained after extrusion, granulation and drying by the twin-screw extruder; wherein, the temperature of each zone of the twin-screw extruder is respectively set to 90° C. for zone 1, 110° C. for zone 2, 130° C. for zone 3, 140° C. for zone 4, 150° C. for zone 5, 160° C. for zone 6, 160° C. for zone 7, 160° C. for zone 8, 170° C. for zone 9, 170° C. for zone 10, 170° C. for zone 11 and 170° C. for zone 12, the screw speed is 300 r / min, and the feeding speed is 20 Hz;
[0069] Step S1: Preparation of premix:
[0070] Weigh 85.8 parts by weight of PBSA, 8 parts by weight of PLA, 3 parts by weight of antibacterial masterbatch, 0.3 parts by weight of benzoyl peroxide (chain extender), 0.5 parts by weight of polydimethylsiloxane (slip agent), 0.4 parts by weight of polymethylphenylsiloxane (slip agent), 0.3 parts by weight of erucic acid amide (slip agent), 0.8 parts by weight of polycarbodiimide (anti-hydrolysis agent), 0.5 parts by weight of dibenzylidene sorbitol derivative (nucleating agent), 0.2 parts by weight of N-N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide) (antioxidant) and 0.2 parts by weight of pentaerythritol tetrakis(3-laurylthiopropionate) (antioxidant), add them into a high-speed mixer, the high-speed mixer rotates at 350 rpm, and mix at a temperature of 65°C for 5 minutes to obtain a premix;
[0071] Step S2: preparing modified non-woven fabric:
[0072] The premix is melt-extruded through a twin-screw extruder, granulated, and dried to obtain a non-woven fabric modified material;
[0073] Among them, the aspect ratio of the twin-screw extruder is 48:1, and the temperature of each zone of the twin-screw extruder is set to 100°C for zone 1, 130°C for zone 2, 150°C for zone 3, 160°C for zone 4, 160°C for zone 5, 170°C for zone 6, 180°C for zone 7, 190°C for zone 8, 190°C for zone 9, 200°C for zone 10, 200°C for zone 11, and 200°C for zone 12. The screw speed is 280r / min, and the feeding speed is 32Hz.
[0074] Step S3: Preparation of non-woven fabric:
[0075] The modified non-woven fabric prepared in step S2 is added into a spunbond device, and a non-woven fabric is obtained through melting, spinning, cooling and blowing, air flow drawing and filament laying;
[0076] Among them, in the spunbond equipment, the temperatures of each melting zone are set to 190°C for zone 1, 200°C for zone 2, 200°C for zone 3, 200°C for zone 4, 200°C for zone 5, and 200°C for zone 6, the die head temperature is 200°C, the operating frequency of the feeding metering pump is 17Hz, the blowing frequency of the air flow drawing is 50Hz, and the set frequency of the filament laying is 38Hz.
[0077] The nonwoven fabric prepared in Example 1 has an average fiber diameter of 17.7 μm, a softness of 16.5 / mN, a 180-day biodegradability of 95.3% under composting conditions, an antibacterial rate of Escherichia coli greater than 99.3%, and an antibacterial rate of Staphylococcus aureus greater than 99.1%.
[0078] from Figure 1 It can be seen from the scanning electron microscope photograph of the non-woven fabric that the fiber diameter of the non-woven fabric prepared in Example 1 is smaller, so it is softer.
[0079] Example 2
[0080] Provided is an antibacterial and degradable PBSA / PLA non-woven fabric, comprising the following components in parts by weight:
[0081] PBSA: 74 parts by weight;
[0082] PLA: 15 parts by weight;
[0083] Antibacterial masterbatch: 6 parts by weight;
[0084] Chain extender: 0.3 parts by weight:
[0085] Lubricant: 3 parts by weight;
[0086] Anti-hydrolysis agent: 0.8 parts by weight;
[0087] Nucleating agent: 0.5 parts by weight;
[0088] Antioxidant: 0.4 parts by weight;
[0089] Among them, the melt index of PBSA at 190°C and 2.16kg is 19g / 10min;
[0090] The melt index of PLA at 190°C and 2.16 kg is 23 g / 10 min.
[0091] The preparation method is as follows:
[0092] Step M: Preparation of antibacterial masterbatch:
[0093] First, a mixture of 1 part by weight of tea tree essential oil, 2 parts by weight of chitosan, 3 parts by weight of ammonium dihydrogen phosphate, 5 parts by weight of nano titanium dioxide, 0.5 parts by weight of ethylene-acrylic acid copolymer, 0.1 parts by weight of N-N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide) and 0.1 parts by weight of pentaerythritol tetrakis(3-laurylthiopropionate) was added into a high-speed mixer, and mixed at a temperature of 60° C. for 5 minutes, with the rotation speed of the high-speed mixer set to 300 rpm, to obtain an antibacterial adjuvant mixture;
[0094] Then, the obtained antibacterial auxiliary agent mixture is fed into a twin-screw extruder from a side feeding system, and 88.3 parts by weight of PBSA is fed into the twin-screw extruder from a main feeding system, and the antibacterial masterbatch is obtained after extrusion, granulation and drying by the twin-screw extruder; wherein, the temperature of each zone of the twin-screw extruder is respectively set to 90° C. for zone 1, 110° C. for zone 2, 130° C. for zone 3, 140° C. for zone 4, 150° C. for zone 5, 160° C. for zone 6, 160° C. for zone 7, 160° C. for zone 8, 170° C. for zone 9, 170° C. for zone 10, 170° C. for zone 11 and 170° C. for zone 12, the screw speed is 300 r / min, and the feeding speed is 20 Hz;
[0095] Step S1: Preparation of premix:
[0096] Weigh 74 parts by weight of PBSA, 15 parts by weight of PLA, 6 parts by weight of antibacterial masterbatch, 0.3 parts by weight of benzoyl peroxide (chain extender), 0.4 parts by weight of polydimethylsiloxane (slip agent), 1.2 parts by weight of polymethylphenylsiloxane (slip agent), 0.4 parts by weight of erucic acid amide (slip agent), 0.8 parts by weight of polycarbodiimide (anti-hydrolysis agent), 0.5 parts by weight of dibenzylidene sorbitol derivative (nucleating agent), 0.2 parts by weight of N-N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide) (antioxidant) and 0.2 parts by weight of pentaerythritol tetrakis(3-laurylthiopropionate) (antioxidant), add them into a high-speed mixer, the high-speed mixer rotates at 350 rpm, and mix at a temperature of 65°C for 5 minutes to obtain a premix;
[0097] Step S2: preparing modified non-woven fabric:
[0098] The premix is melt-extruded through a twin-screw extruder, granulated, and dried to obtain a modified material for non-woven fabrics;
[0099] Among them, the aspect ratio of the twin-screw extruder is 48:1, and the temperature of each zone of the twin-screw extruder is set to 100°C for zone 1, 130°C for zone 2, 150°C for zone 3, 160°C for zone 4, 160°C for zone 5, 170°C for zone 6, 180°C for zone 7, 190°C for zone 8, 190°C for zone 9, 200°C for zone 10, 200°C for zone 11, and 200°C for zone 12. The screw speed is 280r / min, and the feeding speed is 32Hz.
[0100] Step S3: Preparation of non-woven fabric:
[0101] The modified non-woven fabric prepared in step S2 is added into a spunbond device, and a non-woven fabric is obtained through melting, spinning, cooling and blowing, air flow drawing and filament laying;
[0102] Among them, in the spunbond equipment, the temperatures of each melting zone are set to 190°C for zone 1, 200°C for zone 2, 200°C for zone 3, 200°C for zone 4, 200°C for zone 5, and 200°C for zone 6, the die head temperature is 200°C, the operating frequency of the feeding metering pump is 17Hz, the blowing frequency of the air flow drawing is 50Hz, and the set frequency of the filament laying is 38Hz.
[0103] The nonwoven fabric prepared in Example 2 has an average fiber diameter of 18.5 μm, a softness of 14.6 / mN, a 180-day biodegradability rate under composting conditions of 95.5%, an antibacterial rate of Escherichia coli greater than 99.4%, and an antibacterial rate of Staphylococcus aureus greater than 99.5%.
[0104] Example 3
[0105] Provided is an antibacterial and degradable PBSA / PLA non-woven fabric, comprising the following components in parts by weight:
[0106] PBSA: 77.8 parts by weight;
[0107] PLA: 5 parts by weight;
[0108] Antibacterial masterbatch: 10 parts by weight;
[0109] Chain extender: 0.3 parts by weight:
[0110] Lubricant: 5 parts by weight;
[0111] Anti-hydrolysis agent: 1.0 parts by weight;
[0112] Nucleating agent: 0.5 parts by weight;
[0113] Antioxidant: 0.4 parts by weight;
[0114] Among them, the melt index of PBSA at 190°C and 2.16kg is 42g / 10min;
[0115] The melt index of PLA at 190°C and 2.16 kg is 18 g / 10 min.
[0116] The preparation method is as follows:
[0117] Step M: Preparation of antibacterial masterbatch:
[0118] First, a mixture of 1 part by weight of tea tree essential oil, 2 parts by weight of chitosan, 3 parts by weight of ammonium dihydrogen phosphate, 5 parts by weight of nano titanium dioxide, 0.5 parts by weight of ethylene-acrylic acid copolymer, 0.1 parts by weight of N-N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide) and 0.1 parts by weight of pentaerythritol tetrakis(3-laurylthiopropionate) was added into a high-speed mixer, and mixed at a temperature of 60° C. for 5 minutes, with the rotation speed of the high-speed mixer set to 300 rpm, to obtain an antibacterial adjuvant mixture;
[0119] Then, the obtained antibacterial auxiliary agent mixture is fed into a twin-screw extruder from a side feeding system, and 88.3 parts by weight of PBSA is fed into the twin-screw extruder from a main feeding system, and the antibacterial masterbatch is obtained after extrusion, granulation and drying by the twin-screw extruder; wherein, the temperature of each zone of the twin-screw extruder is respectively set to 90° C. for zone 1, 110° C. for zone 2, 130° C. for zone 3, 140° C. for zone 4, 150° C. for zone 5, 160° C. for zone 6, 160° C. for zone 7, 160° C. for zone 8, 170° C. for zone 9, 170° C. for zone 10, 170° C. for zone 11 and 170° C. for zone 12, the screw speed is 300 r / min, and the feeding speed is 20 Hz;
[0120] Step S1: Preparation of premix:
[0121] Weigh 77.8 parts by weight of PBSA, 5 parts by weight of PLA, 10 parts by weight of antibacterial masterbatch, 0.3 parts by weight of benzoyl peroxide (chain extender), 2.5 parts by weight of polydimethylsiloxane (slip agent), 2 parts by weight of polymethylphenylsiloxane (slip agent), 0.5 parts by weight of erucic acid amide (slip agent), 1.0 parts by weight of polycarbodiimide (anti-hydrolysis agent), 0.5 parts by weight of dibenzylidene sorbitol derivative (nucleating agent), 0.2 parts by weight of N-N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide) (antioxidant) and 0.2 parts by weight of pentaerythritol tetrakis(3-laurylthiopropionate) (antioxidant), add them into a high-speed mixer, the high-speed mixer rotates at 350 rpm, and mix at a temperature of 65°C for 5 minutes to obtain a premix;
[0122] Step S2: preparing modified non-woven fabric:
[0123] The premix is melt-extruded through a twin-screw extruder, granulated, and dried to obtain a modified material for non-woven fabrics;
[0124] Among them, the aspect ratio of the twin-screw extruder is 48:1, and the temperature of each zone of the twin-screw extruder is set to 100°C for zone 1, 130°C for zone 2, 150°C for zone 3, 160°C for zone 4, 160°C for zone 5, 170°C for zone 6, 180°C for zone 7, 190°C for zone 8, 190°C for zone 9, 200°C for zone 10, 200°C for zone 11, and 200°C for zone 12. The screw speed is 280r / min, and the feeding speed is 32Hz.
[0125] Step S3: Preparation of non-woven fabric:
[0126] The modified non-woven fabric prepared in step S2 is added into a spunbond device, and a non-woven fabric is obtained through melting, spinning, cooling and blowing, air flow drawing and filament laying;
[0127] Among them, in the spunbond equipment, the temperatures of each melting zone are set to 190°C for zone 1, 200°C for zone 2, 200°C for zone 3, 200°C for zone 4, 200°C for zone 5, and 200°C for zone 6, the die head temperature is 200°C, the operating frequency of the feeding metering pump is 17Hz, the blowing frequency of the air flow drawing is 50Hz, and the set frequency of the filament laying is 38Hz.
[0128] The nonwoven fabric prepared in Example 3 has an average fiber diameter of 16.4 μm, a softness of 15.3 / mN, a 180-day biodegradability of 96.4% under composting conditions, an antibacterial rate of Escherichia coli greater than 99.9%, and an antibacterial rate of Staphylococcus aureus greater than 99.9%.
[0129] Comparative Example 1
[0130] Provided is an antibacterial and degradable PLA non-woven fabric, comprising the following components in parts by weight:
[0131] PLA: 87.3 parts by weight;
[0132] Antibacterial masterbatch: 10 parts by weight;
[0133] Chain extender: 0.3 parts by weight:
[0134] Lubricant: 0.5 parts by weight;
[0135] Anti-hydrolysis agent: 1.0 parts by weight;
[0136] Nucleating agent: 0.5 parts by weight;
[0137] Antioxidant: 0.4 parts by weight;
[0138] The melt index of PLA at 190°C and 2.16 kg is 22 g / 10 min.
[0139] The preparation method is as follows:
[0140] Step M: preparing antibacterial masterbatch;
[0141] First, a mixture of 1 part by weight of tea tree essential oil, 2 parts by weight of chitosan, 3 parts by weight of ammonium dihydrogen phosphate, 5 parts by weight of nano titanium dioxide, 0.5 parts by weight of ethylene-acrylic acid copolymer, 0.1 parts by weight of N-N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide) and 0.1 parts by weight of pentaerythritol tetrakis(3-laurylthiopropionate) was added into a high-speed mixer, and mixed at a temperature of 60° C. for 5 minutes, with the rotation speed of the high-speed mixer set to 300 rpm, to obtain an antibacterial adjuvant mixture;
[0142] Then, the obtained antibacterial auxiliary agent mixture is fed into a twin-screw extruder from a side feeding system, and 88.3 parts by weight of PBSA is fed into the twin-screw extruder from a main feeding system, and the antibacterial masterbatch is obtained after extrusion, granulation and drying by the twin-screw extruder; wherein, the temperature of each zone of the twin-screw extruder is respectively set to 90° C. for zone 1, 110° C. for zone 2, 130° C. for zone 3, 140° C. for zone 4, 150° C. for zone 5, 160° C. for zone 6, 160° C. for zone 7, 160° C. for zone 8, 170° C. for zone 9, 170° C. for zone 10, 170° C. for zone 11 and 170° C. for zone 12, the screw speed is 300 r / min, and the feeding speed is 20 Hz;
[0143] Step S1: Preparation of premix:
[0144] Weigh 87.3 parts by weight of PLA, 3 parts by weight of antibacterial masterbatch, 0.3 parts by weight of benzoyl peroxide (chain extender), 0.5 parts by weight of polydimethylsiloxane (slip agent), 0.4 parts by weight of polymethylphenylsiloxane (slip agent), 0.3 parts by weight of erucic acid amide (slip agent), 0.8 parts by weight of polycarbodiimide (anti-hydrolysis agent), 0.5 parts by weight of dibenzylidene sorbitol derivative (nucleating agent), 0.2 parts by weight of N-N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide) (antioxidant) and 0.2 parts by weight of pentaerythritol tetrakis(3-laurylthiopropionate) (antioxidant), add them into a high-speed mixer, the high-speed mixer rotates at 350 rpm, and mix at a temperature of 65°C for 5 minutes to obtain a premix;
[0145] Step S2: preparing a non-woven fabric modified material;
[0146] The premix is melt-extruded through a twin-screw extruder, granulated, and dried to obtain a non-woven fabric modified material;
[0147] Among them, the aspect ratio of the twin-screw extruder is 48:1, and the temperature of each zone of the twin-screw extruder is set to 100°C for zone 1, 130°C for zone 2, 150°C for zone 3, 160°C for zone 4, 160°C for zone 5, 170°C for zone 6, 180°C for zone 7, 190°C for zone 8, 190°C for zone 9, 200°C for zone 10, 200°C for zone 11, and 200°C for zone 12. The screw speed is 280r / min, and the feeding speed is 32Hz.
[0148] Step S3: preparing non-woven fabric;
[0149] The modified non-woven fabric prepared in step S2 is added into a spunbond device, and a non-woven fabric is obtained through melting, spinning, cooling and blowing, air flow drawing and filament laying;
[0150] Among them, in the spunbond equipment, the temperatures of each melting zone are set to 190°C for zone 1, 200°C for zone 2, 200°C for zone 3, 200°C for zone 4, 200°C for zone 5, and 200°C for zone 6, the die head temperature is 200°C, the operating frequency of the feeding metering pump is 17Hz, the blowing frequency of the air flow drawing is 50Hz, and the set frequency of the filament laying is 38Hz.
[0151] The nonwoven fabric prepared in Comparative Example 1 has an average fiber diameter of 24.3 μm, a softness of 5.3 / mN, a 180-day biodegradability of 96.4% under composting conditions, an antibacterial rate of Escherichia coli greater than 99.9%, and an antibacterial rate of Staphylococcus aureus greater than 99.9%.
[0152] from Figure 2 It can be seen from the scanning electron microscope photograph of the non-woven fabric that the non-woven fabric prepared in Comparative Example 1 has a larger fiber diameter and therefore has a lower softness.
[0153] Comparative Example 2
[0154] Provided is an antibacterial and degradable PBSA / PLA nonwoven fabric, the preparation method of which is as follows:
[0155] Step 1: Preparation of non-woven modified material:
[0156] Weigh 74 parts by weight of PBSA, 15 parts by weight of PLA, 0.06 parts by weight of tea tree essential oil, 0.02 parts by weight of chitosan, 0.03 parts by weight of ammonium dihydrogen phosphate, 0.05 parts by weight of nano titanium dioxide, 0.005 parts by weight of ethylene-acrylic acid copolymer, 0.3 parts by weight of benzoyl peroxide (chain extender), 0.4 parts by weight of polydimethylsiloxane (lubricant), 1.2 parts by weight of polymethylphenylsiloxane (lubricant), 0.4 parts by weight of erucic acid amide (lubricant), 0.8 parts by weight of polycarbonate Diimine (anti-hydrolysis agent), 0.5 parts by weight of dibenzylidene sorbitol derivative (nucleating agent), 0.2 parts by weight of N-N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide) (antioxidant) and 0.2 parts by weight of pentaerythritol tetrakis(3-laurylthiopropionate) (antioxidant) are added into a high-speed mixer, the high-speed mixer rotates at 350 rpm, mixed at a temperature of 65°C for 5 minutes, mixed evenly, added into a twin-screw extruder for extrusion, granulated and dried to obtain a modified material for non-woven fabrics,
[0157] Among them, the aspect ratio of the twin-screw extruder is 48:1, and the temperature of each zone of the twin-screw extruder is set to 100°C for zone 1, 130°C for zone 2, 150°C for zone 3, 160°C for zone 4, 160°C for zone 5, 170°C for zone 6, 180°C for zone 7, 190°C for zone 8, 190°C for zone 9, 200°C for zone 10, 200°C for zone 11, and 200°C for zone 12. The screw speed is 280r / min, and the feeding speed is 32Hz.
[0158] Step 2: preparing non-woven fabric;
[0159] The modified non-woven fabric prepared in step 1 is added into a spunbond device, and a non-woven fabric is obtained by melting, spinning, cooling and blowing, air flow drawing and filament laying;
[0160] Among them, in the spunbond equipment, the temperatures of each melting zone are set to 190°C for zone 1, 200°C for zone 2, 200°C for zone 3, 200°C for zone 4, 200°C for zone 5, and 200°C for zone 6, the die head temperature is 200°C, the operating frequency of the feeding metering pump is 17Hz, the blowing frequency of the air flow drawing is 50Hz, and the set frequency of the filament laying is 38Hz.
[0161] The nonwoven fabric prepared in Comparative Example 2 has a fiber diameter of 18.3 μm, a softness of 14.5 / mN, a 180-day biodegradability of 95.0% under composting conditions, an antibacterial rate of Escherichia coli greater than 96.6%, and an antibacterial rate of Staphylococcus aureus greater than 97.1%.
[0162] Comparative Example 3
[0163] Provided is an antibacterial and degradable PBSA / PLA non-woven fabric, comprising the following components in parts by weight:
[0164] PBSA: 82.3 parts by weight;
[0165] PLA: 5 parts by weight;
[0166] Antibacterial masterbatch: 10 parts by weight;
[0167] Chain extender: 0.3 parts by weight:
[0168] Lubricant: 0.5 parts by weight;
[0169] Anti-hydrolysis agent: 1.0 parts by weight;
[0170] Nucleating agent: 0.5 parts by weight;
[0171] Antioxidant: 0.4 parts by weight;
[0172] The melt index of PBSA at 190°C and 2.16 kg is 42 g / 10 min;
[0173] The melt index of PLA at 190°C and 2.16 kg is 18 g / 10 min.
[0174] The preparation method is as follows:
[0175] Step M: Preparation of antibacterial masterbatch:
[0176] First, 1 part by weight of tea tree essential oil, 2 parts by weight of chitosan, 3 parts by weight of ammonium dihydrogen phosphate, 5 parts by weight of nano titanium dioxide, 0.5 parts by weight of ethylene-acrylic acid copolymer and 0.2 parts by weight of antioxidant were added into a high-speed mixer, and mixed at a temperature of 60° C. for 5 minutes, with the rotation speed of the high-speed mixer set to 300 rpm, to obtain an antibacterial adjuvant mixture;
[0177] Then, the obtained antibacterial auxiliary agent mixture is fed into a twin-screw extruder from a side feeding system, and 88.3 parts by weight of PBSA is fed into the twin-screw extruder from a main feeding system, and the antibacterial masterbatch is obtained after extrusion, granulation and drying by the twin-screw extruder; wherein, the temperature of each zone of the twin-screw extruder is respectively set to 90° C. for zone 1, 110° C. for zone 2, 130° C. for zone 3, 140° C. for zone 4, 150° C. for zone 5, 160° C. for zone 6, 160° C. for zone 7, 160° C. for zone 8, 170° C. for zone 9, 170° C. for zone 10, 170° C. for zone 11 and 170° C. for zone 12, the screw speed is 300 r / min, and the feeding speed is 20 Hz;
[0178] Step S1: Preparation of premix:
[0179] Weigh 82.3 parts by weight of PBSA, 5 parts by weight of PLA, 10 parts by weight of antibacterial masterbatch, 0.3 parts by weight of benzoyl peroxide (chain extender), 0.5 parts by weight of erucic acid amide (slip agent), 1.0 parts by weight of polycarbodiimide (anti-hydrolysis agent), 0.5 parts by weight of dibenzylidene sorbitol derivative (nucleating agent), 0.2 parts by weight of N-N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide) (antioxidant) and 0.2 parts by weight of pentaerythritol tetrakis(3-laurylthiopropionate) (antioxidant), add them into a high-speed mixer, the high-speed mixer rotates at 350 rpm, and mix at a temperature of 65°C for 5 minutes to obtain a premix;
[0180] Step S2: preparing modified non-woven fabric:
[0181] The premix is melt-extruded through a twin-screw extruder, and the modified material for non-woven fabric is obtained after granulation and drying; wherein the aspect ratio of the twin-screw extruder is 48:1, the temperature of each zone of the twin-screw extruder is set to 100°C for zone 1, 130°C for zone 2, 150°C for zone 3, 160°C for zone 4, 160°C for zone 5, 170°C for zone 6, 180°C for zone 7, 190°C for zone 8, 190°C for zone 9, 200°C for zone 10, 200°C for zone 11, and 200°C for zone 12, the screw speed is 280r / min, and the feeding speed is 32Hz;
[0182] Step S3: Preparation of non-woven fabric:
[0183] The modified non-woven fabric prepared in step S2 is added into a spunbond device, and a non-woven fabric is obtained through melting, spinning, cooling and blowing, air flow drawing and filament laying;
[0184] Among them, in the spunbond equipment, the temperatures of each melting zone are set to 190°C for zone 1, 200°C for zone 2, 200°C for zone 3, 200°C for zone 4, 200°C for zone 5, and 200°C for zone 6, the die head temperature is 200°C, the operating frequency of the feeding metering pump is 17Hz, the blowing frequency of the air flow drawing is 50Hz, and the set frequency of the filament laying is 38Hz.
[0185] The nonwoven fabric prepared in Comparative Example 3 has an average fiber diameter of 16.4 μm, a softness of 9.3 / mN, a 180-day biodegradability of 96.4% under composting conditions, an antibacterial rate of Escherichia coli greater than 99.9%, and an antibacterial rate of Staphylococcus aureus greater than 99.9%.
[0186] The experimental data after the performance test of the nonwoven fabrics prepared in Examples 1-3 and Comparative Examples 1-3 are statistically shown in the following Table 2.
[0187] Table 1 Performance test of nonwoven fabrics prepared in Examples 1-3 and Comparative Examples 1-3
[0188]
[0189] From the results in Table 1, it can be seen that compared with Example 1, Comparative Example 1 uses PLA alone for spinning, and the prepared non-woven fabric has a coarse fiber diameter and low softness; Compared with Example 2, Comparative Example 2 extrudes the antibacterial additive, resin and other additives at one time to prepare the non-woven fabric. Due to the poor compatibility between the antibacterial agent and the resin, the antibacterial performance is not significantly improved; Compared with Example 3, Comparative Example 3 only adds a single component of a low content of a lubricant, and the prepared non-woven fabric has a low softness.
[0190] The above description is only a preferred embodiment of the present invention and does not constitute any other form of limitation to the present invention. Any modification or equivalent change made based on the technical essence of the present invention still falls within the scope of protection required by the present invention.
Claims
1. An antibacterial and degradable PBSA / PLA nonwoven fabric, characterized in that: By weight, it includes the following components: PBSA: 9-90 parts by weight; PLA: 5-20 parts by weight; Antibacterial masterbatch: 0.5-10 parts by weight; Chain extender: 0.1-1 parts by weight: Lubricant: 1-8 parts by weight; Anti-hydrolysis agent: 0.1-2 parts by weight; Nucleating agent: 0.1-1 parts by weight; Antioxidant: 0.2-1.0 parts by weight; The fiber diameter of the PBSA / PLA nonwoven fabric is 12-18 μm.
2. The PBSA / PLA nonwoven fabric according to claim 1, characterized in that: The melt index of the PBSA at 190° C. and 2.16 kg is 10-50 g / 10 min.
3. The PBSA / PLA nonwoven fabric according to claim 1 or 2, characterized in that: The melt index of the PLA at 190° C. and 2.16 kg is 15-50 g / 10 min.
4. The PBSA / PLA nonwoven fabric according to claim 3, characterized in that: The antibacterial masterbatch comprises the following components: 40-90 parts by weight of PBSA, 1-3 parts by weight of tea tree essential oil, 2-5 parts by weight of chitosan, 3-8 parts by weight of ammonium dihydrogen phosphate, 5-10 parts by weight of nano titanium dioxide, 0.5-2 parts by weight of dispersant and 0.2-0.5 parts by weight of antioxidant.
5. The PBSA / PLA nonwoven fabric according to claim 4, characterized in that: The preparation method of the antibacterial masterbatch is as follows: first, tea tree essential oil, chitosan, ammonium dihydrogen phosphate, nano titanium dioxide, dispersant and antioxidant are weighed according to respective weight portions and added into a high-speed mixer, and mixed at a temperature of 50-70° C. for 5-10 minutes to obtain an antibacterial auxiliary agent mixture; then, the obtained antibacterial auxiliary agent mixture is evenly mixed with PBSA, and extruded and granulated by a twin-screw extruder to obtain the antibacterial masterbatch.
6. The PBSA / PLA nonwoven fabric according to claim 1, characterized in that: The chain extender includes any one or both of benzoyl peroxide and hexamethylene diisocyanate.
7. The PBSA / PLA nonwoven fabric according to claim 1, characterized in that: The lubricant is a combination of at least three of octadecanoic acid, polydimethylsiloxane, polymethylphenylsiloxane, erucamide, oleamide and stearamide.
8. A method for preparing the PBSA / PLA nonwoven fabric according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: Step S1: Preparation of premix: PBSA, PLA, antibacterial masterbatch, chain extender, lubricant, anti-hydrolysis agent, nucleating agent, and antioxidant are weighed according to weight, and mixed in a high-speed mixer for 3-5 minutes to obtain a premix; Step S2: preparing modified non-woven fabric: The premix prepared in step S1 is melt-extruded through a twin-screw extruder, granulated, and dried to obtain a non-woven fabric modified material; Step S3: Preparation of non-woven fabric: The modified nonwoven fabric prepared in step S2 is used to prepare PBSA / PLA nonwoven fabric in a spunbond device.
9. The preparation method according to claim 8, characterized in that: In step S2, the aspect ratio of the twin screw extruder is 48:1, and the premix enters the twin screw extruder through a main feeding system connected to a zone of the twin screw extruder. The temperatures of each zone of the twin screw extruder are set to 90-120°C for zone one, 100-130°C for zone two, 140-160°C for zone three, 150-170°C for zone four, 150-180°C for zone five, 160-190°C for zone six, 170-200°C for zone seven, 170-200°C for zone eight, 170-200°C for zone nine, 180-200°C for zone ten, 180-200°C for zone eleven, and 180-200°C for zone twelve, the screw speed is 200-600r / min, and the feeding rate is 20-50Hz.
10. The preparation method according to claim 9, characterized in that: In step S3, the parameters of the spunbond equipment are set as follows: the temperatures of the melting zones are set to 180-210°C for zone 1, 180-210°C for zone 2, 190-220°C for zone 3, 190-220°C for zone 4, 190-220°C for zone 5, and 190-220°C for zone 6, the die head temperature is 190-220°C, the operating frequency of the feeding metering pump is 10-30Hz, the blowing frequency of the air flow stretching is 30-55Hz, and the setting frequency of the filament laying is 30-60Hz.
Citation Information
Patent Citations
Fully-degradable polylactic acid fiber melt-blowing nonwoven fabric and preparation method thereof
CN101824708B
A kind of non-woven fabric and its production process and application
CN106048894B
Preparation method of antibacterial PLA nonwoven cloth
CN108823977A
Preparation process of PHBV and PLA biodegradable antibacterial and deodorizing spun-bonded non-woven fabric
CN113584725A
Antistatic and antibacterial ABS color master batch
CN103289298A